Copper paste for bonding, method for producing bonded body, and method for producing semiconductor device
By using copper paste for bonding composed of copper particles of specific particle size and shape in semiconductor devices, the connection reliability and cost problems at high temperatures are solved, and the efficiency and stability of pressurized bonding are achieved.
Patent Information
- Application Number
- CN202010103624.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-09-07
- Filing Date
- 2016-09-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2036-09-07
AI Technical Summary
In the bonding of semiconductor devices, connection reliability is difficult to ensure at high temperatures, especially the operating temperature rise caused by high capacity and space saving, and traditional high melting point lead solder is difficult to ensure connection reliability. At the same time, due to RoHS control, Lead-free bonding materials are required, and the use of silver nanoparticles leads to increased material costs, and copper nanoparticles require protective agents to cause sintering volume shrinkage and density reduction.
Provide a copper paste for bonding containing 0.12 μm to 0.8 μm submicron copper particles and 1 μm to 20 μm sheet-shaped micron copper particles. By limiting the aspect ratio and content of the particles, the strength of the sintered body and the connection reliability are ensured, and the addition of the sintered body is avoided. Crimp joint reduces production costs.
Achieve full bonding strength and connection reliability under no pressurization conditions, improve the chip shear strength and thermal conductivity of semiconductor devices, reduce manufacturing costs, and improve production stability.
Smart Images

Figure BDA0002387724780000351 
Figure BDA0002387724780000361 
Figure BDA0002387724780000371
Abstract
Description
[0001] The present application is a divisional application of Chinese application No. 201680051483.5, whose application date is September 7, 2016 and whose invention name is “Copper paste for bonding, method for manufacturing a bonded body, and method for manufacturing a semiconductor device”. Technical Field
[0002] The present invention relates to a copper paste for bonding, a method for producing a bonded body and a method for producing a semiconductor device using the copper paste for bonding, and a bonded body and a semiconductor device. Background Art
[0003] When manufacturing semiconductor devices, various bonding materials are used to bond semiconductor elements to lead frames (supporting members). In semiconductor devices, high-melting-point lead solder is used as a bonding material for bonding power semiconductors, LSIs, etc. that operate at high temperatures above 150°C. In recent years, due to the high capacity and space saving of semiconductor elements, the operating temperature has risen to near the melting point of high-melting-point lead solder, making it difficult to ensure connection reliability. On the other hand, with the strengthening of RoHS control, lead-free bonding materials are in demand.
[0004] Prior to this, the bonding of semiconductor elements using materials other than lead solder has been studied. For example, Patent Document 1 below proposes a technique for forming a sintered silver layer by sintering silver nanoparticles at low temperature. It is known that such sintered silver has high connection reliability for power cycles (Non-Patent Document 1).
[0005] As other materials, a technology for sintering copper particles to form a sintered copper layer has also been proposed. For example, the following patent document 2 discloses a bonding paste containing copper oxide particles and a reducing agent as a bonding material for bonding a semiconductor element to an electrode. In addition, the following patent document 3 discloses a bonding material containing copper nanoparticles, copper micron particles, copper submicron particles, or both.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 4928639
[0009] Patent Document 2: Japanese Patent No. 5006081
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-167145
[0011] Non-patent literature
[0012] Non-patent document 1: R. Khazaka, L. Mendizabal, D. Henry: J. ElecTron. Mater, 43(7), 2014, 2459-2466 Summary of the invention
[0013] Technical problem to be solved by the invention
[0014] The method described in the above-mentioned patent document 1 requires a hot compression bonding process accompanied by pressurization in order to obtain high connection reliability and densification of the sintered silver layer. When the hot compression bonding process accompanied by pressurization is performed, there are problems such as reduced production efficiency and decreased pass rate. Furthermore, when silver nanoparticles are used, a significant increase in material costs due to silver becomes a problem.
[0015] The method described in Patent Document 2 avoids volume shrinkage when copper oxide is reduced to copper by a thermocompression bonding process. However, the thermocompression bonding process has the above-mentioned problems.
[0016] The method described in the above-mentioned patent document 3 is to sinter without pressurization, but still has deficiencies in the following aspects. That is, the copper nanoparticles need to utilize a protective agent to modify the surface in order to suppress oxidation and improve dispersibility, but because the specific surface area of the copper nanoparticles is relatively large, there is a tendency for the amount of surface protective agent to increase in the bonding material based on the copper nanoparticles. In addition, in order to ensure dispersibility, there is a tendency for the amount of dispersion medium to increase. Thereby, the bonding material described in the above-mentioned patent document 3 has a tendency to increase the proportion of surface protective agent or dispersion medium, volume shrinkage during sintering, and the density after sintering is easy to reduce, and becomes difficult to ensure the sintered body strength.
[0017] An object of the present invention is to provide a copper paste for bonding that can obtain sufficient bonding strength even when bonding is performed without pressure. Another object of the present invention is to provide a method for manufacturing a bonded body and a method for manufacturing a semiconductor device using the copper paste for bonding, as well as a bonded body and a semiconductor device.
[0018] Means for solving technical problems
[0019] The present invention provides a copper paste for bonding, which is a copper paste for bonding containing metal particles and a dispersion medium, wherein the metal particles contain submicron copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less and flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is 50% by mass or less based on the total amount of the flaky micron copper particles.
[0020] According to the copper paste for joining of the present invention, even when joining without pressure is performed, sufficient joining strength can be obtained. For the reason for obtaining this effect, it is believed that by containing the above-mentioned specific submicron copper particles and the above-mentioned specific flaky micron copper particles and limiting the content of micron copper particles with an aspect ratio of less than 2, the flaky micron copper particles in the copper paste for joining become easy to be roughly parallel to the joining surface, and sufficient sintering properties can be obtained. At the same time, the volume shrinkage during sintering can be fully suppressed, and the strength of the sintered body can be ensured and the joining force with the joined surface can be improved. In addition, the copper paste for joining of the present invention can obtain the above-mentioned effect through submicron copper particles and micron copper particles, therefore, compared with the joining material with expensive copper nanoparticles as the main component, it has the advantage of being able to be supplied more cheaply and stably. Thus, for example, when manufacturing a joining body such as a semiconductor device, production stability can be further improved.
[0021] In the present specification, "thin sheet shape" includes flat plate shapes such as plate shape and scale shape. In the present specification, "aspect ratio" refers to the long side / thickness of a particle.
[0022] The copper paste for bonding of the present invention may be for bonding without pressure. In this specification, "without pressure" means a state where the bonding is subjected to the weight of the members to be bonded or to a pressure of 0.01 MPa or less in addition to the weight.
[0023] In the copper paste for bonding of the present invention, the content of submicron copper particles can be 20% by mass or more and 90% by mass or less based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles, and the content of the flaky micron copper particles can be 1% by mass or more and 90% by mass or less based on the total mass of the metal particles. When the submicron copper particles and the flaky micron copper particles are within the above range, it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding, and when the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device tends to show good chip shear strength and connection reliability.
[0024] In the copper paste for bonding of the present invention, the metal particles may contain at least one metal particle selected from nickel, silver, gold, palladium, and platinum. When the copper paste for bonding further contains the above metal particles, a sintered body formed by solid solution or dispersion of multiple metals can be obtained, so that the mechanical properties such as yield stress and fatigue strength of the sintered body can be improved, and the connection reliability can be easily improved.
[0025] The present invention also provides a method for manufacturing a joint body, which comprises the following steps: preparing a stacked body having a first component and, on one side of the direction in which the self-weight of the first component is applied, the above-mentioned copper paste for joining and a second component in sequence; and sintering the copper paste for joining under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa.
[0026] According to the method for producing a joined body of the present invention, by using the above-mentioned copper paste for joining, a joined body in which members are joined with a sufficient joining force by non-pressurized joining can be produced.
[0027] The present invention also provides a method for manufacturing a semiconductor device, which comprises the following steps: preparing a stacked body having a first component and, on one side of the first component in the direction of its own weight, the above-mentioned copper paste for bonding and a second component in sequence; sintering the copper paste for bonding under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa, wherein at least one of the first component and the second component is a semiconductor element.
[0028] According to the method for manufacturing a semiconductor device of the present invention, by using the above-mentioned copper paste for bonding, a semiconductor device having excellent die shear strength can be manufactured by non-pressurized bonding. In addition, the semiconductor device manufactured by the method for manufacturing a semiconductor device of the present invention can have excellent connection reliability.
[0029] The present invention also provides a joint body, which comprises a first member, a second member, and a sintered body of the above-mentioned copper paste for joining the first member and the second member. The first member and the second member of the joint body of the present invention are joined by a sintered body of copper having sufficient joining force. In addition, the joint body of the present invention can have excellent heat dissipation of the member by having a sintered body of copper with excellent thermal conductivity.
[0030] In the above-mentioned joint body, at least one of the first member and the second member may contain at least one metal selected from copper, nickel, silver, gold and palladium on the surface in contact with the sintered body. In this case, the adhesion between at least one of the first member and the second member and the sintered body can be further improved.
[0031] The present invention also provides a semiconductor device, which comprises a first member, a second member, and a sintered body of the above-mentioned copper paste for bonding the first member and the second member, wherein at least one of the first member and the second member is a semiconductor element. The semiconductor device of the present invention can be a semiconductor device having sufficient chip shear strength, excellent connection reliability, and excellent power cycle tolerance by having a sintered body of copper having sufficient bonding strength, thermal conductivity, and high melting point.
[0032] Effects of the Invention
[0033] According to the present invention, a copper paste for bonding that can obtain sufficient bonding strength even when bonding is performed without pressurization can be provided. The present invention can also provide a method for manufacturing a bonded structure and a method for manufacturing a semiconductor device using the copper paste for bonding, as well as a bonded structure and a semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The SEM image shows the flaky micro-copper particles MA-C025.
[0035] Figure 2 This is a schematic cross-sectional view showing an example of a bonded body produced using the copper paste for bonding according to the present embodiment.
[0036] Figure 3 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0037] Figure 4 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0038] Figure 5 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0039] Figure 6 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0040] Figure 7 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0041] Figure 8 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0042] Fig. 9 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0043] Fig.10 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0044] Fig.11 This is a SEM image showing the cross-sectional morphology of the copper paste for bonding of Example 1.
[0045] Fig.12This is a SEM image showing the cross-sectional morphology of the copper paste for bonding of Example 4.
[0046] Fig.13 This is a SEM image showing the cross-sectional morphology of the copper paste for bonding of Example 6.
[0047] Fig.14 This is a SEM image showing the cross-sectional morphology of the copper paste for bonding of Comparative Example 4.
[0048] Fig.15 1 is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Example 1.
[0049] Fig.16 This is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Example 2.
[0050] Fig.17 This is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Example 4.
[0051] Fig.18 1 is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Example 6.
[0052] Fig.19 1 is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Comparative Example 3.
[0053] Fig. 20 1 is a SEM image showing a cross section of a sintered body of a joint body using the copper paste for joining of Comparative Example 4. DETAILED DESCRIPTION
[0054] Hereinafter, a mode for carrying out the present invention (hereinafter also referred to as "this embodiment") will be described in detail. The present invention is not limited to the following embodiment.
[0055] <Copper paste for bonding>
[0056] The copper paste for bonding according to the present embodiment is a copper paste for bonding containing metal particles and a dispersion medium, wherein the metal particles include submicron copper particles and flaky micron copper particles.
[0057] (Metal Particles)
[0058] Examples of the metal particles of the present embodiment include submicron copper particles, flaky micron copper particles, other copper particles, and other metal particles.
[0059] (Submicron copper particles)
[0060] As submicron copper particles, copper particles having a particle size of 0.12 μm or more and 0.8 μm or less can be cited, for example, copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less can be used. If the volume average particle size of the submicron copper particles is 0.12 μm or more, it is easy to obtain the effect of suppressing the synthesis cost of the submicron copper particles, good dispersibility, and suppressing the amount of surface treatment agent used. When the volume average particle size of the submicron copper particles is 0.8 μm or less, it is easy to obtain the effect of excellent sintering of the submicron copper particles. From the viewpoint of further exerting the above-mentioned effects, the volume average particle size of the submicron copper particles can be 0.15 μm or more and 0.8 μm or less, 0.15 μm or more and 0.6 μm or less, 0.2 μm or more and 0.5 μm or less, or 0.3 μm or more and 0.45 μm or less.
[0061] In addition, in the present specification, the volume average particle size refers to the 50% volume average particle size. When calculating the volume average particle size of the copper particles, it can be obtained by using a light scattering particle size distribution measuring device (for example, a Shimadzu nanoparticle size distribution measuring device (SALD-7500nano, manufactured by Shimadzu Corporation)) to measure the material obtained by dispersing the copper particles used as the raw material or the dried copper particles from which the volatile components are removed from the copper paste for bonding in the dispersion medium. When using a light scattering particle size distribution measuring device, hexane, toluene, α-terpineol, etc. can be used as the dispersion medium.
[0062] The submicron copper particles may contain 10% by mass or more of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. From the viewpoint of the sinterability of the copper paste for bonding, the submicron copper particles may contain 20% by mass or more, 30% by mass or more, or 100% by mass of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. When the content ratio of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less in the submicron copper particles is 20% by mass or more, the dispersibility of the copper particles is further improved, and the increase in viscosity and the decrease in paste concentration can be further suppressed.
[0063] The particle size of the copper particles can be calculated by the following method. The particle size of the copper particles can be obtained, for example, from an SEM image. The powder of the copper particles is placed on a carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed at 5000 times using an SEM device. The quadrilateral of the copper particles circumscribed to the SEM image is plotted using image processing software, and one side is used as the particle size of the particle.
[0064] The content of the submicron copper particles can be 20% to 90% by mass, 30% to 85% by mass, 35% to 85% by mass, or 40% to 80% by mass, based on the total mass of the metal particles. When the content of the submicron copper particles is within the above range, it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding, and when the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device tends to show good chip shear strength and connection reliability.
[0065] The content of submicron copper particles is based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles, and can be 20% by mass or more and 90% by mass or less. When the above-mentioned content of submicron copper particles is 20% by mass or more, the flaky micron copper particles can be fully filled, and it becomes easy to ensure the bonding strength of the joint body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. When the above-mentioned content of submicron copper particles is 90% by mass or less, since the volume shrinkage during sintering the copper paste for bonding can be fully suppressed, it becomes easy to ensure the bonding strength of the joint body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above-mentioned effects, the content of the submicron copper particles can be 30% by mass or more and 85% by mass or less, 35% by mass or more and 85% by mass or less, or 40% by mass or more and 80% by mass or less, based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles.
[0066] The shape of the submicron copper particles is not particularly limited. Examples of the shape of the submicron copper particles include spherical, blocky, needle-like, flaky, and roughly spherical shapes and aggregates thereof. From the viewpoint of dispersibility and filling properties, the shape of the submicron copper particles may be spherical, roughly spherical, or flaky. From the viewpoint of combustibility, dispersibility, and miscibility with flaky micron particles, the shape may be spherical or roughly spherical. In this specification, "flaky" includes flat plate shapes such as plate-like and scaly.
[0067] From the viewpoint of dispersibility, filling property and miscibility with flaky micron particles, the aspect ratio of submicron copper particles may be 5 or less, or 3 or less. In this specification, "aspect ratio" means the long side / thickness of a particle. The long side and thickness of a particle can be measured, for example, by calculating from a SEM image of the particle.
[0068] Submicron copper particles can be treated with a specific surface treatment agent. Examples of specific surface treatment agents include organic acids having 8 to 16 carbon atoms. Examples of organic acids having 8 to 16 carbon atoms include octanoic acid, methylheptanoic acid, ethylhexanoic acid, propylpentanoic acid, nonanoic acid, methyloctanoic acid, ethylheptanoic acid, propylhexanoic acid, decanoic acid, methylnonanoic acid, ethyloctanoic acid, propylheptanoic acid, butylhexanoic acid, undecanoic acid, methyldecanoic acid, ethylnonanoic acid, propyloctanoic acid, butylheptanoic acid, lauric acid, methylundecanoic acid, ethyldecanoic acid, propylnonanoic acid, butyloctanoic acid, pentylheptanoic acid, tridecanoic acid, methyldodecanoic acid, ethylundecanoic acid, propyldecanoic acid, butylnonanoic acid, pentyloctanoic acid, myristic acid, methyltridecanoic acid, ethyldodecanoic acid, propylundecanoic acid, butyldecanoic acid, pentylnonanoic acid, hexyloctanoic acid, pentadecanoic acid, methyltetradecanoic acid, ethyl Saturated fatty acids such as octenyl tridecanoic acid, propyl dodecanoic acid, butyl undecanoic acid, pentyl decanoic acid, hexyl nonanoic acid, palmitic acid, methyl pentadecanoic acid, ethyl tetradecanoic acid, propyl tridecanoic acid, butyl dodecanoic acid, pentyl undecanoic acid, hexyl decanoic acid, heptyl nonanoic acid, methyl cyclohexanoic acid, ethyl cyclohexanoic acid, propyl cyclohexanoic acid, butyl cyclohexanoic acid, pentyl cyclohexanoic acid, hexyl cyclohexanoic acid, heptyl cyclohexanoic acid, octyl cyclohexanoic acid, nonyl cyclohexanoic acid; octenyl acid, nonenyl acid, methyl nonenyl acid, decenoic acid, undecenoic acid, dodecenoic acid, tridecenoic acid, tetradecenoic acid, myristic acid, pentadecenoic acid, hexadecenoic acid, palmitoleic acid, 6(Z)-hexadecenoic acid (sapienic acid The organic acid may be used alone or in combination of two or more. By combining such an organic acid with the submicron copper particles, there is a tendency to balance the dispersibility of the submicron copper particles with the separation of the organic acid during sintering.
[0069] The treatment amount of the surface treatment agent can be an amount of one to three molecular layers attached to the surface of the submicron copper particles. This amount can be determined by the number of molecular layers attached to the surface of the submicron copper particles (n), the specific surface area of the submicron copper particles (A p )(Unit: m 2 / g), molecular weight of the surface treatment agent (M s ) (unit: g / mol), minimum coating area of surface treatment agent (S S )(Unit: m 2 / ) and Avogadro's constant (N A )(6.02×10 23 Specifically, the treatment amount of the surface treatment agent is calculated as follows: the treatment amount of the surface treatment agent (mass %) = {(n·A p ·M s) / (S S ·N A +n·A p ·M s )}×100% formula is used to calculate.
[0070] The specific surface area of the submicron copper particles can be determined by measuring the dried submicron copper particles using the BET specific surface area measurement method. The minimum coating area of the surface treatment agent is 2.05×10 -19 m 2 / 1 molecule. In the case of a surface treatment agent other than these, it can be measured, for example, by calculation by a molecular model or by the method described in "Chemistry and Education" (Kamieda, Inafuku, Mori, 40 (2), 1992, p114-117). An example of a quantitative method for a surface treatment agent is shown below. The surface treatment agent can be identified by a heat-leaving gas-gas chromatograph mass spectrometer of a dry powder after the dispersion medium is removed from the copper paste for bonding, thereby determining the carbon number and molecular weight of the surface treatment agent. The carbon fraction ratio of the surface treatment agent can be analyzed by carbon fraction analysis. As a carbon fraction analysis method, for example, a high-frequency induction heating furnace combustion / infrared absorption method can be cited. The surface treatment amount can be calculated using the above formula from the carbon number, molecular weight and carbon fraction ratio of the identified surface treatment agent.
[0071] The treatment amount of the surface treatment agent may be 0.07% by mass or more and 2.1% by mass or less, 0.10% by mass or more and 1.6% by mass or less, or 0.2% by mass or more and 1.1% by mass or less.
[0072] Since the submicron copper particles have good sinterability, they can reduce problems such as high synthesis cost, poor dispersibility, and reduced volume shrinkage after sintering that are seen in bonding materials that mainly use copper nanoparticles.
[0073] As the submicron copper particles of the present embodiment, commercially available products can be used. As commercially available submicron copper particles, for example, CH-0200 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.36 μm), HT-14 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.41 μm), CT-500 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.72 μm), and Tn-Cu100 (manufactured by Taiyo Nippon Sanso Corporation, with a volume average particle size of 0.12 μm) can be cited.
[0074] (Flake-like micron copper particles)
[0075] As the flaky micron copper particles, particles containing copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be cited. For example, copper particles with an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be used. When the average maximum diameter and aspect ratio of the flaky micron copper particles are within the above range, the volume shrinkage during sintering of the copper paste for bonding can be sufficiently reduced, and it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the bonding copper paste is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above effect, the average maximum diameter of the flaky micron copper particles can be 1 μm or more and 10 μm or less, and can also be 3 μm or more and 10 μm or less. The maximum diameter and average maximum diameter of the flaky micron copper particles can be obtained, for example, from the SEM image of the particles, as the long diameter X of the flaky micron copper particles described later and the average value Xav of the long diameter.
[0076] The flaky micron copper particles may contain 50% or more of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoint of orientation in the joint body, reinforcement effect, and filling property of the joint paste, the flaky micron copper particles may contain 70% or more, 80% or more, or 100% of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoint of suppressing joint failure, the flaky micron copper particles preferably do not contain particles having a size exceeding the joint thickness, such as particles having a maximum diameter exceeding 20 μm.
[0077] The aspect ratio of the flaky micron copper particles can be 4 or more, and can also be 6 or more. When the aspect ratio is within the above range, the flaky micron copper particles in the copper paste for bonding are oriented approximately parallel to the bonding surface, thereby suppressing the volume shrinkage when the copper paste for bonding is sintered, and it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding semiconductor elements, the semiconductor device tends to show good chip shear strength and connection reliability.
[0078] The content of the flaky micron copper particles can be 1% by mass or more and 90% by mass or less, 10% by mass or more and 70% by mass or less, or 20% by mass or more and 50% by mass or less, based on the total mass of the metal particles. When the content of the flaky micron copper particles is within the above range, it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device tends to show good chip shear strength and connection reliability.
[0079] The sum of the content of submicron copper particles and the content of flaky micron copper particles can be 80% or more by mass based on the total mass of the metal particles. When the content of submicron copper particles and the sum of the content of micron copper particles are within the above range, the volume shrinkage during sintering of the copper paste for bonding can be sufficiently reduced, and it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above-mentioned effects, the sum of the content of submicron copper particles and the content of flaky micron copper particles can be 90% or more by mass, 95% or more by mass, or 100% by mass based on the total mass of the metal particles.
[0080] The shape of the flaky micron copper particles of the present embodiment can also be specified by the parameters of the long diameter (maximum diameter) X, the median diameter Y (width), and the short diameter (thickness) T. The long diameter X is the distance between two parallel planes selected in a manner that the distance between the two planes is maximized in the three-dimensional shape of the flaky micron copper particles. The median diameter Y is the distance between two parallel planes selected in a manner that is orthogonal to the two parallel planes that give the long diameter X and are circumscribed in a manner that the distance between the two parallel planes is maximized. The short diameter T is the distance between two parallel planes selected in a manner that is orthogonal to the two parallel planes that give the long diameter X and the two parallel planes that are circumscribed in a manner that the distance between the two parallel planes is maximized.
[0081] The average value Xav of the major diameter can be 1 μm to 20.0 μm, 1 μm to 10 μm, or 3 μm to 10 μm. When Xav is within the above range, the sintered body of the copper paste for sintering bonding can be easily formed with an appropriate thickness in the bonded body manufactured by the copper paste for sintering bonding.
[0082] Xav / Tav, which is the ratio (aspect ratio) of the average value of the long diameter Xav to the average value of the short diameter Tav, can be 4.0 or more, 6.0 or more, or 10.0 or more. When Xav / Tav is within the above range, the flaky micron copper particles in the copper paste for bonding are easily oriented roughly parallel to the bonding surface, which can suppress the volume shrinkage during sintering of the copper paste for bonding, and make it easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, it is easy to improve the chip shear strength and connection reliability of the semiconductor device.
[0083] Xav / Yav, which is the ratio of the average value Xav of the major diameter to the average value Yav of the median diameter, can be less than 2.0, less than 1.7, or less than 1.5. When Xav / Yav is within the above range, the shape of the flaky micron copper particles becomes a flaky particle with a certain degree of area, and the flaky micron copper particles in the copper paste for bonding are easily oriented roughly parallel to the bonding surface, which can suppress the volume shrinkage during sintering of the copper paste for bonding, and become easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, it is easy to improve the chip shear strength and connection reliability of the semiconductor device. When Xav / Yav exceeds 2.0, it means that the shape of the flaky micron copper particles is close to a slender line.
[0084] Yav / Tav, which is the ratio of the average value of the median diameter Yav to the average value of the short diameter Tav, can be 2.5 or more, 4.0 or more, or 8.0 or more. When Yav / Tav is within the above range, the flaky micron copper particles in the copper paste for bonding are easily oriented roughly parallel to the bonding surface, which can suppress the volume shrinkage during sintering of the copper paste for bonding, and make it easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, it is easy to improve the chip shear strength and connection reliability of the semiconductor device.
[0085] The method of obtaining the major diameter X and median diameter Y of the flaky micron copper particles from the SEM image is exemplified. The powder of the flaky micron copper particles is placed on a carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed using a SEM device at 5000 times magnification. Figure 1 This is a SEM image of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.), which is an example of a flaky micron copper particle. A rectangle of a flaky micron copper particle 9 circumscribed in the SEM image is plotted using image processing software, with the long side of the rectangle being the major diameter X of the particle and the short side of the rectangle being the median diameter Y of the particle. Using a plurality of SEM images, the measurement is performed on more than 50 flaky micron copper particles, and the average value Xav of the major diameter and the average value Yav of the median diameter are calculated.
[0086] An example of a method for determining the short diameter T of flaky micron copper particles from an SEM image is given. A copper paste containing flaky micron copper particles is printed on a copper substrate and a silicon chip is mounted. The copper paste is dried in air at 100°C for 30 minutes using a heating plate or the like, thereby preparing a joint in which the copper plate and the silicon chip are weakly bonded by the dried copper paste for bonding. The joint is cured using epoxy injection molding resin, and the cured sample is ground using abrasive paper to expose a cross section near the center of the joint. The cross section is processed using a cross section polisher (CP) using argon ions to prepare a sample for SEM. The sample for SEM is observed using an SEM device at 5000 times. Figure 6 The SEM image of the dried film of the copper paste for bonding when the copper paste for bonding was dried at 100°C for 30 minutes in order to sandwich the copper paste for bonding described in Example 6 between the chip and the substrate. The shape of the flaky micron copper particles in the SEM image was plotted using image processing software to circumscribe the rectangle, and the short side of the rectangle was taken as the short diameter T of the particle. Using multiple SEM images, the measurement was performed on more than 50 flaky micron copper particles to obtain the average value Tav of the short diameter.
[0087] The image processing software is not particularly limited, and for example, Microsoft PowerPoint (manufactured by Microsoft Corporation) or ImageJ (manufactured by the National Institutes of Health, USA) can be used.
[0088] There is no particular limitation on whether the flaky micron copper particles are treated with a surface treatment agent. From the viewpoint of dispersion stability and oxidation resistance, the flaky micron copper particles can be treated with a surface treatment agent. The surface treatment agent can also be removed during bonding. Examples of such surface treatment agents include aliphatic carboxylic acids such as palmitic acid, stearic acid, arachidic acid, and oleic acid; aromatic carboxylic acids such as terephthalic acid, pyromellitic acid, and o-phenoxybenzoic acid; aliphatic alcohols such as cetyl alcohol, stearyl alcohol, isobornyl cyclohexanol, and tetraethylene glycol; aromatic alcohols such as p-phenylphenol; alkylamines such as octylamine, dodecylamine, and stearylamine; aliphatic nitriles such as stearonitrile and decanoonitrile; silane coupling agents such as alkylalkoxysilanes; polymer treatment agents such as polyethylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, and silicone oligomers. The surface treatment agent can be used alone or in combination of two or more.
[0089] The treatment amount of the surface treatment agent can be an amount of more than one molecular layer on the particle surface. The treatment amount of this surface treatment agent varies with the specific surface area of the flaky micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent. The treatment amount of the surface treatment agent is usually 0.001 mass % or more. For the specific surface area of the flaky micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent, the above method can be used to obtain.
[0090] When the copper paste for bonding is prepared only from the above-mentioned submicron copper particles, the volume shrinkage and sintering shrinkage accompanying the drying of the dispersion medium are large, so it is easy to peel off from the bonded surface during the sintering of the copper paste for bonding, and it is difficult to obtain sufficient chip shear strength and connection reliability in the bonding of semiconductor elements, etc. By using submicron copper particles and flaky micron copper particles in combination, the volume shrinkage during sintering of the copper paste for bonding can be suppressed, and the bonded body can have sufficient bonding strength. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device can obtain the effect of showing good chip shear strength and connection reliability.
[0091] In the copper paste for bonding of the present embodiment, the content of the micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is preferably 50% by mass or less, and more preferably 30% by mass or less, based on the total amount of the flaky micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more. By limiting the content of the micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2, the flaky micron copper particles in the copper paste for bonding become easy to be oriented roughly parallel to the bonding surface, and the volume shrinkage during sintering of the copper paste for bonding can be further effectively suppressed. As a result, it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding, and when the copper paste for bonding is used for bonding of semiconductor elements, it is easy to improve the chip shear strength and connection reliability of the semiconductor device. From the perspective of making it easier to obtain this effect, the content of micron copper particles with a maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2 can be 20 mass % or less, or 10 mass % or less, based on the total amount of flaky micron copper particles with a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more.
[0092] As the flaky micron copper particles of the present embodiment, commercially available products can be used. As commercially available flaky micron copper particles, for example, MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd., with an average maximum diameter of 4.1 μm), 3L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with a volume maximum diameter of 7.3 μm), 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd., with an average maximum diameter of 5.8 μm), and 2L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with an average maximum diameter of 9 μm) can be cited.
[0093] In the copper paste for bonding of the present embodiment, as the micron copper particles to be blended, flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be used, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 can be used, based on the total amount of the flaky micron copper particles, and preferably 30% or less. When commercially available flaky micron copper particles are used, flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be selected, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 can be used, based on the total amount of the flaky micron copper particles, and preferably 30% or less.
[0094] (Other metal particles except copper particles)
[0095] As metal particles, other metal particles other than submicron copper particles and micron copper particles may be contained, for example, particles such as nickel, silver, gold, palladium, and platinum may be contained. Other metal particles may have a volume average particle size of 0.01 μm or more and 10 μm or less, 0.01 μm or more and 5 μm or less, or 0.05 μm or more and 3 μm or less. When other metal particles are contained, their content may be less than 20% by mass or less than 10% by mass based on the total mass of the metal particles from the viewpoint of obtaining sufficient bonding. Other metal particles may also be contained. The shape of other metal particles is not particularly limited.
[0096] By containing metal particles other than copper particles, a sintered body formed by solid solution or dispersion of multiple metals can be obtained, thereby improving the mechanical properties of the sintered body such as yield stress and fatigue strength, and the connection reliability is easily improved. In addition, by adding multiple metal particles, the sintered body of the copper paste for bonding can have sufficient bonding strength relative to a specific bonded body. When the copper paste for bonding is used for bonding semiconductor elements, the chip shear strength and connection reliability of the semiconductor device are easily improved.
[0097] (Dispersion Medium)
[0098] The dispersion medium is not particularly limited and may be a volatile dispersion medium. Examples of the volatile dispersion medium include monohydric and polyhydric alcohols such as pentanol, hexanol, heptanol, octanol, decanol, ethylene glycol, diethylene glycol, propylene glycol, butanediol, α-terpineol, and isobornylcyclohexanol (MTPH); ethylene glycol butyl ether, ethylene glycol phenyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, triethylene glycol methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol propyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol Ethers such as propyl ether, dipropylene glycol butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol methyl ether, and tripropylene glycol dimethyl ether; esters such as ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate (DPMA), ethyl lactate, butyl lactate, γ-butyrolactone, and propylene carbonate; acid amides such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide; aliphatic hydrocarbons such as cyclohexanone, octane, nonane, decane, and undecane; aromatic hydrocarbons such as benzene, toluene, and xylene; mercaptans having an alkyl group with a carbon number of 1 to 18; mercaptans having a cycloalkyl group with a carbon number of 5 to 7. Examples of the mercaptans having an alkyl group having 1 to 18 carbon atoms include ethyl mercaptan, n-propyl mercaptan, isopropyl mercaptan, n-butyl mercaptan, isobutyl mercaptan, tert-butyl mercaptan, pentyl mercaptan, hexyl mercaptan, and dodecyl mercaptan. Examples of the mercaptans having a cycloalkyl group having 5 to 7 carbon atoms include cyclopentyl mercaptan, cyclohexyl mercaptan, and cycloheptyl mercaptan.
[0099] The content of the dispersion medium may be 5 to 50 parts by mass based on 100 parts by mass of the total mass of the metal particles. When the content of the dispersion medium is within the above range, the viscosity of the copper paste for bonding can be adjusted to be more appropriate, and the sintering of the copper particles is less likely to be inhibited.
[0100] (additive)
[0101] The copper paste for bonding may further contain, as required, a wettability enhancer such as a nonionic surfactant or a fluorine-based surfactant, a defoamer such as silicone oil, an ion scavenger such as an inorganic ion exchanger, or the like.
[0102] As one form of the copper paste for joining according to the present embodiment, the following copper paste for joining can be cited: the above-mentioned metal particles contain submicron copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less, preferably 0.15 μm or more and 0.8 μm or less, and flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is 50 mass % or less, preferably 30 mass % or less, based on the total amount of the above-mentioned flaky micron copper particles.
[0103] As the copper paste for bonding, the following substances may be mixed:
[0104] (1) submicron copper particles having a volume average particle size of 0.12 μm to 0.8 μm, preferably 0.15 μm to 0.8 μm; and
[0105] (2) The present invention contains flaky micron copper particles having an average maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, wherein the content of micron copper particles having an average maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2 is 50% by mass or less, preferably 30% by mass or less, based on the total amount of the flaky micron copper particles.
[0106] In addition, as another embodiment of the copper paste for bonding of the present embodiment, the following copper paste for bonding can be cited: containing metal particles and a dispersion medium, the metal particles contain submicron copper particles with a maximum diameter of 0.12 μm or more and 0.8 μm or less, preferably 0.15 μm or more and 0.8 μm or less, and flaky micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more, and the content of micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is 50% by mass or less, preferably 30% by mass or less, based on the total amount of flaky micron copper particles. The maximum diameter of the particles is obtained by observing the copper particles used as the raw material or the dry copper particles from which the volatile components are removed from the copper paste for bonding using a scanning electron microscope (SEM). The content of the submicron copper particles and flaky micron copper particles of the present embodiment can be the same as the above range.
[0107] (Preparation of copper paste for bonding)
[0108] The copper paste for bonding can be prepared by mixing the above-mentioned submicron copper particles, flaky micron copper particles, other metal particles and any additives in a dispersion medium. After mixing the components, stirring treatment can also be performed. The copper paste for bonding can also adjust the maximum particle size of the dispersion by classification operation. At this time, the maximum particle size of the dispersion can be less than 20 μm, and can also be less than 10 μm.
[0109] The copper paste for bonding can also be prepared by mixing submicron copper particles, a surface treatment agent, and a dispersion medium in advance, performing a dispersion treatment to prepare a dispersion of submicron copper particles, and then mixing thin flaky micron copper particles, other metal particles, and any additives. By following this sequence, the dispersibility of the submicron copper particles is improved, the miscibility with the thin flaky micron copper particles becomes good, and the performance of the copper paste for bonding is further improved. It is also possible to remove agglomerates from the dispersion of submicron copper particles by a classification operation.
[0110] The stirring treatment can be performed using a stirrer. Examples of the stirrer include a rotation-revolution type stirring device, a Raikai machine, a twin-screw kneader, a three-roll mill, a planetary mixer, and a thin-layer shear disperser.
[0111] The classification operation can be performed by, for example, filtration, natural sedimentation, or centrifugal separation. Examples of the filter for filtration include metal meshes, metal filters, and nylon meshes.
[0112] Examples of the dispersion treatment include a thin layer shear disperser, a bead mill, an ultrasonic homogenizer, a high shear stirrer, a narrow gap three-roll mill, a wet ultrafine particle device, a supersonic jet mill, and an ultrahigh pressure homogenizer.
[0113] The viscosity of the copper paste for bonding can be adjusted to be suitable for various printing and coating techniques during molding. The viscosity of the copper paste for bonding can be, for example, 0.05 Pa·s to 2.0 Pa·s as the Casson viscosity at 25°C, or 0.06 Pa·s to 1.0 Pa·s.
[0114] When the copper paste for bonding of the present embodiment is disposed on or between components by coating or the like, the flaky micron copper particles tend to be oriented roughly parallel to the interface with the component (interface between the paste layer and the component). At this time, the degree of orientation order S can be used to indicate how horizontal the flaky micron copper particles are relative to the interface. The degree of orientation order S can be calculated using formula (1).
[0115] S=1 / 2×(3<cos 2 θ>-1) (1)
[0116] Where θ represents the angle between the interface and the thin-film copper particles, <cos 2θ> represents multiple cos 2 The average value of θ.
[0117] The degree of orientation order S may be greater than or equal to 0.88 and less than or equal to 1.00. When the degree of orientation order S is within this range, the flaky micron copper particles in the copper paste for bonding are oriented approximately parallel to the bonding surface. Therefore, the volume shrinkage during sintering of the copper paste for bonding can be suppressed, and it becomes easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, it is easy to improve the chip shear strength and connection reliability of the semiconductor device.
[0118] The degree of orientation order S can be obtained, for example, from the SEM image of the dried body of the copper paste for bonding. The following is an example of a method for obtaining the degree of orientation order S from the SEM image. The copper paste for bonding is printed on a copper substrate and a silicon chip is mounted. It is sintered in air at 100°C for 30 minutes using a heating plate or the like to prepare a bond in which the copper plate and the silicon chip are weakly bonded by the dried copper paste for bonding. The bond is injected into the bond in such a way that the entire bond is embedded in an epoxy injection molding resin and cured. The bond after injection molding is sheared near the cross section to be observed, and the cross section is ground by grinding and CP processing is performed to prepare a sample. The cross section of the sample is observed at 5000 times using an SEM device. For the obtained cross-sectional image, the angle between the major axis of the source shape of the flaky micron copper particles and the interface is measured using image processing software with an angle measurement function. The shape of 50 or more flaky micron copper particles selected at random is measured and substituted into formula (1) to obtain the degree of orientation order S. There is no particular limitation on the image processing software, and for example, ImageJ (manufactured by the National Institutes of Health) can be used. The degree of orientation order S takes a value of 0 to 1, 1 in a completely oriented state and 0 in a completely random state.
[0119] According to the copper paste for joining of the present embodiment, by using the above-mentioned submicron copper particles and the above-mentioned flaky micron copper particles and limiting the content of specific micron copper particles, good sintering properties can be obtained, and then the volume shrinkage during sintering can be suppressed. Therefore, the copper paste for joining of the present embodiment can ensure the joining force with the component without applying excessive pressure, and the joining body manufactured by the sintering copper paste for joining can have sufficient joining strength. When the copper paste for joining is used for the joining of semiconductor elements, the semiconductor device shows good chip shear strength and connection reliability. That is, the copper paste for joining of the present embodiment can also be used as a joining material for non-pressurized joining. In addition, according to the copper paste for joining of the present embodiment, by using relatively cheap copper particles, the manufacturing cost can be suppressed and mass production can be carried out. In particular, the copper paste for joining of the present embodiment can obtain the above-mentioned effect through submicron copper particles and micron copper particles, so compared with the joining material with expensive copper nanoparticles as the main component, it has the advantage of being cheaper and more stably supplied. Thus, when manufacturing joining bodies such as semiconductor devices, for example, production stability can be further improved.
[0120] <Joint body and semiconductor device>
[0121] The following is a reference to the attached Figure 1 The preferred embodiment will be described in detail. In addition, in the drawings, the same or corresponding parts are given the same symbols, and repeated descriptions are omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0122] Figure 2 This is a schematic cross-sectional view showing an example of a bonded body manufactured using the bonding copper paste of the present embodiment. The bonded body 100 of the present embodiment includes a first member 2, a second member 3, and a sintered body 1 of the bonding copper paste bonding the first member and the second member.
[0123] As the first component 2 and the second component 3, for example, there can be cited semiconductor elements such as IGBT, diode, Schottky barrier diode, MOS-FET, thyristor, logic circuit, sensor, analog integrated circuit, LED, semiconductor laser, signal transmitter, etc., lead frame, ceramic substrate with metal plate (such as DBC), LED package and other semiconductor element mounting substrate, metal wiring such as copper tape and metal frame, blocks such as metal blocks, power supply components such as terminals, heat dissipation plates, water-cooling plates, etc.
[0124] The first component 2 and the second component 3 may contain metal in the surfaces 4a and 4b in contact with the sintered body of the copper paste for bonding. As metals, for example, copper, nickel, silver, gold, palladium, platinum, lead, tin, cobalt, etc. can be cited. One metal can be used alone, or two or more metals can be used in combination. In addition, the surface in contact with the sintered body can be an alloy containing the above metals. As metals used in alloys, in addition to the above metals, zinc, manganese, aluminum, beryllium, titanium, chromium, iron, molybdenum, etc. can also be cited. As components containing metal in the surface in contact with the sintered body, for example, components with various metal plating, wires, chips with metal plating, heat sinks, ceramic substrates with metal plates, lead frames with various metal plating or lead frames formed by various metals, copper plates, copper foils. In addition, when the second component 3 is a semiconductor element, the first component 2 can also be a block with thermal conductivity and electrical conductivity such as a metal wiring such as a metal frame, a metal block, etc.
[0125] The die shear strength of the bonded body may be 10 MPa or more, 15 MPa or more, 20 MPa or more, or 30 MPa or more, from the viewpoint of sufficiently bonding the first member and the second member. The die shear strength may be measured using a universal bond strength tester (4000 series, manufactured by DAGE).
[0126] The thermal conductivity of the sintered body of the copper paste for bonding may be 100 W / (m·K) or more, 120 W / (m·K) or more, or 150 W / (m·K) or more from the viewpoint of heat dissipation and connection reliability at high temperatures. The thermal conductivity can be obtained from the thermal diffusivity, specific heat capacity, and density of the sintered body of the copper paste for bonding.
[0127] The orientation order S of the flaky micron copper particles in the bonded body may be 0.88 or more and 1.00 or less. The orientation order S of the bonded body can be determined by the above method using the bonded body as the analysis object instead of the weakly bonded body formed by the dried copper paste for bonding.
[0128] Hereinafter, a method for producing a joined body using the copper paste for joining according to the present embodiment will be described.
[0129] The method for manufacturing a joint body using the copper paste for joining of the present embodiment comprises the following steps: preparing a stacked body having a first component, and the copper paste for joining and a second component sequentially arranged on one side in the direction of the self-weight of the first component, and sintering the copper paste for joining under the self-weight of the first component or under the self-weight of the first component and a pressure of less than 0.01 MPa.
[0130] The above-mentioned laminated body can be prepared, for example, by providing the copper paste for bonding of the present embodiment on a necessary portion of the second member and then placing the first member on the copper paste for bonding.
[0131] As a method of setting the copper paste for bonding of the present embodiment on the necessary part of the second member, a method of depositing the copper paste for bonding may be used. As such method, for example, screen printing, transfer printing, offset printing, inkjet printing, dispenser, jet dispenser, needle dispenser, comma coater, slit coater, die coater, gravure coater, slit coating, relief printing, gravure printing, gravure printing, steel screen printing, soft etching, rod coating, applicator, particle deposition method, spray coater, spin coater, dip coater, electrodeposition coating, etc. may be used. The thickness of the copper paste for bonding may be greater than 1 μm and less than 1000 μm, greater than 10 μm and less than 500 μm, greater than 50 μm and less than 200 μm, greater than 10 μm and less than 3000 μm, greater than 15 μm and less than 500 μm, greater than 20 μm and less than 300 μm, greater than 5 μm and less than 500 μm, greater than 10 μm and less than 250 μm, or greater than 15 μm and less than 150 μm.
[0132] The copper paste for bonding provided on the second member can also be properly dried from the viewpoint of suppressing the flow and occurrence of pores during sintering. The ambient gas during drying can be in the atmosphere, or in an oxygen-free ambient gas such as nitrogen or a rare gas, or in a reducing ambient gas such as hydrogen or formic acid. The drying method can be drying by placing at room temperature, or heating drying, or reduced pressure drying. For example, heating drying or reduced pressure drying can use a heating plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, a hot plate pressing device, etc. The drying temperature and time can be appropriately adjusted according to the type and amount of the dispersion medium used. As the drying temperature and time, for example, it can be above 50°C and below 180°C, and dried for more than 1 minute and less than 120 minutes.
[0133] Examples of a method for placing the first member on the copper paste for bonding include a chip mounter, a flip chip bonding machine, and a positioning jig made of carbon or ceramics.
[0134] The copper paste for bonding can be sintered by heating the laminate. The heating treatment can be performed using, for example, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, etc.
[0135] The atmosphere during sintering may be an oxygen-free atmosphere from the viewpoint of suppressing oxidation of the sintered body, the first component, and the second component. The atmosphere during sintering may also be a reducing atmosphere from the viewpoint of removing the surface oxides of the copper particles of the copper paste for bonding. As an oxygen-free atmosphere, for example, nitrogen, a rare gas, or the like may be introduced or vacuum may be used. As a reducing atmosphere, for example, pure hydrogen, a mixed gas of hydrogen and nitrogen representing the composition gas, nitrogen containing formic acid gas, a mixed gas of hydrogen and a rare gas, a rare gas containing formic acid gas, etc. may be used.
[0136] The maximum temperature during the heat treatment may be 250° C. or higher and 450° C. or lower, 250° C. or higher and 400° C. or lower, or 250° C. or higher and 350° C. or lower, from the viewpoint of reducing thermal damage to the first member and the second member and improving the yield. When the maximum temperature is 200° C. or higher and the maximum temperature holding time is 60 minutes or less, sintering tends to proceed sufficiently.
[0137] The holding time at the maximum temperature may be 1 minute to 60 minutes, 1 minute to less than 40 minutes, or 1 minute to less than 30 minutes, from the viewpoint of completely volatilizing the dispersion medium and improving the yield.
[0138] By using the copper paste for bonding of the present embodiment, when the stack is sintered, the bonded body has sufficient bonding strength even when bonding is performed without pressure. That is, sufficient bonding strength can be obtained when only the deadweight generated by the first member stacked on the copper paste for bonding is applied, or when a pressure of less than 0.01MPa, preferably less than 0.005MPa, is applied in addition to the deadweight of the first member. When the pressure applied during sintering is within the above range, since no special pressurized connection is required, the porosity can be reduced without compromising the pass rate, and the chip shear strength and connection reliability can be further improved. As a method for subjecting the copper paste for bonding to a pressure of less than 0.01MPa, for example, a method of placing a weight on the first member can be cited.
[0139] In the above-mentioned joint body, at least one of the first component and the second component can be a semiconductor element. As semiconductor elements, for example, power modules, signal transmitters, amplifiers, LED modules, etc. formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, etc. can be cited. At this time, the above-mentioned joint body becomes a semiconductor device. The resulting semiconductor device can have sufficient chip shear strength and connection reliability.
[0140] Figure 3 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment. Figure 3 The semiconductor device 110 shown is formed of a semiconductor element 8 connected to a lead frame 5a via a sintered body 1 of a copper paste for bonding according to the present embodiment, and a molding resin 7 molding the semiconductor element 8. The semiconductor element 8 is connected to the lead frame 5b via a wire 6.
[0141] Examples of semiconductor devices manufactured using the copper paste for bonding according to this embodiment include power modules formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, etc., signal transmitters, amplifiers, high-brightness LED modules, sensors, and the like.
[0142] The semiconductor device can be manufactured in the same manner as the manufacturing method of the above-mentioned joint body. That is, the manufacturing method of the semiconductor device comprises the following steps: at least one of the first component and the second component uses a semiconductor element, a laminated body having a first component, and the above-mentioned copper paste for bonding and a second component are sequentially prepared on one side of the direction in which the self-weight of the first component acts, and the copper paste for bonding is sintered under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa. For example, a step of providing a copper paste for bonding on the lead frame 5a and configuring a semiconductor element 8 for heating can be cited. The obtained semiconductor device can have sufficient chip shear strength and connection reliability even when bonding is performed without pressure. The semiconductor device of this embodiment has a sintered body of copper having sufficient bonding force, thermal conductivity and high melting point, and has sufficient chip shear strength, excellent connection reliability, and excellent power cycle tolerance.
[0143] The above method can reduce the damage to the semiconductor element when the metal wiring or bulk as the first member is bonded to the semiconductor element when the second member is a semiconductor element. A semiconductor device in which a member such as a metal wiring or bulk is bonded to a semiconductor element is described below.
[0144] As an embodiment of such a semiconductor device, the following semiconductor device can be cited: a semiconductor device comprising a first electrode, a semiconductor element electrically connected to the first electrode, and a second electrode electrically connected to the semiconductor element via a metal wiring, and a sintered body having the above-mentioned copper paste for bonding between the semiconductor element and the metal wiring and between the metal wiring and the second electrode.
[0145] Figure 4 It is a schematic cross-sectional view showing an example of the above-mentioned semiconductor device. Figure 4The semiconductor device 200 shown in the figure includes an insulating substrate 21 having a first electrode 22 and a second electrode 24, a semiconductor element 23 bonded to the first electrode 22 via a sintered body 1 of the above-mentioned copper paste for bonding, and a metal wiring 25 electrically connecting the semiconductor element 23 and the second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded respectively via the sintered body 1 of the copper paste for bonding. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The semiconductor device 200 includes a copper plate 28 on the side opposite to the surface on which the above-mentioned electrodes and the like are mounted of the insulating substrate 21. The above-mentioned structure of the semiconductor device 200 is sealed with an insulator 29. The semiconductor device 200 has one semiconductor element 23 on the first electrode 22, or may have two or more. In this case, the plurality of semiconductor elements 23 can be bonded to the metal wiring 25 via the sintered body 1 of the copper paste for bonding.
[0146] Figure 5 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 5 The semiconductor device 210 shown in the figure has a block 30 provided between the semiconductor element 23 and the metal wiring 25, and the semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered body 1 of a bonding copper paste, and has other Figure 4 The structure is the same as that of the semiconductor device 200 shown in FIG.
[0147] Figure 6 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 6 The semiconductor device 220 shown in the figure further includes a semiconductor element 23 and a block 30 on the first electrode 22, and a sintered body 1 of a copper paste for bonding them. Figure 5 The semiconductor device 220 has the same structure as the semiconductor device 210 shown in the figure. The semiconductor device 220 has two semiconductor elements on the first electrode 22, and may also have three or more. In this case, the three or more semiconductor elements 23 may also be bonded to the metal wiring 25 through the sintered body 1 of the bonding copper paste via the block 30. In addition, the position of the block 30 may be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0148] Examples of the insulating substrate 21 include ceramics such as alumina, aluminum nitride, and silicon nitride, highly thermally conductive particle / resin composites, polyimide resins, and polymaleimide resins.
[0149] As metals constituting the first electrode 22, the second electrode 24 and the third electrode 26, for example, copper, nickel, silver, gold, palladium, platinum, lead, tin, cobalt, etc. can be cited. One of these metals can be used alone, or two or more can be used in combination. In addition, the electrode can also have an alloy containing the above metals on the surface in contact with the copper paste for bonding and the sintered body 1. As metals used in the alloy, in addition to the above metals, zinc, manganese, aluminum, beryllium, titanium, chromium, iron, molybdenum, etc. can also be cited.
[0150] As metal wiring, there can be mentioned metal frames having shapes such as strip, plate, cube, cylinder, L-shaped, U-shaped, and E-shaped. As the material of the metal wiring, for example, there can be mentioned silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or alloys thereof. For the purpose of oxidation resistance and adhesion, the surfaces of these metal wirings can also be coated with nickel, copper, gold, silver, etc. by plating, sputtering, etc. In addition, the width of the metal wiring can be 1 μm to 30 μm, and the thickness can be 20 μm to 5 mm.
[0151] As the block, those with excellent thermal conductivity and electrical conductivity are preferred, for example, silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or alloys thereof can be used. For oxidation resistance and adhesion, the surface of the block can also be coated with nickel, copper, gold, silver, etc. by plating, sputtering, etc. By arranging the block on the semiconductor element, the heat dissipation is further improved. The number of blocks can be appropriately changed.
[0152] Examples of the insulator 29 include silicone rubber, polymaleimide resin, polyimide resin, and polyamide-imide resin.
[0153] Figures 4 to 6 The semiconductor device shown can be used for a power module requiring a large capacity and high reliability.
[0154] Figures 4 to 6 The semiconductor device shown can be manufactured, for example, by a method comprising the following steps: preparing an insulating substrate comprising a first electrode and a second electrode, arranging a bonding copper paste, a semiconductor element, further bonding copper paste as required, a block, and a bonding copper paste on the first electrode in order from the first electrode side, arranging a bonding copper paste on the second electrode, and arranging metal wiring on the bonding copper paste on the semiconductor element or the block and the bonding copper paste on the second electrode in a manner such that the bonding copper pastes are cross-linked; and sintering the bonding copper paste under the self-weight of each component or under the self-weight of each component and a pressure of less than 0.01 MPa.
[0155] According to this manufacturing method, a semiconductor device can be manufactured without applying pressure, so bonding can be performed without deforming the metal wiring having a bridge portion, and even when a component having a smaller bonding area than the semiconductor element is bonded to the semiconductor element, damage to the semiconductor element can be further reduced.
[0156] Figure 7 It is a schematic cross-sectional view showing still another example of a semiconductor device. Figure 7 The semiconductor device 300 shown in the figure includes a first electrode 22, a semiconductor element 23 bonded to the first electrode 22 via a sintered body 1 of a copper paste for bonding, and a metal wiring 25 electrically connecting the semiconductor element 23 and the second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded respectively via the sintered body 1 of the copper paste for bonding. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The above-mentioned structure of the semiconductor device 300 is sealed with a sealing material 31. The semiconductor device 300 has one semiconductor element 23 on the first electrode 22, and may have two or more. In this case, the plurality of semiconductor elements 23 can be bonded to the metal wiring 25 via the sintered body 1 of the copper paste for bonding.
[0157] Figure 8 It is a schematic cross-sectional view showing still another example of a semiconductor device. Figure 8 The semiconductor device 310 shown in the figure has a block 30 provided between the semiconductor element 23 and the metal wiring 25, and the semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered body 1 of a bonding copper paste. Figure 7 The structure of the semiconductor device 300 is the same as that of the semiconductor device 300 shown in FIG.
[0158] Fig. 9 It is a schematic cross-sectional view showing still another example of a semiconductor device. Fig. 9 The semiconductor device 320 shown in the figure further includes a semiconductor element 23 and a bulk body 30 on the first electrode 22, and a sintered body 1 of a copper paste for bonding them. Figure 8 The semiconductor device 320 has the same structure as the semiconductor device 310 shown in the figure. The semiconductor device 320 has two semiconductor elements on the first electrode 22, and may also have three or more. In this case, the three or more semiconductor elements 23 may also be bonded to the metal wiring 25 through the block 30 and the sintered body 1 of the bonding copper paste. In addition, the position of the block 30 may be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0159] Figures 7 to 9The first electrode 22 and the second electrode 24 shown may also be a lead frame, a copper plate, a copper / molybdenum sintered body, etc.
[0160] Examples of the sealing material 31 include heat-resistant solid sealing materials and highly thermally conductive composite materials.
[0161] The sintered body 1 of the copper paste for bonding may be the same as that described in connection with the semiconductor devices 200 to 220 .
[0162] Figures 7 to 9 The semiconductor device of the embodiment shown can be used for a miniaturized power module by using a lead frame or the like as the first electrode and the second electrode. This semiconductor device can be manufactured in the same manner as the manufacturing method of the semiconductor device described above.
[0163] Furthermore, another embodiment of a semiconductor device having a structure in which a bulk body is bonded to a semiconductor element will be described.
[0164] The semiconductor device may include a first heat conducting member, a second heat conducting member, and a semiconductor element disposed between the first heat conducting member and the second heat conducting member, and a sintered body of the copper paste for bonding is provided between at least one of the first heat conducting member and the semiconductor element and between the semiconductor element and the second heat conducting member.
[0165] Fig.10 It is a schematic cross-sectional view showing an example of this embodiment. Fig.10 The semiconductor device 400 shown in the figure comprises a first heat-conducting member 32, a semiconductor element 23 joined to the first heat-conducting member 32 by a sintered body 1 of a copper paste for joining, a block 30 joined to the semiconductor element 23 by a sintered body 1 of a copper paste for joining, and a second heat-conducting member 33 joined to the block 30 by a sintered body 1 of a copper paste for joining. The semiconductor element 23 is connected to an electrode 34 via a wire 35. The first heat-conducting member 32 and the second heat-conducting member of the semiconductor device 400 are sealed with a sealing material 31. The semiconductor device 400 may have two semiconductor elements, or may have one or more than three semiconductor elements, and the number of blocks may also be appropriately changed. In addition, the position of the block 30 may also be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0166] The heat conducting member has both the function of releasing heat generated from the semiconductor element 23 to the outside and the function of serving as an electrode for electrically connecting the semiconductor element to the outside. For example, copper, aluminum, or an alloy thereof is used for such a heat conducting member.
[0167] Fig.10The semiconductor device shown can have a double-sided cooling structure with excellent heat dissipation by having heat-conducting members on both sides of the semiconductor element. This semiconductor device can be manufactured by a method having the following steps: preparing a stacked body in which a copper paste for bonding, a semiconductor element, a copper paste for bonding, a block, a copper paste for bonding, and a second heat-conducting member are stacked in order from the first heat-conducting member side on the first heat-conducting member, and sintering the copper paste for bonding under the weight of each member or under the weight of each member and a pressure of 0.01 MPa or less. In addition, the stacked body can also be stacked in the opposite order to the above.
[0168] Example
[0169] The present invention will be described in more detail below by way of examples, but the present invention is not limited to the following examples.
[0170] <Measurement conditions>
[0171] The properties of each example and comparative example were measured by the following methods.
[0172] (1) Determination of the major diameter (maximum diameter) and median diameter of the flaky micronized copper particles and determination of the average values of the major diameter and median diameter
[0173] Use a spatula to place the flaky micron copper particles on a carbon tape for SEM to make a SEM sample. Use a SEM device (ESEM XL30 manufactured by Philips or NeoScope JCM-5000 manufactured by JEOL Ltd.) to apply a voltage of 10kV to observe the SEM sample. Use Microsoft PowerPoint (manufactured by Microsoft) to read the resulting 2000 times SEM image (when reading, the image size is 17.07cm high × 22.75cm wide). Draw a straight line from one end to the other end of the scale bar at the bottom of the image (in this case, it is a scale representing 10μm), and record the length of the straight line (3.7cm in this case). Next, draw a rectangle in the shape of the source of the flaky micron copper particles. For the shape of a certain source of flaky micron copper particles, draw a rectangle of 1.81cm×1.37cm. Here, the long side of the rectangle (1.81 cm in this example) is set as the major diameter X of the flaky micron copper particle, and the short side of the rectangle (1.37 cm in this example) is set as the median diameter Y of the flaky micron copper particle. The major diameter X and median diameter Y are calculated as follows from the ratio of the 10 μm scale bar to the 3.7 cm straight line.
[0174] Long diameter X = 1.81 cm × 10 μm / 3.7 cm = 4.89 μm
[0175] Middle diameter Y = 1.37 cm × 10 μm / 3.7 cm = 3.70 μm
[0176] For the shape of the source of the flaky micron copper particles on the screen, this operation is repeated without repetition. However, the shape of the source of the flaky micron copper particles that overflows from the end of the screen and the image is cut off is not selected. The shapes of more than 50 sources of flaky micron copper particles are measured, and the average of the length measurement results is calculated. As a result, the average value Xav of the long diameter and the average value Yav of the median diameter of the flaky micron copper particles are obtained.
[0177] (2) Cross-sectional morphology observation of copper paste for bonding
[0178] On the copper plate (19×25×3mm 3 ) is placed on a stainless steel plate with a thickness of 70 μm and a metal mask with 3 rows and 3 columns of 3×3 mm square openings is applied using a metal scraper and screen printing. A 3×3 mm square with titanium, nickel and other materials formed in this order is placed on the applied copper paste. 2 A silicon chip (chip thickness: 600μm) with a nickel surface to be bonded is gently pressed with tweezers. It is mounted on a heating plate (EC HOTPLATE EC-1200N manufactured by AS ONE Co., Ltd.) and dried in air at 100°C for 30 minutes. Thus, a bond is obtained in which the copper plate and the silicon chip are weakly bonded by a dried copper paste for bonding. The bond is fixed in a cup using a sample fixture (Samplklip I, Buehler), and epoxy injection molding resin (エポマウント, Refinetec Co., Ltd.) is flowed around until the entire bond is embedded, and it is allowed to stand in a vacuum dryer and decompressed for 1 minute for degassing. Afterwards, the degassed bond is placed at room temperature for 10 hours, the epoxy injection molding resin is cured, and a sample is prepared. Use a Refine Soxel (manufactured by Refinetec Co., Ltd.) to cut the sample near the silicon chip. Use a polishing device (Refine Polisher Hv, manufactured by Refinetec Co., Ltd.) with water-resistant abrasive paper (Carbon Mac Paper, manufactured by Refinetec Co., Ltd.) to scrape the sample until it is near the center of the adhesive to expose the cross section. For the polished sample, the excess epoxy injection resin is shaved off to make it a size that can be processed by an ion milling device. Use an ion milling device (IM4000, manufactured by Hitachi High-Technologies Co., Ltd.) in CP processing mode at an argon gas flow rate of 0.07 to 0.1 cm 3The sample processed by the size processing was subjected to cross-section processing under the conditions of 1000 nm / min and 120 minutes of processing time to prepare a sample for SEM. The sample for SEM was observed by using a SEM device (NeoScope JCM-5000 manufactured by JEOL Ltd.) at an applied voltage of 10 kV.
[0179] (3) Determination of the short diameter of the flaky micron copper particles
[0180] Use Microsoft PowerPoint (manufactured by Microsoft Corporation) to read the 5000-fold SEM image obtained in "(2) Cross-sectional morphological observation of copper paste for bonding" (the image size when reading is 9.9 cm high × 11.74 cm wide). Draw a straight line from one end to the other end of the scale bar at the bottom of the image (in this case, the scale represents 5 μm), and record the length of the straight line (2.5 cm in this case). Next, draw a rectangle in the shape of the source of the flaky micron copper particles. For the shape of a certain source of flaky micron copper particles, draw a rectangle of 1.79 cm × 0.36 cm. Here, the long side of the rectangle (1.79 cm in this case) is equivalent to the long diameter X or the median diameter Y of the flaky micron copper particles. The short side of the rectangle (0.36 cm in this case) is set to the short diameter T of the flaky micron copper particles. The short diameter T is calculated as follows from the ratio of the 5 μm scale bar to the 2.5 cm straight line.
[0181] Short diameter T = 0.36cm × 5μm / 2.5cm = 0.72μm
[0182] This operation is not repeated for the shape of the source of the flaky micron copper particles on the screen. However, the flaky micron copper particles that overflow from the end of the screen and whose image is cut off are not selected. The shapes of more than 50 flaky micron copper particles are measured, and the average of the length measurement results is calculated. As a result, the average value Tav of the short diameter of the flaky micron copper particles is obtained. Using the average value Tav of the short diameter, the average value Xav of the long diameter and the average value Yav of the medium diameter obtained by "(1) Determination of the long diameter and medium diameter of flaky micron copper particles", the ratios of the long diameter / medium diameter (Xav / Yav), the long diameter / short diameter (Xav / Tav), and the medium diameter / short diameter (Yav / Tav) of the flaky micron copper particles are calculated respectively.
[0183] (4) Determination of the Orientation Order of the Copper Paste for Bonding
[0184] Use ImageJ (manufactured by the National Institutes of Health, USA) to read the 5000-fold SEM image obtained in "(2) Cross-sectional morphological observation of copper paste for bonding". As the SEM image, use the image of the interface between the substrate or silicon chip and the copper paste for bonding. Press the [T] key to display the ROI Manager window, and check the Show All check box. Select Straight Line from the main window. Use click → drag to draw a line from one end of the cross section of the flaky micron copper particle on the image to the other end, and press the [T] key to log in to the ROI Manager window. For the shape of the source of the flaky micron copper particles on the screen, this operation is repeated without repetition. However, do not select the shape of the source of the flaky micron copper particles that overflow from the end of the screen and the image is cut off. Next, press the Measure key in the ROI Manager window. Since the measured angle is displayed in the Results window, use [File] → [Save As] to save it in a file. When the interface between the substrate or silicon chip and the copper paste for bonding deviates from the horizontal relative to the image, measure its angle in the same way. The saved result file was read using Microsoft Excel. When the interface between the substrate or silicon chip and the copper paste for bonding was not horizontal with respect to the image, the angle of the bonding interface was subtracted from the measured angle data. For each angle data θ, cos 2 θ, find its average value <cos 2 θ>, substitute into S=1 / 2×(3<cos 2 θ>-1), calculate the orientation order S.
[0185] (5) Determination of chip shear strength
[0186] On the copper plate (19×25×3mm 3 ) is placed on a stainless steel plate with a thickness of 70 μm and a metal mask with 3 rows and 3 columns of 3×3 mm square openings is applied using a metal scraper and screen printing. A 3×3 mm square with titanium, nickel and other materials formed in this order is placed on the applied copper paste. 2 A silicon chip (chip thickness: 600μm) with nickel on the surface to be bonded is gently pressed with small tweezers. It is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 1L / min to replace the air with argon gas. After that, while hydrogen gas flows in at 300mL / min, the temperature is raised for 10 minutes, and sintering treatment is performed at 350℃ for 10 minutes to obtain a joint body in which the copper plate and the silicon chip are bonded by a copper sintered body. After that, the argon gas is replaced at 0.3L / min for cooling, and the joint body is taken out into the air below 50℃.
[0187] The bonding strength of the joint body was evaluated by die shear strength. A universal bonding strength tester (4000 series, manufactured by DAGE) equipped with a 1 kN load cell was used to press the silicon chip in the horizontal direction at a measuring speed of 500 μm / s and a measuring height of 100 μm to measure the die shear strength of the joint body. The average value of the values measured for 8 joint bodies was taken as the die shear strength.
[0188] (6) Density of sintered body
[0189] A 15×15 mm thick Teflon (registered trademark) plate was set 2 Opening. Place the Teflon (registered trademark) plate on a glass plate, fill the opening with copper paste for bonding, and use a metal scraper to remove the copper paste overflowing from the opening. Remove the Teflon (registered trademark) plate, install it in a tube furnace, and heat it to 150°C while flowing argon gas at 0.3L / min. Keep it for 1 hour to remove the dispersion medium. In this state, replace the gas with hydrogen at 300mL / min, raise the temperature to 350°C, and sinter for 60 minutes to obtain a sintered body. Thereafter, replace the argon gas at 0.3L / min for cooling, and take out the bonded body into the air below 50°C. Peel off the plate-shaped sintered body from the glass plate and grind it with sandpaper (No. 800) to obtain a 10×10mm 2 The plate sample is a flat plate sample with a size of . The length, width and thickness of the plate sample are measured, and the weight of the plate sample is measured. The density of the plate sample is calculated from these values.
[0190] (7) Cross-sectional morphological observation of the joint body
[0191] The conjugate was manufactured using the method described in "(5) Determination of chip shear strength". The manufactured conjugate was fixed in a cup using a sample fixture (Samplklip I, manufactured by Buehler), and epoxy injection resin (Epomer, manufactured by Refinetec Co., Ltd.) was poured around it until the entire conjugate was embedded, and the conjugate was allowed to stand in a vacuum dryer and decompressed for 1 minute for degassing. After that, the conjugate was allowed to stand at room temperature for 10 hours to cure the epoxy injection resin and prepare a sample. A Refinery Solder (manufactured by Refinetec Co., Ltd.) was used to cut the sample near the silicon chip. A polishing device (Refine Polisher Hv, manufactured by Refinetec Co., Ltd.) with water-resistant polishing paper (Carbon Mac Paper, manufactured by Refinetec Co., Ltd.) was used to cut near the center of the conjugate to expose the cross section. The excess epoxy resin was cut off from the polished sample to a size that could be processed by an ion milling device. An ion milling device (IM4000, manufactured by Hitachi High-Technologies Co., Ltd.) was used in the CP processing mode with an argon gas flow rate of 0.07 to 0.1 cm 3 The sample processed by the size processing was subjected to cross-section processing under the conditions of 1000 nm / min and 120 minutes of processing time to prepare a SEM sample. The copper sintered body cross section of the SEM sample was observed using a SEM device (NeoScope JCM-5000 manufactured by JEOL Ltd.) at an applied voltage of 10 kV.
[0192] (8) Determination of the degree of orientation order of the sintered body
[0193] The 5000-fold SEM image obtained in "(7) Cross-sectional morphological observation of the joint body" was read using ImageJ (manufactured by the National Institutes of Health, USA). As the SEM image, an image of the interface between the substrate or silicon chip and the copper paste for joining was used. The orientation order S of the joint body was obtained using the same procedure as in "(4) Determination of the orientation order of the copper paste for joining".
[0194] (9) Thermal conductivity
[0195] The thermal diffusivity was measured by a laser flash method (LFA467, manufactured by Netch) using the plate-shaped sample prepared in "(6) Density of sintered body". The thermal conductivity [W / (m·K)] of the sintered body at 25°C was calculated by the product of the thermal diffusivity, the specific heat capacity obtained by a differential scanning calorimeter (DSC8500, manufactured by PerkinElmer) and the density calculated in "(6) Density of sintered body".
[0196] (10) Temperature cycle connection reliability test
[0197] In the same manner as in "(5) Measurement of die shear strength", a copper plate (19×25×3 mm 3 ) and 3×3mm 2 A bonded body is formed by bonding a silicon chip (chip thickness: 600 μm) whose bonding surface is nickel. On the bonded body, a silicone resin (SE1880, manufactured by Dow Corning Toray Co., Ltd.) is applied using a glass pipette in a manner to cover the silicon chip, and degassed in a reduced pressure dryer for 3 minutes. After degassed, it is kept in a warm air circulation oven at 70°C for 30 minutes and in a warm air circulation oven at 150°C for 60 minutes to cure and obtain a temperature cycle test piece. The temperature cycle test piece is installed in a temperature cycle tester (TSA-72SE-W, manufactured by Espec Co., Ltd.), and a temperature cycle connection reliability test is carried out under the conditions of -40°C on the low temperature side, 200°C on the high temperature side, 15 minutes for each gradient, automatic defrost cycle, and 300 cycles. Using an ultrasonic flaw detector (Insight Insight-300), SAT images of the bonding state of the copper sintered body and the bonded body interface before and after the temperature cycle connection reliability test were obtained to check for peeling. If peeling occurred in 20% or more of the bonding area, it was evaluated as poor (×).
[0198] (Example 1)
[0199] 0.5 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.5 g of isobornyl cyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd. of Japan) as a dispersion medium and 7 g of HT-14 (manufactured by Mitsui Mining and Smelting Co., Ltd.) as submicron copper particles were mixed in a plastic bottle, and an ultrasonic homogenizer (US-600, manufactured by Nippon Seiki Co., Ltd.) was used to perform a treatment at 19.6 kHz, 600 W, and 1 minute to obtain a dispersion. 3 g of MA-C025 (manufactured by Mitsui Mining and Smelting Co., Ltd.) as flaky micron copper particles was added to the dispersion, and stirred with a spatula until the dry powder disappeared. The plastic bottle was tightly covered, and stirred at 2000 rpm for 2 minutes using a rotation-revolution type stirring device (Planetary Vacuum Mixer ARV-310, manufactured by Shinkey Co., Ltd.), and stirred at 2000 rpm for 2 minutes under reduced pressure to obtain a copper paste 1 for bonding. Various measurements and analyses were performed using the copper paste 1 for bonding.
[0200] In addition, the content of the flaky micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more in the submicron copper particles and flaky micron copper particles used above, and the content of the micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 were converted from the particle size distribution obtained by measuring 50 or more particles. Based on the converted values, the content ratio of the micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 was calculated based on the total amount of the flaky micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more.
[0201] (Example 2)
[0202] A joining copper paste 2 was obtained by the same method as in Example 1 except that 3L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd.) was used as the flaky micron copper particles. Using the joining copper paste 2, various measurements and analyses were performed.
[0203] (Example 3)
[0204] A joining copper paste 3 was obtained by the same method as in Example 1 except that 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd.) was used as the flaky micron copper particles. Using the joining copper paste 3, various measurements and analyses were performed.
[0205] (Example 4)
[0206] A copper paste 4 for bonding was obtained by the same method as in Example 1 except that TN-Cu100 (manufactured by Taiyo Nippon Sanso Corporation) was used as the submicron copper particles. Using the copper paste 4 for bonding, various measurements and analyses were performed.
[0207] (Example 5)
[0208] A joining copper paste 5 was obtained by the same method as in Example 1 except that CH-0200 (manufactured by Mitsui Mining & Smelting Co., Ltd.) was used as the submicron copper particles. Using the joining copper paste 5, various measurements and analyses were performed.
[0209] (Example 6)
[0210] A joining copper paste 6 was obtained by the same method as in Example 1 except that CT-500 (manufactured by Mitsui Mining & Smelting Co., Ltd.) was used as the copper particles. Using the joining copper paste 6, various measurements and analyses were performed.
[0211] (Example 7)
[0212] A copper paste 7 for bonding was obtained by the same method as in Example 1 except that silver particles LM1 (manufactured by Tokusen Kogyo Co., Ltd.) were used as an additive. Using the copper paste 7 for bonding, various measurements and analyses were performed.
[0213] (Example 8)
[0214] A joining copper paste 8 was obtained by the same method as in Example 1 except that nickel particles Ni-HWQ (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd.) were used as an additive. Using the joining copper paste 8, various measurements and analyses were performed.
[0215] (Example 9)
[0216] A bonding copper paste 9 was obtained by the same method as in Example 1 except that spherical copper particles 1300Y (manufactured by Mitsui Mining & Smelting Co., Ltd.) were used as micron copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2. Using the bonding copper paste 9, various measurements and analyses were performed.
[0217] (Comparative Example 1)
[0218] A copper paste 10 for bonding was obtained by the same method as in Example 1 except that no flaky micron copper particles were added. Using the copper paste 10 for bonding, various measurements and analyses were performed.
[0219] (Comparative Example 2)
[0220] A joining copper paste 11 was obtained by the same method as in Example 1 except that spherical copper particles 1300Y (manufactured by Mitsui Mining & Smelting Co., Ltd.) were used instead of the flaky micron copper particles. Using the joining copper paste 11, various measurements and analyses were performed.
[0221] (Comparative Example 3)
[0222] A joining copper paste 12 was obtained by the same method as in Example 1 except that spherical copper particles 1100Y (manufactured by Mitsui Mining & Smelting Co., Ltd.) were used instead of the flaky micron copper particles. Using the joining copper paste 12, various measurements and analyses were performed.
[0223] (Comparative Example 4)
[0224] A joining copper paste 13 was obtained by the same method as in Example 1 except that spherical copper particles 1050Y (manufactured by Mitsui Mining & Smelting Co., Ltd.) were used instead of the flaky micron copper particles. Using the joining copper paste 13, various measurements and analyses were performed.
[0225] (Comparative Example 5)
[0226] A joining copper paste 14 was obtained by the same method as in Example 1 except that spherical copper particles 1020Y (manufactured by Mitsui Mining & Smelting Co., Ltd.) were used instead of the flaky micron copper particles. Using the joining copper paste 14, various measurements and analyses were performed.
[0227] The compositions and test results of Examples and Comparative Examples are shown in Tables 1 to 3.
[0228] The shapes of the copper particles used in Examples and Comparative Examples are as follows.
[0229] (Submicron copper particles)
[0230] HT-14: 50% volume average particle size is 0.36 μm, and the content of copper particles with a particle size of 0.12 μm or more and 0.8 μm or less is 100 mass%
[0231] TN-Cu100: 50% volume average particle size is 0.12 μm, and the content of copper particles with a particle size of 0.12 μm or more and 0.8 μm or less is 90 mass %
[0232] CH-0200: 50% volume average particle size of 0.36 μm, content of copper particles with a particle size of 0.12 μm or more and 0.8 μm or less is 100 mass%
[0233] CT-500: 50% volume average particle size is 0.72 μm, and the content of copper particles with a particle size of 0.12 μm or more and 0.8 μm or less is 80 mass%
[0234] Among the submicron copper particles, the content of flaky micron copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, and the content of micron copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2 were both 0 mass %.
[0235] (Flake-like micron copper particles)
[0236] MA-C025: average maximum diameter of 4.1 μm, aspect ratio of 7.9, content of copper particles with a maximum diameter of 1 μm or more and 20 μm or less is 100 mass %
[0237] 3L3: average maximum diameter of 7.3 μm, aspect ratio of 26, content of copper particles with a maximum diameter of 1 μm or more and 20 μm or less is 100 mass %
[0238] 1110F: average maximum diameter of 5.8 μm, aspect ratio of 20, content of copper particles with a maximum diameter of 1 μm or more and 20 μm or less is 100 mass %
[0239] Among the above-mentioned flaky micron copper particles, the content of flaky micron copper particles with a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more is 100 mass%, and the content of micron copper particles with a maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2 is 0 mass%.
[0240] (Micron copper particles)
[0241] 1300Y: average maximum diameter is 3.3μm, aspect ratio is 1
[0242] In addition, the said volume average particle diameter is calculated|required by the following method.
[0243] (50% volume average particle size)
[0244] The 50% volume average particle size was measured according to the following (1) to (5) using a Shimadzu nanoparticle size distribution measuring apparatus (SALD-7500nano, manufactured by Shimadzu Corporation) and accompanying software (WingSALDII-7500-for Japanese V3., manufactured by Shimadzu Corporation).
[0245] (1) Software settings
[0246] Start WingSALDII-7500-for Japanese V3.1 using the computer attached to the measuring device, press the manual control to initialize the device. After the initialization is completed, specify the save file name, click "Next", set the measurement conditions and particle size distribution calculation conditions as follows, and click "Next".
[0247] (Measurement conditions)
[0248] Detection of diffracted / scattered light
[0249] Average times (number of measurements: 1): 128, number of measurements: 1, measurement interval (seconds): 2
[0250] ·Measurement absorbance range
[0251] Maximum value: 0.2, Minimum value: 0
[0252] Blank area / Measurement area
[0253] Maximum allowable variation of blank measurement: 150, optimal measurement range (MAX): 45000, optimal measurement range (MIN): 15000
[0254] (Particle size distribution calculation conditions)
[0255] Refractive index selection: reference sample / pure metal / semiconductor, etc. (solid value)
[0256] Sample material: 4Copper
[0257] Refractive index selection: 1.18-2.21, check "Evaluate side / rear sensors"
[0258] (2) Blank determination
[0259] The Shimadzu nanoparticle size distribution measuring device SALD-7500nano batch cell (SALD-BC75, manufactured by Shimadzu Corporation) was installed in the SALD-7500nano for measurement. α-Terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) was dripped into the batch cell with a funnel attached to the SALD-BC75 (component number S347-61030-41, manufactured by Shimadzu Corporation, hereinafter referred to as the "batch cell") using a glass pipette to reach between the two marking lines of the batch cell. Select "Diagnosis" and "Adjustment" on the screen of WingSALDII-7500-for Japanese V3. to confirm that the position sensor power is within the allowable range of the device. Click "Cancel" to return to the original screen and select blank measurement for measurement.
[0260] (3) Preparation of assay solution
[0261] 2 mg of the copper paste for bonding to be measured was placed on the stirring rod of the batch cell holder (part number S347-62301, manufactured by Shimadzu Corporation) attached to SALD-BC75, and installed in the batch cell with a funnel. Next, "Stirring" was selected on the screen of WingSALDII-7500-for Japanese V3., and stirring was performed for 15 minutes.
[0262] (4) Determination
[0263] After stirring, select "Measure" on the screen of WingSALDII-7500-for Japanese V3. to perform measurement. Repeat the steps (1) to (4) 4 times to perform 4 measurements.
[0264] (5) Statistics
[0265] Start WingSALDII-7500-for Japanese V3., click "Open", select the measured file, and display the measured data on the screen of WingSALDII-7500-for Japanese V3. Click "Overlay", and the 50.000% diameter will be displayed in the lower part of the screen, and the average value of the four times will be the 50% volume average particle diameter.
[0266] Table 1
[0267]
[0268] Table 2
[0269]
[0270] Table 3
[0271]
[0272] As shown in Tables 1 to 3, as described in "(5) Determination of chip shear strength", the bonded body using the bonding copper paste of the embodiment has good chip shear strength, thermal conductivity and connection reliability only by the pressure generated by the chip's own weight without applying special pressure when manufacturing the bonded body. On the other hand, the bonded body using the bonding copper paste of the comparative example that does not contain flaky micron copper particles cannot fully bond the chip and the substrate without applying pressure when manufacturing the bonded body.
[0273] (Cross-sectional morphology observation)
[0274] Figures 11 to 13 SEM images of dried films of copper pastes for bonding prepared by sandwiching the copper pastes for bonding of Examples 1, 4 and 6 between a chip 12 and a substrate and subjecting them to a heat treatment at 100°C for 30 minutes. In the copper pastes for bonding, a structure is adopted in which the non-flaky copper particles 11 (submicron copper particles) fill the gaps between the flaky micron copper particles 10. These copper pastes for bonding have a specific average maximum diameter and aspect ratio, and the flaky micron copper particles 10 are easily oriented approximately parallel to the interface with the chip 12 or the substrate by the shear force when printing and coating on the substrate or the slight pressure when the chip 12 is mounted.
[0275] Figures 15 to 18 SEM images of the bonded bodies prepared by sandwiching the bonding copper pastes of Examples 1, 2, 4 and 6 between the chip 12 and the substrate and performing a sintering treatment at 350°C for 25 minutes. It can be seen from these figures that the state of the bonding copper paste before sintering is reflected even after sintering. That is, the shape 14 derived from the non-flake-like copper particles fills the gap of the shape 13 derived from the flake-like micron copper particles, and the shape 13 derived from the flake-like micron copper particles is oriented roughly parallel to the bonding surface of the chip 12 or the substrate 15. The bonded body prepared using the bonding copper paste of the present invention can have a copper sintered body with higher connection reliability compared to the sintered body formed by the bonding copper paste containing only non-flake-like copper particles (such as spherical copper particles) due to the enhanced effect of the dense filling of the above-mentioned oriented structure.
[0276] Fig.14This is a SEM image of a dried film of the copper paste for bonding prepared by sandwiching the copper paste for bonding of Comparative Example 4 between a chip and a substrate and subjecting it to a heat treatment at 100° C. for 30 minutes. The copper paste for bonding of Comparative Example 4 is a copper paste for bonding containing only the non-flaky copper particles 11 . Fig.19 and 20 The SEM image of the bonded body prepared by sandwiching the bonding copper paste of Comparative Examples 3 and 4 between the chip 12 and the substrate 15 and performing a sintering treatment at 350°C for 25 minutes. The bonding copper paste prepared using only non-flaky copper particles cannot ensure sufficient bonding because the non-flaky copper particles are sintered in a form close to point contact, and the bonding area cannot be sufficiently ensured with respect to the bonded surface, and the results of the connection reliability test after bonding are not good.
[0277] From the above results, it can be seen that in an electronic device having a sintered body formed by the copper paste for bonding of the present invention as a bonding layer, even when the thermal stress generated by the difference in thermal expansion coefficients between the bonded components is applied to the bonding layer, high connection reliability can be maintained. It is believed that the reason is that the orientation structure derived from the flaky micron copper particles will hinder the propagation of cracks generated in the sintered body of the copper paste for bonding due to thermal stress, so the connection reliability is improved. In addition, since the sintered body is composed of metallic copper connected by metal bonds, it exhibits a high thermal conductivity of more than 100W / (m·K), and can quickly release heat during the installation of electronic devices with large heat release. In addition, according to the copper paste for bonding of the present invention, since it is firmly bonded by metal bonding even without pressure, the material of the bonded surface can make the chip shear strength representing the bonding strength more than 20MPa relative to copper, nickel, silver, and gold. In this way, the copper paste for bonding of the present invention has a very effective property for bonding electronic devices with large heat release such as power supply devices, logic circuits, and amplifiers. Therefore, when the copper paste for bonding of the present invention is used, a higher input power can be allowed, and the bonding agent can be operated at a high operating temperature.
[0278] Explanation of symbols
[0279] 1 Sintered body of copper paste for bonding, 2 First member, 3 Second member, 5a, 5b Lead frame, 6 Electric wire, 7 Molding resin, 8 Semiconductor element, 9 Flake-shaped micron copper particles, 10 Flake-shaped micron copper particles (unsintered), 11 Non-flake-shaped micron copper particles (unsintered), 12 Chip (material: Si, copper), 13 Shape of source of flake-shaped micron copper particles (after sintering), 14 Shape of source of non-flake-shaped micron copper particles (after sintering), 15 Substrate (copper), 100 Bonding body, 110 Semiconductor device, 21 insulating substrate, 22 first electrode, 23 semiconductor element, 24 second electrode, 25 metal wiring, 26 third electrode, 27 electric wire, 28 copper plate, 29 insulator, 30 block, 31 sealing material, 32 first heat-conducting member, 33 second heat-conducting member, 34 electrode, 35 electric wire, 200 semiconductor device, 210 semiconductor device, 220 semiconductor device, 300 semiconductor device, 310 semiconductor device, 320 semiconductor device, 400 semiconductor device.
Claims
1. A copper paste for bonding, comprising metal particles and a dispersion medium, wherein: The metal particles contain submicron copper particles having a volume average particle size of 0.3 μm or more and 0.8 μm or less and flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is 50% by mass or less, based on the total amount of the flaky micron copper particles, the content of the flaky micron copper particles is 1% by mass or more and 90% by mass or less, based on the total mass of the metal particles, and the content of the submicron copper particles is 20% by mass or more and 90% by mass or less, based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles. 2 . The copper paste for bonding according to claim 1 , which is for non-pressurized bonding.
3. The copper paste for bonding according to claim 1 or 2, wherein The metal particles include at least one metal particle selected from the group consisting of nickel, silver, gold, palladium, and platinum.
4. A method for manufacturing a joint body, comprising the following steps: preparing a stacked body having a first component, and a copper paste for joining according to any one of claims 1 to 3 and a second component on one side of the first component in the direction of its own weight, and sintering the copper paste for joining under the condition of being subjected to the own weight of the first component, or under the condition of being subjected to the own weight of the first component and a pressure of 0.01 MPa or less.
5. A method for manufacturing a semiconductor device, comprising the following steps: preparing a stacked body having a first component, and on one side of the first component in a direction in which its own weight acts, the copper paste for bonding according to any one of claims 1 to 3 and a second component in sequence, sintering the copper paste for bonding under the own weight of the first component, or under the own weight of the first component and a pressure of 0.01 MPa or less, at least one of the first component and the second component being a semiconductor element. 6 . A joined body comprising a first member, a second member, and a sintered body of the joining copper paste according to claim 1 , which joins the first member and the second member.
7. The conjugate according to claim 6, wherein: At least one of the first member and the second member contains at least one metal selected from the group consisting of copper, nickel, silver, gold, and palladium on a surface in contact with the sintered body. 8 . A semiconductor device comprising a first member, a second member, and a sintered body of the copper paste for bonding according to claim 1 for bonding the first member and the second member, wherein at least one of the first member and the second member is a semiconductor element.