Production method of hydrogen sulfide corrosion resistant oil casing and hydrogen sulfide corrosion resistant oil casing

By adopting steelmaking, heat treatment and reasonable chemical composition control in the production process of oil casing, the problem of insufficient corrosion resistance of hydrogen sulfide in the oil casing is solved, high yield strength and tensile strength are achieved, and hydrogen sulfide resistance is resistant to hydrogen sulfide A 95% pass rate was achieved in the corrosion test.

CN119040592AActive Publication Date: 2024-11-29JIANGSU CHANGBAO STEELTUBE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411266468.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-29
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing oil casing cannot effectively resist hydrogen sulfide corrosion during use. Although the lateral impact work is improved, it cannot solve the problem of hydrogen sulfide corrosion resistance.

Method used

A production method is adopted, including steelmaking, continuous casting into a tube blank, heating, perforation, hot rolling, diameter reduction, quenching and two-stage tempering, heat straightening and stacking cooling, controlling chemical composition and wall thickness deviations, forming Oil casing with high yield strength and tensile strength improves its anti-hydrogen sulfide corrosion performance.

Benefits of technology

Through quenching and tempering heat treatment of two-stage tempering, a fine precipitation phase is formed, which reduces residual stress and dislocation density. Combined with the reasonable addition of Cr and Mo, the anti-hydrogen sulfide corrosion performance of the oil casing is significantly improved and meets the C110 steel grade. Required mechanical properties and high pass rate anti-hydrogen sulfide corrosion test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a production method of a hydrogen sulfide corrosion resistant oil casing and the hydrogen sulfide corrosion resistant oil casing. The production method comprises the following steps that S1, after steelmaking, continuous casting is conducted to form a pipe blank; s2, sawing the pipe blank, and then sequentially carrying out pipe blank heating, punching, hot rolling of a continuous rolling unit and reducing of a reducing mill to prepare a semi-finished product of the oil sleeve; the pipe blank is heated to 1170-1225 DEG C, and the heat preservation time is 2-3 h; the temperature before punching is 1145-1200 DEG C, the temperature before hot rolling is 960-1150 DEG C, and the temperature before tension reducing is 820-950 DEG C; s3, quenching and tempering heat treatment is conducted on the oil casing semi-finished product, wherein quenching and tempering heat treatment sequentially comprises quenching and two-section tempering; the quenching temperature is 920-950 DEG C, and the heat preservation time is 30-50 minutes; in the two-stage tempering process, in the first-stage tempering process, the temperature is 700-710 DEG C; second-stage tempering: the temperature is 680-685 DEG C; and S4, carrying out thermal straightening after quenching and tempering heat treatment, and then carrying out stack cooling to obtain an oil casing finished product. By means of the method, the mechanical property of the oil casing is guaranteed, and the hydrogen sulfide stress corrosion resistance of the oil casing is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a production method of an oil casing resistant to hydrogen sulfide corrosion and the oil casing resistant to hydrogen sulfide corrosion. Background Art

[0002] At present, oil casing is used in oil field exploitation, and is a steel pipe used to support the well wall of oil and gas wells to ensure the normal operation of the entire oil well during the drilling process and after completion. The Chinese patent application publication number CN110303066A discloses a high transverse impact energy steel for oil casing and a preparation method thereof. In the method, molten steel is smelted and continuously cast into a slab, and then the slab is heated, rough rolled, finished rolled and laminar cooled in sequence to obtain a finished product. No heat treatment is used in the method. Through the corresponding rolling process, although the transverse impact energy of the steel is improved, the hydrogen sulfide corrosion resistance of the oil casing is not solved. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide a production method for oil casing resistant to hydrogen sulfide corrosion, by which not only the mechanical properties of the oil casing are guaranteed, but also its resistance to hydrogen sulfide stress corrosion is improved.

[0004] In order to solve the above technical problems, the technical solution of the present invention is: a production method of oil casing resistant to hydrogen sulfide corrosion, the production method comprises the following steps: S1: Continuous casting into tube billet after steelmaking; S2: sawing the tube billet, and then successively heating the tube billet, piercing, hot rolling by a continuous rolling mill, and reducing the diameter by a reducing mill to make a semi-finished oil casing pipe; wherein the tube billet is heated to 1170℃~1225℃, and the holding time is 2~3h; the temperature before piercing is 1145℃~1200℃, the temperature before hot rolling is 960℃~1150℃, and the temperature before tension reducing is 820℃~950℃; S3: The semi-finished oil casing is subjected to quenching and tempering heat treatment, which includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 920℃~950℃, and the holding time is 30-50min; in the two-stage tempering process, the first stage tempering: temperature 700℃-710℃, holding time 20-25min; the second stage tempering: temperature 680℃-685℃, holding time 100-120min; S4: After the quenching and tempering heat treatment, hot straightening is performed, and then stack cooling is performed to obtain the finished oil casing; wherein, the hot straightening temperature is above 550°C, and the cooling rate of stack cooling is ≤3°C / min.

[0005] Furthermore, steelmaking includes: molten iron pretreatment, converter smelting, refining outside the furnace, vacuum degassing and calcium treatment.

[0006] Further, the molten iron is pretreated: the molten iron is pretreated with desulfurization, and the sulfur content of the molten iron after the desulfurization pretreatment is not higher than 0.005%; Converter smelting: add the pretreated molten iron into the converter for smelting, and add auxiliary materials for smelting at the same time. The tapping temperature is controlled at 1625~1675℃. The mass percentage of P during tapping is ≤0.01%. When 1 / 3 of the steel is tapped, add ferrochrome and ferromolybdenum into the ladle for alloying. Refining outside the furnace: After the steel is tapped, the ladle is refined outside the furnace, the basicity of the refined slag is controlled at 2.5-3.5, the white slag time is 25-30 minutes, ferrovanadium and ferroniobium are added during the refining process for alloying, samples are taken from the refined molten steel to determine the composition, and the mass percentage of the chemical composition is adjusted according to the test results; Vacuum degassing: When the chemical composition and mass percentage meet the target requirements, the ladle is vacuum degassed, and the degassing time is ≥15min. After the degassing is completed, the hydrogen content is determined and the hydrogen content should be ≤2ppm.

[0007] Furthermore, in order to control the wall thickness deviation within a smaller range during the preparation process, reduce the deformation of the pipeline during the subsequent heat treatment process, reduce the internal stress after straightening, and improve the material's resistance to hydrogen sulfide corrosion, in step S2, the wall thickness deviation is controlled to be ≤10% during the perforation, hot rolling of the continuous rolling mill, and reducing of the reducing mill.

[0008] Furthermore, in order to reasonably control the wall thickness deviation during the preparation process, in step S2, during punching, the rolling center line is kept consistent with the punching machine center line, so that the force on the tube billet is balanced during punching, avoiding one-sided force on the tube billet during rolling and affecting the wall thickness accuracy.

[0009] Furthermore, in order to reasonably control the wall thickness deviation during the preparation process, in step S2, during punching, the deviation between the three-roller centering center line for centering the tube blank and the center line of the punching machine is ≤1 mm.

[0010] Furthermore, in order to reasonably control the wall thickness deviation during the preparation process, in step S2, when the continuous rolling mill is hot-rolling, the center line of the continuous rolling mill and the rolling mill arch should be kept consistent, with a deviation of ≤0.5 mm.

[0011] Furthermore, the performance parameters of the finished oil casing are as follows: yield strength: 770~810MPa, tensile strength: 850~900MPa, elongation ≥20%, impact toughness: longitudinal 0℃, ≥150J, transverse 0℃, ≥120J.

[0012] Further, in order to better ensure its mechanical properties and better improve its resistance to hydrogen sulfide stress corrosion, in step S1, steelmaking is carried out according to the chemical composition and mass percentage of the oil casing; wherein the chemical composition and mass percentage of the oil casing are as follows: C: 0.25-0.30%, Si: 0.2-0.6%, Mn: 0.3-0.7%, Cr: 0.3-0.6%, Mo: 0.7-1.0%, V: 0.05-0.15%, Nb: 0.03-0.1%, P≤0.015%, S≤0.0015%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein 1.2%≤Cr+Mo≤1.4%.

[0013] The present invention also provides an oil casing pipe resistant to hydrogen sulfide corrosion prepared by the above production method. The chemical composition and mass percentage of the oil casing pipe are as follows: C: 0.25~0.30%, Si: 0.2~0.6%, Mn: 0.3~0.7%, Cr: 0.3~0.6%, Mo: 0.7~1.0%, V: 0.05~0.15%, Nb: 0.03~0.1%, P≤0.015%, S≤0.0015%, the rest are Fe and unavoidable impurities, totaling 100%; among which 1.2%≤Cr+Mo≤1.4%.

[0014] After adopting the above technical solution, the present invention has the following beneficial effects: 1. The present invention adopts quenching + two-stage tempering to perform quenching and tempering heat treatment; wherein, the heat treatment quenching temperature is between 920℃ and 950℃, which can not only ensure that the oil casing steel of the present invention is completely austenitized, but also avoid the grain size enlargement caused by excessive temperature. The present invention controls the morphology of the precipitated phase by two-stage tempering during the quenching and tempering heat treatment stage, forming a dispersed fine precipitated phase to avoid the precipitated phase from growing locally. The first stage tempering temperature is 700℃-710℃, and the holding time is 20-25min; the main function is to quickly eliminate the quenching stress and increase the nucleation driving force of the precipitated phase; the second stage tempering temperature is 680℃-685℃, and the holding time is 100-120min. The use of a longer tempering time can reduce the temperature difference between the core and the surface of the material, and the core and surface performance differences are smaller, and the performance fluctuations are small. The straightening temperature of the oil casing after tempering is above 550℃. After straightening, the stacking and slow cooling are carried out to reduce the residual stress. The above measures are used to control the metallographic structure, thereby ultimately improving the material's resistance to hydrogen sulfide corrosion. 2. The cooling speed during quenching is very fast, which will produce large thermal stress. At the same time, martensitic phase transformation will occur, generating phase transformation stress. If the wall thickness difference is large, the steel pipe will easily deform and bend. In the subsequent straightening process, it will produce large plastic deformation. As a result, large internal stress and high dislocation density are generated in the pipeline, which will significantly reduce the material's resistance to hydrogen sulfide corrosion. The present invention improves the wall thickness control accuracy through a series of means, minimizes the deformation during the quenching process, and reduces the residual stress and dislocation density in the material through a higher straightening temperature and slow cooling measures, thereby improving the material's resistance to hydrogen sulfide corrosion.

[0015] 3. In addition, by adding Cr and Mo to improve the strength, promote the precipitation of fine precipitated phases in the steel, and avoid the precipitation of large-sized M23C6 at the grain boundaries. Cr and Mo are both strong carbide-forming elements. The fine carbides precipitated during the tempering process can not only improve the yield strength of the material, but also are good hydrogen traps, which can improve the material's resistance to hydrogen sulfide corrosion. However, when the Cr content is too high, large-sized carbides M23C6 will be generated at the grain boundaries, which reduces the grain boundary strength and affects the material's resistance to hydrogen sulfide corrosion. If only Mo is added for strengthening, the material cost will be greatly increased. Therefore, the present invention not only stipulates the composition range of Cr and Mo, Cr: 0.3~0.6%, Mo: 0.7~1.0%, but also limits the total amount of the two added, 1.2≤Cr+Mo≤1.4. It can not only ensure the yield strength of the material, but also avoid the production of large-sized M23C6 at the grain boundaries.

[0016] 4. The present invention also improves the material's hydrogen sulfide corrosion resistance by controlling the purity of the oil casing steel, that is, controlling the content of P and S, improving the purity, and avoiding the occurrence of grain boundary embrittlement and large-sized manganese sulfide inclusions. DETAILED DESCRIPTION

[0017] The present invention provides a method for producing oil casing resistant to hydrogen sulfide corrosion and oil casing resistant to hydrogen sulfide corrosion. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be pointed out in particular that all similar replacements and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.

[0018] A method for producing oil casing resistant to hydrogen sulfide corrosion, the method comprising the following steps: S1: After steelmaking, the tubes are continuously cast into billets, which are cut into fixed lengths and then placed in a slow cooling pit for slow cooling. The slow cooling time is ≥ 48h. During the casting process, the tundish is heated by induction to ensure that the superheat is stable at 20-30℃. S2: sawing the tube billet according to the requirements, the cutting slope of the tube billet section is ≤3mm, and then the tube billet is heated, pierced, hot rolled by a continuous rolling mill and reduced by a reducing mill in sequence to form a semi-finished oil casing pipe; wherein, the tube billet is heated to 1170℃~1225℃, and the holding time is 2~3h. If the holding time is too short, the temperature uniformity of the tube billet is poor, and the piercing process is prone to uneven wall thickness. If the holding time is too long, oxidation and burning are serious, so the holding time is limited to 2~3h; the temperature before piercing is 1145℃~1200℃, the temperature before hot rolling is 960℃~1150℃, and the temperature before tension reducing is 820℃~950℃; S3: The semi-finished oil casing is subjected to quenching and tempering heat treatment, which includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 920℃~950℃, and the holding time is 30-50min; in the two-stage tempering process, the first stage tempering: temperature 700℃-710℃, holding time 20-25min; the second stage tempering: temperature 680℃-685℃, holding time 100-120min; S4: After the quenching and tempering heat treatment, hot straightening is performed, and then stack cooling is performed to obtain the finished oil casing; wherein, the hot straightening temperature is above 550°C, and the cooling rate of stack cooling is ≤3°C / min.

[0019] The present invention adopts quenching + two-stage tempering to perform quenching and tempering heat treatment; wherein, the heat treatment quenching temperature is between 920℃ and 950℃, which can not only ensure that the oil casing steel of the present invention is completely austenitized, but also avoid the increase of grain size due to excessive temperature. The present invention controls the morphology of the precipitated phase by two-stage tempering during the quenching and tempering heat treatment stage, forms a dispersed fine precipitated phase, and avoids the precipitated phase from growing locally. The first stage tempering temperature is 700℃-710℃, and the holding time is 20-25min; the main function is to quickly eliminate the quenching stress and increase the nucleation driving force of the precipitated phase; the second stage tempering temperature is 680℃-685℃, and the holding time is 100-120min. The use of a longer tempering time can reduce the temperature difference between the core and the surface of the material, and the core and surface performance differences are smaller, and the performance fluctuations are small. The straightening temperature of the oil casing after tempering is above 550℃. After straightening, the stacking and slow cooling are carried out to reduce the residual stress. The above measures are used to control the metallographic structure, thereby ultimately improving the material's resistance to hydrogen sulfide corrosion. Specifically, steelmaking includes: molten iron pretreatment, converter smelting, refining outside the furnace, vacuum degassing and calcium treatment.

[0020] Specifically, hot metal pretreatment: hot metal is subjected to desulfurization pretreatment, and the sulfur content of the hot metal after desulfurization pretreatment is not higher than 0.005%; Converter smelting: add the pretreated molten iron into the converter for smelting, and add scrap steel, lime and other auxiliary materials for smelting at the same time. The tapping temperature is controlled at 1625~1675℃. The mass percentage of P during tapping is ≤0.01%. When 1 / 3 of the steel is tapped, add ferrochrome and ferromolybdenum into the ladle for alloying. The ferrochrome and ferromolybdenum used are low S and low P alloys to avoid introducing too many impurity elements. Refining outside the furnace: After the steel is tapped, the ladle is refined outside the furnace, the basicity of the refined slag is controlled at 2.5-3.5, the white slag time is 25-30 minutes, ferrovanadium and ferroniobium are added during the refining process for alloying, samples are taken from the refined molten steel to determine the composition, and the mass percentage of the chemical composition is adjusted according to the test results; Vacuum degassing: When the chemical composition and mass percentage meet the target requirements, the ladle is vacuum degassed. The degassing treatment should be carried out under high vacuum conditions (≤0.26kpa) to achieve the purpose of dehydrogenation and removal of deoxidized inclusions in the steel. The degassing time is ≥15min. After the degassing is completed, the hydrogen content is determined and the hydrogen content should be ≤2ppm.

[0021] Specifically, in step S2, during the perforation, hot rolling of the continuous rolling mill, and the diameter reduction of the diameter reducing mill, the wall thickness deviation is controlled to be ≤10%. If the wall thickness deviation is controlled within a small range, the pipe deformation in the subsequent heat treatment process is small, and the internal stress after straightening is small, which is conducive to improving the material's resistance to hydrogen sulfide corrosion.

[0022] The cooling speed during quenching is very fast, which will produce large thermal stress. At the same time, martensitic phase transformation will occur, generating phase transformation stress. If the wall thickness difference is large, the steel pipe will easily deform and bend. In the subsequent straightening process, large plastic deformation will occur. As a result, large internal stress and high dislocation density will be generated in the oil casing, which will significantly reduce the material's resistance to hydrogen sulfide corrosion. The present invention improves the wall thickness control accuracy through a series of means, minimizes the deformation during the quenching process, and reduces the residual stress and dislocation density in the material through a higher straightening temperature and slow cooling measures, thereby improving the material's resistance to hydrogen sulfide corrosion.

[0023] Specifically, in step S2, during punching, the rolling center line is consistent with the punching machine center line, so that the force is balanced during the punching of the tube billet, and the wall thickness accuracy is not affected by the force on one side during the rolling of the tube billet; during punching, the deviation between the three-roller centering center line for centering the tube billet and the punching machine center line is ≤1mm; during hot rolling of the continuous rolling mill, the center line of the continuous rolling mill and the mill arch should be consistent, with a deviation of ≤0.5mm. The above measures are all for the purpose of reasonably controlling the wall thickness deviation during the preparation process, thereby reducing the deformation of the subsequent heat treatment and the internal stress after straightening, which is conducive to improving the material's resistance to hydrogen sulfide corrosion.

[0024] Specifically, the performance parameters of the finished oil casing are as follows: yield strength: 770~810MPa, tensile strength: 850~900MPa, elongation ≥20%, impact toughness: longitudinal 0℃, ≥150J, transverse 0℃, ≥120J.

[0025] Specifically, in step S1, steelmaking is performed according to the chemical composition and mass percentage of the oil casing; wherein the chemical composition and mass percentage of the oil casing are as follows: C: 0.25-0.30%, Si: 0.2-0.6%, Mn: 0.3-0.7%, Cr: 0.3-0.6%, Mo: 0.7-1.0%, V: 0.05-0.15%, Nb: 0.03-0.1%, P≤0.015%, S≤0.0015%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein 1.2%≤Cr+Mo≤1.4%.

[0026] C is an important element to ensure strength. When the C content is less than 0.25%, the strength is difficult to ensure. When the C content is greater than 0.3%, the stress is large during quenching, which not only easily causes cracks during the quenching process, but also leads to reduced material toughness and increased stress corrosion sensitivity. Therefore, the present invention controls the C content to be between 0.25 and 0.3%.

[0027] Si is an important deoxidizing element. When the Si content is too low, the deoxidizing effect is poor and the number of inclusions is large. However, when it is too much, the cold brittle tendency of the steel will increase. The present invention limits the Si content to 0.2-0.6%.

[0028] Mn has the function of increasing hardenability. Adding an appropriate amount of Mn can ensure that the material completely produces martensite after quenching. However, Mn is also an important element that promotes the formation of banded structure. If too much Mn is added, segregation will increase, the performance difference between different structures will increase, the uniformity of the material will decrease, and the resistance to hydrogen sulfide corrosion will be affected. Therefore, the Mn content is set to 0.3~0.7%.

[0029] Cr and Mo are both strong carbide-forming elements. The fine carbides precipitated during tempering can not only improve the yield strength of the material, but also are good hydrogen traps, which can improve the material's resistance to hydrogen sulfide corrosion. However, when the Cr content is too high, large-sized carbides M23C6 will be generated at the grain boundaries, reducing the grain boundary strength and affecting the material's resistance to hydrogen sulfide corrosion. If only Mo is added for strengthening, the material cost will increase significantly. Therefore, this patent not only stipulates the composition range of Cr and Mo, Cr: 0.3~0.6%, Mo: 0.7~1.0%, but also limits the total amount of both added, 1.2≤Cr+Mo≤1.4. It can not only ensure the yield strength of the material, but also avoid the production of large-sized M23C6 at the grain boundaries.

[0030] V and Nb are important grain-refining elements, and can also produce fine precipitates, improving the yield strength and hydrogen sulfide corrosion resistance of the material. However, if too much is added, coarse carbides will be formed, especially if too much Nb is added, serious liquid precipitation will occur, reducing the mechanical properties of the material. Therefore, the present invention sets V: 0.05~0.15%, Nb: 0.03~0.1%.

[0031] P and S are harmful elements. P is prone to form abnormal structural segregation and increase the cold brittleness of steel. S is prone to form sulfide inclusions, which seriously affects the anti-sulfur performance. Therefore, the content of P and S should be reduced as much as possible, and controlled within P≤0.015% and S≤0.0015%.

[0032] A hydrogen sulfide corrosion resistant oil casing prepared by the above production method, the chemical composition and mass percentage of the oil casing are as follows: C: 0.25~0.30%, Si: 0.2~0.6%, Mn: 0.3~0.7%, Cr: 0.3~0.6%, Mo: 0.7~1.0%, V: 0.05~0.15%, Nb: 0.03~0.1%, P≤0.015%, S≤0.0015%, the rest are Fe and unavoidable impurities, totaling 100%; among which 1.2%≤Cr+Mo≤1.4%.

[0033] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments.

[0034] Embodiment 1: A method for producing oil casing resistant to hydrogen sulfide corrosion, the production method comprising the following steps: S1: Steelmaking is carried out according to the chemical composition and mass percentage of the oil casing, and after steelmaking, it is continuously cast into tube billets, which are cut into fixed lengths and then placed in a slow cooling pit for slow cooling, and the slow cooling time is ≥48h; during the casting process, the tundish adopts induction heating to ensure that the superheat is stable at 20-30℃; steelmaking includes: molten iron pretreatment, converter smelting, refining outside the furnace, vacuum degassing and calcium treatment in sequence; the chemical composition and mass percentage of the oil casing are as follows: C: 0.25%, Si: 0.3%, Mn: 0.3%, Cr: 0.4%, Mo: 1.0%, V: 0.05%, Nb: 0.03%, P: 0.009%, S: 0.0011%, and the rest are Fe and unavoidable impurities, totaling 100%; Cr+Mo=1.4%; S2: saw the tube billet according to the requirements, the cutting slope of the tube billet section is ≤3mm, and then the tube billet is heated, pierced, hot rolled by the continuous rolling mill and reduced by the reducing mill in sequence to form a semi-finished oil casing pipe; wherein, the tube billet is heated to 1170℃ and the holding time is 2h; the temperature before piercing is 1145℃, the temperature before hot rolling is 960℃, and the temperature before tension reducing is 820℃; during piercing, hot rolling by the continuous rolling mill and reducing by the reducing mill, the wall thickness deviation is controlled to be ≤10%; the rolling center line is consistent with the center line of the piercing mill, so that the force is balanced when the tube billet is pierced, and the wall thickness accuracy is not affected by the single-sided force during the rolling of the tube billet; during piercing, the deviation between the three-roller centering center line for centering the tube billet and the center line of the piercing mill is ≤1mm; during hot rolling by the continuous rolling mill, the center lines of the continuous rolling mill and the rolling mill arch should be consistent, with a deviation of ≤0.5mm; S3: The semi-finished oil casing is subjected to quenching and tempering heat treatment, which includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 920°C and the holding time is 30 minutes; in the two-stage tempering process, the first stage tempering: temperature 700°C, holding time 20 minutes; the second stage tempering: temperature 680°C, holding time 100 minutes; S4: After the quenching and tempering heat treatment, hot straightening is performed, followed by stack cooling to obtain the finished oil casing; wherein, the hot straightening temperature is 600°C, and the cooling rate of stack cooling is about 2.3°C / min.

[0035] Embodiment 2: The production method of the oil casing resistant to hydrogen sulfide corrosion in this embodiment is basically the same as that in Embodiment 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.4%, Mn: 0.45%, Cr: 0.45%, Mo: 0.9%, V: 0.07%, Nb: 0.04%, P: 0.008%, S: 0.001%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.35%; in step S2, the tube blank is heated to 1225°C, and the heat preservation time is The time is 3h; the temperature before piercing is 1200℃, the temperature before hot rolling is 1150℃, and the temperature before tension reducing is 950℃; in step S3, the semi-finished oil casing is subjected to tempering heat treatment, and the tempering heat treatment includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 950℃, and the holding time is 50min; in the two-stage tempering process, the first stage tempering: temperature 710℃, holding time 25min; the second stage tempering: temperature 685℃, holding time 120min; in step S4, the hot straightening temperature is 550℃, and the cooling rate of stack cooling is about 2.9℃ / min.

[0036] Embodiment 3: The production method of the oil casing resistant to hydrogen sulfide corrosion in this embodiment is basically the same as that in Embodiment 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.30%, Si: 0.45%, Mn: 0.5%, Cr: 0.55%, Mo: 0.8%, V: 0.07%, Nb: 0.04%, P: 0.011%, S: 0.0009%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.35%; in step S2, the tube blank is heated to 1200°C and kept warm. The time is 2.5h; the temperature before piercing is 1160℃, the temperature before hot rolling is 1050℃, and the temperature before tension reducing is 900℃; in step S3, the semi-finished oil casing is subjected to tempering heat treatment, and the tempering heat treatment includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 935℃, and the holding time is 40min; in the two-stage tempering process, the first stage tempering: temperature 705℃, holding time 22min; the second stage tempering: temperature 682℃, holding time 110min; in step S4, the hot straightening temperature is 650℃, and the cooling rate of stack cooling is about 2℃ / min.

[0037] Example 4: The production method of the hydrogen sulfide corrosion resistant oil casing of the embodiment is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.35%, Mn: 0.47%, Cr: 0.55%, Mo: 0.75%, V: 0.12%, Nb: 0.06%, P: 0.012%, S: 0.0012%, and the rest are Fe and unavoidable impurities, totaling 100%; among which Cr+Mo: 1.3%.

[0038] Example 5: The production method of the oil casing resistant to hydrogen sulfide corrosion in this example is basically the same as that in Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.4%, Mn: 0.46%, Cr: 0.6%, Mo: 0.7%, V: 0.15%, Nb: 0.03%, P≤0.01%, S≤0.0008%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.3%.

[0039] Comparative Example 1 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.4%, Mn: 0.46%, Cr: 0.6%, Mo: 0.7%, V: 0.15%, Nb: 0.03%, P: 0.011%, S: 0.0012%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.3%; in step S4, the hot straightening temperature is 300°C, and air cooling is adopted after hot straightening.

[0040] Comparative Example 2 The production method of the oil casing of this comparative example is basically the same as that of comparative example 1, except that in step S3, the semi-finished oil casing is subjected to a tempering heat treatment, and the tempering heat treatment sequentially includes quenching and a tempering stage; wherein the quenching temperature is 935°C and the holding time is 40 minutes; the first tempering stage: temperature is 705°C and the holding time is 22 minutes.

[0041] Comparative Example 3 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.23%, Si: 0.4%, Mn: 0.56%, Cr: 0.6%, Mo: 0.71%, V: 0.15%, Nb: 0.03%, P: 0.01%, S: 0.0012%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.31%.

[0042] Comparative Example 4 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.23%, Si: 0.4%, Mn: 0.56%, Cr: 0.6%, Mo: 0.71%, V: 0.15%, Nb: 0.03%, P: 0.012%, S: 0.0011%, and the rest are Fe and unavoidable impurities, totaling 100%; Cr+Mo=1.31%. Second stage tempering: temperature 650°C, heat preservation 120min.

[0043] Comparative Example 5 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.32%, Si: 0.37%, Mn: 0.45%, Cr: 0.6%, Mo: 0.67%, V: 0.15%, Nb: 0.03%, P: 0.01%, S: 0.0012%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.31%.

[0044] Comparative Example 6 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.27%, Si: 0.4%, Mn: 0.46%, Cr: 0.9%, Mo: 0.5%, V: 0.15%, Nb: 0.03%, P: 0.009%, S: 0.0014%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.3%.

[0045] Comparative Example 7 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.45%, Mn: 0.56%, Cr: 0.2%, Mo: 0.75%, V: 0.15%, Nb: 0.03%, P: 0.011%, S: 0.001%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=0.95%.

[0046] Comparative Example 8 The production method of the oil casing of this comparative example is basically the same as that of Example 1, except that the chemical composition and mass percentage of the oil casing are as follows: C: 0.26%, Si: 0.4%, Mn: 0.46%, Cr: 0.6%, Mo: 0.9%, V: 0.15%, Nb: 0.03%, P: 0.012%, S: 0.0007%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein Cr+Mo=1.5%.

[0047] Comparative Example 9 The production method of the oil casing in this comparative example is basically the same as that in Example 1, except that in step S2, during the perforation, hot rolling by the continuous rolling mill and the diameter reducing by the reducing mill, the wall thickness deviation is relatively large, which is 12.4%.

[0048] The properties of the oil casing produced by the production methods of the above embodiments and comparative examples are shown in the following table after testing:

[0049] In the above embodiments and comparative examples, the hydrogen sulfide corrosion resistance test was carried out in accordance with the A-NACE standard tensile test in ANSI / NACE TM0177-2016. Each test case tested 20 specimens, and the pass rate was calculated based on the specimens that passed the test. The components of Examples 1-5 meet the requirements, and quenching + two-stage tempering and straightening temperature above 550°C + stack slow cooling are adopted. The mechanical properties such as yield strength meet the requirements of C110 steel grade, and the pass rate of hydrogen sulfide corrosion resistance test is ≥95%. The straightening temperature used in Comparative Example 1 is lower than 550°C, and air cooling is used after straightening, and the pass rate of hydrogen sulfide corrosion resistance test is reduced to 70%. Comparative Example 2 adopts one-stage tempering, and the pass rate of hydrogen sulfide corrosion resistance test is also significantly reduced. The carbon content of Comparative Example 3 is lower than the lower limit, and the strength is significantly reduced, which does not meet the requirements of C110 steel grade. Comparative Example 4 is substantially the same as Comparative Example 3. The strength is increased to C110 steel grade by adjusting the tempering temperature, but the pass rate of hydrogen sulfide corrosion resistance test is greatly reduced. In Comparative Example 5, the carbon content exceeds the upper limit, the strength is relatively high, and the pass rate of the hydrogen sulfide corrosion test is only 50%. In Comparative Example 6, the Cr content exceeds the upper limit of this patent, and the pass rate of the hydrogen sulfide corrosion test is only 30%. In Comparative Example 7, the Cr content is lower than the lower limit of this patent, and the strength does not meet the requirements. In Comparative Example 8, the Cr+Mo content exceeds the upper limit of this patent, and the pass rate of the hydrogen sulfide corrosion test drops to 50%; in Comparative Example 9, the wall thickness deviation is large, the bending phenomenon after quenching is serious, the residual stress after straightening is large, and the pass rate of hydrogen sulfide corrosion resistance drops to 70%.

[0050] The specific embodiments described above further illustrate the technical problems, technical solutions and beneficial effects solved by the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing oil casing resistant to hydrogen sulfide corrosion, characterized in that: The production method comprises the following steps: S1: Continuous casting into tube billet after steelmaking; S2: sawing the tube billet, and then successively heating the tube billet, piercing, hot rolling by a continuous rolling mill, and reducing the diameter by a reducing mill to make a semi-finished oil casing pipe; wherein the tube billet is heated to 1170℃~1225℃, and the holding time is 2~3h; the temperature before piercing is 1145℃~1200℃, the temperature before hot rolling is 960℃~1150℃, and the temperature before tension reducing is 820℃~950℃; S3: The semi-finished oil casing is subjected to quenching and tempering heat treatment, which includes quenching and two-stage tempering in sequence; wherein, the quenching temperature is 920℃~950℃, and the holding time is 30-50min; in the two-stage tempering process, the first stage tempering: temperature 700℃-710℃, holding time 20-25min; the second stage tempering: temperature 680℃-685℃, holding time 100-120min; S4: After the quenching and tempering heat treatment, hot straightening is performed, and then stack cooling is performed to obtain the finished oil casing; wherein, the hot straightening temperature is above 550°C, and the cooling rate of stack cooling is ≤3°C / min.

2. The production method according to claim 1, characterized in that Steelmaking includes: molten iron pretreatment, converter smelting, refining outside the furnace, vacuum degassing and calcium treatment.

3. The production method according to claim 2, characterized in that: Hot metal pretreatment: The hot metal is subjected to desulfurization pretreatment. The sulfur content of the hot metal after desulfurization pretreatment is not higher than 0.005%; Converter smelting: add the pretreated molten iron into the converter for smelting, and add auxiliary materials for smelting at the same time. The tapping temperature is controlled at 1625~1675℃. The mass percentage of P during tapping is ≤0.01%. When 1 / 3 of the steel is tapped, add ferrochrome and ferromolybdenum into the ladle for alloying. Refining outside the furnace: After the steel is tapped, the ladle is refined outside the furnace, the basicity of the refined slag is controlled at 2.5-3.5, the white slag time is 25-30 minutes, ferrovanadium and ferroniobium are added during the refining process for alloying, samples are taken from the refined molten steel to determine the composition, and the mass percentage of the chemical composition is adjusted according to the test results; Vacuum degassing: When the chemical composition and mass percentage meet the target requirements, the ladle is vacuum degassed, and the degassing time is ≥15min. After the degassing is completed, the hydrogen content is determined and the hydrogen content should be ≤2ppm.

4. The production method according to claim 1, characterized in that In step S2, during the piercing, hot rolling by the continuous rolling mill and the diameter reducing by the diameter reducing mill, the wall thickness deviation is controlled to be ≤10%.

5. The production method according to claim 1, characterized in that: In step S2, during punching, the rolling center line is kept consistent with the punching machine center line, so that the force on the tube billet is balanced during punching, and the wall thickness accuracy is not affected by the one-sided force during rolling of the tube billet.

6. The production method according to claim 1, characterized in that: In step S2, during punching, the deviation between the three-roll centering center line for centering the tube blank and the center line of the punching machine is ≤1 mm.

7. The production method according to claim 1, characterized in that: In step S2, when the continuous rolling mill is hot rolling, the center line of the continuous rolling mill and the rolling mill arch should be kept consistent, with a deviation of ≤0.5mm.

8. The production method according to claim 1, characterized in that: The performance parameters of finished oil casing are as follows: yield strength: 770~810MPa, tensile strength: 850~900MPa, elongation ≥20%, impact toughness: longitudinal 0℃, ≥150J, transverse 0℃, ≥120J.

9. The production method according to claim 1, characterized in that: In step S1, steelmaking is performed according to the chemical composition and mass percentage of the oil casing; wherein the chemical composition and mass percentage of the oil casing are as follows: C: 0.25-0.30%, Si: 0.2-0.6%, Mn: 0.3-0.7%, Cr: 0.3-0.6%, Mo: 0.7-1.0%, V: 0.05-0.15%, Nb: 0.03-0.1%, P≤0.015%, S≤0.0015%, and the rest are Fe and unavoidable impurities, totaling 100%; wherein 1.2%≤Cr+Mo≤1.4%.

10. An oil casing resistant to hydrogen sulfide corrosion produced by the production method according to any one of claims 1 to 8, characterized in that: The chemical composition and mass percentage of oil casing are as follows: C: 0.25~0.30%, Si: 0.2~0.6%, Mn: 0.3~0.7%, Cr: 0.3~0.6%, Mo: 0.7~1.0%, V: 0.05~0.15%, Nb: 0.03~0.1%, P≤0.015%, S≤0.0015%, the rest are Fe and unavoidable impurities, totaling 100%; among which 1.2%≤Cr+Mo≤1.4%.

Citation Information

Patent Citations

  • Ultrahigh-strength hydrogen sulfide corrosion resistant oil well pipe and production method thereof

    CN101724785A

  • High strength and ductility oil casing with hydrogen sulfide corrosion resistance and manufacturing method for oil casing

    CN102618791A

  • High-toughness corrosion-resistant steel and manufacturing method thereof

    CN102839331A

  • High-strength seamless steel pipe with excellent resistance to sulfide stress cracking for oil well, and process for producing same

    CN104011251A

  • Low-alloy high-strength sulfur-resistant oil casing material and preparation method thereof

    CN111961973A