Latent curing agent as well as preparation method and application thereof
By adding specific additives to the B-order phenolic resin and controlling the reaction conditions, a latent curing agent with long-term stability and low curing shrinkage rate was prepared, which solved the storage stability and curing shrinkage of latent curing agents in the prior art. The problem of insufficient rate improves the overall performance and safety of the material.
Patent Information
- Application Number
- CN202411321857.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-27
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
The existing latent curing agents have shortcomings in storage stability and curing shrinkage, and are expensive, making them difficult to be well compatible with epoxy resins, affecting the overall performance of the material.
By adding copolymer, superbranching material, sealing material, compounding material, anti-shrinking agent and functional resin to the B-order phenolic resin, controlling the reaction conditions and addition amount, a kind of long-term storage stability and low curing shrinkage rate was prepared. latent curing agent.
It realizes long-term stable storage of latent curing agents and low curing shrinkage, improving the comprehensive performance of the material, including high and low temperature resistance, impact resistance, hardness and toughness, and complies with environmental protection and safety requirements.
Smart Images

Figure CN119060277A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of compound preparation, and specifically relates to a latent curing agent and a preparation method and application thereof. Background Art
[0002] Chemicals that have a long application life / storage life in epoxy resin at room temperature and can rapidly cure epoxy resin when heated to a certain temperature are collectively referred to as "latent curing agents". They may be additives added in trace amounts or resins added in larger amounts.
[0003] At present, the latent curing agents on the market mainly include:
[0004] ①Dicyandiamide and its modified products
[0005] ② Boron trifluoride-amine complexes
[0006] 3 Boron heterocyclic boron amines
[0007] 4Organic hydrazides
[0008] 5 Imidazoles
[0009] 6 Supercoordinated silicates
[0010] They are all key raw materials for preparing single-component epoxy resin products (commonly known as single-component glue), such as single-component epoxy adhesives, epoxy coatings, epoxy inks, as well as epoxy potting materials, epoxy casting materials, and epoxy composite prepregs. According to literature and patent searches, there are several technical solutions for latent curing agents on the market, and their advantages and disadvantages are as follows:
[0011] 1Dicyandiamide powder
[0012] Dicyandiamide (DICY) is a white crystalline powder with a melting point of 207-209°C. Its molecular structure contains conjugated double bonds and cyano groups. The alkalinity is greatly reduced after the alkyl group replaces the guanidine. After mixing with epoxy resin, it has a long stable period at room temperature. It is insoluble in epoxy resin and is in a suspended and dispersed state. The compatibility of ultrafinely crushed dicyandiamide is significantly improved.
[0013] The advantages are long storage period, easy use, simple operation and high Tg of the cured product.
[0014] The disadvantages are poor compatibility and solubility, the curing temperature needs to be between 180-200°C, it is easy to oxidize and discolor at high temperature, and the cured product is hard and brittle. It is generally not used alone, but usually combined with other latent curing agents, and the price is relatively high.
[0015] 2 Liquefied dicyandiamide
[0016] The dicyandiamide is grafted and modified and then liquefied, mainly using NCO monomer for grafting to generate urea derivatives. The second is modification with imidazole.
[0017] The advantages are easy use and operation, good compatibility and solubility, the curing temperature is reduced to 130-150℃, and the curing speed is increased.
[0018] The disadvantage is that the application period is short and it needs to be stored at low temperature. The storage period at room temperature is about 30 days. The heat resistance, electrical insulation and impact resistance of the cured product decrease. It is expensive and easy to yellow, which is not conducive to making light-colored or colorless and transparent products.
[0019] 3 Boron trifluoride-amine complexes
[0020] Boron trifluoride can form a stable complex with amines, making the amines less active. It has a longer shelf life with epoxy resin at room temperature. When heated, it quickly decomposes into BF3 and amines. Amines and epoxy resins react and solidify, and BF3 acts as a promoter.
[0021] The advantages are good compatibility and long-term storage.
[0022] The disadvantage is BF 3 It is corrosive to metals and is not suitable for insulating materials. It is sensitive to humidity and water vapor and can easily become cloudy and deteriorate if not stored properly, making it inconvenient to store and use.
[0023] 4-boron heterocyclic boron amine complex
[0024] A latent epoxy resin curing agent developed by the American Boron Chemical Company in 1962.
[0025] The advantages are low viscosity, not easy to hydrolyze, miscible with epoxy resin, low volatility; the storage period at room temperature is more than 3 months, and no BF is generated during curing 3 , no corrosion to metal.
[0026] The disadvantages are that it is expensive, affects electrical insulation, has high moisture absorption, large shrinkage, large internal stress, is easy to crack, and has poor impact resistance.
[0027] 5Organic hydrazides
[0028] High melting point powder, made from methyl carboxylate and hydrazine, general structural formula: H 2 N-NH-CO-R-CO-NH-NH 2 , heated to the critical temperature to quickly cure the epoxy resin.
[0029] The disadvantages are that the powder is not suspended and dispersed in the epoxy resin, has poor compatibility, and is insoluble; it is relatively expensive; it requires high temperature of about 180°C for curing, has high energy consumption, and the curing process is relatively complicated, making it inconvenient to use and operate.
[0030] The advantage is that the storage period at room temperature is greater than 4 months.
[0031] 6 Supercoordinated silicate
[0032] Boil the methanol solution of trimethoxyphenylsilane, catechol and benzylamine for 10-15 minutes, precipitate the generated crystals, filter them, wash them with cold methanol and dry them to obtain benzyldimethylamine bis(o-phenylenedioxy)phenyl silicate, with the structural formula: PhCH 2 NHMe 2 PhSi(C 6 H 4 O 2 ) 2 . Take 2 parts of the silicate, 14 parts of trimellitic anhydride and 100 parts of bisphenol A epoxy resin to prepare glue. The storage period at room temperature is 5 months. It is unstable at high temperature. The silicate decomposes into free amine and coordinated silicon compound. It is mainly used as an accelerator for anhydride epoxy curing agent, used for casting, bonding, lamination, etc. The curing condition is 200℃ for about 8.5s.
[0033] The advantage is that it is stable at room temperature and has a long storage period.
[0034] The disadvantage is that it is expensive and the performance of the cured product is far inferior to that of two-component products.
[0035] 7-ethylenediamine silicate
[0036] Structural formula (H 2 NCH 2 CH 2 NH 3 )2Si 2 (C 6 H 4 O 2 ) 3 The dosage in liquid bisphenol A epoxy resin is about 25%, the storage period at room temperature is more than 300 days, the curing condition is 175℃130min, and the tensile strength is 20.67MPa.
[0037] The advantages are good compatibility and long storage period;
[0038] The disadvantages are that the curing temperature is high, the curing speed is slow, and some physical and chemical properties of the cured product are quite different from those of two-component products.
[0039] 8 Imidazole-metal salt complex
[0040] It is a complex of imidazole and metal salts such as copper, nickel, and cobalt. It dissolves in liquid epoxy resin, has a storage period of more than 6 months at room temperature, and cures at 150-170℃ for 5-15 minutes. It is usually used as an accelerator for dicyandiamide to improve the bonding strength of its cured product.
[0041] The advantages are good compatibility, good solubility, easy use and operation, and strong bonding strength. At a specific temperature, as the degree of curing increases, the color continues to deepen, and finally reaches a dark brown-red, which is conducive to intuitively judging the degree of curing and process, such as for optical fiber crystal head packaging detection;
[0042] The disadvantages are that it is colored, which affects the electrical insulation performance, has a high curing temperature and is expensive.
[0043] 9 Imidazole derivatives
[0044] It can be synthesized from imidazole and NCO, imidazole and acid anhydride, imidazole and acid, imidazole and linear phenolic resin, etc.
[0045] The advantages are good compatibility and solubility;
[0046] The disadvantages are that it is expensive, has a relatively short shelf life, and needs to be stored at low temperatures. The performance of the solidified material varies with the type and formula, and the differences between them are large, so it is not universal.
[0047] For example, the reaction product of methylimidazole and pyromellitic acid or succinic acid, in epoxy resin, has a storage period of more than 2 months at 20°C, a curing condition of 150°C for 6-8 minutes, and the insulation grade of the cured product is H grade;
[0048] For example, the reaction product of 2-ethyl-4-methylimidazole, benzyl glycidyl ether 692 and cupric chloride has a storage period of more than 1 month at 25°C, a curing condition of 130-150°C for 5-10 minutes, and a glass transition temperature of the cured product of up to 208°C.
[0049] For example, the reaction product of imidazole and isocyanate is usually used as a curing accelerator for dicyandiamide. It is a urea derivative and is also the most commonly used latent curing agent. The isocyanate reactant of 2-methylimidazole contains a urea structure and has a stronger promoting effect on dicyandiamide than Monuron. After mixing with epoxy resin, the storage period at room temperature is more than 3 months, and the curing condition is 120℃ for 10min.
[0050] 10 Cyclic amides
[0051] Obtained by the reaction of aliphatic polyamines and acid anhydrides.
[0052] The advantages are low curing temperature and fast curing speed;
[0053] The disadvantages are short shelf life, average compatibility and solubility, and high price.
[0054] For example, the cyclic amide generated by the reaction of diethylenetriamine and phthalic anhydride is an amorphous yellow powder with a melting point of 96-113°C. When heated to 80°C, diethylenetriamine is produced to cause the epoxy resin to cure, and it itself is converted into o-phenylimide. The storage period at 25°C is greater than 1 month, and the curing condition is 150°C for 40-50s;
[0055] For example, the amide acid generated by the reaction of phthalic anhydride or 3-methylphthalic anhydride and NN-dimethylaminoethylamine is a crystalline latent curing agent. When heated, it generates imine, which produces secondary amine to cure epoxy resin. It is used as a curing accelerator for epoxy / polyester hybrid powder coatings (especially in formulations containing TGIC). The dosage is 0.5% to 1%, the stable period at room temperature is greater than 3 months, and the curing conditions are 150-160°C for 5-15 minutes. The comparative curing conditions without it are 180-200°C for 15-30 minutes.
[0056] Obviously, the existing latent curing agents on the market all have problems to varying degrees: those that are stable and have a long storage period are incompatible and insoluble with epoxy resins, require high-temperature curing, and the cured products are brittle; they are either expensive, such as the liquefied latent curing agent, which will also cause certain properties of the cured product to decline after the curing temperature drops; or they have a short storage period, affecting certain properties of the material, such as electrical insulation properties; they usually need to be used in conjunction with other curing agents, accelerators or catalysts, and are rarely used alone; they have high requirements for the formulation design of epoxy adhesives, high technical barriers, and are monopolized by foreign technology; they are difficult to compound and modify with other resins, have high shrinkage rates, high internal stresses, and poor dimensional accuracy and dimensional stability; latent curing agents are not compatible with oils and water, and most of them are oily systems, and are easily ineffective when exposed to water or moisture absorption; they cannot be secondary vulcanized by compounding with resins, and cannot be deeply cured and modified.
[0057] The latent curing agent that is really needed on the market is: compatible and miscible with epoxy resin to form a transparent and clear liquid, easy to operate, simple to use, evenly dispersed and easy to use; long service life and storage period at room temperature, no restrictions on operation, long storage period of single-group glue, usually required to be more than 6 months; cheap, can be used as main resin, as well as as latent curing agent and accelerator, everyone can afford it; can modify epoxy resin by itself to improve the comprehensive performance of the cured product; can be compounded and modified with a variety of other resins, additives, etc., and has a variety of curing methods and deep curing, and further improves material performance through secondary vulcanization modification; low shrinkage rate, curing temperature It has low temperature, short curing time, mild reaction, no internal stress concentration, high and low temperature impact resistance, both hard and tough, mechanical impact resistance without cracking, strong adhesion, strong shear resistance, and meets the technical requirements of structural material production process; it is used in composite material prepregs, potting materials, castings, etc., with good wettability, no bubbles, good dimensional stability after curing, and insulation, flame retardancy, thermal conductivity and other functions can be added; the raw materials for large-scale production are easy to obtain, the formula process is stable and reliable, the production process and products meet the requirements of safety, environmental protection, non-toxicity and non-hazardousness, the engineering is easy to achieve and is stable and reliable, the cured product complies with the regulations of the EU and ROHs, and does not contain banned substances. Summary of the invention
[0058] Purpose of the invention: The purpose of the present invention is to address the deficiencies in the prior art and to provide a latent curing agent with long-term storage stability and low curing shrinkage, as well as a preparation method and application thereof.
[0059] Technical solution: The first object of the present invention is to provide a method for preparing a latent curing agent, comprising the following steps:
[0060] S1: Add aldehyde, phenol and alkaline catalyst to the reaction vessel, slowly heat to 60-70°C under stirring, keep warm, the system becomes turbid after the materials start to react, use the reaction heat to raise the system temperature to 80-90°C, and control the temperature; after reacting for 1-3h, the material becomes transparent and clear again, and the first stage reaction is completed;
[0061] S2: Start the vacuum system, and gradually increase the vacuum degree from -0.01Mpa to -0.05Mpa, dehydration and polycondensation, control the temperature at 85-95℃, maintain vacuuming for 1-3h, and after the water output drops significantly, gradually increase the vacuum degree to -0.1Mpa under the condition of maintaining the temperature at 85-95℃, and maintain it under full vacuum for 1-2h; stop vacuuming, take samples to measure the drawing property, curing property and viscosity of the sample on the glass plate, and stop heating after reaching the specified indicators; qualified products are obtained as bulk B-stage phenolic resin;
[0062] S3: Cool down to 50-60℃, add copolymer, hyperbranched material and blocking material to the bulk B-stage phenolic resin system, control the temperature at 70-80℃ for 1-2 hours, the color of the material gradually decreases from light yellow to colorless, and the viscosity decreases to water state, indicating that the reaction is over and the synthesis is terminated; cool down to 50-55℃;
[0063] S4: Add compounding ingredients, anti-shrinkage agent, functional resin and initiator to the system, keep stirring at 50-55°C for 30-60 minutes, discharge and filter to obtain latent curing agent; its viscosity range at 25°C is 300-900cp.
[0064] Further, as a preferred embodiment, the phenol in step S1 is one or more of phenol, o-cresol, mixed phenols or cardanol;
[0065] The aldehyde is formaldehyde or furfural or a mixture of the two; the mol ratio of aldehyde / phenol is in the range of 1.1-1.6; the mol ratio of aldehyde / phenol is more preferably in the range of 1.3-1.5; the design of the added amount can avoid the problem of gelation in the subsequent modification and sealing stages caused by excessive phenol; and avoid the problem of excessive aldehyde residue, low molecular weight of bulk B-stage phenolic resin, increased by-products in the subsequent modification and sealing stages, slow curing speed, high curing temperature, and decreased comprehensive performance of the cured product caused by too little phenol.
[0066] Furthermore, as a preferred embodiment, the alkaline catalyst in step S1 is selected from a Lewis type weak base, including one or more of amine water, sodium carbonate, sodium acetate, zinc acetate, barium sulfate, magnesium oxide, ammonium acetate, triethylamine, TPP, triethylbenzylammonium chloride, butylammonium bromide, ammonium phosphate, and sodium hypophosphite; the addition amount of the alkaline catalyst is 1-5% of the total mass of phenol and aldehyde.
[0067] Further, as a preferred embodiment, the amount of the copolymer added in step S3 is 1%-10% of the total mass of the bulk B-stage phenolic resin; the addition of the copolymer can eliminate or reduce the residual free phenol and aldehyde while copolymerizing and modifying the bulk B-stage phenolic resin; it may include the following categories:
[0068] The first category is cyclized compounds containing oxygen / nitrogen elements: such as oxabutane OXT-1, cyclopropyl carbonate PC, epoxyhexacyclic ring, tetrahydrofuran, pyridine and its derivatives, caprolactone, melamine, triglycidyl isocyanurate TGIC, etc.
[0069] The second category is single-terminal tertiary amines or secondary amines containing long carbon chains: for example, monomethyl dodecyl secondary amine, monomethyl octadecyl secondary amine, dimethyl dodecyl tertiary amine, dimethyl octadecyl tertiary amine, etc.
[0070] The third category is saturated monohydroxy raw materials with long carbon chains: such as monomethyl ether polyethylene glycol MPEG (molecular weight 200, 400, 500), fatty alcohol polyoxyethylene ether AEO-7, fatty alcohol polyoxyethylene ether AEO-9;
[0071] The fourth category, hydroxyl monomers containing C=C (1 or 2 OH groups are allowed): (meth) hydroxyl acrylates, such as hydroxyethyl methacrylate HEMA, hydroxyethyl acrylate HEA, pentaerythritol triacrylate PETA, hydroxypropyl acrylate HPA, hydroxypropyl methacrylate HPMA; polyether monoacrylate monomers, such as monoacrylate polyethylene glycol APEG200 / 400, monoacrylate polypropylene glycol APPG200 / 400 / 600; oleic acid single-end polyether esters, such as monooleic acid polyethanol ether acid-PEG200 / 400 product; single OH monomers of hydroxyethyl acrylate HEA or hydroxyethyl methacrylate HEMA and caprolactone ring opening.
[0072] Further, as a preferred embodiment, the amount of the hyperbranched material added in step S3 is 1%-10% of the total mass of the bulk B-stage phenolic resin; the prepolymer of the hyperbranched material is a gradient / block synthesis product obtained by Michael addition reaction, ring opening reaction or click reaction of epoxy resin or epoxy reactive diluent and secondary amine, thiol, organic acid or acid anhydride; the specific methods for obtaining the hyperbranched material may include the following categories:
[0073] The first category, the product of diethylamine DEA or methylethanolamine MEA and tert-butyl vinyl carbonate V10, has a terminal dendritic structure, which is conducive to hyperbranching to reduce viscosity and reduce the water absorption of the solid;
[0074] The second type uses the product of tert-butyl glycidyl carbonate E10P and diethylamine DEA / methylethanolamine MEA, which has a tert-butyl carbon ester structure, good toughness and good insulation.
[0075] The third type uses the ester of glycidyl methacrylate GMA and acrylic acid, which has high reactivity and dicumyl peroxide DCP secondary vulcanization activity, and has both lipophilic and hydrophilic activities;
[0076] The fourth category is the graft product of sodium (methyl) allyl sulfonate MAS / AS and dicyandiamide, which has excellent permeability, surface activity and self-emulsifying water solubility;
[0077] The fifth category is the product of epoxy active diluent (such as epichlorohydrin ECH, benzyl glycidyl ether 692, butyl glycidyl ether 510, neopentyl glycol diglycidyl ether 678, ethylene glycol glycidyl ether 207, etc.) and dicyandiamide or diethylenetriamine (commonly known as solid Y or GY), which has excellent hydrophilicity, wettability and viscosity reduction and anti-settling properties for fillers, good color development and color fixation;
[0078] The sixth category, the product of (meth) acrylic acid and epichlorohydrin or the product of (meth) acrylic acid and epichlorohydrin and phthalic anhydride (both commonly known as polyester PEA, typical UV polyester resin), has excellent toughness, both hard and tough, high curing activity, and high activity of diisopropyl peroxide DCP secondary vulcanization;
[0079] The seventh category, the product of acetic acid / propionic acid / butyric acid and polyether epoxy reactive diluent, has long-term storage stability and excellent flexibility. It is the first choice for making elastic or low-temperature, high-stretchability, soft epoxy adhesive;
[0080] The eighth category, the products of polyester / long-chain fatty alcohol / polyether and acid anhydride (mainly succinic anhydride, tetrahydrophthalic anhydride THPA, phthalic anhydride PA, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride) and epoxy active diluent have excellent flexibility, stretchability, high curing activity, toughness, high and low temperature resistance, and chemical resistance.
[0081] The amount of the sealant added in step S3 is 1%-10% of the total mass of the bulk B-stage phenolic resin. The addition of the sealant seals the bulk B-stage phenolic resin and can eliminate or reduce the residual free phenol and aldehyde; there are the following categories:
[0082] The first category, (methyl)aziridine and its dispersible polymers: mainly (methyl)aziridine and adducts of (methyl)aziridine and acrylate monomers (trihydroxymethyl triacrylate TM, pentaerythritol triacrylate PETA) (commonly known as curing agent 110, 105 on the market); its nitrogen ring can be retained through OH reaction, and can also be opened and connected to the B-stage resin as needed, which is very effective in improving curing activity, promoting curing, and reducing curing temperature; but it is sensitive to pH acidic systems, which is not conducive to the storage stability of acidic systems, and is mainly used in alkaline formulas or water-based anionic formulas;
[0083] The second category is heterocyclic resins containing N / S / P: for example, melamine amino resin B325, prepolymers of triglycidyl isocyanurate TGIC and n-dodecyl mercaptan NDM mercaptan, prepolymers of triglycidyl isocyanurate TGIC and propionic acid / acrylic acid / tartaric acid / citric acid / succinic acid, prepolymers of hydroxyethyl acrylate HEA / hydroxyethyl methacrylate HEMA and tetrahydrophthalic anhydride THPA / phthalic anhydride PA / methyltetrahydrophthalic anhydride / methylhexahydrophthalic anhydride and triglycidyl isocyanurate TGIC, adducts of imidazole and hydroxy acrylate, urea derivatives of imidazole and isocyanate group NCO, and prepolymers of hydroxy (meth) acrylate and isocyanate group NCO. They are mainly used to improve curing activity, promote curing, reduce curing temperature, improve chemical resistance, improve adhesion and long-term storage stability, and improve the strength of prepregs;
[0084] The third category is thiols, which mainly include n-dodecyl mercaptan NDM, isooctyl 3-mercaptopropionate IOMP, pentaerythritol trimercaptopropionate PETMP405, and trimethylolpropane tris(3-mercaptopropionate) (TMPMP).
[0085] Further, as a preferred embodiment, the amount of the compounding material added in step S4 is 10%-60% of the total mass of the bulk B-stage phenolic resin; the compounding material is preferably the following:
[0086] The first category may preferably include ethanol, ethylene glycol, propylene glycol, diethylene glycol, benzyl alcohol, Nongru 601, PEG200, PPG200, PPG400, linear saturated polyester (such as XCP-500N, T1136), etc., so that the latent curing agent has low viscosity, long-term storage stability, participates in or cooperates with epoxy resin curing, and improves the comprehensive mechanical properties, adhesion and strength of the cured product;
[0087] The second category can preferably use oleic acid, sucrose / chitosan, epoxy soybean oil ESO, BX penetrant, sodium (methyl) allyl sulfonate, octadecyl acrylate, castor oil, linseed oil, tung oil, etc., so that the latent curing agent has the characteristics of penetration, infiltration, hydrophobicity, flexibility, and impact crack resistance;
[0088] The third category may preferably contain, for example, C=C acrylate monomers (tripropylene glycol diacrylate TP / trimethylolpropane triacrylate TM / hexylene glycol diacrylate HDDA / hydroxyethyl methacrylate HEMA / trimethylolpropane formal acrylate CTFA / tetrahydrofuran acrylate THFA / isoborneol acrylate IBOA)
[0089] / lauryl (meth)acrylate LOMA or LOA), octadecyl acrylate SMA, sodium (meth)allyl sulfonate MSA (SA), allyl monomer DMDAAC and diallylamine, etc.; in combination with isopropyl peroxide DCP high temperature initiator, deep curing can be carried out at 100-150°C, and isopropyl peroxide DCP secondary vulcanization is carried out according to the free radical reaction mechanism, so that it can be compounded with a variety of other resins (polyether with C=C, polyester PEA, unsaturated polyester UPR, modified epoxy EA, polyurethane PUA, amino acrylate resin, polyacrylate resin, alkyd resin) for deep / secondary vulcanization modification, further strengthening and toughening, and improving hydrophobicity, flexibility, self-catalytic and curing promotion, wettability, permeability, oil resistance, etc.
[0090] Further, as a preferred embodiment, the anti-shrinkage agent in step S4 is polystyrene; the amount of the anti-shrinkage agent added is 0.1%-5% of the total mass of the bulk B-stage phenolic resin; the anti-shrinkage agent polystyrene is dissolved in the bulk B-stage phenolic resin, so that the bulk B-stage phenolic resin latent curing agent has anti-expansion characteristics, anti-shrinkage or micro-expansion function, can inhibit or eliminate the shrinkage generated during the curing of epoxy resin, the shrinkage rate can be reduced to 0 or micro-expansion, and the water absorption rate can be reduced; in the manufacture of potting materials, casting materials, and composite material prepregs, this technology can ensure the dimensional accuracy and dimensional stability of the final product, and has great value and extraordinary significance;
[0091] The initiator is cumene peroxide DCP; the added amount of the initiator is 1%-5% of the total mass of the bulk B-stage phenolic resin.
[0092] Furthermore, as a preferred embodiment, the functional resin in step S4 includes a flame retardant resin and a water-based resin, wherein the flame retardant resin includes trishydroxymethylphosphine oxide THPO modified polyester or 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide DOPO open-ring polyester; the water-based resin includes water-based pure acrylic resin or PUD polyurethane; the added amount of the functional resin is 10%-50% of the total mass of the bulk B-stage phenolic resin; the addition of the functional resin can adjust the curing speed, curing temperature, flame retardancy, etc., so that the flame retardancy reaches UL-94V0 level.
[0093] Furthermore, as a preferred embodiment, a specific auxiliary agent is added, and the addition amount of the specific auxiliary agent is 5%-30% of the total mass of the bulk B-stage phenolic resin; the specific auxiliary agent may include the following components:
[0094] Functional powders: nano-spherical corundum powder, nano-spherical aluminum hydroxide, nano-barium sulfate, nano-ceramic powder (BN, SiC, zirconium oxide), etc. with special surface treatment;
[0095] Super wetting dispersant: such as TEG5010, to prevent powder precipitation and reduce viscosity; the dosage is 0.1%-0.5% of the mass of functional powder;
[0096] Defoamer: BYK341, to eliminate bubbles; the dosage is 0.1%-0.5% of the mass of the functional powder;
[0097] Silane coupling agent: KH560, the dosage is 1%-5% of the mass of the functional powder, to modify the surface of the functional powder and improve the bonding strength and mechanical strength.
[0098] The second purpose of the present invention is to protect the latent curing agent obtained by the above preparation method.
[0099] The third object of the present invention is to use the latent curing agent in the preparation of epoxy adhesive, water-based acrylic varnish, and fiber-reinforced composite material prepreg.
[0100] Beneficial effects:
[0101] (1) The present invention is the first to use an alkaline catalyst to synthesize a low-viscosity B-stage phenolic resin that can be stored stably for a long time alone or mixed with epoxy, and has excellent latent curing properties, a curing temperature of 80-150°C, a curing time of 5-30 minutes, an adjustable curing speed, and a room temperature storage stability period of more than 12 months for a single set of adhesives. It is easy to construct and has good curing properties.
[0102] (2) The present invention introduces blocking groups, branched or hyperbranched group copolymers, latent curing groups, etc. into the molecular structure of bulk B-stage phenolic resin for the first time, and controls its mol ratio, degree of polymerization, molecular weight, functionality, functional groups, etc., which not only eliminates the problem of phenol and aldehyde residues, but also makes the latent curing agent have a longer shelf life, is more stable, safer, more environmentally friendly, and non-toxic.
[0103] (3) The present invention is the first to use a variety of non-epoxy resins to compound and modify bulk B-stage phenolic resins, such as polyester, polyurethane, amino, polyacrylic acid / ester, UPR, silicone, etc., which can be stored for a long time and deeply modified, significantly improving the comprehensive performance of potting, casting, and composite materials;
[0104] (4) The present invention discovers for the first time that bulk B-stage phenolic resin has latent curing properties in certain water-based resins, is universal in oil and water, and has better performance of the cured product. For example, the cured product of bulk B-stage phenolic resin and water-based acrylic resin has the characteristics of resistance to water boiling, alcohol boiling, long-term immersion in chemicals, both hardness and toughness, high hardness, scratch resistance, impact resistance, scratch resistance, and high-grade insulation, while the cured product of water-based acrylic resin (with its supporting curing agent) without bulk B-stage phenolic resin absorbs moisture or becomes sticky when heated, is not resistant to high and low temperatures, becomes brittle when frozen, and cracks or powders when impacted;
[0105] (5) The scheme of the present invention realizes for the first time the use of C=C monomer to access the B-type phenolic resin, which has the characteristic of free radical high-temperature initiation curing, and can perform secondary vulcanization modification on the material, making the material both hard and tough, with more balanced performance, significantly improving the strength of the material, and also giving the material more characteristics and functions. Its application value is very important in military industry and major equipment, and is conducive to giving the material the characteristics of force / sound / heat / electricity / light / wave / magnetism; it is safer, environmentally friendly, odorless, non-toxic and rational, and can replace styrene-containing products on the market;
[0106] (6) The present invention introduces the anti-shrinkage agent polystyrene into the epoxy industry for the first time, and discovers for the first time that it has the characteristics of micro-expansion, negative shrinkage, and reduced moisture absorption rate in epoxy cured products, which completely solves the problems of always large shrinkage rate, large deformation, poor dimensional accuracy, poor dimensional stability, large internal stress, and high water absorption rate during epoxy resin curing;
[0107] (7) The present invention uses a compound type B-stage phenolic resin with a variety of alcohols, ethers, esters, additives, etc., and it is found that the latent curing property is better, the storage period is longer, and the curing promotion property is better.
[0108] (8) The product obtained by the scheme of the present invention can be widely used, complies with the EU safety and environmental protection ban requirements, and meets ROHs requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0109] Figure 1 This is the infrared spectrum of the latent curing agent product obtained in Example 1. DETAILED DESCRIPTION
[0110] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0111] The following four implementation cases are provided with reference formulas, application fields, and comprehensive conclusions of test data, including storage period, curing conditions, shrinkage, properties of cured products, and comparative results; the added materials in the following embodiments are calculated by mass fraction. Unless otherwise specified in the implementation examples, the added drugs are all commercially available, including:
[0112] Super wetting dispersant TEG5010 was purchased from Shanghai Tiger Polymer Co., Ltd.;
[0113] Defoamer BYK341 was purchased from BYK Company of Germany;
[0114] Urea-based imidazole was purchased from Ajinomoto Co., Ltd. of Japan and Azken Co., Ltd. of Germany;
[0115] OH-type amine propionidine diffraction polymer was purchased from Ningxia Jiafeng Chemical Co., Ltd.;
[0116] E10P is purchased from Momentive, an American company;
[0117] Glycidyl methacrylate GMA was purchased from Henan Xiayi County Yuhao Additive Co., Ltd.
[0118] Embodiment 1:
[0119] (1) Assemble synthesis, vacuum, heating, temperature control and other systems, check the safety and reliability of each subsystem, confirm that the raw materials are complete and of correct and stable quality, start the stirring, temperature control, heating and other systems, and start feeding;
[0120] (2) Add 1000 parts of formaldehyde, 100 parts of furfural, 950 parts of phenol, 180 parts of ammonia water, 20 parts of sodium carbonate, and 10 parts of barium sulfate according to the formula. Heat, stir, and control the temperature to slowly rise to 60-70°C, stop heating, and keep warm. At this time, the material begins to become turbid. Continue to control the temperature and use the reaction heat to slowly raise the temperature to 80-90°C. After about 1 hour, the material becomes transparent and clear again; indicating that the first stage of the reaction is complete; start the vacuum system for dehydration and condensation;
[0121] (3) Gradually increase the vacuum degree from -0.01Mpa to -0.05Mpa to prevent the vacuum degree from being too high, which may cause the material to boil or rush. Also avoid dehydration too violently and cooling too quickly, which may cause the material temperature to drop sharply, the reaction to stop, fail, or produce isomerization and side reactions. Improper vacuum operation may easily cause gelation, or the product may be opaque or unclear, or have no storage stability. Always control the temperature at 85-95°C and keep the vacuum for 1 hour. After the water outlet rate drops significantly, continue heating, keep the temperature at 85-95°C, and gradually increase the vacuum degree until it reaches -0.1Mpa, keep the temperature stable at 85-95°C, and keep it under full vacuum for 1-2 hours. Stop the vacuum, take a sample and test the wire drawing property on a glass plate. At room temperature, the wire drawing is extremely fine and does not break or crystallize, which is qualified. Test its low-temperature freezing crystallization at -20°C. It is qualified if it does not crystallize after low-temperature freezing for 10-30 minutes and still has good wire drawing property. After it reaches the specified indicators, stop heating and prepare to add the second step of synthetic raw materials;
[0122] (4) Cooling down to 50-60°C, accurately weighing according to the formula, adding copolymer material OXT-140 parts, fatty alcohol polyvinyl alcohol AEO-960 parts; hyperbranching material: OH-type aminopropane dismutase 40 parts, tert-butyl carbonate glycidyl ester E10P 120 parts; blocking material: urea imidazole 50 parts, controlling the temperature at 70-80°C for 1-2 hours, the color of the material gradually decreases from light yellow to nearly colorless, and the viscosity decreases to nearly water state, indicating that the reaction is completed, and the synthesis is terminated; Cooling down to 50-55°C;
[0123] (5) Add the following ingredients according to the formula: 800 parts of a mixture of ethanol and benzyl alcohol, 200 parts of PPG400, 100 parts of XCP-500N; 100 parts of an anti-shrinkage agent: polystyrene; 500 parts of a flame retardant functional resin: THPO modified polyester; and 0 parts of an initiator: DCP. Stirring is continued at 50-55° C. for 30 minutes. The material is discharged, filtered, and packaged to obtain a latent curing agent. The viscosity of the latent curing agent at 25° C. is 300-900 cp.
[0124] like Figure 1As shown, it is the infrared spectrum of the latent curing agent prepared in this embodiment, and the characteristic peaks of the infrared spectrum show that the absorption peak at 2900-3200 is the characteristic peak of -NHCO, the absorption peak at 1700-1800 is the characteristic peak of C=O, the absorption peak at 1400-1600 is the characteristic peak of benzene ring, and the absorption peak at 1000-1100 is the characteristic peak of Si-C. The peak position assignment proves that the synthetic material is successful.
[0125] The latent curing agent obtained in this embodiment is used to prepare a one-component F-class insulating, thermally conductive, and flame-retardant electrical appliance potting epoxy adhesive. The specific method is as follows: in the pull cylinder of a high-speed disperser, a measured amount of latent curing agent is added according to the formula, 60 parts of nano-spherical corundum powder, 30 parts of ATH, 5 parts of KH560 are added, and high-speed dispersion is performed at 500-1500rpm for 15-45min, the material temperature is controlled at 30-50°C, and 3 parts of defoaming agent BYK341 are added to obtain a functional latent curing agent with a viscosity range of 500-1500cp at 25 degrees; it is mixed with YD128 epoxy resin at 10-100% as needed to obtain a one-component epoxy adhesive electrical appliance potting adhesive, which is suitable for various medium and high voltage electrical appliances; the room temperature storage period is greater than 6 months, the curing temperature is 80-150°C, and the curing time is 5-30min. F-class insulation, withstand voltage>10Kv / mm, flame retardant UL-94V0 level, thermal conductivity 1.2-1.5w / mk.
[0126] Example 2: The method for preparing a latent curing agent in this example is basically the same as that in Example 1, except that phenol is added in this example: 1050 parts of phenol and 100 parts of cardanol; aldehyde: 1300 parts of formaldehyde; alkaline catalyst: 270 parts of ammonia water, 10 parts of sodium carbonate, and 5 parts of barium sulfate; copolymer: 40 parts of C12NH and 60 parts of AEO-9; hyperbranched material: 40 parts of melamine-type amino resin B325 and 120 parts of tert-butyl glycidyl carbonate E10P; sealing material: 50 parts of urea diamino ester; compounding material: 900 parts of a mixture of ethanol and benzyl alcohol, 200 parts of PEG200, 100 parts of T1136, and 50 parts of ESO; anti-shrinkage agent: 120 parts of polystyrene; flame retardant functional resin: 500 parts of DOPO open-ring polyester.
[0127] The latent curing agent obtained in this embodiment is used to prepare a single-component thermally conductive, flame-retardant, and insulating epoxy adhesive for new energy battery packaging. The specific method is as follows: 100g of latent curing agent, 30g of nano-spherical corundum powder, 25g of ATH, 15g of flame retardant DOPO modifier, about 80-100g of epoxy resin 128YD, about 3-7g of epoxy reactive diluent 692, stir evenly, and package. The storage period at room temperature is greater than 1 year, and the viscosity is stable at 600-1200cp. Curing conditions: 80-120℃15-30min. Flame retardant UL-94V0 level, thermal conductivity 1.5-2.0w / mk, F-level insulation, withstand voltage>10kv / mm, impact resistance and high and low temperature resistance without cracking, electrolyte resistance, and aging resistance.
[0128] Example 3: The method for preparing a latent curing agent in this example is basically the same as that in Example 1, except that phenol is added in this example: 1000 parts of o-cresol and 100 parts of cardanol; aldehyde: 1200 parts of formaldehyde and 100 parts of furfural; alkaline catalyst: 240 parts of ammonia water, 5 parts of sodium carbonate and 20 parts of barium sulfate; copolymer: 20 parts of OXT-1, 20 parts of C12MH and 60 parts of AEO-9; hyperbranched material: 40 parts of B325 and 120 parts of E10P; sealing material: 10 parts of urea imidazole and 10 parts of urea diamino ester; compounding material: 850 parts of a mixture of ethanol and benzyl alcohol, 100 parts of PPG400, 200 parts of XCP-500N and 50 parts of ESO; anti-shrinkage agent: 80 parts of polystyrene; flame retardant functional resin: 300 parts of THPO modified polyester and 200 parts of DOPO open-ring polyester.
[0129] The latent curing agent obtained in this embodiment is used to prepare a brilliant blue water-based acrylic varnish for cosmetic bottles, specifically as follows: 10-30g of latent curing agent, 100g of water-based acrylic resin varnish, 10-30 parts of polyurethane modified epoxy resin 168A, dispersed evenly to obtain a transparent and clear varnish, 1.0g of water-based transparent blue dye, 0.1g of brilliant blue, 50-100g of pure water are added, dispersed evenly to obtain a blue finished varnish; viscosity 50-200cp. Sprayed on a glass bottle for cosmetics, the thickness is 25-35 microns, first dried by hot air at 70-80℃ for 3-5min, and then cured at 130-150℃ for 10-15min. The adhesion is measured to be level 0, it is resistant to impact and collision without cracking or bursting, high and low temperature without cracking, high temperature and UV aging test without powdering, high temperature without stickiness, low temperature without hardness or brittleness, hardness 2-3H, scratch resistance, water boiling resistance, alcohol boiling resistance, chemical immersion resistance, no yellowing, bright blue color.
[0130] Comparative sample situation: The varnish without this product is used. According to its matching curing agent, blocked isocyanate or aziridine derivative, after curing, it will become sticky above 80℃ and soften significantly above 120℃. It will crack and burst when stressed at low temperature of -20℃. It is not scratch-resistant and will fall off after being soaked in alcohol for 5 minutes.
[0131] Example 4: The method for preparing a latent curing agent in this example is basically the same as that in Example 1, except that phenol is added in this example: 100 parts of phenol, 1000 parts of mixed phenol, and 100 parts of cardanol; aldehyde: 1450 parts of formaldehyde; alkaline catalyst: 270 parts of ammonia water, 20 parts of sodium carbonate, and 10 parts of barium sulfate; copolymer: 20 parts of OXT-1, 60 parts of AEO-9, 200 parts of AAPEG-200, and 100 parts of low-viscosity PEA polyester; hyperbranched material: 40 parts of E10P, 100 parts of GMA, 240 parts of NDM-69, and 20 parts of HEA-RMCO; sealing material: 40 parts of NN dimethyl diallylamine DMDAAC; compounding materials: 100 parts of C18 acrylate, 450 parts of a mixture of ethanol and benzyl alcohol, and XCP-500N 100 parts; anti-shrinkage agent: polystyrene 150 parts; flame retardant functional resin: THPO modified polyester 500 parts; water-based functional polyester: water-based pure acrylic resin 200 parts, PUD polyurethane 300 parts; initiator: DCP 150 parts.
[0132] In this embodiment, NDM-692 is synthesized from n-dodecyl mercaptan NDM and benzyl glycidyl ether;
[0133] HEA-RMCO is synthesized from hydroxyethyl acrylate and IPDI;
[0134] The fiber-reinforced composite material prepreg for UAV, automobile, or major equipment is prepared by using the latent curing agent obtained in this embodiment, as follows:
[0135] Latent curing agent (5-50% of functional materials such as electrical insulation, thermal conductivity, flame retardancy, magnetic conductivity, waveguide, color paste, etc. have been added according to the formula) 100g, epoxy resin 128YD 80-100g, electrical grade 0.1mm alkali-free glass fiber cloth 20-50g, and 300g / m 2 The alkali-free needle felt is about 30-60g, and the thinning agent is 100g of thinner / white oil / butanone. The prepreg made after being impregnated with glass fiber has a storage period of more than 6 months at room temperature. Curing conditions: 120-150℃ / 5-50 tons hydraulic four-column molding machine insulation for 3-5min. The strength of the cured product is close to that of epoxy board FR4, phenolic FX530, and unsaturated polyester SMC, and is 1.2-1.5 times higher than that of phenolic molding compound 4230 and unsaturated polyester molding compound BMC.
[0136] The above examples prove that the latent curing agent obtained by the scheme of the present invention has good performance after application.
[0137] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. A method for preparing a latent curing agent, characterized in that The steps include: S1: Add aldehyde, phenol and alkaline catalyst to the reaction vessel, slowly heat to 60-70°C under stirring, keep warm, the system becomes turbid after the materials start to react, use the reaction heat to raise the system temperature to 80-90°C, and control the temperature; after reacting for 1-3h, the material becomes transparent and clear again, and the first stage reaction is completed; S2: Start the vacuum system, and gradually increase the vacuum degree from -0.01Mpa to -0.05Mpa, dehydration and polycondensation, control the temperature at 85-95℃, maintain vacuuming for 1-3h, and after the water output drops significantly, gradually increase the vacuum degree to -0.1Mpa under the condition of maintaining the temperature at 85-95℃, and maintain it under full vacuum for 1-2h; stop vacuuming, take samples to measure the drawing property, curing property and viscosity of the sample on the glass plate, and stop heating after reaching the specified indicators; qualified products are obtained as bulk B-stage phenolic resin; S3: Cool down to 50-60℃, add copolymer, hyperbranched material and blocking material to the bulk B-stage phenolic resin system, control the temperature at 70-80℃ for 1-2 hours, the color of the material gradually decreases from light yellow to colorless, and the viscosity decreases to water state, indicating that the reaction is over and the synthesis is terminated; cool down to 50-55℃; S4: Add compounding ingredients, anti-shrinkage agent, functional resin and initiator to the system, keep stirring at 50-55°C for 30-60 minutes, discharge and filter to obtain latent curing agent; its viscosity range at 25°C is 300-900cp.
2. The method for preparing a latent curing agent according to claim 1, characterized in that: The phenol in step S1 is one or a combination of phenol, o-cresol, mixed phenols or cardanol; The aldehyde is formaldehyde or furfural or a mixture of the two; The molar ratio of aldehyde to phenol is in the range of 1.1-1.
6.
3. The method for preparing a latent curing agent according to claim 1, characterized in that: The alkaline catalyst in step S1 is selected from Lewis type weak base, including one or more of amine water, sodium carbonate, sodium acetate, zinc acetate, barium sulfate, magnesium oxide, ammonium acetate, triethylamine, triethylbenzylammonium chloride, butylammonium bromide, ammonium phosphate, sodium hypophosphite; the addition amount of the alkaline catalyst is 1-5% of the total mass of phenol and aldehyde.
4. The method for preparing a latent curing agent according to claim 1, characterized in that: The copolymer in step S3 is one of oxygen / nitrogen cyclized products, single-terminal tertiary amines or secondary amines containing long carbon chains, saturated monohydroxy compounds containing long carbon chains, and hydroxyl monomers containing C=C; the amount of the copolymer added is 1%-10% of the total mass of the bulk B-stage phenolic resin; The prepolymer of the hyperbranched material in step S3 is a gradient / block synthesis product obtained by Michael addition reaction, ring opening reaction or click reaction of epoxy resin or epoxy reactive diluent with secondary amine, thiol, organic acid or acid anhydride; the addition amount of the hyperbranched material is 1%-10% of the total mass of bulk B-stage phenolic resin; In step S3, the sealing material is one or more of (methyl)aziridine and its disproportionate polymer, N / S / P-containing heterocyclic polymer or thiol compound; the addition amount of the sealing material is 1%-10% of the total mass of the bulk B-stage phenolic resin.
5. The method for preparing a latent curing agent according to claim 1, characterized in that: The compounding material in step S4 is one or more compounds of alcohol, polyether, polyester or diluent; the addition amount of the compounding material is 10%-60% of the total mass of the bulk B-stage phenolic resin. The alcohol is one or more of ethanol, ethylene glycol, propylene glycol, diethylene glycol, benzyl alcohol, Nongru 601, PEG200, PPG200, PPG400 or linear saturated polyester; The polyester is one or more of UPR unsaturated polyester, alkyd resin, polyurethane acrylate, acrylic melamine resin or polyacrylic resin.
6. The method for preparing a latent curing agent according to claim 1, characterized in that: The anti-shrinkage agent in step S4 is polystyrene; the amount of the anti-shrinkage agent added is 0.1%-5% of the total mass of the bulk B-stage phenolic resin; The initiator is cumene peroxide; the added amount of the initiator is 1%-5% of the total mass of the bulk B-stage phenolic resin.
7. The method for preparing a latent curing agent according to claim 1, characterized in that: The functional resin in step S4 includes a flame retardant resin and a water-based resin, wherein the flame retardant resin includes THPO modified polyester or 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ring-opening polyester; the water-based resin includes a water-based pure acrylic resin or PUD polyurethane; and the added amount of the functional resin is 10%-50% of the total mass of the bulk B-stage phenolic resin.
8. The method for preparing a latent curing agent according to claim 1, characterized in that: Specific additives are also added; the specific additives include one or more of functional powders, wetting and dispersing agents, defoaming agents, and silane coupling agents, as follows: Functional powder: one or more of nano-spherical corundum powder, nano-spherical aluminum hydroxide, nano-barium sulfate, and nano-ceramic powder (BN, SiC, zirconium oxide); the added amount of the functional powder is 5%-30% of the total mass of the bulk B-stage phenolic resin; Wetting dispersant: TEG5010; Defoamer: BYK341; Silane coupling agent: KH560, the dosage is 1%-5% of the mass of the functional powder to achieve surface modification of the functional powder.
9. A latent curing agent obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the latent curing agent of claim 9 in the preparation of epoxy adhesive, water-based acrylic varnish, and fiber-reinforced composite material prepreg.
Citation Information
Patent Citations
One component epoxy resin composition
CN103228696A
Phenalkamine epoxy latent curing agent and preparation method and application thereof
CN110746581A
Latent curing agent and one-pack curable epoxide composition containing the same
JP2019099754A