Bottle liner pad of thermos bottle
A thermos bottle and gall pad technology, which is used in household appliances, heat-insulating utensils, applications, etc., can solve the problems of asbestos piercing into the cavity wall of the respiratory tract and inflammation of the respiratory tract of operators, and achieve the effect of eliminating harm and simple production process.
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2012-12-19
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a liner pad for a thermos bottle. Background technique
[0002] At present, asbestos is the main ingredient used in thermos liner pads, and its material form is fiber and powder. Due to the special form of asbestos, during a series of production processes such as preparation, molding, and drying, asbestos fibers or The powder is easily scattered in the air and inhaled by the operator into the respiratory tract, causing inflammation of the operator's respiratory tract, and even fibrous asbestos penetrates into the cavity wall of the respiratory tract, resulting in silicosis. Because asbestos is carcinogenic, there is the possibility of infecting cancerous mesothelioma and lung cancer in the serious environment of asbestos dust. Therefore, the production of this liner liner needs to be improved. Contents of the invention
[0003] The technical problem to be solved by the present invention is to provide a thermos liner liner, w...
Examples
Example Embodiment
[0028] Example 1:
[0029] A thermos flask bottle liner pad, its formula composition and weight are:
[0030] Alumina fiber: 550g
[0031] Light calcium carbonate: 50g
[0032] Clay: 1900g
[0033] Montmorillonite: 250g
[0034] Quartz: 550g
[0035] Deionized water: 1000g.
[0036] Preparation method: fully stir and mix alumina fiber, light calcium carbonate, clay, montmorillonite and quartz at a stirring speed of 1500 rpm, stirring for 10 minutes to obtain a mixed material; add deionization to the mixed material Continue to stir the water for 30 minutes, the stirring speed is 1000 rpm, and then pour the material into the mold to dry and shape, the drying temperature is 60 ℃, the drying time is 15 minutes, and the bottle gasket can be obtained after demolding .
Example Embodiment
[0037] Example 2:
[0038] A thermos flask bottle liner pad, its formula composition and weight are:
[0039] Alumina fiber: 1000g
[0040] Light calcium carbonate: 240g
[0041] Clay: 3000g
[0042] Montmorillonite: 750g
[0043] Quartz: 1000g
[0044] Deionized water: 2500g.
[0045] Preparation method: fully stir and mix alumina fiber, light calcium carbonate, clay, montmorillonite, and quartz at a stirring speed of 2000 rpm, stirring for 30 minutes to obtain a mixed material; add deionization to the mixed material The water continues to stir for 60 minutes, the stirring speed is 1500 rpm, and then the material is poured into the mold to dry and shape, the drying temperature is 200 ℃, the drying time is 5 minutes, and the bottle gasket can be obtained after demolding .
Example Embodiment
[0046] Example 3:
[0047] A thermos flask bottle liner pad, its formula composition and weight are:
[0048] Alumina fiber: 150g
[0049] Light calcium carbonate: 30g
[0050] Clay: 570g
[0051] Montmorillonite: 100g
[0052] Quartz: 150g
[0053] Deionized water: 350g.
[0054] Preparation method: fully stir and mix alumina fiber, light calcium carbonate, clay, montmorillonite, and quartz at a stirring speed of 2000 rpm, stirring for 20 minutes to obtain a mixed material; add deionization to the mixed material Continue to stir the water for 450 minutes, the stirring speed is 1500 rpm, and then pour the material into the mold to dry and shape, the drying temperature is 120 ℃, the drying time is 10 minutes, after demolding, the bottle gasket can be prepared .