Preparation method and application of high-energy-storage polyetherimide-polymethyl methacrylate organic composite material
Preparation of high-energy storage polyetherimide-polymethyl methacrylate organic composite materials through solution blending method, solving the problem of low energy storage density of traditional polymer dielectric capacitors, and achieving higher energy storage density and breakdown Strength, suitable for advanced electrical and electronic equipment.
Patent Information
- Application Number
- CN202411166093.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polymer dielectric capacitors use polyetherimide as the main material lead to lower energy storage density, limiting their miniaturization applications in actual engineering and equipment.
The solution blending method is used to prepare high-energy storage polyetherimide-polymethyl methacrylate organic composite material. By dissolving polymethyl methacrylate particles in N,N-dimethylacetamide solution, and with 4,4'-diamined diphenyl ether and 4,4'-(4,4'-isopropyldiphenoxy) diphthalic anhydride are mixed, and cured by mechanical stirring and gradient heating to form a complete high energy storage Organic composite film.
It improves the insulation and dielectric properties of polyetherimide, enhances energy storage performance, and significantly improves breakdown strength and energy storage density. It is suitable for electrical, electronic and new energy vehicles and other fields.
Smart Images

Figure CN119039614A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyetherimide-based composite film preparation, and in particular to a preparation method and application of a high-energy storage polyetherimide-polymethyl methacrylate organic composite material. Background Art
[0002] As a component for storing energy, capacitors play an important role in tuning, bypassing, coupling and filtering in circuits. Compared with other electrochemical energy storage systems, dielectric capacitors have faster charging and discharging speeds, higher power density and good self-healing properties. They have great application potential in high pulse power technology, new energy vehicles, inverters, power grids and other electronic equipment, as well as power systems and medical systems. With the development and progress of technology, the demand for small, lightweight and highly reliable capacitors has gradually expanded in the fields of hybrid electric vehicles and renewable energy grid converters. The realization of high energy storage density dielectric materials is not only conducive to the effective use and storage of electric energy, but also conducive to the miniaturization and lightweight development of modern electrical and electronic devices, and has great practical application value. Polyetherimide (PEI) is a thermoplastic polyimide (PI) containing ether bonds in the main chain. It is widely used in aerospace and electronic instrumentation industries due to its advantages of high temperature resistance, low dielectric loss and good flexibility. However, the discharge energy density of polyetherimide as a polymer dielectric capacitor is relatively low, which limits its miniaturized application in practical engineering and equipment. Summary of the invention
[0003] The purpose of the present invention is to solve the problem of low energy storage density caused by using polyetherimide as the main material of traditional polymer dielectric capacitors, and to provide a preparation method and application of a high energy storage polyetherimide-polymethyl methacrylate organic composite material.
[0004] A method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material is carried out according to the following steps:
[0005] Step S1: preparing a polymethyl methacrylate mixed solution a;
[0006] Adding polymethyl methacrylate particles into N,N-dimethylacetamide solution, stirring at 50-55° C. until the polymethyl methacrylate particles are completely dissolved, and naturally cooling to room temperature to obtain a polymethyl methacrylate mixed solution a;
[0007] Step S2: preparing a polyetherimide-polymethyl methacrylate organic composite material by a solution blending method;
[0008] 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonic dispersion is performed to obtain a mixed solution b; the polymethyl methacrylate mixed solution a obtained in step S1 is mixed with the mixed solution b to obtain a mixed solution c; 4,4'-(4,4'-isopropyldiphenyloxy) diphthalic anhydride is added to the mixed solution c, and mechanical stirring is performed for 3-5 hours to obtain a mixed solution d; the mixed solution d is evacuated, and then evenly coated on one surface of a pretreated substrate, and after curing, the substrate is gradually heated to 250°C and kept at 250°C for 1-2 hours, and naturally cooled to room temperature after the end of the heat preservation, and finally the film on the substrate is peeled off to obtain a high-energy storage polyetherimide-polymethyl methacrylate organic composite material; the mass fraction of the polymethyl methacrylate particles in the high-energy storage polyetherimide-polymethyl methacrylate organic composite material is 10%, 20%, 30%, 40% or 50%.
[0009] An application of a high-energy storage polyetherimide-polymethyl methacrylate organic composite material, and an application of the high-energy storage polyetherimide-polymethyl methacrylate organic composite material in a dielectric capacitor.
[0010] Beneficial effects of the present invention:
[0011] (1) The preparation method of the high energy storage polyetherimide-polymethyl methacrylate organic composite material of the present invention comprises the following steps: firstly, polymethyl methacrylate is added to N,N-dimethylacetamide solution, and the mixture is stirred at a temperature of 50°C and a rotation speed of 200 r / min; then, polyetherimide is used as a matrix, and the polymethyl methacrylate mixed solution is added thereto, and the mixture is prepared by a solution blending method. Polyetherimide and polymethyl methacrylate have good compatibility. The introduction of polymethyl methacrylate into the polyetherimide matrix not only does not cause phase separation, but also improves the amorphous phase space of polyetherimide, optimizes the polymer chain structure to reduce the internal defects of the polymer, and increases the breakdown strength. At the same time, polymethyl methacrylate can improve the interchain interaction and spatial structure of polyetherimide, and the obtained all-organic composite film reduces the interchain distance of the polymer, effectively hinders the input of charge carriers and alleviates the electric field distortion, thereby improving the insulation and dielectric properties of polyetherimide, and thus improving the energy storage performance of the composite material. In addition, the introduction of polymethyl methacrylate, which has its own unique high breakdown performance, can also optimize the insulation properties of the original polyetherimide.
[0012] (2) The high energy storage polyetherimide-polymethyl methacrylate organic composite material prepared by the method of the present invention has improved breakdown and dielectric properties compared to pure polyetherimide, and has enhanced energy storage performance, and can be widely used in advanced fields such as electrical, electronic and new energy vehicles. The preparation process of the present invention is simple, economical and practical, effectively saves resources, is suitable for large-scale industrial production, and provides a good strategy for developing new application paths for polyetherimide insulating composite media.
[0013] The invention can obtain a preparation method and application of a high-energy storage polyetherimide-polymethyl methacrylate organic composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Represents the discharge energy storage density test results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate, ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%;
[0015] Figure 2 The test results of charge and discharge efficiency of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate are shown in Figure 2. ■ indicates pure polyetherimide film material, ● indicates pure polymethyl methacrylate film material, ▼ indicates that the mass fraction of polymethyl methacrylate is 10%, ▲ indicates that the mass fraction of polymethyl methacrylate is 20%, ◆ indicates that the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%;
[0016] Figure 3 The figure represents the DC breakdown Weibull distribution results of polyetherimide-polymethyl methacrylate organic composites with different mass fractions of polymethyl methacrylate. ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%;
[0017] Figure 4 The dielectric properties test results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate are shown in Figure 1. ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%;
[0018] Figure 5 The Fourier infrared spectrum characterization results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate, A represents pure polyetherimide film material, B represents pure polymethyl methacrylate film material, C represents 10% mass fraction of polymethyl methacrylate, D represents 20% mass fraction of polymethyl methacrylate, E represents 30% mass fraction of polymethyl methacrylate, F represents 40% mass fraction of polymethyl methacrylate, and G represents 50% mass fraction of polymethyl methacrylate. DETAILED DESCRIPTION
[0019] Specific implementation method 1: This implementation method is a method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material, which is carried out according to the following steps:
[0020] Step S1: preparing a polymethyl methacrylate mixed solution a;
[0021] Adding polymethyl methacrylate particles into N,N-dimethylacetamide solution, stirring at 50-55° C. until the polymethyl methacrylate particles are completely dissolved, and naturally cooling to room temperature to obtain a polymethyl methacrylate mixed solution a;
[0022] Step S2: preparing a polyetherimide-polymethyl methacrylate organic composite material by a solution blending method;
[0023] 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonic dispersion is performed to obtain a mixed solution b; the polymethyl methacrylate mixed solution a obtained in step S1 is mixed with the mixed solution b to obtain a mixed solution c; 4,4'-(4,4'-isopropyldiphenyloxy) diphthalic anhydride is added to the mixed solution c, and mechanical stirring is performed for 3-5 hours to obtain a mixed solution d; the mixed solution d is evacuated, and then evenly coated on one surface of a pretreated substrate, and after curing, the substrate is gradually heated to 250°C and kept at 250°C for 1-2 hours, and naturally cooled to room temperature after the end of the heat preservation, and finally the film on the substrate is peeled off to obtain a high-energy storage polyetherimide-polymethyl methacrylate organic composite material; the mass fraction of the polymethyl methacrylate particles in the high-energy storage polyetherimide-polymethyl methacrylate organic composite material is 10%, 20%, 30%, 40% or 50%.
[0024] Specific embodiment 2: The difference between this embodiment and specific embodiment 1 is that the ratio of the mass of the polymethyl methacrylate particles described in step S1 to the volume of the N,N-dimethylacetamide solution is (1.2-10.9) g: (19.5-20.5) mL.
[0025] The other steps are the same as those in the first specific implementation.
[0026] Specific implementation method three: This implementation method is different from specific implementation method one or two in that: in step S1, magnetic stirring is performed at a temperature of 50 to 55°C and a rotation speed of 100 to 300 r / min for 8 to 12 hours.
[0027] The other steps are the same as those in the first or second embodiment.
[0028] Specific embodiment 4: The difference between this embodiment and specific embodiments 1 to 3 is that the ratio of the mass of 4,4'-diaminodiphenyl ether, the volume of N,N-dimethylacetamide solution and the mass of 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic anhydride described in step S2 is (2.9~3.1) g: (19.5~20.5) mL: (7.7~7.9) g.
[0029] The other steps are the same as those in Specific Embodiments 1 to 3.
[0030] Specific embodiment five: The difference between this embodiment and specific embodiments one to four is that before adding 4,4'-(4,4'-isopropyldiphenoxy) diphthalic anhydride to the mixed solution c in step S2, it is first dried under vacuum conditions at 50-70°C for 8-10 hours; 4,4'-(4,4'-isopropyldiphenoxy) diphthalic anhydride is added to the mixed solution c in four times, with 1 / 2 of the total mass added in the first time, 1 / 4 of the total mass added in the second time, and 1 / 8 of the total mass added in the third and fourth times, and the interval time between each addition is 30 minutes.
[0031] The other steps are the same as those in Specific Embodiments 1 to 4.
[0032] Specific embodiment 6: The difference between this embodiment and specific embodiments 1 to 5 is that the ultrasonic dispersion time in step S2 is 15 to 30 minutes, and the curing temperature is 80 to 100°C.
[0033] The other steps are the same as those in Specific Embodiments 1 to 5.
[0034] Specific embodiment seven: The difference between this embodiment and specific embodiments one to six is that the pretreated substrate described in step S2 is processed according to the following steps: first, the substrate is cleaned with clean water for 1 to 3 times, then rinsed with deionized water for 3 to 5 times, and then cleaned with anhydrous ethanol for 3 to 5 times, and finally dried at 50°C to 60°C for 1 to 2 hours to obtain a pretreated substrate, which is a glass plate.
[0035] The other steps are the same as those in Specific Embodiments 1 to 6.
[0036] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that the step of gradient heating the substrate in step S2 is as follows: first place the substrate in a blast oven and heat it to 60-80°C, and keep it at 60-80°C for 10-12 hours, then heat it to 100°C, 150°C, 200°C and 250°C in sequence, and keep it at 100°C, 150°C, 200°C and 250°C for 1-2 hours respectively.
[0037] The other steps are the same as those in Specific Embodiments 1 to 7.
[0038] Specific embodiment 9: The difference between this embodiment and specific embodiments 1 to 8 is that in step S2, the cooled substrate is first placed in deionized water and soaked for 10 to 15 minutes, and then the film on the substrate is peeled off.
[0039] The other steps are the same as those in Specific Embodiments 1 to 8.
[0040] Specific implementation method ten: This implementation method provides an application of a high energy storage polyetherimide-polymethyl methacrylate organic composite material, and the application of the high energy storage polyetherimide-polymethyl methacrylate organic composite material in a dielectric capacitor.
[0041] The following examples are used to verify the beneficial effects of the present invention:
[0042] Example 1: A method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material, comprising the following steps:
[0043] Step S1: preparing a polymethyl methacrylate mixed solution a;
[0044] 1.2 g of polymethyl methacrylate particles were added to 20 mL of N,N-dimethylacetamide solution, and magnetically stirred at 200 r / min for 8 h at a temperature of 50° C. until the polymethyl methacrylate particles were completely dissolved, and then naturally cooled to room temperature to obtain a polymethyl methacrylate mixed solution a;
[0045] Step S2: preparing a polyetherimide-polymethyl methacrylate organic composite material by a solution blending method;
[0046] 3.0 g of 4,4'-diaminodiphenyl ether was added to 20 mL of N,N-dimethylacetamide solution, and ultrasonically dispersed for 15 min to obtain a mixed solution b; the polymethyl methacrylate mixed solution a obtained in step S1 was mixed with the mixed solution b to obtain a mixed solution c; 7.8 g of 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic anhydride was added to the mixed solution c, and mechanically stirred for 4 h until it became viscous to obtain a mixed solution d; before adding 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic anhydride to the mixed solution c, it was dried under vacuum conditions at 60° C. for 8 h; 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic anhydride was added to the mixed solution c in four times, 1 / 2 of the total mass was added in the first time, 1 / 4 of the total mass was added in the second time, and 1 / 8 of the total mass was added in the third and fourth times, and the interval between each addition was 30 min.
[0047] First, prepare a glass plate with a size of 200 mm × 16 mm × 4 mm, wash the glass plate with clean water for 3 times, then rinse with deionized water for 3 times, and then wash with anhydrous ethanol for 3 times, and finally dry it at 60°C for 1 h to obtain a pretreated glass plate.
[0048] The mixed solution d is evacuated and then evenly coated on one surface of a pretreated glass plate. After curing at 80°C, the glass plate is first placed in a blast oven and heated to 80°C, and kept at 80°C for 12 hours, then heated to 100°C, 150°C, 200°C and 250°C in sequence, and kept at 100°C, 150°C, 200°C and 250°C for 1 hour respectively. After the insulation is completed, it is naturally cooled to room temperature, the cooled glass plate is first immersed in deionized water for 15 minutes, and then the film on the glass plate is peeled off to obtain a high-energy storage polyetherimide-polymethyl methacrylate organic composite material, wherein the mass fraction of the polymethyl methacrylate particles in the high-energy storage polyetherimide-polymethyl methacrylate organic composite material is 10%.
[0049] Example 2: In this example, the mass fraction of polymethyl methacrylate particles in the high energy storage polyetherimide-polymethyl methacrylate organic composite material is 20%. Other experimental conditions are the same as those in Example 1.
[0050] Example 3: In this embodiment, the mass fraction of polymethyl methacrylate particles in the high energy storage polyetherimide-polymethyl methacrylate organic composite material is 30%. Other experimental conditions are the same as those in Example 1.
[0051] Example 4: In this embodiment, the mass fraction of polymethyl methacrylate particles in the high energy storage polyetherimide-polymethyl methacrylate organic composite material is 40%. Other experimental conditions are the same as those in Example 1.
[0052] Example 5: In this embodiment, the mass fraction of polymethyl methacrylate particles in the high energy storage polyetherimide-polymethyl methacrylate organic composite material is 50%. Other experimental conditions are the same as those in Example 1.
[0053] Figure 1 Represents the discharge energy storage density test results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate, ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%.
[0054] like Figure 1 As shown in Figure 2, with the continuous addition of polymethyl methacrylate with good energy storage performance, the energy storage density of polyetherimide-based composite materials also increases. At an applied field strength of 400 MV / m, the energy density of pure polyetherimide is 3.80 J / cm3 When the mass fraction of polymethyl methacrylate is 50%, the discharge energy storage density of polyetherimide-polymethyl methacrylate organic composite material is 5.75 J / cm 3 , compared with pure polyetherimide, the energy storage density is increased by 51.31%.
[0055] Figure 2 The test results of charge and discharge efficiency of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate are shown in Figure 2. ■ indicates pure polyetherimide film material, ● indicates pure polymethyl methacrylate film material, ▼ indicates that the mass fraction of polymethyl methacrylate is 10%, ▲ indicates that the mass fraction of polymethyl methacrylate is 20%, ◆ indicates that the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%.
[0056] like Figure 2 As shown, while improving the discharge energy storage density, the polyetherimide-polymethyl methacrylate organic composite material also retains the advantages of polyetherimide of low loss and high energy storage efficiency. As the mass fraction of polymethyl methacrylate continues to increase, the energy storage efficiency of the polyetherimide-polymethyl methacrylate organic composite material always remains above 90%.
[0057] Figure 3 The figure represents the DC breakdown Weibull distribution results of polyetherimide-polymethyl methacrylate organic composites with different mass fractions of polymethyl methacrylate. ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%.
[0058] like Figure 3 As shown in the figure, with the increase of the mass fraction of polymethyl methacrylate, the breakdown field strength first increases and then decreases. The breakdown field strength of pure polyimide is 554.00MV / m. When the mass fraction of polymethyl methacrylate is 30%, the breakdown field strength reaches the maximum value of 652.49kV / mm, which is 18.7% higher than that of pure polyimide. With the addition of polymethyl methacrylate, the internal free volume of polyetherimide-polymethyl methacrylate organic composite material decreases, the carrier transport is restricted, and the breakdown field strength is improved.
[0059] Figure 4 The dielectric properties test results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate are shown in Figure 1. ■ represents pure polyetherimide film material, ● represents pure polymethyl methacrylate film material, ▼ represents the mass fraction of polymethyl methacrylate is 10%, ▲ represents the mass fraction of polymethyl methacrylate is 20%, ◆ represents the mass fraction of polymethyl methacrylate is 30%, Indicates that the mass fraction of polymethyl methacrylate is 40%, It means that the mass fraction of polymethyl methacrylate is 50%.
[0060] like Figure 4 As shown in the figure, at a frequency of 100Hz, the dielectric constant of pure polyetherimide is 3.21, the dielectric constant of pure polymethyl methacrylate is 4.25, and the dielectric constant of polyetherimide-polymethyl methacrylate organic composite material increases with the increase of polymethyl methacrylate mass fraction. The dielectric loss maintains the low loss characteristic of polyetherimide, and although it increases slightly with the content of polymethyl methacrylate, it is basically kept below 0.01.
[0061] Figure 5 The Fourier infrared spectrum characterization results of polyetherimide-polymethyl methacrylate organic composite materials with different mass fractions of polymethyl methacrylate, A represents pure polyetherimide film material, B represents pure polymethyl methacrylate film material, C represents 10% mass fraction of polymethyl methacrylate, D represents 20% mass fraction of polymethyl methacrylate, E represents 30% mass fraction of polymethyl methacrylate, F represents 40% mass fraction of polymethyl methacrylate, and G represents 50% mass fraction of polymethyl methacrylate.
[0062] like Figure 5 As shown in the figure, the addition of polymethyl methacrylate makes the polyetherimide-polymethyl methacrylate organic composite material have a high -1 A strong hydroxyl (C=O) vibration absorption peak appears at 1272 cm -1 A COC asymmetric stretching vibration peak appeared, which not only represents the existence of polyetherimide-polymethyl methacrylate organic composite materials, indicating that polyetherimide and polymethyl methacrylate have good compatibility, but also the inherent molecular structure of polyetherimide is not destroyed, and the composite material still has the high breakdown field strength and low dielectric loss characteristics of polyetherimide.
Claims
1. A method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material, characterized in that The preparation method is carried out according to the following steps: Step S1: preparing a polymethyl methacrylate mixed solution a; Adding polymethyl methacrylate particles into N,N-dimethylacetamide solution, stirring at 50-55° C. until the polymethyl methacrylate particles are completely dissolved, and naturally cooling to room temperature to obtain a polymethyl methacrylate mixed solution a; Step S2: preparing a polyetherimide-polymethyl methacrylate organic composite material by a solution blending method; 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonic dispersion is performed to obtain a mixed solution b; the polymethyl methacrylate mixed solution a obtained in step S1 is mixed with the mixed solution b to obtain a mixed solution c; 4,4'-(4,4'-isopropyldiphenyloxy) diphthalic anhydride is added to the mixed solution c, and mechanical stirring is performed for 3-5 hours to obtain a mixed solution d; the mixed solution d is evacuated, and then evenly coated on one surface of a pretreated substrate, and after curing, the substrate is gradually heated to 250°C and kept at 250°C for 1-2 hours, and naturally cooled to room temperature after the end of the heat preservation, and finally the film on the substrate is peeled off to obtain a high-energy storage polyetherimide-polymethyl methacrylate organic composite material; the mass fraction of the polymethyl methacrylate particles in the high-energy storage polyetherimide-polymethyl methacrylate organic composite material is 10%, 20%, 30%, 40% or 50%.
2. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that The ratio of the mass of the polymethyl methacrylate particles described in step S1 to the volume of the N,N-dimethylacetamide solution is (1.2-10.9) g: (19.5-20.5) mL.
3. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that In step S1, the mixture is stirred magnetically at a speed of 100 to 300 r / min for 8 to 12 hours at a temperature of 50 to 55°C.
4. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that The ratio of the mass of 4,4'-diaminodiphenyl ether, the volume of N,N-dimethylacetamide solution and the mass of 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic anhydride described in step S2 is (2.9-3.1) g: (19.5-20.5) mL: (7.7-7.9) g.
5. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that In step S2, before adding 4,4'-(4,4'-isopropyldiphenoxy) diphthalic anhydride to the mixed solution c, it is first dried under vacuum conditions at 50-70° C. for 8-10 hours; 4,4'-(4,4'-isopropyldiphenoxy) diphthalic anhydride is added to the mixed solution c in four times, with 1 / 2 of the total mass added in the first time, 1 / 4 of the total mass added in the second time, and 1 / 8 of the total mass added in the third and fourth times, and the interval time between each addition is 30 minutes.
6. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that The ultrasonic dispersion time in step S2 is 15 to 30 minutes, and the curing temperature is 80 to 100°C.
7. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that The pretreated substrate described in step S2 is treated according to the following steps: first, the substrate is cleaned with clean water for 1 to 3 times, then rinsed with deionized water for 3 to 5 times, then cleaned with anhydrous ethanol for 3 to 5 times, and finally dried at 50°C to 60°C for 1 to 2 hours to obtain a pretreated substrate, wherein the substrate is a glass plate.
8. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that The steps of gradient heating the substrate in step S2 are as follows: first place the substrate in a blast oven and heat it to 60-80°C, and keep it at 60-80°C for 10-12 hours, then heat it to 100°C, 150°C, 200°C and 250°C in sequence, and keep it at 100°C, 150°C, 200°C and 250°C for 1-2 hours respectively.
9. The method for preparing a high energy storage polyetherimide-polymethyl methacrylate organic composite material according to claim 1, characterized in that In step S2, the cooled substrate is first placed in deionized water and soaked for 10 to 15 minutes, and then the thin film on the substrate is peeled off.
10. Use of a high energy storage polyetherimide-polymethyl methacrylate organic composite material prepared by the method according to any one of claims 1 to 9, characterized in that The application of the high energy storage polyetherimide-polymethyl methacrylate organic composite material in dielectric capacitors.
Citation Information
Patent Citations
Preparation method and application of polyacrylic acid rubber dielectric elastomer / polyimide insulating composite material
CN116218215A
High-dielectric polyimide film and preparation method thereof
CN116693903A
Preparation method and application of thermoplastic polyurethane elastomer-polyetherimide composite material
CN117467171A
Preparation method and application of polyacrylate rubber elastomer and polyimide-based multilayer structure composite film
CN118221989A
Polyimide film and preparation method thereof
CN118240247A
Cited By
Dielectric energy storage material and preparation method and application thereof
CN119661936A
Preparation method and application of polyetherimide-based three-phase blended dielectric film
CN122277960A