Additive, reaction liquid and method for alkali etching and polishing of silicon wafer and application of additive and reaction liquid
By using alkali etching and polishing technology of specific additives and alkali solutions in solar cell manufacturing, the silicon wafer tower base structure is rounded, and the problems of environmental pollution and efficiency improvement in traditional processes are solved, achieving efficient and environmentally friendly silicon wafer surface treatment , improves battery efficiency.
Patent Information
- Application Number
- CN202411523343.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-30
AI Technical Summary
In solar cell manufacturing, traditional hydrofluoric acid etching method is harmful to the environment. Although alkali etching and polishing technology is environmentally friendly, the contact resistance increases when improving the battery efficiency, resulting in a decrease in overall efficiency and cannot meet the needs of higher efficiency.
The additives composed of defoaming agent, modifier and accelerator are used to combine alkaline solution for alkali etching and polishing. By adjusting the additive composition and process conditions, the surface morphology of the silicon wafer is optimized, the tower base structure is rounded, the contact resistance is reduced, and the contact resistance is improved. Reflectivity and passivation properties.
The reflectivity of the silicon wafer reaches more than 51%, the tower base is rounded and the passivation performance is good, the contact resistance is reduced, and the conversion efficiency of solar cells is improved.
Smart Images

Figure CN119039991A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon wafer processing, and relates to an additive, a reaction liquid, a method and an application thereof for alkali etching and polishing of silicon wafers. Background Art
[0002] In the field of solar cell manufacturing, traditional production technology relies on a mixed acid etching method of nitric acid and hydrofluoric acid, aiming to achieve precise edge etching and effective removal of the PSG (phosphorus silicon glass) layer. The PSG layer is formed on the surface of the silicon wafer due to the introduction of oxygen during the diffusion process. At high temperature, POCl3 and O2 form P2O5. Some P atoms enter Si to replace some Si atoms on the lattice to form n-type semiconductors, and some remain in SiO2 to form PSG. The presence of the PSG layer makes the surface of the silicon wafer susceptible to moisture in the air, resulting in a decrease in current and power attenuation. In terms of enhancing cell efficiency, the etching and polishing process gradually deepens the degree of polishing, making the tip of the pyramid structure rounded and the surface smoothness significantly improved, thereby achieving a delicate balance between surface passivation and photoelectric contact characteristics, and promoting the improvement of cell conversion efficiency. However, given its potential impact on the environment, this process is not an ideal long-term solution.
[0003] As an alternative, alkaline etching and polishing technology has demonstrated its dual advantages in environmental protection and efficiency improvement. This technology not only abandons the environmentally unfriendly acid in the traditional process, realizes green production, but also significantly improves the conversion efficiency of solar cells. Specifically, the alkaline etching and polishing process can deeply optimize the surface morphology of the battery, making the top of the pyramid structure completely flat, the base presents a regular square outline, and the surface flatness reaches an unprecedented level. Although this highly flattened surface enhances the passivation effect and is conducive to reducing carrier recombination, it is also accompanied by a significant increase in contact resistance, which to a certain extent restricts the further improvement of the overall efficiency of the battery, resulting in a decrease in overall efficiency compared to traditional processes under certain optimized conditions. The higher the reflectivity, the flatter the tower base and the relatively uniform coating. Adding additives to alkaline etching and polishing is a suitable method. Patent CN118240485A uses compound additives such as polishing agents and amphoteric inorganic ion salts to obtain silicon wafers with a reflectivity of 48.59%, but it still cannot meet the pursuit of higher efficiency in this field. Therefore, when exploring more efficient and environmentally friendly solar cell production processes, how to optimize contact characteristics while maintaining high passivation performance has become a key technical challenge that needs to be solved urgently. Summary of the invention
[0004] The purpose of the present invention is to optimize the surface morphology of silicon wafers, round the base of the pyramid on the back surface of the silicon wafer after texturing, improve passivation and reduce contact resistance, thereby improving battery efficiency. To this end, the present invention provides an additive, reaction solution, method and application for alkaline etching and polishing of silicon wafers to solve this need in the field.
[0005] On the one hand, the present invention relates to an additive for alkaline etching and polishing of silicon wafers, wherein the additive is composed of: 0.3-1.0% of a defoamer, 0.1-1.0% of a modifier, 0.1-1.0% of an accelerator, and the balance of deionized water, in terms of mass percentage; The defoaming agent is selected from at least one of non-ionic surfactants; The modifier is selected from at least one of a phenyl-containing phosphorus oxide compound and a phenyl-containing ester compound; The promoter is selected from at least one of a strong base weak acid salt with oxidizing properties and a borate with oxidizing properties.
[0006] Furthermore, in the additive for alkaline etching and polishing of silicon wafers provided by the present invention, the nonionic surfactant is selected from polyoxyethylene polyoxypropylene pentaerythritol ether, polydimethylsiloxane, and polyoxypropylene glycerol ether; The phenyl-containing phosphorus oxide compound is triphenylphosphine oxide, and the phenyl-containing ester compound is ethyl o-toluate and monobenzyl phthalate; The strong base and weak acid salt with oxidizing property are sodium hypochlorite and sodium percarbonate, and the borate with oxidizing property is potassium perborate.
[0007] Furthermore, in the additive for silicon wafer alkaline etching and polishing provided by the present invention, the resistivity of the deionized water is greater than 18 MΩ.
[0008] On the other hand, the present invention relates to a reaction solution for alkali etching and polishing of silicon wafers, which is obtained by mixing an alkali solution with a concentration of 1-3wt% and the additive.
[0009] Furthermore, in the reaction solution for alkaline etching and polishing of silicon wafers provided by the present invention, the volume ratio of the alkaline solution in the reaction solution to the additive is 30-100:6.
[0010] Furthermore, in the reaction solution for alkaline etching and polishing of silicon wafers provided by the present invention, the alkali in the reaction solution is sodium hydroxide and / or potassium hydroxide.
[0011] On the other hand, the present invention relates to a method for preparing a silicon wafer containing a rounded tower base structure, comprising: surface treating the texturized silicon wafer to remove the PSG layer, and performing alkaline etching and polishing after cleaning; the alkaline etching and polishing comprises: placing the silicon wafer in the reaction solution for reaction.
[0012] Furthermore, in the method for preparing a silicon wafer having a rounded tower base structure provided by the present invention, the temperature of the alkaline etching and polishing is 60-80° C., and the time is 150s-300s.
[0013] On the other hand, the present invention relates to a silicon wafer containing a rounded tower base structure, which is prepared by using the method for preparing a silicon wafer containing a rounded tower base structure.
[0014] Furthermore, in the silicon wafer containing a rounded tower base structure provided by the present invention, the reflectivity of the silicon wafer containing a rounded tower base structure is not less than 51%, and the side length of the tower base is not greater than 9 μm.
[0015] On the other hand, the present invention relates to the use of the additive for alkaline etching and polishing of silicon wafers, or the reaction solution for alkaline etching and polishing of silicon wafers in alkaline etching and polishing of silicon wafers, wherein the additive or the reaction solution improves the reflectivity of the silicon wafer.
[0016] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages: The present invention uses high-molecular green reagents such as defoamers, modifiers, and promoters. When used as additives for alkaline etching and polishing of silicon wafers, the reflectivity of the silicon wafer can reach more than 51%, and the pyramid on the back of the silicon wafer is corroded and flat, and the pyramid base is rounded. Different from the conventional square pyramid base, the rounded pyramid base has good passivation performance and low contact resistance, and can ultimately achieve the purpose of improving efficiency by increasing the short-circuit current. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 The pyramid morphology of the surface on the back of the silicon wafer prepared in Example 1.
[0019] Figure 2 The pyramid morphology of the surface on the back of the silicon wafer prepared in Example 2.
[0020] Figure 3 This is the surface pyramid morphology of the back side of the silicon wafer prepared in Example 3.
[0021] Figure 4 This is the surface pyramid morphology of the back side of the silicon wafer prepared in Comparative Example 1.
[0022] Figure 5This is the surface pyramid morphology of the back side of the silicon wafer prepared in Comparative Example 2. DETAILED DESCRIPTION
[0023] The technical scheme of the present invention is described below in conjunction with the embodiments, but the present invention is not limited to the following embodiments. The experimental methods and detection methods described in each embodiment are conventional methods unless otherwise specified; the reagents and materials can be purchased on the market unless otherwise specified. The % in the following embodiments, unless otherwise specified, are all mass percentages. The ratios in the following embodiments, unless otherwise specified, are all mass ratios.
[0024] Example 1 This embodiment provides an alkali polishing additive process for preparing a rounded tower base on a texturing silicon wafer.
[0025] The additive is composed of the following ingredients, by mass percentage: 0.3% of polyoxyethylene polyoxypropylene pentaerythritol ether, 0.1% of triphenylphosphine oxide, 0.1% of sodium hypochlorite, and the balance of deionized water (resistivity is 18 MΩ).
[0026] The preparation process is as follows: Step 1: Surface treatment is performed on the texturized silicon wafer to remove the PSG layer on the back side, and the removal liquid is 1.0% hydrofluoric acid solution (mass ratio).
[0027] Step 2: Place the silicon wafer treated in step 1 into deionized water (resistivity of 18 MΩ) for 60 seconds.
[0028] Step 3, mixing a sodium hydroxide solution with a concentration of 1.08wt% with an additive to form a reaction solution, placing the silicon wafer obtained in step 2 into the reaction solution for reaction, and obtaining a silicon wafer containing a rounded tower base structure; the volume ratio of the alkaline solution in the reaction solution to the additive is 60:6, the reaction temperature is 60°C, and the time is 150s.
[0029] Figure 1 The pyramid morphology of the surface on the back of the silicon wafer prepared in Example 1.
[0030] Example 2 This embodiment provides an alkali polishing additive process for preparing a rounded tower base on a texturing silicon wafer.
[0031] The additive is composed of the following ingredients, by mass percentage: 0.3% of polyoxyethylene polyoxypropylene pentaerythritol ether, 0.2% of polydimethylsiloxane, 0.2% of triphenylphosphine oxide, 0.3% of ethyl o-methylbenzoate, 0.3% of sodium hypochlorite, 0.3% of sodium percarbonate, and the balance of deionized water (resistivity is 18 MΩ).
[0032] The preparation process is as follows: Step 1: Surface treatment is performed on the texturized silicon wafer to remove the PSG layer on the back side, and the removal liquid is 1.0% hydrofluoric acid solution (mass ratio).
[0033] Step 2: Place the silicon wafer treated in step 1 into deionized water (resistivity of 18 MΩ) for 60 seconds.
[0034] Step 3, mixing a sodium hydroxide solution with a concentration of 2.05wt% with an additive to form a reaction solution, placing the silicon wafer obtained in step 2 into the reaction solution for reaction, and obtaining a silicon wafer containing a rounded tower base structure; the volume ratio of the alkaline solution in the reaction solution to the additive is 30:6, the reaction temperature is 70°C, and the time is 180s.
[0035] Figure 2 The pyramid morphology of the surface on the back of the silicon wafer prepared in Example 2.
[0036] Example 3 This embodiment provides an alkali polishing additive process for preparing a rounded tower base on a texturing silicon wafer.
[0037] The additive is composed of the following ingredients, by mass percentage: 1.0% of polyoxypropylene glyceryl ether, 1.0% of monobenzyl phthalate, 1.0% of potassium perborate, and the balance of deionized water (resistivity is 18 MΩ).
[0038] The preparation process is as follows: Step 1: Surface treatment is performed on the texturized silicon wafer to remove the PSG layer on the back side, and the removal liquid is 1.0% hydrofluoric acid solution (mass ratio).
[0039] Step 2: Place the silicon wafer treated in step 1 into deionized water (resistivity of 18 MΩ) for 60 seconds.
[0040] Step 3, mixing a 3.01wt% sodium hydroxide solution with an additive to form a reaction solution, placing the silicon wafer obtained in step 2 into the reaction solution for reaction, and obtaining a silicon wafer containing a rounded tower base structure; the volume ratio of the alkaline solution in the reaction solution to the additive is 100:6, the reaction temperature is 80°C, and the time is 300s.
[0041] Figure 3 This is the surface pyramid morphology of the back side of the silicon wafer prepared in Example 3.
[0042] Comparative Example 1 This comparative example is intended to illustrate that each functional component in the present application is indispensable. This comparative example is the same as Example 2, except that no modifier is added, that is, the additive is composed of the following ingredients, by mass percentage, 0.3% polyoxyethylene polyoxypropylene pentaerythritol ether, 0.2% polydimethylsiloxane, 0.3% sodium hypochlorite, 0.3% sodium percarbonate, and the balance deionized water (resistivity is 18MΩ).
[0043] Figure 4 This is the surface pyramid morphology of the back side of the silicon wafer prepared in Example 4.
[0044] The silicon wafers prepared in Examples 1 to 3 and Comparative Example 1 were tested, and the test results are shown in Table 1.
[0045] Table 1: Performance test results
[0046] As can be seen from Table 1, the present invention has a significant impact on the morphology and performance of the silicon wafer surface by applying a combination of specific defoamers, modifiers, and promoters. By adjusting the additives provided by the present invention, the reflective performance and surface flatness of the silicon wafer can be optimized.
[0047] Comparative Example 2 This comparative example provides a silicon wafer obtained without adding additives. This comparative example is the same as Example 2, except that no additives are added. The test results are as follows Figure 5 As shown. Figure 5 It can be seen that the top of the conventional alkali-polished pyramid is completely flattened, the base is square, and the surface is smoother. Although the passivation performance is improved, the contact resistance is significantly deteriorated and the overall efficiency is reduced.
[0048] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.
Claims
1. An additive for alkaline etching and polishing of silicon wafers, characterized in that: In terms of mass percentage, the additives are composed of: 0.3-1.0% defoamer, 0.1-1.0% modifier, 0.1-1.0% accelerator, and the balance of deionized water; The defoaming agent is selected from at least one of non-ionic surfactants; The modifier is selected from at least one of a phenyl-containing phosphorus oxide compound and a phenyl-containing ester compound; The promoter is selected from at least one of a strong base weak acid salt with oxidizing properties and a borate with oxidizing properties.
2. The additive for alkaline etching and polishing of silicon wafers according to claim 1, characterized in that: The nonionic surfactant is selected from polyoxyethylene polyoxypropylene pentaerythritol ether, polydimethylsiloxane, and polyoxypropylene glycerol ether; The phenyl-containing phosphorus oxide compound is triphenylphosphine oxide, and the phenyl-containing ester compound is ethyl o-toluate and monobenzyl phthalate; The strong base and weak acid salt with oxidizing property are sodium hypochlorite and sodium percarbonate, and the borate with oxidizing property is potassium perborate.
3. The additive for alkaline etching and polishing of silicon wafers according to claim 1, characterized in that: The resistivity of the deionized water is greater than 18 MΩ.
4. A reaction solution for alkaline etching and polishing of silicon wafers, characterized in that: The invention is obtained by mixing an alkaline solution with a concentration of 1-3 wt% and the additive according to any one of claims 1-3.
5. The reaction solution for alkaline etching and polishing of silicon wafers according to claim 4, characterized in that: The volume ratio of the alkali in the reaction solution to the additive is 0.1-100:
6.
6. The reaction solution for alkaline etching and polishing of silicon wafers according to claim 4, characterized in that: The alkali in the reaction solution is sodium hydroxide and / or potassium hydroxide.
7. A method for preparing a silicon wafer having a rounded tower base structure, comprising: The silicon wafer after texturing is subjected to surface treatment to remove the PSG layer, and then subjected to alkaline etching and polishing after cleaning, wherein the alkaline etching and polishing comprises: placing the silicon wafer in the reaction solution according to any one of claims 4 to 6 for reaction.
8. The method for preparing a silicon wafer having a rounded tower base structure according to claim 7, characterized in that: The temperature of the alkaline etching polishing is 60-80° C., and the time is 150s-300s.
9. A silicon wafer having a rounded tower base structure, characterized in that: The method for preparing a silicon wafer having a rounded tower base structure according to any one of claims 7 to 8 is adopted; The reflectivity of the silicon wafer containing the rounded tower base structure is not less than 51%, and the side length of the tower base is not more than 9 μm.
10. Use of the additive according to any one of claims 1 to 3, or the reaction solution according to any one of claims 4 to 6 in alkaline etching and polishing of silicon wafers, characterized in that: The additive or the reaction solution improves the reflectivity of the silicon wafer.
Citation Information
Patent Citations
Methods and compositions for polishing silicon-containing substrates
CN102149783A
Crystalline silicon surface fine polishing method based on alkaline polishing gel
CN111690987A
Crystalline silicon polishing gel special for Topcon battery and using method thereof
CN111808533A
Additive for alkali polishing in solar cell preparation and polishing process thereof
CN112111279A
Method for etching and polishing single surface of silicon wafer
CN112309849A
Cited By
Solar cell, photovoltaic module and semiconductor substrate
CN119584716A
Silicon wafer back contact cell grooving additive and preparation method and use method thereof
CN120018620A
Alkali polishing additive, polishing solution and polishing method
CN121873800A
Alkaline polishing additives, polishing solutions and polishing methods
CN121873800B