Aerogel fireproof heat-insulating coating and preparation method thereof
Porous aerogel particles are prepared through suspension dispersion technology and atmospheric pressure and high-temperature drying method. Combined with high-temperature colloidal solution, the problem of aging and cracking of existing aerogel coatings at high temperatures is solved, and smoke-free, non-toxic, and high fire-proof. High-insulated aerogel fire-resistant and thermal insulation coating, suitable for high-temperature protection applications such as lithium battery modules in electric vehicles.
Patent Information
- Application Number
- CN202310662026.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The existing aerogel thermal insulation coatings are prone to aging and cracking in high temperature environments, producing toxic gases and dust. The traditional preparation methods are time-consuming and costly, making it difficult to meet the high-temperature protection needs of thermal runaway battery modules for electric vehicles.
The mixed solution of the silicone precursor and hydrophobic silicone compound is prepared by suspension dispersion technology, and the surface stable aerogel wet glue particles are formed through hydrolysis and condensation reactions, and then dried with a porous structure is obtained by drying the airflow using normal pressure and high temperature. Gel particles and evenly disperse them in a high-temperature resistant colloid solution to form smoke-free, non-toxic, high-fire-proof, and high-heat-insulated aerogel fire-resistant and thermal insulation coating.
Achieve smoke-free, non-toxic, high fire-proof and high heat insulation performance under high temperature flames, simplify the preparation process, reduce costs, and is suitable for electric vehicle lithium battery modules and other high-temperature protection applications, improving safety and production efficiency.
Smart Images

Figure CN119081452A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high temperature resistant aerogel fireproof and heat insulating coating, and in particular to an aerogel composite coating having the characteristics of being smokeless, highly heat insulating and highly fireproof, and a preparation method thereof. Background Art
[0002] As is known to all, aerogel is a porous material with a three-dimensional network structure, a porosity higher than 80% (even higher than 95%), and a low density (about 0.005 to 0.2 g / cm 3 ), high specific surface area (500 to 2000m 2 / g), low thermal conductivity (k = 15 to 40 mW / mk) and low dielectric properties (D k =1.3 to 2.0), low dielectric loss (D f<0.003 or less) and other characteristics, making aerogel or its composite materials have excellent characteristics such as high thermal insulation, high fire resistance, and low dielectric. Because aerogel or its composite materials have a large amount of porosity and extremely low density, they have a very high value in applications such as high thermal insulation, high fire resistance, low signal transmission resistance, and high electrical shock resistance. Therefore, they have a strategic position in energy-saving and carbon-reducing applications in various industries in the future, such as high-temperature fire protection, high-energy-consuming production equipment or transmission pipelines. Although general organic foam materials currently have good thermal insulation effects at room temperature or below 120°C, the preparation process of these organic foam materials has caused environmental pollution, and the products are used in environments with temperatures above 120°C. They will quickly crack and lose their thermal insulation effects. In environments with temperatures of 120°C or higher, organic foam materials will have their application limitations. In addition, the current general high-temperature fireproof and thermal insulation coatings are mainly thermal expansion organic coatings. The above products are products made by mixing organic coatings with thermal expansion metal oxides. Thermally expandable metal oxides use the thermal expansion characteristics of metal oxides or carbon to achieve fireproof and heat-insulating effects under high-temperature flames. However, in high-temperature applications of the above products, organic coatings such as epoxy resins will carbonize and crack under high-temperature flames above 500°C to form toxic dioxins and other substances, and the metal oxide layer after thermal expansion will also crack and fall off under high-temperature flames, resulting in the disappearance of protective properties. Therefore, the above thermally expandable metal oxide organic fire retardant coatings cannot achieve long-term fireproof and heat-insulating effects under 800 to 1200°C environments. Therefore, when the lithium battery module in the electric vehicle instantly generates 800 to 1200°C high-temperature flames and explosion impacts under thermal runaway, the fireproof and heat source barrier properties of the thermally expandable metal oxide organic fire retardant coatings are not superior. Therefore, in the future, for the thermal runaway protection of lithium battery modules in motor vehicles, it is necessary to develop better fire retardant coatings to replace traditional thermally expandable metal oxide organic fire retardant coatings. Aerogel is a material with a nano-porous inorganic silica three-dimensional network structure. Aerogel or its related composite materials can replace traditional organic foaming materials or thermal expansion metal oxides or thermal expansion carbons and add organic fire retardant coatings to form a novel fireproof and heat-insulating product. According to basic material theory, a large amount of nano-porosity inside the aerogel material will significantly reduce the transmission of heat energy. Therefore, the higher the porosity of the material structure, the better its thermal insulation properties. On the other hand. Inorganic silica aerogel materials are highly fireproof materials that are resistant to high temperatures and do not burn or spread. Therefore, nano-porous silica aerogel materials can prevent thermal runaway and also have high fireproof properties. In the future, thermal runaway of lithium battery modules in electric vehicles or safety protection of new generation high-temperature molten batteries are necessary.In this regard, the present invention team hopes to develop a kind of aerogel fireproof and heat-insulating coating with high fireproof and heat-insulating properties and smokeless and non-toxicity for the safety protection needs of thermal runaway of lithium battery modules of electric vehicles or new generation of high-temperature molten batteries in aerogel-related products. It is expected that the prevention products that effectively solve the safety hazards of thermal runaway of lithium battery modules of electric vehicles or new generation of high-temperature molten batteries are the goals that need to be worked hard on. At present, the patent technologies of various thermal insulation coatings or high-temperature fireproof coatings disclosed by international published patents still have the above doubts, especially at high temperatures above 600°C. The aerogels used in the currently disclosed technologies are added with organic coatings (for example: epoxy resin, polyamide ester, polyacrylate, etc.). The highest heat-resistant temperature of these products is about 200°C. When heated in a high temperature environment for a long time, the relevant organic coatings will gradually carbonize and crack, and will cause the organic coatings to crack and produce toxic gases. The shortcomings of the above fireproof and heat-insulating coatings are still an important and must-be-solved problem for thermal runaway of lithium battery modules of electric vehicles.
[0003] The traditional method for preparing aerogels is the sol-gel synthesis method, which mainly involves mixing precursors such as alkoxysilane, methyl orthosilicate or water glass with a large amount of organic mixed solvents, and then adding an acid catalyst to perform a hydrolysis reaction. After the hydrolysis reaction has been going on for a certain period of time, an alkali catalyst is added to perform a condensation reaction. During the condensation reaction, a sol is gradually formed, and the molecules in the sol continue to react and bond, gradually forming a semi-solid polymer gel. Then, after a period of aging, the gel forms a three-dimensional network structure with a stable structure. Finally, a hydrophobic solvent such as n-butanol, n-hexanol, n-hexane or cyclohexane is used for solvent replacement, and then the solvent in the aerogel structure is extracted and dried using supercritical drying technology. In addition to consuming a large amount of expensive organic solvents and supercritical equipment, the traditional process technology also requires the use of hydrophobic solvents for long-term solvent replacement, so the cost of preparing aerogels is high and time-consuming.
[0004] On the other hand, the preparation method of hydrophobic aerogel also adopts the sol-gel synthesis method, which mainly involves mixing methyl alkoxy silicon precursors such as methyltrimethoxysilane (MTMS) or methyltriethoxysilane (MTES) with organic solvents, and then adding an alkali catalyst to perform a hydrolysis reaction. After a certain period of hydrolysis reaction, a condensation reaction is performed, and a sol is gradually formed during the condensation reaction. The molecules in the sol continue to react and bond, gradually forming a semi-solid polymer gel. After a period of aging, solvent replacement is performed for two to three days using solvents such as isopropanol, acetone, n-hexane or cyclohexane, so that the hydrophobic gel forms a stable three-dimensional network structure. Finally, the solvent in the aerogel structure is dried using atmospheric pressure drying technology to obtain a porous dry aerogel block. The process of preparing hydrophobic aerogels also requires the consumption of a large amount of expensive organic solvents, and a long period of solvent replacement with alcohols or alkanes is required, so the preparation is time-consuming and costly.
[0005] Since the process technology used in the above-mentioned aerogel preparation method requires the use of a large amount of hydrophobic solvents; such as organic solvents such as alkanes, multiple solvent replacements are carried out for two to three days, and then supercritical drying technology or normal pressure high temperature drying technology is used to prevent the aerogel structure from shrinking or cracking due to the surface tension of water molecules during the normal pressure drying process. "Supercritical drying" means that water and organic solvents are in a supercritical state under high temperature and high pressure, so that the organic solvent and water have gas-liquid mixing properties at the same time, and the solvent is directly vaporized and dried under the supercritical state. Therefore, the remaining solvent in the network structure can be removed under supercritical conditions without causing the wet glue to shrink. However, the use of multiple hydrophobic solvent replacement technology and supercritical drying technology in the relevant process is quite time-consuming and costly, which is not conducive to the competitiveness of aerogel mass production and future applications. The above-mentioned hydrophobic modification uses a multi-stage solvent replacement technology at normal temperature and pressure, but this modification technology must be carried out for more than 24 hours, and the process takes too long and is not cost-effective.
[0006] The Chinese invention patent publication number CN106479297A states that "an aerogel water-based intumescent fire-retardant coating and its preparation method" is related to providing an aerogel water-based intumescent fire-retardant coating and its preparation method. The fire-retardant coating comprises the following components by weight: 10-50 parts of emulsion, 30-70 parts of intumescent flame retardant, 0.1-10 parts of first neutralizer, 1-10 parts of plasticizer, 2-20 parts of flux, 0.1-10 parts of first dispersant, 0.1-10 parts of first stabilizer, 5-20 parts of aerogel slurry and 5-60 parts of pigments and fillers; wherein the emulsion is a mixture of core-shell silicone modified acrylate emulsion and pure acrylic emulsion. The above-mentioned aerogel water-based intumescent fire-retardant coating uses organosilicon-modified acrylate emulsion and pure acrylic emulsion as the emulsion system, wherein the organosilicon-modified acrylate emulsion has both excellent physical and chemical properties such as weather resistance, stain resistance, good air permeability and high hydrophobicity, and has excellent expansion effect and fire retardant performance. The pure acrylic emulsion can improve the mechanical properties such as adhesion of the fire retardant coating, ensure the effective performance of the fire retardant performance of the carbonized coating, have good fire retardant performance, stable performance, and easy production. Among them, the emulsion is a mixture of core-shell organosilicon-modified acrylate emulsion and pure acrylic emulsion. The aerogel water-based intumescent fire retardant coating is characterized in that the core-shell organosilicon-modified acrylate emulsion is prepared by a silicone-acrylic emulsion polymerization reaction of a mixture of vinyltriethoxysilane and styrene and a mixture of butyl acrylate and methyl methacrylate.
[0007] The "aerogel water-based thermal insulation fire retardant coating and its preparation method" described in the Chinese invention patent publication number CN107267006A mainly relates to an aerogel water-based thermal insulation fire retardant coating and its preparation method, which is mainly composed of aerogel powder, water-based resin and flame retardant. The aerogel powder is composed of an internal hydrophobic layer and a surface hydrophilic layer, and the thickness of the surface hydrophilic layer is 0.1 to 100 μm. The preparation method of an aerogel water-based thermal insulation fire retardant coating disclosed in the invention comprises the following steps: (1) aerogel powder modification; 2) mixing the aerogel powder of step (1) with the water-based resin and the flame retardant, stirring or ball milling. The present invention adds aerogel powder to the water-based coating system to ensure that the nanoporous structure of the aerogel is not destroyed, give full play to the thermal insulation and heat preservation performance of the aerogel, and improve the fire resistance limit of the coating. The aerogel water-based thermal insulation fire retardant coating provided by the invention can be applied to steel structures, wood, concrete structures, tunnels, cables and other fields. The preparation process is simple, practical, excellent in performance, low in price, and suitable for industrial production. The invention is characterized in that it is mainly composed of aerogel powder, water-based resin and flame retardant, the aerogel powder is composed of an internal hydrophobic layer and a surface hydrophilic layer, and the thickness of the surface hydrophilic layer is 0.1 to 100 μm.
[0008] The "SiO2 aerogel thermal insulation coating and its preparation method" described in Chinese invention patent publication number CN107858050A relates to a SiO2 aerogel thermal insulation coating, which includes the following components by weight: 50-100 parts of base paint, 5-20 parts of SiO2 aerogel, 2-10 parts of hollow glass microspheres with titanium dioxide coating, 0.05-0.2 parts of dimethylhydroxy silicone oil, 0.05-0.2 parts of hexadecyltrimethylammonium bromide, 10-25 parts of curing agent and 2-10 parts of additives; the additives include dispersants, wetting agents, defoaming agents, and leveling agents. In the SiO2 aerogel thermal insulation coating, SiO2 aerogel is combined with hollow glass microspheres with a coating to synergistically improve the thermal insulation effect; through the method provided by the present invention, a thermal insulation coating with good homogeneity can be obtained, which is characterized in that it includes the following components in parts by weight: 50-100 parts of base paint, 5-20 parts of SiO2 aerogel, 2-10 parts of hollow glass microspheres with a titanium dioxide coating, 0.05-0.2 parts of dimethylhydroxy silicone oil, 0.05-0.2 parts of hexadecyltrimethylammonium bromide, 10-25 parts of a curing agent and 2-10 parts of an auxiliary agent; the auxiliary agent includes a dispersant, a wetting agent, a defoaming agent, and a leveling agent.
[0009] The "SiO2 aerogel thermal insulation coating and its preparation method" described in Chinese invention patent publication number CN107858050A involves wetting a fiber material including at least one of inorganic fiber and organic fiber; stacking the wetted fiber material and the spacer in a winding structure or in a flat form; filling the fiber material into a container; preparing a gel-fiber composite by injecting a precursor into the container and gelling the precursor while removing residual bubbles under vacuum; taking out the aerogel-fiber composite from the container and removing the spacer; using a solvent to replace and organically surface modify the gel-fiber composite, and then drying the organically surface modified gel-fiber composite by atmospheric pressure drying or supercritical drying.
[0010] The "method for preparing a reinforced silica aerogel super thermal insulation coating" described in Chinese invention patent publication number CN107858050A relates to a method for preparing a reinforced silica aerogel super thermal insulation coating, comprising the following steps: S1, in a mixed solution of 10 parts of ethanol and 2-10 parts of pure water, 1 part of ethyl orthosilicate is added dropwise, and then 0.2-0.5 parts of titanium tetrachloride are added dropwise, and a solution is obtained by stirring; S2, a mixed solution of ammonia and ethanol is added dropwise to obtain a sol; S3, the sol is injection molded, and aged to obtain a wet gel; S4, the wet gel is impregnated with a n-hexane solution of trimethylchlorosilane to perform hydrophobic modification on the wet gel; S5, the wet gel is crushed after drying at normal pressure to obtain a gel powder; S6, 100 parts of gel powder F are added to 10-50 parts of the coating, 2-6 parts of a dispersant, 2-6 parts of a defoamer, and 2-6 parts of a leveling agent are added, and the finished coating is obtained by high-speed stirring. The product prepared by the invention has the advantages of high strength and good thermal insulation, and the finished product quality and construction quality of the aerogel coating are good, and it is suitable for both water-based and oil-based coatings, and is suitable for large-scale promotion. The coating is a water-based coating, and the water-based coating is specifically a water-based polyurethane, a water-based epoxy resin or a water-based alcohol ester resin.
[0011] The "aerogel invisible fire retardant coating" described in the Chinese invention patent publication number CN108587264A is a kind of aerogel invisible fire retardant coating, which includes two stages: hydrophobic enhancement modification of silicon aerogel and preparation of coating. The raw materials used in the hydrophobic enhancement modification stage of silicon aerogel are: water glass, carbon nanofiber, anhydrous ethanol, acetone, n-butanol, hexadecyltrimethylammonium bromide, trimethylchlorosilane, styrene exchange resin, ammonia water, kerosene; the raw materials used in the preparation stage of coating are hydrophobic enhancement silicon aerogel modified by the above steps, sodium sulfite, talcum powder, sodium chloride, carbon-forming catalyst, carbon-forming agent, foaming agent, and antioxidant. Pentaerythritol carbon-forming agent is added to the coating to expand the carbon source in the carbon layer to enhance the barrier function of aerogel.
[0012] The Chinese invention patent publication number CN112745698A describes a method for preparing a modified aerogel, a modified aerogel, a thermal insulation coating and its application, wherein the method for preparing the modified aerogel comprises the following steps: adding a certain amount of modifier to a certain amount of water-alcohol solution, adding a certain amount of silane coupling agent, stirring at a certain temperature for a certain time, adding a certain amount of aerogel, continuing to stir for a certain time, washing, drying, and obtaining the modified aerogel; wherein the modifier comprises one or more of glass microspheres, SiO2, fiber alumina, and fiber silica. The modified aerogel prepared by the method of the invention can be uniformly dispersed in an aqueous solvent system, and its microstructure will not be destroyed. At the same time, it has excellent mechanical strength and can be used as a filler to meet the requirements of coating hardness and adhesion. The coating is prepared by mixing modified aerogel into 55 ml of silicone resin emulsion, adding polyether dispersant and silicone defoamer, stirring for 30 minutes, and then adding hydroxypropyl cellulose after uniform dispersion, and continuing to stir until uniform; finally, adding chitosan and mica powder, stirring evenly, and obtaining the thermal insulation coating.
[0013] The "Nano-silicon aerogel thermal insulation coating and its preparation method" described in the Chinese invention patent publication number CN113831765A is related to a nano-silicon aerogel thermal insulation coating and its preparation method, which mainly uses a drum ball mill to finely grind the prepared silicon aerogel dispersion to create a nano-silicon aerogel dispersion, and then the nano-silicon aerogel dispersion is further fully stirred with a specially selected composite solid filler to prepare the original nano-silicon aerogel thermal insulation coating, which has the functions of convenient coating, easy adhesion, high hardness, weather resistance, and good heat preservation and heat insulation effects. The water-based coating is at least one of the water-based acrylic, acrylic emulsion, styrene-acrylate emulsion and acetic acid acrylate emulsion.
[0014] The "aerogel thick thermal insulation textured coating" described in Chinese invention patent publication number CN113881300A relates to an aerogel thick thermal insulation textured coating, which includes the following components by weight: 6 parts of silica aerogel, 0.45 parts of wetting agent, 0.5 parts of dispersant, 13 parts of deionized water, 0.35 parts of defoaming agent, 72 parts of water-based acrylic resin, and 7.7 parts of film-forming aid. The invention uses silica aerogel as a functional filler, and its thermal insulation performance is far superior to titanium dioxide, glass beads and far-infrared ceramic powder coatings, because the nanopores and unique three-dimensional network structure of silica aerogel destroy the heat conduction path of the matrix, and its unique nanostructure pores limit the free flow of air molecules, inhibit the convection conduction of air, and make it have an extremely low thermal conductivity. Therefore, using silica aerogel as a filler for the coating can maximize the thermal insulation performance of the coating.
[0015] The "aerogel fireproof and heat-insulating coating and its preparation method" described in the Chinese invention patent announcement number CN108997911B is related to an aerogel fireproof and heat-insulating coating and its preparation method. By adding hydrophilically modified aerogel powder and ceramic powder, and then adding additives and fillers according to different formula proportions, a coating with fireproof and heat-insulating properties is prepared. The coating is prepared by utilizing the performance characteristics of the three-dimensional network structure of aerogel, which solves the shortcomings of existing coatings that are only fireproof but not heat-insulating, and makes it have heat-insulating properties. At the same time, nano-ceramic powder is added to the coating. The nano-ceramic powder in the coating is ceramicized after heating, forming a layer of expanded ceramic film on the surface of the substrate. There is an air layer between the film and the substrate, which isolates the flame from contacting the surface of the vehicle metal material product, and relies on the low thermal conductivity of the aerogel in the coating to prevent heat from being transferred to the metal surface. This fireproof and heat-insulating synergistic effect can ensure that the metal parts in the vehicle have a good barrier effect against heat and flames regardless of normal use or in extreme fire accidents. It is characterized in that the resin emulsion includes one or more of water-based acrylic emulsion, water-based polyurethane emulsion, and water-based epoxy resin emulsion.
[0016] The "aerogel thermal insulation coating and its preparation method" described in the Chinese invention patent announcement number CN112226137B relates to an aerogel thermal insulation coating and its preparation method. It is prepared according to the following components in parts by weight: 40wt%-60wt% aldehyde-ketone resin, 20-40% activated carbon, 10wt%-15wt% nano-silicon dioxide, 5wt%-10wt% aerogel, and 2wt% dispersant. The aerogel thermal insulation coating prepared by the invention has good thermal insulation and air purification effects, and is particularly suitable for thermal insulation and anti-corrosion treatment of inner surfaces of vehicles. It is characterized in that the aerogel thermal insulation coating on the inner metal surface of the vehicle, the aldehyde-ketone resin is at least one of KR-120 aldehyde-ketone resin and KR-80F aldehyde-ketone resin.
[0017] The "A high-temperature aerogel thermal insulation and fire-retardant coating and its preparation method" described in the Chinese invention patent announcement number CN112500770B, which involves a high-temperature aerogel thermal insulation and fire-retardant coating, is made of the following raw materials in parts by weight: 10-20 parts of aerogel powder, 35-46 parts of organic binder, 15-20 parts of inorganic binder, 12-15 parts of filler, 2-3 parts of toughening agent, 10-15 parts of flame retardant, and 50-60 parts of deionized water. The invention also discloses a preparation method of the high-temperature aerogel thermal insulation and fire-retardant coating. The high-temperature aerogel thermal insulation and fire-retardant coating provided by the invention has good thermal insulation and fire-retardant properties. The organic binder is one or more of unsaturated polyester emulsion, PVC emulsion, epoxy resin emulsion, acrylic resin emulsion, silicone resin emulsion, and alkyd resin emulsion, and the inorganic binder is one or more of cement mortar, gypsum powder, and silicate.
[0018] The "aerogel coating and aerogel coating obtained from aerogel coating" described in the Chinese invention patent announcement number CN113292894B is an aerogel coating, which includes: a film-forming emulsion; SiC-SiO2 composite aerogel; a dispersant; a wetting agent; a defoaming agent; rutile titanium dioxide nanoparticles; hollow glass microspheres; a thickener; a film-forming aid; ammonia water; and a balance of deionized water. In addition, the invention also discloses an aerogel coating obtained from aerogel coating. The aerogel improves the surface energy and the connection area of the secondary particles, thereby improving the mechanical properties and thermal insulation properties. The aerogel coating, wherein the film-forming emulsion is selected from a flexible acrylic emulsion, and the solid content is 50-60%.
[0019] The Chinese invention patent announcement number CN114479602B states that "a repair coating for aerogel surface defects and its preparation method and application" relates to a repair coating for aerogel surface defects and its preparation method and application, which is applied to the surface to be repaired of phenolic aerogel materials. The mass fraction of each component in the repair coating is: 10-70% phenolic resin solution, 10-30% aerogel, 10-30% nano inorganic oxide and 10-30% inorganic fiber. The repair coating provided by the present invention can be used for defect repair of phenolic aerogel materials, is easy to operate, has excellent compatibility with phenolic aerogel materials, and has excellent maintainability and ablation resistance.
[0020] The "method for preparing nano-silicon aerogel thermal insulation coating" described in Taiwan Invention Patent Publication No. TWI770931 is a method for preparing a nano-silicon aerogel dispersion, which is carried out through the following steps: (1) dissolving triton x-100 in a water solution to form a first solution, wherein the amount of triton x-100 is between 0.1 and 1.2 grams and the amount of the water solution is between 15 and 30 grams; (2) adding a silicon aerogel to the first solution, and continuously mechanically stirring to obtain a silicon aerogel slurry; (3) mixing sodium dodecylbenzene sulfonate, sodium dodecyl polyoxyethylene ether sulfate, hydroxy cellulose thickener and water solution, and continuously stirring to obtain a second solution, wherein the amount of sodium dodecylbenzene sulfonate is between 0.3 and 1.2 grams, the amount of sodium dodecyl polyoxyethylene ether sulfate is between 0.05 and 1 gram, the amount of hydroxy cellulose thickener is between 0.1 and 0.3 grams, and the amount of the water solution is between 15 and 30 grams. 15-30 grams; (4). Add an aqueous acrylic into the second solution and stir it continuously to obtain a third solution, the ratio of which is 30-50 grams; (5). Add the third solution into the silica aerogel slurry and stir it continuously to obtain a silica aerogel dispersion; (6). Grind the silica aerogel dispersion on a drum ball mill to produce a grinding liquid, the grinding balls are zirconium beads with a size of 2 mm and a ball filling rate of 1:1 to the volume of silica aerogel; (7). Finally, filter the grinding liquid containing the grinding balls with a filter screen to obtain a nano silica aerogel dispersion.
[0021] The applicant's invention patent publication No. TWI793839 in Taiwan, China, describes "low dielectric gel powder, low dielectric gel suspension, composite film and preparation method thereof", which relates to the preparation and application of a high-purity aerogel powder with low dielectric constant and low dielectric loss. The preparation is completed by the following steps: (1) mixing and hydrolysis, (2) condensation dispersion, and (3) drying. This process improves the sol-gel technology and does not require the addition of a large amount of organic solvents and surfactants during the reaction. Therefore, this process does not require solvent replacement and deionized water rinsing to prepare high-purity aerogel powder materials with low dielectric loss. The density of low dielectric gel is between about 0.05 and 0.12 g / cm 3 Since there are no other impurities in the process, the thermal conductivity and dielectric loss are significantly reduced. The thermal conductivity coefficient of the aerogel powder is about 0.013 to 0.016 W / mk, the dielectric constant of the aerogel powder is about 1.28 to 1.8, and the dielectric loss is 0.0012 to 0.0036. In addition, the dry powder or semi-dry powder is further dispersed with an organic solvent to form an aerogel suspension containing an organic solvent. The preparation can be completed by the following steps: (4) impregnation with a specific organic solvent, (5) three-roller refinement, and (5) uniform mixing of a specific polymer concentrated solution. The suspension formed by impregnation with a specific organic solvent can be adjusted according to the solvent of the specific polymer concentrated solution. The mixed specific polymer concentrated solution forms a uniform and porous low-dielectric composite film after drying, especially a low-dielectric polymer composite film with a thickness of less than 300 μm, which can be used as a dielectric layer in a high-frequency circuit, an insulating layer in a semiconductor device, or a microwave circuit in a communication integrated circuit.
[0022] In addition, the applicant's invention patent publication No. TWI764584 in Taiwan, China, describes "low dielectric gel and its preparation method", which relates to the preparation and application of a low dielectric organic / inorganic aerogel composite material formed by impregnating a low dielectric gel into a polymer solution. The preparation is completed through the following steps: (1) mixing, (2) hydrolysis, (3) condensation, (4) aging, (5) drying, (6) impregnation with a polymer solution, (7) curing and phase separation, and (8) drying and cross-linking. This process prepares a high-strength low dielectric organic / inorganic aerogel composite material. The low dielectric gel is a porous structure with a porosity of more than 70% and a density of approximately 0.12 to 0.45 g / cm 3 The dielectric properties decrease with the increase of porosity, with the dielectric constant being 1.28 to 1.89 and the dielectric loss being 0.012 to 0.023. It can be used as dielectric layers in high-frequency circuits, insulating layers in semiconductor devices, or microwave circuits in communication integrated circuits.
[0023] In addition, the team's invention patent publication number TWI760728 in Taiwan, China, described in the "Method for preparing hydrophobic aerogel composite colloid for cold-resistance and heat-insulation and related products thereof" relates to a method for preparing a hydrophobic aerogel composite colloid comprising the following steps: (S1) a mixing step; (2) a hydrolysis step; (3) a condensation step; (4) an aging step; (5) a high-temperature pulse water washing step; (6) a drying step; and (7) a compounding step. The hydrophobic aerogel composite colloid is a high-viscosity colloid formed by mixing the prepared hydrophobic aerogel with inorganic fibers, inorganic glue, and natural cellulose adhesive. The developed product has excellent cold-resistance and heat-insulation properties, as well as the advantages of appropriate strength, light weight, good flame retardancy, and good water repellency.
[0024] In addition, the applicant's invention patent publication No. TWI717257 in Taiwan, China, described in "Preparation method of high temperature resistant, heat insulating, and fireproof aerogel / inorganic fiber composite adhesive and application of its products", which is related to a preparation method of a hydrophilic aerogel / inorganic fiber composite adhesive comprising the following steps: (1) mixing step; (2) hydrolysis step; (3) condensation step; (4) aging step; (5) high temperature solvent replacement step; (6) evaporation drying step; and (7) compounding step. The obtained product is a viscous aerogel composite colloid formed by mixing aerogel particles, inorganic fibers, inorganic adhesives and natural cellulose adhesives. After drying, the content of aerogel and inorganic fibers is 25-90wt%. In addition, the obtained product can be used for a long time at a high temperature of more than 600°C without the phenomenon of organic matter decomposition and carcinogens being produced.
[0025] Although the above-mentioned prior arts are all about the manufacturing technology of aerogel organic thermal insulation coating or thermal expansion type organic coating, these prior arts all use the thermal expansion of inorganic substances at high temperature by several to dozens of times, and use the thermal expansion air layer for thermal insulation. At present, the gap between the lithium battery packs of electric vehicles is extremely thin. The use of the above thermal expansion products will cause other lithium batteries to be harmed by high pressure under the condition of thermal runaway of lithium batteries. These prior arts generally use aerogel or aerogel mixed with inorganic powder and organic coating, such as epoxy resin, water-based polyamide ester coating ( Commonly known as water-based PU coatings), water-based polyacrylate coatings (commonly known as water-based acrylic coatings), etc., the maximum heat-resistant temperature of water-based coatings is mostly below 200°C, so these prior arts use flame retardants to increase the heat-resistant temperature; the organic coatings used in these prior arts will gradually age under long-term sunlight, resulting in a decrease in the coating effect of the organic coatings and causing a large number of aerogel particles to fall off. In addition, when the environment is above 200°C, the organic coatings will cause rapid aging and cracking, resulting in the shedding of the aerogel insulation coating and the generation of toxic smoke.
[0026] The high-temperature cracking of the above organic coatings will cause the leakage of aerogel dust or the shedding of thermal insulation coatings and produce toxic smoke, which will cause pollution in the application of high-tech components such as clean rooms or inside electric vehicles. This is the biggest disadvantage of aerogel organic thermal insulation coatings; therefore, silicon-based aerogel organic thermal insulation coatings or thermal expansion fire retardant coatings are very likely to produce nano to micron-sized dust pollutants during high-temperature applications. These aerogel dusts have always been the main problem that prevents aerogels from being quickly applied in high-tech industries; the shortcomings of the above fire-retardant and thermal insulation coatings have always been the main concerns or main problems that prevent high-insulation aerogel energy-saving materials from being applied in high-tech industry production lines for thermal runaway of lithium battery modules in electric vehicles.
[0027] In view of the several deficiencies in application caused by the above-mentioned aerogel dust pollutants, the inventors came up with the idea of improvement and carried out in-depth improvement research and development and creation. After a long period of hard work, the present invention was finally produced; the main purpose of the present invention is to provide a silicon-based aerogel fire-retardant and heat-insulating coating that is smokeless and non-toxic and has high fire resistance and high heat insulation performance under high-temperature flames, and a preparation method thereof. Summary of the invention
[0028] Therefore, in order to improve the shortcomings of the current thermal insulation coatings or fire retardant coatings using epoxy resins, water-based polyamide ester coatings, water-based polymethyl methacrylate coatings mixed with aerogels or thermal expansion metal oxides, such as the organic coatings are easily cracked due to aging and causing aerogel dust to fall during long-term sunlight application and in high-temperature environments above 300°C, or the shortcomings of the above organic coatings causing rapid burning when the lithium battery module is thermally runaway and produces flames above 500°C; the main purpose of the present invention is to provide a preparation method for preparing aerogel fire-retardant and heat-insulating coatings, and such aerogel fire-retardant and heat-insulating coatings are both smokeless and non-toxic and have high fire resistance and high heat insulation properties under high-temperature flames, and can be used in clean room high-temperature processes and safety protection of thermal runaway of lithium battery modules of electric vehicles.
[0029] Therefore, another main purpose of the present invention is to provide a method for preparing aerogel fireproof and heat-insulating coatings, and such aerogel fireproof and heat-insulating coatings have strong adhesion to the surface of metal materials, and no aging and cracking under long-term sunlight environment, and have excellent salt resistance and low moisture absorption in rainwater or aqueous solution containing trace salts. Silicon-based aerogel fireproof and heat-insulating coatings are suitable for use in automobiles and electric vehicles that need to be placed outdoors for a long time; another purpose of the present invention is to provide a method for preparing aerogel fireproof and heat-insulating coatings, and such aerogel fireproof and heat-insulating coatings combine high fireproof coatings and high thermal insulation aerogel particles, and are particularly suitable for thermal runaway or thermal dissipation of lithium battery modules of electric vehicles. Spraying aerogel fireproof coatings on the outer shell of the lithium battery module of electric vehicles or the chassis of electric vehicles can avoid thermal runaway of the lithium battery module of electric vehicles, which causes high temperature and high heat to be quickly transmitted through the chassis of the electric vehicle and penetrate into the driver's space, thereby increasing the safety of electric vehicle personnel.
[0030] In the present invention, firstly, in the process of preparing aerogel, the condensation solution is quickly stirred and dispersed in a large amount of dispersed solution by using a suspension dispersion technology, and then the silicon oxide suspension droplets in the suspended dispersed solution are gelled to form wet gel particles, and then a large amount of dispersed solution can be removed by using a filtering device or a reaction tank solution removal pipeline to form silicon aerogel wet gel particles with a particle size ranging from tens of nanometers to tens of microns, and then after drying in the reaction tank with high-temperature gas at normal pressure, aerogel micron or nano particles with low thermal conductivity and high fire resistance can be prepared; then, the dried aerogel particles are further mixed in a mixing tank with a large amount of inorganic glue aqueous solution, so that the dried aerogel particles can be uniformly dispersed in the inorganic glue aqueous solution, and the combined product will have aerogel fire retardant coatings with extremely strong adhesion to the surface of metal plates, high thermal insulation efficiency, high fire resistance and smokeless under high-temperature flames.
[0031] The method provided by the present invention can be used to prepare an aerogel fire retardant coating that has extremely strong adhesion to the surface of a metal plate, is smokeless and non-toxic under high-temperature flames, and has high fire resistance and high heat insulation performance, especially for aerogel fire retardant coatings used in thermal runaway protection of lithium battery modules in electric vehicles, fireproof door metal panels or H-steel steel frame structures for buildings, or internal fireproof and heat insulation of military aerospace high-speed vehicles, wherein the method comprises: a mixing and hydrolysis step (S1): adding a siloxane precursor to an ethanol aqueous solution and stirring and mixing to form a mixed solution, wherein the siloxane precursor includes a siloxane compound and a hydrophobic siloxane compound substituted with alkyl groups of different chain lengths or a combination thereof, and then adding an acid catalyst to the mixed solution to carry out a hydrolysis reaction; a condensation dispersion step (S2): adding an alkali catalyst solution to the mixed solution and stirring it evenly to carry out a condensation reaction to obtain a condensation solution, and then adding a large amount of dispersed aqueous solution, and quickly stirring and dispersing it with a dispersing device such as an emulsifier or a homogenizer, so that the condensation solution is suspended and dispersed in a large amount of dispersed aqueous solution, wherein the dispersed solution includes suspended and dispersed submicron-sized condensation droplets formed by the condensation reaction, and a large amount of dispersed aqueous solution, and then continuously stirring the dispersed solution, so that the suspended and dispersed submicron-sized condensation solution system is gelled during continuous stirring to form surface-stable aerogel wet gel particles, and the aerogel wet gel particles are suspended and dispersed in a large amount of dispersed aqueous solution; a normal pressure drying step ( S3): the surface-stabilized aerogel wet colloid particles are suspended and dispersed in a dispersion aqueous solution, and the surface-stabilized aerogel wet colloid particles are filtered by a filter, and then a normal pressure high-temperature dry airflow is provided in a drying tank to promote the rapid vaporization of the dispersion solvent contained in the surface-stabilized aerogel wet colloid particles to obtain dry aerogel particles. Since the surface-stabilized aerogel wet colloid particles contain a large number of alkyl hydrophobic structures of different chain lengths, the shrinkage and rupture of the aerogel structure caused by the interfacial tension of water molecules in the aerogel wet colloid particles can be suppressed during the drying process. Combining the above technologies, dry aerogel particles with a porous structure and low heat transfer and high fire resistance can be quickly obtained; high temperature resistant glue mixing step (S4): prepare a high temperature resistant glue above 500°C a high temperature resistant colloidal solution, adding the dry aerogel particles to the high temperature resistant colloidal solution, and slowly stirring to disperse the dry aerogel particles in the high temperature resistant colloidal solution; a blending and dispersing step (S5): further blending and dispersing the high temperature resistant colloidal solution impregnated with the dry aerogel particles with a stirring device. In this step, a wetting agent, a defoaming agent and a dispersant can be added to the high temperature resistant colloidal solution impregnated with the dry aerogel particles to make the aerogel particles completely and evenly dispersed in the high temperature resistant colloidal solution to form a uniform aerogel fire retardant and heat insulation coating. Through the above preparation steps, a silicon-based aerogel fire retardant and heat insulation coating that is smokeless, non-toxic, has high fire resistance and high heat insulation performance under high temperature flames can be obtained.
[0032] Furthermore, in the mixed hydrolysis step (S1), the siloxane compound comprises tetramethoxysilane (TMOS), tetraethoxysilane (TEOS) or a combination thereof; the hydrophobic modified siloxane compound comprises methyltrimethoxysilane (MTMS), propyltrimethoxysilane (PTMS), hexyltrimethoxysilane (HTMS), octyltrimethoxysilane (Octyltrimethoxysilane , OTS), hexamethyldisilane (HMDS) and other hydrophobic siloxanes substituted with different chain lengths or a combination thereof, wherein in the siloxane precursor, the molar ratio of the siloxane compound to the hydrophobic modified siloxane compound is between (0:100 mol%) and (95:5 mol%), and the purpose of adding the hydrophobic modified siloxane compound substituted with different chain lengths of alkyl groups is to reduce the shrinkage and cracking of the aerogel structure during the drying process and reduce the thermal conductivity; on the other hand, the purpose of adding the siloxane compound is to provide a microstructure for regulating the internal structure of the aerogel structure and to increase the pore structure and porosity in the structure, so as to reduce the thermal conductivity or improve the fireproof property.
[0033] Furthermore, in the mixed hydrolysis step (S1), when the content ratio of the acid catalyst in the mixed solution is higher, the hydrolysis rate is faster, but a large amount of acid ions will produce ionic conductivity under the action of the electric field, thereby significantly increasing the dielectric constant of the aerogel structure and reducing the dielectric strength; relatively, the lower the content ratio of the acid catalyst, the slower the hydrolysis rate, and the dielectric constant of the aerogel structure will be significantly reduced and the resistivity and dielectric strength will be improved; therefore, the present invention can significantly reduce the content of acid radical ions and condensed base ions added in the overall system by reducing the content of the acid catalyst and increasing the process temperature to increase the hydrolysis rate; on the other hand, the siloxane compound and the hydrophobic siloxane compound will produce a large amount of alcohol molecules during the hydrolysis process, so that deionized water is used to replace organic solvents such as ammonia and alkanes during the hydrolysis process, thereby reducing the addition of organic solvents such as ammonia and alkanes. In addition to reducing the influence of organic solvents such as ammonia on the dielectric properties of aerogels, it can also reduce the harm and environmental pollution of organic solvent treatment in the process, and can also reduce the overall preparation cost of aerogels.
[0034] Furthermore, in the mixed hydrolysis step (S1), in the overall mixed solution, the higher the content of the alcohol aqueous solution is, the higher the porosity in the subsequently dried wet glue particles is; relatively, in the overall mixed solution, the lower the content of the alcohol aqueous solution is, the lower the porosity in the subsequently dried wet glue particles is; wherein the alcohol aqueous solution comprises ethanol, recovered ethanol aqueous solution, recovered methanol aqueous solution, recovered water, deionized water, filtered water, distilled water or a combination thereof.
[0035] Further, in the condensation dispersion process (S2), an alkali catalyst solution is added to the mixed hydrolysis solution and stirred evenly to make it undergo a condensation reaction, and then a large amount of dispersed aqueous solution is added and quickly stirred and dispersed by a dispersing device such as an emulsifier or a homogenizer, so that the condensation solution is suspended and dispersed in a large amount of dispersed aqueous solution, and the dispersed solution includes a suspended and dispersed submicron-sized condensation droplet and a large amount of dispersed aqueous solution to form a suspended and dispersed submicron-sized condensation droplet and a large amount of dispersed aqueous solution, and then the suspended and dispersed submicron-sized condensation droplet is continuously stirred in the suspended and dispersed submicron-sized condensation solution system, waiting for the suspended and dispersed submicron-sized condensation droplet to gel to form a surface-stable aerogel wet gel particles, and the particles are suspended and dispersed in a large amount of dispersed aqueous solution. One of the main purposes of using this step is to accelerate the gelation rate of the nano-scale submicron-sized siloxane molecules or hydrophobic siloxane molecules in a large amount of dispersed aqueous solution, so as to form nano-scale to submicron-scale circular molecular suspended wet gel particles; another purpose of using this step is that the nano-scale to submicron-sized wet gel particles formed in the subsequent drying process will significantly increase their specific surface area due to the small particle size of the gel particles, so that the drying rate will also be increased.
[0036] Furthermore, in the above-mentioned condensation dispersion step (S2), the aerogel wet gel particles with a particle size of nanometers to submicrometers contain a large number of hydrophobic siloxane molecules substituted with alkyl groups of different chain lengths. Due to the presence of these hydrophobic siloxane molecules substituted with alkyl groups of different chain lengths in the dispersed aqueous solution system, the mixture of the siloxane compound and the hydrophobic modified siloxane compound can form an aerogel wet gel particle in the dispersed aqueous solution, which has a stable gelled hydrophobic surface layer and is uniformly dispersed in the dispersed aqueous solution; in the condensation dispersion process, the aerogel wet gel particles with a particle size of nanometers to submicrometers can form stable suspended particles in the dispersed aqueous solution system without directly dissolving in the dispersed aqueous solution, so that aerogel particles with a large porosity can be prepared without adding a large amount of hydrophobic organic solvents such as toluene and n-hexane or eliminating multiple replacement steps of hydrophobic organic solvents.
[0037] Furthermore, the atmospheric pressure drying step (S3) comprises: a vaporization step (S3-1): a dispersed aqueous solution system in which the surface-stabilized aerogel wet colloid particles are suspended and dispersed is used to filter the surface-stabilized aerogel wet colloid particles by using a filter, and then a atmospheric pressure high-temperature drying airflow is provided in a drying tank to promote rapid vaporization of water and alcohol solvents in the surface-stabilized submicron aerogel wet colloid particles. In the atmospheric pressure drying step, since the surface-stabilized aerogel wet colloid particles contain a large number of hydrophobic alkyl structures with different chain lengths, the shrinkage and rupture of the aerogel structure caused by the interfacial tension of the water molecules in the aerogel wet colloid particles can be suppressed during the drying process; therefore, a porous structure and dry aerogel particles with low heat transfer and high fire resistance can be quickly obtained through the atmospheric pressure high-temperature airflow drying technology; combined with reducing the aerogel particle size and adding a large number of hydrophobic alkyl structures with different chain lengths, the water molecules and alcohol molecules inside the aerogel structure can be quickly dried. Generally, a large amount of mixed solvent in the aerogel wet colloid particles is quickly evaporated. The rapid azeotropic vaporization temperature is between 60 and 90° C.; a recovery step (S3-2): at the azeotropic vaporization temperature, the vaporized steam of the mixed solvent is guided to a heat exchange recovery device; the mixed solvent is condensed and recovered in the heat exchange recovery device, and the purpose of the recovery is to reduce costs and reduce pollution to the environment; and a sudden boiling step (S3-3): adjusting the drying temperature of the dried aerogel particles to a temperature above the sudden boiling temperature of the mixed solvent, and combining with the rapid rotation of the microwave frequency to destroy the hydrogen bonding of the water molecules in the aerogel structure, and quickly providing friction heat to the solvent molecules, so that the remaining mixed solvent in the nearly dry aerogel produces a rapid sudden boiling to form a positive pressure, and the positive pressure inside the aerogel structure is used to promote the expansion behavior of the aerogel during the drying process, and the aerogel structure produces a large number of nano-scale to sub-micron-scale micropores during the expansion process, so as to improve the porosity and thermal insulation properties of the aerogel product, wherein the sudden boiling temperature is between 110 and 180° C.
[0038] Furthermore, in the above-mentioned high temperature resistant glue mixing step (S4), a high temperature resistant colloidal solution that can withstand temperatures above 500°C is prepared, and the dry aerogel particles are added to the stirring high temperature resistant colloidal solution under stirring conditions of a stirrer. In this step, a wetting agent, a defoaming agent and a dispersant may be added to disperse and immerse the dry aerogel particles in the high temperature resistant colloidal solution; the high temperature resistant colloidal solution contains a high temperature resistant glue material that can withstand temperatures above 500°C, which includes an inorganic glue material, an organic glue material, a thermosetting resin or any combination thereof; specifically, the high temperature resistant glue material includes a pure inorganic glue material or a large amount of inorganic glue material mixed with a trace amount of organic glue material, for example, 75 to 97 v / v% of an inorganic glue material mixed with 3 to 2 5v / v% organic thermosetting resin; further, the inorganic adhesive material includes water glass, inorganic silicone resin, copper oxide-phosphate glue, silicate glue, phosphate-silicate glue, sulfate glue, magnesium oxide-silicon dioxide-borax inorganic glue or any combination thereof; in addition, the organic adhesive material includes polyimide, polyetherimide, polyphenylene ether, polyphenylene sulfide, polyether ketone liquid crystal polymer, polytetrafluoroethylene, polymelamine, polyphenolic acid, polymelamine-formaldehyde, high temperature resistant silica gel, silicone modified polyurethane, silicone modified acrylate, silicone modified polyvinyl alcohol, organic thermosetting resin includes one of epoxy resin, organic high temperature resistant silicone resin and silicone modified epoxy resin, or any combination thereof.
[0039] Furthermore, in the above-mentioned blending and dispersing step (S5), the high-temperature resistant colloidal solution impregnated with and dispersed with the dry aerogel particles is further blended and dispersed by a stirring device. In this step, a wetting agent, a defoaming agent and a dispersant can be added to make the dry aerogel particles completely and evenly dispersed in the high-temperature resistant colloidal solution to form a uniform aerogel fire-retardant and heat-insulating coating. Through the above preparation steps, a silicon-based aerogel fire-retardant and heat-insulating coating that is smokeless, non-toxic, has high fire resistance and high heat insulation performance under high-temperature flames can be obtained. The purpose of the present invention is to provide a method for preparing an aerogel fireproof and heat-insulating coating, which improves the shortcomings of traditional aerogel organic coatings or thermal expansion metal oxide organic fire-retardant coatings, so as to prepare an aerogel fireproof and heat-insulating coating that has excellent adhesion properties to metal or plastic plates, and has smokeless, high heat insulation efficiency and high fireproof function under high-temperature flames; another purpose of the present invention is to provide a method for preparing an aerogel fireproof and heat-insulating coating, which improves the traditional fireproof door or fireproof iron rolling door sprayed with aerogel inorganic fire-retardant coating, under the condition of high-temperature flame spraying at 850 to 1250°C for 1 to 3 hours, the back of the iron plate of the fireproof door or fireproof iron rolling door can be obviously maintained below 500 degrees; on the other hand, another purpose of the present invention is to provide a method for preparing an aerogel fireproof and heat-insulating coating. The gel fireproof and heat-insulating coating is suitable for the insulation layer or heat-insulating fireproof layer of the surface of high-temperature smelting boiler structure or military aerospace high-speed vehicle. It can block the heat loss in pipelines or tool platform interfaces, thereby improving energy saving and carbon reduction effects, or it can block the high heat generated by air friction to reduce the damage of precision detection components inside military aerospace high-speed vehicles; the aerogel fireproof and heat-insulating coating provided by the present invention is particularly suitable for blocking thermal runaway or thermal dissipation of electric vehicle lithium battery modules. The aerogel fireproof coating is sprayed on the outer shell of the electric vehicle lithium battery module or the chassis of the electric vehicle to avoid the thermal runaway of the electric vehicle lithium battery module, which causes high temperature and high heat to be quickly transmitted through the chassis of the electric vehicle and penetrate into the driver's space, thereby increasing the safety of electric vehicle personnel.
[0040] Furthermore, in the above preparation method, the aerogel fire retardant coating is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames, and the dry aerogel particles contained therein have a porous structure, a porosity of 50.0 to 75.0%, and a density of 0.06 to 0.12 g / cm 3, its heat transfer coefficient is between 0.020 and 0.045 W / mk, its dielectric constant is between 1.30 and 1.85, and its flame retardancy is above UL94-V0; wherein, the aerogel fireproof and heat-insulating coating is further combined with a high heat-resistant inorganic adhesive or an inorganic-organic mixed adhesive to form a high heat-insulating and high fire-retardant aerogel inorganic fire-retardant coating; when the high heat-insulating and high fire-retardant aerogel inorganic fire-retardant coating is sprayed on the front of the aluminum plate to a thickness of 150 to 200 microns, it will dry in 1 When sprayed under a high-temperature flame of 200°C for at least 5 minutes, the temperature of the back side of the aluminum plate relative to the front side is 300 to 350°C, so the aluminum plate will not burn through; in contrast, another aluminum plate that is not sprayed with the high-insulation and high-fireproof aerogel inorganic fire retardant coating, its front side is sprayed under a high-temperature flame of 1200°C for 1 minute, the aluminum plate is melted through, and the temperature of its back side reaches a high temperature of 950 to 1050°C, indicating that the aerogel inorganic fire retardant coating has excellent fireproof and heat-insulating properties.
[0041] The preparation method provided by the present invention has the following effects:
[0042] 1. The preparation method provided by the present invention improves the shortcomings of traditional aerogel thermal insulation coatings and thermal expansion organic coatings in high-temperature fire prevention, and promotes the wide application of aerogel thermal insulation materials, and prepares an aerogel fire retardant coating that is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames; wherein the aerogel particles are prepared by using an improved sol-gel suspension dispersion technology, and a large amount of organic solvents, surfactants, adhesives and other substances are not added in the process, so that the preparation of aerogel particles does not require long-term solvent replacement and the use of supercritical drying technology, and only the atmospheric pressure high-temperature airflow drying technology with solvent recovery can be used to quickly prepare aerogel particles with high porosity. The overall process is simple, safe and economically advantageous, and the batch process speed can be reduced to 4 to 10 hours to complete the sub-micron aerogel particle product, and the fluidized bed dynamic drying or high-temperature airflow drying technology can be used to continuously produce and prepare aerogel particles to improve production efficiency.
[0043] 2. In the preparation method provided by the present invention, the porosity and pore size inside the porous aerogel particles, the porosity between the aerogel particles and the compactness of the aerogel structure can be easily controlled by utilizing factors such as the ratio of the siloxane compound and the hydrophobic siloxane substituted with alkyl groups of different chain lengths, the content of the hydrolysis solvent, the content of the dispersed aqueous solution, the stirring rate of the dispersing equipment such as an emulsifier or a homogenizer, and the content and ratio of the acid catalyst and the base catalyst.
[0044] 3. In the preparation method provided by the present invention, the repulsive force of the hydrophilic-hydrophobic property and rapid stirring are used to make the siloxane compound and the hydrophobic siloxane substituted with different chain length alkyl groups form wet gel particles of nanometer to micrometer scale, so as to improve the drying rate of the wet gel particles and reduce the shrinkage property; therefore, no other hydrophobic organic solvents such as cyclohexane, benzene, isopropanol, ammonia water or a large amount of surfactants are added except for alcohols, and the acid catalyst and the base catalyst are controlled at extremely low concentrations, which can further regulate the thermal conductivity, fireproof properties and dielectric properties of the aerogel material, so as to reduce the manufacturing cost of the aerogel composite material.
[0045] 4. In the preparation method provided by the present invention, a technique for rapidly condensing a dispersed solution using an emulsifier or a homogenizer is provided, and the condensed dispersed solution is gelled so that siloxane compounds and hydrophobic siloxane oil droplets substituted with alkyl groups of different chain lengths form aerogel wet gel particles with a stable hydrophobic surface layer in a large amount of dispersed aqueous solution; further, in the subsequent gelation process, a phase-separated structure is formed inside the aerogel wet gel particles due to the hydrophilic-hydrophobic repulsion phenomenon, so as to further form a network aerogel structure; the hydrophobic siloxanes substituted with alkyl groups of different chain lengths inside the aerogel wet gel particles are distributed at the molecular level, so that the formed aerogel wet gel particles have excellent hydrophobic properties inside, and in the subsequent normal pressure drying step, aerogel particles with different pore sizes can be prepared; compared with other technologies, the products prepared using this technology not only save a large amount of organic solvents but also have a fast process.
[0046] 5. To solve the problems related to the shortcomings of traditional aerogel organic coatings, the present invention improves the previous aerogel manufacturing process technology, and also develops a high-temperature resistant colloidal solution formed by using inorganic glue or inorganic glue mixed with organic glue materials in the preparation of aerogel fire retardant coatings, so that the prepared high-temperature resistant glue can achieve no smoke and odor release under 1200℃ high-temperature flame spraying, and can form excellent bonding with different materials such as metals, ceramics, plastics, inorganic fibers, organic fibers, etc.; then the aerogel particles are mixed with the prepared high-temperature resistant glue materials, and the aerogel particles are used to form a high-temperature resistant glue material. The pores in the particles achieve a heat insulation mechanism, and then a high-temperature resistant colloidal solution is used to achieve a high-temperature resistance and fire prevention mechanism, thus forming an aerogel fire retardant coating that is smokeless, non-toxic, highly fire-resistant and highly heat-insulating under high-temperature flames; based on this technology, aerogel fire retardant coatings can be used to prevent thermal runaway or thermal dissipation of lithium battery modules in electric vehicles. Spraying aerogel fire retardant coatings on the outer shell of the lithium battery module of electric vehicles or the chassis of electric vehicles can prevent the high temperature and heat caused by the thermal runaway of the lithium battery module of electric vehicles from being quickly transmitted through the chassis of the electric vehicle into the driver's space, so as to increase the safety of electric vehicle personnel.
[0047] 6. The preparation method provided by the present invention can further improve the fireproof effect of traditional fire doors or fireproof iron rolling doors. When the aerogel fire retardant coating is sprayed, the back of the iron plate of the fire door or fireproof iron rolling door can be significantly lowered to below 500°C under a high-temperature flame spraying of 850 to 1250°C for 1 to 3 hours; on the other hand, the aerogel fire retardant coating prepared by the method provided by the present invention is also suitable for use as a fireproof layer on the surface of a high-temperature smelting boiler structure, or as an insulating layer or a heat-insulating fireproof layer for military aerospace high-speed vehicles to block the high heat generated by air friction and reduce the damage to the precision detection components inside the military aerospace high-speed vehicles; the aerogel material contained in the above-mentioned aerogel fire retardant coating is a porous structure with a porosity of 50.0 to 75.0% and a density of 0.06 to 0.12 g / cm 3 , its heat transfer coefficient is between 0.020 and 0.045 W / mk, its dielectric constant is between 1.30 and 1.85, and its flame retardancy is above UL94-V0. The above-mentioned aerogel material is combined with a high heat-resistant inorganic adhesive or an inorganic-organic mixed adhesive to form an aerogel inorganic fire retardant coating with high heat insulation and high fire resistance; the aerogel inorganic fire retardant coating is sprayed on the surface of the aluminum plate to a thickness of 150 to 200 microns, and after drying, it can withstand spraying for 30 minutes under a high temperature flame of 1200°C, and maintain the back temperature at 300 to 350°C to protect the aluminum plate from being burned through; in contrast, the surface of the aluminum plate without spraying is sprayed for 1 minute under a high temperature flame of 1200°C, and the aluminum plate is melted through, showing that the above-mentioned aerogel inorganic fire retardant coating has excellent fireproof and heat insulation properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The present invention is a step flow chart for explaining the first embodiment of the preparation process of aerogel fire retardant coating which is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flame.
[0049] Figure 2 This is a photograph of the appearance of aerogel particles with high thermal insulation efficiency and low density prepared by the preparation method according to the first embodiment of the present invention.
[0050] Figure 3 The scanning electron microscope (SEM) observation photograph of the aerogel particles with high thermal insulation efficiency and low density prepared by the preparation method of the first embodiment of the present invention has a magnification of 10,000 times.
[0051] Figure 4 This is a photograph of the appearance of an aerogel fire retardant coating prepared by the preparation method according to the first embodiment of the present invention, which is smokeless, non-toxic, has high fire resistance and high heat insulation performance under high temperature flames.
[0052] Figure 5This is a scanning electron microscope (SEM) observation photograph of a cross-section of an aerogel fire-retardant coating prepared by the preparation method of the first embodiment of the present invention, which is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames, with a magnification of 5,000 times.
[0053] Figure 6 The photos are used to show the appearance of a general aluminum plate with a thickness of 1mm before and after being sprayed under a high-temperature flame of 1200℃.
[0054] Figure 7 The photographs are used to show the appearance of an aluminum plate sprayed with an aerogel fire retardant coating prepared according to the first embodiment of the preparation method, which has smokeless, non-toxic, high fire resistance and high heat insulation performance under a high temperature flame, before and after being sprayed under a high temperature flame of 1200°C. DETAILED DESCRIPTION
[0055] See also Figure 1 The present invention provides a first embodiment of a method for preparing an aerogel fire retardant coating, which is formed by adding an inorganic glue solution or an inorganic glue / organic glue solution to aerogel particles of different particle sizes and hydrophilicity and hydrophobicity, and the aerogel fire retardant coating has both smokeless and non-toxic properties and high fireproof and high heat insulation properties under high-temperature flames. The steps include: a mixing and hydrolysis step (S1), a condensation and dispersion step (S2), a normal pressure drying step (S3), a high temperature resistant glue mixing step (S4), and a blending and dispersion step (S5), wherein:
[0056] The mixing and hydrolysis step (S1) is as follows: a siloxane precursor is added to an ethanol aqueous solution to form a mixed solution, wherein the siloxane precursor comprises a hydrophobic modified siloxane compound, a siloxane compound or a combination thereof, and then an acid catalyst is added to the mixed solution to perform a hydrolysis reaction; in some embodiments, the siloxane compound comprises tetramethoxysilane (TMOS), tetraethoxysilane (TEOS) or any combination thereof; in these embodiments, the hydrophobic modified siloxane compound comprises methyltrimethoxysilane (MTMS), propyltrimethoxysilane (PTMS), hexyltrimethoxysilane (Hexyltrimethoxysilane) The invention relates to a hydrophobic siloxane having different chain lengths and alkyl groups substituted with octyl trimethoxysilane (HTMS), octyl trimethoxysilane (OTMS), hexamethyldisilane (HMDS) or any combination thereof; specifically, the purpose of adding the hydrophobic modified siloxane is to reduce the cracking phenomenon of the aerogel structure during the drying process, and the purpose of adding the siloxane compound is to regulate the internal microstructure of the aerogel structure to increase the pore content in the structure; in these embodiments, for the overall mixed solution, the total molar percentage of the siloxane compound and the hydrophobic siloxane molecules having different chain lengths and alkyl groups substituted with octyl trimethoxysilane (HTMS), hexamethyldisilane (HMDS) or any combination thereof; specifically, the purpose of adding the hydrophobic modified siloxane is to reduce the cracking phenomenon of the aerogel structure during the drying process, and the purpose of adding the siloxane compound is to regulate the internal microstructure of the aerogel structure to increase the pore content in the structure; in these embodiments, for the overall mixed solution, the total molar percentage of the siloxane compound and the hydrophobic siloxane molecules having different chain lengths and alkyl groups substituted with octyl trimethoxysilane (OTMS), hexamethyldisilane (HMDS) or any combination thereof; and the molar ratio of the content of the ethanol aqueous solution is between 99.5 mol% and 60 mol%.
[0057] In this embodiment, the molar ratio of the siloxane compound to the hydrophobic siloxane compound substituted with alkyl groups of different chain lengths is from (0:100) to (95:5.0); in a preferred embodiment, the molar ratio of the siloxane compound to the hydrophobic siloxane compound substituted with alkyl groups of different chain lengths is 5:95; in the ethanol-water solution, the molar ratio of ethanol to water is from 0:100 to 50:50; in a preferred embodiment, the molar ratio of ethanol to water is 15:85.
[0058] In the mixing and hydrolysis step (S1), the siloxane compound, the hydrophobic siloxane compound substituted with alkyl groups of different chain lengths and a large amount of ethanol aqueous solution containing a trace amount of acid catalyst are fully mixed. During the above mixing process, a hydrolysis reaction (hydrolysis) will be carried out simultaneously, wherein the ethanol aqueous solution containing a trace amount of acid catalyst includes ethanol, deionized water, treated water, secondary treated water or a mixture of any combination thereof, and the molar ratio of the total content of the mixture of the siloxane compound and the hydrophobic siloxane compound substituted with alkyl groups of different chain lengths to the content of the acid catalyst is 1:0.01 to 1:0.0005; when the content ratio of the acid catalyst in the mixed solution is higher, the hydrolysis rate is faster; but on the other hand, the higher the content ratio of the acid catalyst, the greater the ion content in the overall aerogel structure, and the greater the dielectric loss of the aerogel will be; in a preferred embodiment, the molar ratio of the total content of the mixture of the siloxane compound and the hydrophobic siloxane compound substituted with alkyl groups of different chain lengths to the content of the acid catalyst is 1:0.0015.
[0059] Condensation dispersion step (S2): adding an alkali catalyst solution to the mixed solution and stirring it evenly to make it undergo a condensation reaction to obtain a condensation solution, then adding a large amount of dispersed aqueous solution to the condensation solution, and using a dispersing device such as an emulsifier or a homogenizer to quickly stir and disperse it, so that the condensation solution is suspended and dispersed in a large amount of dispersed aqueous solution, so that the hydrolyzed mixed siloxane compound in the condensation solution undergoes a condensation reaction to form sol oil droplets, which are sub-micron condensed oil droplets suspended and dispersed in the dispersed aqueous solution, and then continuously stirring the suspended and dispersed sub-micron condensed solution system, waiting for the sub-micron condensed oil droplets to gel to form surface-stable aerogel wet gel particles, and the aerogel wet gel particles are suspended and dispersed in a large amount of dispersed aqueous solution; the volume ratio of the dispersed aqueous solution to the ethanol aqueous solution is from 100:0 to 30:70; in a preferred embodiment, the volume ratio of the dispersed aqueous solution to the ethanol aqueous solution is 100:0.
[0060] In the condensation dispersion step, the increase in temperature helps to significantly shorten the condensation reaction time, that is, the gelation time of the aerogel is effectively shortened in the dispersion condensation step (S2); wherein, when the content equivalent ratio of the base catalyst to the acid catalyst is 1.0:1.0, the condensation reaction temperature is 20 to 55°C, and the condensation reaction time is 20 to 250 minutes; in some preferred embodiments, the condensation reaction temperature is 25°C, and the condensation reaction time is about 220 minutes. When the condensation reaction temperature is 50°C, the condensation reaction time is about 15 minutes.
[0061] In the condensation dispersion step, since the aerogel wet gel particles with nanometer to submicron particle sizes contain a large amount of hydrophobic siloxane compounds substituted with alkyl groups of different chain lengths, the aerogel wet gel particles are dispersed in the aqueous solution system. Due to the presence of the hydrophobic siloxane compounds substituted with alkyl groups of different chain lengths, the mixture of the siloxane compound and the hydrophobic modified siloxane compound can form a stable gelled hydrophobic surface layer in the dispersed aqueous solution, and the initial structural size of the siloxane aerogel molecules and the hydrophobic siloxane molecules substituted with alkyl groups of different chain lengths inside the particles can be controlled to be 5 to 10 nm, and the initial structures are stacked to form aerogel wet gel molecules of 50 to 100 nm, and are interconnected to form a three-dimensional network structure; therefore, in the condensation dispersion process, the aerogel wet gel particles with nanometer to submicron particle sizes are Stable suspended particles can be formed in a dispersed aqueous solution system and will not be directly dissolved in the aqueous solution; therefore, aerogel wet gel particles with a large amount of porosity can be prepared without adding a large amount of hydrophobic organic solvents such as toluene and n-hexane, or without multiple replacement steps of hydrophobic organic solvents; wherein the volume ratio of the added siloxane compound or the mixture of hydrophobic siloxane compounds substituted with alkyl groups of different chain lengths to the dispersed aqueous solution is between (1.0:1.0) and (1.0:5.0); in other embodiments, the volume ratio is 1.0:1.0, and the condensation reaction time is 70 minutes; preferably, the volume ratio is 1.0:3.0, and the condensation reaction time is 30 minutes; more preferably, the volume ratio is 1.0:1.5, the condensation reaction time is reduced to 55 minutes, and a higher aerogel particle yield is achieved.
[0062] In some other embodiments, increasing the content of the alkali catalyst will also significantly shorten the condensation reaction time, wherein the content equivalent ratio of 1.0M alkali catalyst to 1.0M acid catalyst is (0.8:1.0) to (2.0:1.0), and the condensation reaction time is 360 to 3 minutes; preferably, the content equivalent ratio is 0.8:1.0, and the condensation reaction time is 360 minutes; more preferably, the content equivalent ratio is 1.6:1.0, and the condensation reaction time is about 10 minutes; it should be further explained that when the content equivalent ratio is less than 1.0:1.0, the condensation reaction time gradually increases, and the dielectric loss of the prepared aerogel will be significantly reduced; when the content equivalent ratio is greater than 1.0:1.0, the condensation reaction time gradually decreases, but the dielectric loss of the prepared aerogel will be significantly increased due to the increase in ion content; in a preferred embodiment of this embodiment, the content volume ratio is 1.2:1.0.
[0063] Furthermore, the atmospheric pressure drying step (S3) includes a solvent vaporization step (S3-1), a solvent recovery step (S3-2) and a solvent sudden boiling step (S3-3).
[0064] Normal pressure drying step (S3): using a filter to filter out the dispersed aqueous solution system in which the surface-stable submicron aerogel wet colloid particles are suspended and dispersed, and leaving the submicron aerogel wet colloid particles, and then providing a normal pressure high temperature drying airflow in a drying tank to promote rapid vaporization of the residual water and alcohol solvents in the surface-stable submicron aerogel wet colloid particles. In the normal pressure drying step, since the submicron aerogel wet colloid particles contain a large number of hydrophobic alkyl structures with different chain lengths, the shrinkage and rupture of the aerogel structure caused by the interfacial tension of the water molecules in the submicron aerogel wet colloid particles is suppressed during the drying process; therefore, the normal pressure high temperature airflow drying technology can quickly obtain aerogel particles with a porous structure and low heat transfer and high fire resistance; combined with reducing the aerogel particle size and adding a large number of hydrophobic alkyl structures with different chain lengths, the water molecules and alcohol molecules inside the aerogel structure can be quickly dried, and the rapid azeotropic vaporization temperature of a large number of mixed solvents in the aerogel wet colloid particles is between 60 and 90°C; preferably, the azeotropic vaporization temperature is 90°C.
[0065] Specifically, in the atmospheric pressure drying step, a solvent recovery device can be designed to perform a solvent recovery step (S3-2), in which the drying process is carried out in a atmospheric pressure high-temperature airflow, and the vaporized steam is guided to a heat exchange recovery device under an azeotropic vaporization temperature environment; in the heat exchange recovery device, the aqueous alcohol is condensed and recovered, and the purpose of the recovery is to reduce costs and reduce pollution to the environment.
[0066] Boiling step (S3-3): after most of the solvent in the wet aerogel particles is vaporized to obtain a dry aerogel structure, the drying air flow temperature of the dry aerogel structure is adjusted to a temperature above the boiling temperature of the mixed solvent, and the microwave frequency is combined with rapid rotation to destroy the hydrogen bonds of the water molecules in the aerogel structure to provide friction heat for the solvent molecules, so that the remaining mixed solvent inside the dry aerogel structure produces rapid boiling to form a positive vapor pressure, and the positive vapor pressure is used to cause the dry aerogel structure to expand during further drying, thereby causing the dry aerogel structure to produce a large number of nano-scale to sub-micron-scale micropores during the expansion process, so as to obtain dryer gel particles, which specifically improves the porosity and thermal insulation properties of the dry aerogel particles and the back-end products; preferably, the boiling temperature is 110 to 180°C; more preferably, the boiling temperature is 150 to 180°C.
[0067] On the other hand, since no large amount of organic solvents such as alkanes, aromatic benzenes, amines, and surfactants are added, the drying process is safer and aerogel products with higher purity can be produced. Since the prepared high-porosity dry aerogel particles do not contain various impurities, the thermal insulation properties, dielectric constant, dielectric loss and other properties of the back-end products will be better.
[0068] The step of mixing a high temperature resistant glue (S4): preparing a high temperature resistant colloidal solution that can withstand temperatures above 500°C, adding the dry aerogel particles to the stirred high temperature resistant colloidal solution under slow stirring in a stirrer, and dispersing and impregnating the dry aerogel particles in the high temperature resistant colloidal solution under slow stirring; the high temperature resistant colloidal solution comprises a high temperature resistant glue material that can withstand temperatures above 500°C, which comprises a pure inorganic glue, or an inorganic glue material mixed with a trace amount of organic glue material, wherein the inorganic glue material mixed with a trace amount of organic glue material can be, for example, 75 to 97 v / v% of the inorganic glue material mixed with 3 to 25v / v% organic thermal adhesive; in some embodiments, the inorganic adhesive comprises water glass, inorganic silicone resin, copper oxide-phosphate adhesive, silicate adhesive, inorganic silicon polymer adhesive, phosphate-silicate adhesive, sulfate adhesive, magnesium oxide-silicon dioxide-borax inorganic adhesive or any combination thereof; the organic adhesive comprises polyimide, polyetherimide, polyphenylene ether, polyphenylene sulfide, polyetherketone liquid crystal polymer, polytetrafluoroethylene, polymelamine, polyphenolic formaldehyde, high temperature resistant silica gel, silicone modified polyurethane, silicone modified acrylate, organic The silicon-modified polyvinyl alcohol or organic thermosetting resin includes one of epoxy resin, organic high-temperature resistant silicone resin and organic silicon-modified epoxy resin, or any combination thereof; as for the aerogel fire retardant coating as a whole, the weight content ratio of the dry aerogel particles is between 10.0 and 45.0 wt%, and the weight content ratio of the high-temperature resistant colloid solution is between 55.0 and 90 wt%; wherein, the lower the weight content ratio of the high-temperature resistant colloid solution, the lower the bonding strength of the overall aerogel fire retardant coating to metals, ceramics, and plastics, and the prepared aerogel fire retardant coating has a heat insulation performance. The properties are superior; relatively, the higher the weight content ratio of the high temperature resistant colloidal solution, the higher the bonding strength of the aerogel fire retardant coating to metals, ceramics, and plastics, the higher the high temperature fire retardant performance and the better the density of the prepared aerogel fire retardant coating, but the thermal insulation property is poor, and there is obvious sag when sprayed on the surface of the substrate; therefore, in order to optimize the formulation of the aerogel fire retardant coating so that it has smokeless, high thermal insulation efficiency, and high fire retardant function under high temperature flames, preferably, the weight content ratio of the dry aerogel particles is between 13.0 and 15.0wt%.
[0069] Blending and dispersing step (S5): the high temperature resistant colloidal solution impregnated with the dried aerogel particles is further blended and dispersed by a stirring device. In this step, a trace amount of wetting agent, defoaming agent and dispersant can be further added to make the dried aerogel particles completely and evenly dispersed in the high temperature resistant colloidal solution to form a uniform aerogel fireproof and heat-insulating coating. Through the above preparation steps, a silicon-based aerogel fireproof and heat-insulating coating that is smokeless, non-toxic, has high fireproof and high heat-insulating properties under high temperature flames can be obtained. The main purpose of the present invention is to improve the shortcomings of traditional aerogel organic coatings or thermal expansion metal oxide organic fire-retardant coatings, so as to prepare an aerogel inorganic fire-retardant coating that has excellent adhesion properties to metal or plastic plates, and smokeless, high heat-insulating efficiency and high fireproof function under high temperature flames. The aerogel inorganic fire-retardant coating can also be used to improve the serious deformation of the iron plate caused by the traditional fire door or fireproof iron rolling door under high temperature flame spraying. Spraying on the surface of the iron plate After the aerogel inorganic fire retardant coating is applied, the back of the iron plate of the fire door or fireproof iron rolling door can still be obviously maintained below 500°C after being sprayed with a high-temperature flame of 850 to 1250°C for 1 to 3 hours; on the other hand, the aerogel inorganic fire retardant coating is also suitable for the surface of high-temperature smelting boiler structure or military aerospace high-speed vehicle as an insulation layer or insulation fireproof layer to reduce heat loss in pipelines or tool platform interfaces, improve the effectiveness of energy saving and carbon reduction, or to block the high heat generated by air friction to reduce the damage of precision detection components inside military aerospace high-speed vehicles; on the other hand, the aerogel inorganic fire retardant coating is particularly suitable for thermal runaway or thermal dissipation of electric vehicle lithium battery modules. The aerogel fire retardant coating is sprayed on the outer shell of the electric vehicle lithium battery module or the chassis of the electric vehicle to avoid the high temperature and high heat caused by the thermal runaway of the electric vehicle lithium battery module from being quickly transmitted through the chassis of the electric vehicle into the driver's space to increase the safety of electric vehicle personnel.
[0070] Several embodiments are presented below with accompanying drawings to illustrate the technical effects achieved by the method provided by the present invention; Figure 2 , the appearance photo of the aerogel particles with high thermal insulation efficiency and low density prepared by the preparation method of the first embodiment, the photo shows that the prepared aerogel particles are white powder with excellent uniformity.
[0071] See also Figure 3 , a scanning electron microscope (SEM) observation photograph of aerogel particles with high thermal insulation efficiency and low density prepared by the preparation method of the first embodiment of the present invention, with a magnification of 10,000 times; under electron microscope observation, its microstructure shows obvious spherical aerogel particles, the particle size of the spherical aerogel particles is approximately in the scale of 100 to 200 nm, and the size of the agglomerates of the aerogel particles is approximately between sub-micron and ten micron levels.
[0072] See also Figure 4, is a photograph of the appearance of an aerogel fire retardant coating that is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames and is prepared according to the preparation method of the first embodiment; specifically, the prepared aerogel fire retardant coating has a white and viscous appearance, and the color of the aerogel fire retardant coating is also mixed into black or other colors using inorganic pigments; the aerogel fire retardant coating contains sub-micron to ten-micron aerogel particles to provide high temperature resistance and high heat insulation properties, and also contains high temperature resistant adhesive materials to provide higher high temperature resistance, high bonding strength and high fire resistance properties; the above combination can form an aerogel fire retardant coating that is smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames to enhance the application field of aerogel.
[0073] See also Figure 5 , a cross-sectional scanning electron microscope (SEM) observation photograph of an aerogel fire retardant coating having both smokeless and non-toxic properties and high fire resistance and high heat insulation properties under high temperature flames prepared according to the preparation method of the first embodiment, with a magnification of 5,000 times; Figure 5 It is shown that in this embodiment, the interior of the aerogel fire retardant coating is a composite material of high-temperature resistant glue coated with sub-micron to ten-micron aerogel agglomerates, specifically, a large number of sub-micron aerogel molecular aggregates are dispersed in the high-temperature resistant glue, and in the cross-section of the aerogel fire retardant coating film, it can be clearly seen that the interior of the aerogel molecular aggregates in the high-temperature resistant glue still contains a large number of holes. Therefore, in the cross-sectional structure of the overall aerogel fire retardant coating film, the large number of aerogels and holes provide the aerogel fire retardant coating with the characteristics of low heat transfer and high thermal insulation.
[0074] See also Figure 6 , are photos of the appearance of a general aluminum plate with a thickness of 1mm before and after being sprayed with a high-temperature flame at 1200℃. During the 1200℃ high-temperature flame spraying process, the temperature of the back of the aluminum plate reached about 600℃ in 50 seconds, and the aluminum plate was burned through in about 1 minute under the 1200℃ high-temperature flame spraying. Figure 6 Shown on the right.
[0075] See also Figure 7 , photos of the appearance of an aluminum plate sprayed with an aerogel fire retardant coating prepared according to the first embodiment, which has both smokeless, non-toxic, high fire resistance and high heat insulation performance under high temperature flames, before and after being sprayed with a 1200°C high temperature flame; specifically, the spraying thickness of the aerogel fire retardant coating is about 150μm, which shows the back temperature of the aluminum plate during the flame spraying process. The back temperature of the aluminum plate sprayed with the aerogel fire retardant coating is about 350°C, and the aluminum plate is sprayed with a 1200°C high temperature flame for 30 minutes without burning through, such as Figure 7 As shown on the right. This shows that aerogel fire retardant coatings that are smokeless, non-toxic, highly fireproof and highly heat-insulating under high-temperature flames do have excellent fireproof and heat-insulating effects and can be used to prevent thermal runaway of lithium battery modules in electric vehicles.
[0076] In summary, the manufacture, application and effects of the present invention should have been clearly disclosed. However, the above-described embodiments are only preferred embodiments of the present invention and should not be used to limit the scope of patent protection of the present invention. That is, simple equivalent changes and modifications made according to the scope of patent protection of the present invention and the content of the invention description all fall within the scope of patent protection of the present invention.
[0077]
Explanation of symbols
[0078] (S1) Mixing and hydrolysis step
[0079] (S2) Condensation and dispersion step
[0080] (S3) Normal pressure drying step
[0081] (S4) High temperature resistant glue mixing step
[0082] (S5) Blending and Dispersing Step
[0083] (S3-1) Solvent Vaporization Step
[0084] (S3-2) Solvent recovery step
[0085] (S3-3) Solvent Boiling Step
Claims
1. A method for preparing an aerogel fireproof and heat-insulating coating, characterized in that: The method comprises adding an inorganic glue solution or an inorganic glue / organic glue solution to aerogel particles of different particle sizes and hydrophilicity and hydrophobicity, and includes the following steps: Mixing and hydrolysis step: adding a siloxane precursor to an ethanol aqueous solution to form a mixed solution, wherein the siloxane precursor includes a hydrophobic modified siloxane compound with different chain length alkyl groups, a siloxane compound or a combination thereof, and then adding an acid catalyst to the mixed solution to perform a hydrolysis reaction; Condensation and dispersion step: adding an alkali catalyst solution to the mixed solution to carry out a condensation reaction to obtain a condensation solution, then adding a dispersed aqueous solution to the condensed solution, and rapidly stirring with an emulsifier or a homogenizer to condense the hydrolyzed mixed siloxane compound in the condensed solution to form sol oil droplets, which are suspended and dispersed in the dispersed aqueous solution, and then the sol oil droplets are condensed to form aerogel wet gel particles, which have a stable hydrophobic shell and are uniformly dispersed in the dispersed aqueous solution; Normal pressure drying step: filtering the dispersed aqueous solution with a filter under normal pressure and drying temperature to obtain the wet aerogel particles, and then providing a normal pressure high temperature drying airflow to rapidly vaporize the solvent contained in the wet aerogel particles to obtain dry aerogel particles, wherein the drying temperature is between 60 and 150° C.; A high temperature resistant glue mixing step: preparing a high temperature resistant colloid solution, slowly stirring the high temperature resistant colloid solution, adding the dry aerogel particles into the high temperature resistant colloid solution, and slowly stirring the dry aerogel particles so that they are dispersed and impregnated in the high temperature resistant colloid solution, wherein the high temperature resistant colloid solution can withstand a high temperature of at least 500° C.; and The mixing and dispersing step is to mix and disperse the high temperature resistant colloidal solution impregnated with the dry aerogel particles by a stirrer, and add a wetting agent, a defoaming agent and a dispersant to the high temperature resistant colloidal solution impregnated with the dry aerogel particles, so that the dry aerogel particles are completely and evenly dispersed in the high temperature resistant colloidal solution to form an aerogel fireproof and heat-insulating coating, which has the properties of being smokeless, non-toxic, highly fireproof and highly heat-insulating under high temperature flames.
2. The preparation method according to claim 1, characterized in that: The aerogel fireproof and heat-insulating coating improves the shortcomings of traditional aerogel organic coatings or thermal expansion metal oxide organic fireproof coatings, and has excellent adhesion properties to metal or plastic plates, and has smokeless, non-toxic, high fireproof and high heat insulation properties under high-temperature flames; The aerogel fireproof and heat-insulating coating is suitable for thermal runaway or thermal escape of lithium battery modules of electric vehicles. The aerogel fireproof coating is sprayed on the outer shell of the lithium battery module of electric vehicles or the chassis of electric vehicles to prevent the thermal runaway of the lithium battery module of electric vehicles from causing high temperature and high heat to be quickly transmitted through the chassis of the electric vehicle and penetrate into the driver's space, thereby increasing the safety of electric vehicle personnel.
3. The preparation method according to claim 1, characterized in that: The atmospheric pressure drying step comprises: Vaporization step: Rapidly azeotropically vaporize the solvent in the structure of the aerogel wet gel particles at an azeotropic vaporization temperature to distill and dry the solvent and obtain a dry aerogel structure, wherein the azeotropic vaporization temperature is 60 to 90° C.; Recovery step: directing the azeotropic vapor of the solvent to a heat exchange recovery device to cause the solvent to condense and be recovered; and Boiling step: adjusting the drying temperature to the boiling temperature so that the solvent and water molecules contained in the dried aerogel structure boil rapidly and generate positive vapor pressure to inhibit the drying shrinkage of the dried aerogel structure and generate a large number of fine pores to obtain the dried aerogel particles, which have a higher thermal insulation effect, wherein the boiling temperature is 110 to 180°C.
4. The preparation method according to claim 1, characterized in that: The high temperature resistant colloidal solution comprises a pure inorganic glue, or an inorganic glue mixed with an organic glue, wherein the inorganic glue mixed with an organic glue comprises 75 to 97 v / v% of the inorganic glue and 3 to 25 v / v% of the organic glue; The inorganic adhesive material comprises water glass, inorganic silicone resin, copper oxide-phosphate adhesive, silicate adhesive, inorganic silicon polymer adhesive, phosphate-silicate adhesive, sulfate adhesive, magnesium oxide-silicon dioxide-borax inorganic adhesive or any combination thereof; Among them, the organic adhesive material includes polyimide, polyetherimide, polyphenylene ether, polyphenylene sulfide, polyether ketone liquid crystal polymer, polytetrafluoroethylene, polymelamine, polyphenolic acid, polymelamine-formaldehyde, high temperature resistant silicone, silicone modified polyurethane, silicone modified acrylate, silicone modified polyvinyl alcohol, organic thermosetting resin selected from the group consisting of epoxy resin, organic high temperature resistant silicone resin and silicone modified epoxy resin, or any combination thereof.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The siloxane compound comprises tetramethoxysilane, tetraethoxysilane or a combination thereof; the hydrophobic modified siloxane compound comprises methyltrimethoxysilane, propyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, hexamethyldisilazane or any combination thereof, wherein in the siloxane precursor, the molar ratio of the siloxane compound and the hydrophobic siloxane molecules substituted with alkyl groups of different chain lengths is between (0:100 mol%) and (95:5.0 mol%).
6. The preparation method according to any one of claims 1 to 4, characterized in that: The blending and dispersing step includes blending and dispersing the high temperature resistant colloid solution impregnated with the dry aerogel particles by using a stirring and dispersing device.
7. The preparation method according to any one of claims 1 to 4, characterized in that: Taking the aerogel fireproof and heat-insulating coating as a whole as an example, the weight content percentage of the dry aerogel particles is between 10.0 and 45.0 wt %, and the weight content percentage of the high temperature resistant colloid solution is between 55.0 and 90 wt %; Among them, the lower the weight content percentage of the high temperature resistant colloidal solution, the lower the bonding strength of the aerogel fireproof and thermal insulation coating to metal, ceramic, or plastic, and its thermal insulation properties are more superior; relatively, the higher the weight content percentage of the high temperature resistant colloidal solution, the higher the bonding strength of the aerogel fireproof and thermal insulation coating to metal, ceramic, and plastic, the higher its high temperature fireproof performance and the better its density, but the thermal insulation properties are poor, and there is an obvious sag phenomenon when sprayed on the substrate.
8. The preparation method according to any one of claims 1 to 4, characterized in that: The dry aerogel particles contained in the aerogel fireproof and heat-insulating coating have a porous structure, a porosity of which is between 50.0 and 75.0%, and a density of which is between 0.06 and 0.12 g / cm 3 , its heat transfer coefficient is between 0.020 and 0.045 W / mk, its dielectric constant is between 1.30 and 1.85, and its flame retardancy is above UL94-V0; The aerogel fireproof and heat-insulating coating is further combined with a high heat-resistant inorganic glue or an inorganic-organic mixed glue to form a high heat-insulating and high fire-resistant aerogel inorganic fire-retardant coating. When the high heat-insulating and high fire-resistant aerogel inorganic fire-retardant coating is sprayed on the front of an aluminum plate to a thickness of 150 microns, it is sprayed at a high temperature of 1200°C for 30 minutes after drying. The temperature of the back of the aluminum plate relative to the front is 300 to 350°C, and the aluminum plate will not be burned through. In contrast, another aluminum plate that is not sprayed with the high heat-insulating and high fire-resistant aerogel fire-retardant coating has its front sprayed at a high temperature of 1200°C for about 1 minute, and the aluminum plate is burned through.
9. The preparation method according to any one of claims 1 to 4, characterized in that: The aerogel fireproof and heat-insulating coating is used to prevent thermal runaway or thermal escape of lithium battery modules in electric vehicles; The aerogel fireproof and heat-insulating coating is used to reduce the serious deformation of the iron plate caused by the high temperature difference when the fire door or fireproof iron rolling door is sprayed with a high temperature flame of 850 to 1250°C for 1 to 3 hours; The aerogel fireproof and heat-insulating coating is used on the surface of high-temperature smelting boiler structures or military aerospace high-speed carriers as an insulation layer or insulation fireproof layer to reduce heat loss in pipelines or equipment platform interfaces, improve energy conservation and carbon reduction effects, or to block high heat generated by air friction to reduce damage to precision detection components inside military aerospace high-speed vehicles.
10. An aerogel fireproof and heat-insulating coating, characterized in that: Aerogel particles of different particle sizes and hydrophilicity and hydrophobicity are formed by adding an inorganic glue solution or an inorganic glue / organic glue solution, wherein the inorganic glue comprises water glass, inorganic silicone resin, copper oxide-phosphate glue, silicate glue, inorganic silicon polymer glue, phosphate-silicate glue, sulfate glue, magnesium oxide-silicon dioxide-borax inorganic glue or any combination thereof; The organic glue comprises polyimide, polyetherimide, polyphenylene ether, polyphenylene sulfide, polyetherketone liquid crystal polymer, polytetrafluoroethylene, polymelamine, polyphenolic acid, polymelamine-formaldehyde, high temperature resistant silicone, silicone modified polyurethane, silicone modified acrylate, silicone modified polyvinyl alcohol, organic thermosetting resin selected from the group consisting of epoxy resin, organic high temperature resistant silicone resin and silicone modified epoxy resin, or any combination thereof.
Citation Information
Patent Citations
Aerogel thermal insulation coating and preparation method thereof
CN104497688A
Method for producing aerogel and inorganic fiber composite gel material having high temperature resistance, heat insulation and fire resistance, and use of product thereof
JP2021172565A
Low-k dielectric aerogel powder and low-k dielectric aerogel suspension, composite film and preparation method therefor
TWI793839B
Method for producing a high temperature resistant, heat insulating, and fireproof composite glue composed of an aerogel and an inorganic fiber and the application of the related product
US20210332270A1
Cited By
Hydrophobic non-intumescent aerogel fireproof coating for steel structure and preparation method of hydrophobic non-intumescent aerogel fireproof coating
CN120865745A
Fire-resistant and heat-insulating aerogel coating, preparation method therefor and use thereof
JP2026039691A