Copper paste for bonding, method for producing bonded body, and method for producing semiconductor device
By using a copper paste for bonding with a specific proportion of submicron and micron copper particles, the problem of difficulty in ensuring bonding strength and reliability during pressurized bonding is solved, and efficient and economical bonding of semiconductor components is achieved, reducing material costs And improve production stability.
Patent Information
- Application Number
- CN202010141856.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-09-07
- Filing Date
- 2016-09-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2036-09-07
AI Technical Summary
The prior art is difficult to ensure bonding strength and connection reliability when semiconductor components are bonded without pressurization, and the use of high-priced copper nanoparticles leads to increased material costs and reduced production efficiency.
Using a copper paste for bonding containing 0.12 μm to 0.8 μm submicron copper particles and 2 μm to 50 μm copper particles, the density and bonding force of the sintered body are ensured through a combination of specific proportions and a surface treatment agent, thereby avoiding volume shrinkage, and realizing No pressurized bonding.
High bonding strength and connection reliability of semiconductor devices under pressure-free conditions are achieved, material costs are reduced, production stability and chip shear strength are improved.
Smart Images

Figure BDA0002399360070000301 
Figure BDA0002399360070000311 
Figure BDA0002399360070000321
Abstract
Description
[0001] The present application is a divisional application of Chinese application No. 201680051482.0, whose application date is September 7, 2016 and whose invention name is “Copper paste for bonding, method for manufacturing a bonded body, and method for manufacturing a semiconductor device”. Technical Field
[0002] The present invention relates to a copper paste for bonding, a method for producing a bonded body and a method for producing a semiconductor device using the copper paste for bonding, and a bonded body and a semiconductor device. Background Art
[0003] When manufacturing semiconductor devices, various bonding materials are used to bond semiconductor elements to lead frames (supporting members). In semiconductor devices, high-melting-point lead solder is used as a bonding material for bonding power semiconductors, LSIs, etc. that operate at high temperatures above 150°C. In recent years, due to the high capacity and space saving of semiconductor elements, the operating temperature has risen to near the melting point of high-melting-point lead solder, making it difficult to ensure connection reliability. On the other hand, with the strengthening of RoHS control, lead-free bonding materials are in demand.
[0004] Prior to this, the bonding of semiconductor elements using materials other than lead solder has been studied. For example, Patent Document 1 below proposes a technique for forming a sintered silver layer by sintering silver nanoparticles at low temperature. It is known that such sintered silver has high connection reliability for power cycles (Non-Patent Document 1).
[0005] As other materials, a technology for sintering copper particles to form a sintered copper layer has also been proposed. For example, the following patent document 2 discloses a bonding paste containing copper oxide particles and a reducing agent as a bonding material for bonding a semiconductor element to an electrode. In addition, the following patent document 3 discloses a bonding material containing copper nanoparticles, copper micron particles, copper submicron particles, or both.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 4928639
[0009] Patent Document 2: Japanese Patent No. 5006081
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-167145
[0011] Non-patent literature
[0012] Non-patent document 1: R. Khazaka, L. Mendizabal, D. Henry: J. ElecTron. Mater, 43(7), 2014, 2459-2466 Summary of the invention
[0013] Technical problem to be solved by the invention
[0014] The method described in the above-mentioned patent document 1 requires a hot compression bonding process accompanied by pressurization in order to obtain high connection reliability and densification of the sintered silver layer. When the hot compression bonding process accompanied by pressurization is performed, there are problems such as reduced production efficiency and decreased pass rate. Furthermore, when silver nanoparticles are used, a significant increase in material costs due to silver becomes a problem.
[0015] The method described in Patent Document 2 avoids volume shrinkage when copper oxide is reduced to copper by a thermocompression bonding process. However, the thermocompression bonding process has the above-mentioned problems.
[0016] The method described in the above-mentioned patent document 3 is to sinter without pressurization, but still has deficiencies in the following aspects. That is, the copper nanoparticles need to utilize a protective agent to modify the surface in order to suppress oxidation and improve dispersibility, but because the specific surface area of the copper nanoparticles is relatively large, there is a tendency for the amount of surface protective agent to increase in the bonding material based on the copper nanoparticles. In addition, in order to ensure dispersibility, there is a tendency for the amount of dispersion medium to increase. Thereby, the bonding material described in the above-mentioned patent document 3 has a tendency to increase the proportion of surface protective agent or dispersion medium, volume shrinkage during sintering, and the density after sintering is easy to reduce, and becomes difficult to ensure the sintered body strength.
[0017] An object of the present invention is to provide a copper paste for bonding that can obtain sufficient bonding strength even when bonding is performed without pressure. Another object of the present invention is to provide a method for manufacturing a bonded body and a method for manufacturing a semiconductor device using the copper paste for bonding, as well as a bonded body and a semiconductor device.
[0018] Means for solving technical problems
[0019] The present invention provides a copper paste for bonding, which is a copper paste for bonding containing metal particles and a dispersion medium, wherein the metal particles contain submicron copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less and micron copper particles having a volume average particle size of 2 μm or more and 50 μm or less, the content of the submicron copper particles and the sum of the content of the micron copper particles are 80% by mass or more based on the total mass of the metal particles, and the content of the submicron copper particles is 30% by mass or more and 90% by mass or less based on the sum of the mass of the submicron copper particles and the mass of the micron copper particles.
[0020] According to the copper paste for joining of the present invention, even when joining is performed without pressure, sufficient joining strength can be obtained. For the reason for obtaining this effect, it is believed that by containing the above-mentioned submicron copper particles and the above-mentioned micron copper particles in a specific ratio, the volume shrinkage during sintering caused by the surface protective agent or the dispersion medium can be fully suppressed while maintaining sufficient sinterability, and the strength of the sintered body and the bonding force with the joined surface can be ensured. In addition, the copper paste for joining of the present invention has the advantage of being cheaper and more stably supplied compared to the joining material with expensive copper nanoparticles as the main component because it can obtain the above-mentioned effect through submicron copper particles and micron copper particles. Thus, for example, production stability can be further improved when manufacturing a joining body such as a semiconductor device.
[0021] In the above-mentioned copper paste for bonding, the micron copper particles may be in the form of thin sheets. When thin sheet-shaped micron copper particles are used, for example, the chip shear strength and connection reliability of the semiconductor device can be more easily improved. In addition, as the reasons for obtaining such an effect, it is considered that: the micron copper particles in the copper paste for bonding are oriented approximately parallel to the bonding surface, so that the volume shrinkage when the copper paste for bonding is sintered can be suppressed; the bonding force is improved due to the increase in the overlapping area of the thin sheet-shaped micron copper particles; and the thin sheet-shaped micron copper particles align the submicron copper particles in a straight line, so that a reinforcing effect can be obtained.
[0022] The copper paste for bonding of the present invention may be for bonding without pressure. In this specification, "without pressure" means a state where the bonding is subjected to the dead weight of the members to be bonded, or a state where the bonding is subjected to a pressure of 0.01 MPa or less in addition to the dead weight.
[0023] The present invention also provides a method for manufacturing a joint body, which comprises the following steps: preparing a stacked body having a first component and, on one side of the direction in which the self-weight of the first component is applied, the above-mentioned copper paste for joining and a second component in sequence; and sintering the copper paste for joining under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa.
[0024] According to the method for producing a joined body of the present invention, by using the above-mentioned copper paste for joining, a joined body in which members are joined with a sufficient joining force by non-pressurized joining can be produced.
[0025] The present invention also provides a method for manufacturing a semiconductor device, which comprises the following steps: preparing a stacked body having a first component and, on one side of the first component in the direction of its own weight, the above-mentioned copper paste for bonding and a second component in sequence; sintering the copper paste for bonding under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa, wherein at least one of the first component and the second component is a semiconductor element.
[0026] According to the method for manufacturing a semiconductor device of the present invention, by using the above-mentioned copper paste for bonding, a semiconductor device having excellent die shear strength can be manufactured by non-pressurized bonding. In addition, the semiconductor device manufactured by the method for manufacturing a semiconductor device of the present invention can have excellent connection reliability.
[0027] The present invention also provides a joint body, which comprises a first member, a second member, and a sintered body of the above-mentioned copper paste for joining the first member and the second member. The first member and the second member of the joint body of the present invention are joined by a sintered body of copper having sufficient joining force. In addition, the joint body of the present invention can have excellent heat dissipation of the member by having a sintered body of copper with excellent thermal conductivity.
[0028] In the above-mentioned joint body, at least one of the first member and the second member may contain at least one metal selected from copper, nickel, silver, gold and palladium on the surface in contact with the sintered body. In this case, the adhesion between at least one of the first member and the second member and the sintered body can be further improved.
[0029] The present invention also provides a semiconductor device, which comprises a first member, a second member, and a sintered body of the above-mentioned copper paste for bonding the first member and the second member, wherein at least one of the first member and the second member is a semiconductor element. The semiconductor device of the present invention can be a semiconductor device having sufficient chip shear strength, excellent connection reliability, and excellent power cycle tolerance by having a sintered body of copper having sufficient bonding strength, thermal conductivity, and high melting point.
[0030] Effects of the Invention
[0031] According to the present invention, a copper paste for bonding that can obtain sufficient bonding strength even when bonding is performed without pressurization can be provided. The present invention can also provide a method for manufacturing a bonded structure and a method for manufacturing a semiconductor device using the copper paste for bonding, as well as a bonded structure and a semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic cross-sectional view showing an example of a bonded body produced using the copper paste for bonding according to the present embodiment.
[0033] Figure 2 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0034] Figure 3 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0035] Figure 4 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0036] Figure 5 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0037] Figure 6 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0038] Figure 7 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0039] Figure 8 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0040] Fig. 9 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0041] Fig.10 This is a SEM image of a cross section of the bonded body of Example 1.
[0042] Fig.11 This is a SEM image of a cross section of the bonded body of Example 12.
[0043] Fig.12 This is a SEM image of a cross section of the bonded body of Example 13.
[0044] Fig.13 The SEM image of the cross section of the bonded body of Comparative Example 2 is shown. DETAILED DESCRIPTION
[0045] Hereinafter, a mode for carrying out the present invention (hereinafter also referred to as "this embodiment") will be described in detail. The present invention is not limited to the following embodiment.
[0046] <Copper paste for bonding>
[0047] The copper paste for bonding according to the present embodiment is a copper paste for bonding containing metal particles and a dispersion medium, wherein the metal particles include submicron copper particles and micron copper particles.
[0048] (Metal Particles)
[0049] Examples of the metal particles of the present embodiment include submicron copper particles, micron copper particles, and other metal particles other than copper particles.
[0050] (Submicron copper particles)
[0051] As submicron copper particles, copper particles having a particle size of 0.12 μm or more and 0.8 μm or less can be cited, for example, copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less can be used. If the volume average particle size of the submicron copper particles is 0.12 μm or more, it is easy to obtain the effect of suppressing the synthesis cost of the submicron copper particles, good dispersibility, and suppressing the amount of surface treatment agent used. When the volume average particle size of the submicron copper particles is 0.8 μm or less, it is easy to obtain the effect of excellent sintering of the submicron copper particles. From the viewpoint of further exerting the above-mentioned effects, the volume average particle size of the submicron copper particles can be 0.15 μm or more and 0.8 μm or less, 0.15 μm or more and 0.6 μm or less, 0.2 μm or more and 0.5 μm or less, or 0.3 μm or more and 0.45 μm or less.
[0052] In addition, in the present specification, the volume average particle size refers to the 50% volume average particle size. When calculating the volume average particle size of the copper particles, it can be obtained by using a light scattering particle size distribution measuring device (for example, a Shimadzu nanoparticle size distribution measuring device (SALD-7500nano, manufactured by Shimadzu Corporation)) to measure the material obtained by dispersing the copper particles used as the raw material or the dried copper particles from which the volatile components are removed from the copper paste for bonding in the dispersion medium. When using a light scattering particle size distribution measuring device, hexane, toluene, α-terpineol, etc. can be used as the dispersion medium.
[0053] The submicron copper particles may contain 10% by mass or more of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. From the viewpoint of the sinterability of the copper paste for bonding, the submicron copper particles may contain 20% by mass or more, 30% by mass or more, or 100% by mass of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. When the content ratio of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less in the submicron copper particles is 20% by mass or more, the dispersibility of the copper particles is further improved, and the increase in viscosity and the decrease in paste concentration can be further suppressed.
[0054] The particle size of the copper particles can be calculated by the following method. The particle size of the copper particles can be obtained, for example, from an SEM image. The powder of the copper particles is placed on a carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed at 5000 times using an SEM device. The quadrilateral of the copper particles circumscribed to the SEM image is plotted using image processing software, and one side is used as the particle size of the particle.
[0055] The content of submicron copper particles can be 20% by mass or more and 90% by mass or less, based on the total mass of the metal particles, or 30% by mass or more and 90% by mass or less, or 35% by mass or more and 85% by mass or less, or 40% by mass or more and 80% by mass or less. When the content of submicron copper particles is within the above range, it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, if the content of submicron copper particles is within the above range, the semiconductor device has a tendency to show good chip shear strength and connection reliability.
[0056] The content of submicron copper particles is based on the sum of the mass of submicron copper particles and the mass of micron copper particles, preferably 20% by mass or more and 90% by mass or less. When the above-mentioned content of submicron copper particles is 20% by mass or more, the micron copper particles can be fully filled, and it is easy to ensure the bonding strength of the joint body manufactured by sintering copper paste for bonding, and when the bonding copper paste is used for the bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. When the content of submicron copper particles is 90% by mass or less, since the volume shrinkage during sintering copper paste for bonding can be fully suppressed, it is easy to ensure the bonding strength of the joint body manufactured by sintering copper paste for bonding. When the bonding copper paste is used for the bonding of semiconductor elements, when the content of submicron copper particles is 90% by mass or less, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above-mentioned effects, the content of the submicron copper particles can be 30% by mass or more and 85% by mass or less, 35% by mass or more and 85% by mass or less, or 40% by mass or more and 80% by mass or less, based on the sum of the mass of the submicron copper particles and the mass of the micron copper particles.
[0057] The shape of the submicron copper particles is not particularly limited. Examples of the shape of the submicron copper particles include spherical, blocky, needle-like, flaky, and roughly spherical shapes and aggregates thereof. From the viewpoint of dispersibility and filling properties, the shape of the submicron copper particles may be spherical, roughly spherical, or flaky. From the viewpoint of combustibility, dispersibility, and miscibility with flaky micron particles, the shape may be spherical or roughly spherical. In this specification, "flaky" includes flat plate shapes such as plate-like and scaly.
[0058] From the viewpoint of dispersibility, filling property and miscibility with flaky micron particles, the aspect ratio of submicron copper particles may be 5 or less, or 3 or less. In this specification, "aspect ratio" means the long side / thickness of a particle. The long side and thickness of a particle can be measured, for example, by calculating from a SEM image of the particle.
[0059] Submicron copper particles can be treated with a specific surface treatment agent. Examples of specific surface treatment agents include organic acids having 8 to 16 carbon atoms. Examples of organic acids having 8 to 16 carbon atoms include octanoic acid, methylheptanoic acid, ethylhexanoic acid, propylpentanoic acid, nonanoic acid, methyloctanoic acid, ethylheptanoic acid, propylhexanoic acid, decanoic acid, methylnonanoic acid, ethyloctanoic acid, propylheptanoic acid, butylhexanoic acid, undecanoic acid, methyldecanoic acid, ethylnonanoic acid, propyloctanoic acid, butylheptanoic acid, lauric acid, methylundecanoic acid, ethyldecanoic acid, propylnonanoic acid, butyloctanoic acid, pentylheptanoic acid, tridecanoic acid, methyldodecanoic acid, ethylundecanoic acid, propyldecanoic acid, butylnonanoic acid, pentyloctanoic acid, myristic acid, methyltridecanoic acid, ethyldodecanoic acid, propylundecanoic acid, butyldecanoic acid, pentylnonanoic acid, hexyloctanoic acid, pentadecanoic acid, methyltetradecanoic acid, ethyl Saturated fatty acids such as octenyl tridecanoic acid, propyl dodecanoic acid, butyl undecanoic acid, pentyl decanoic acid, hexyl nonanoic acid, palmitic acid, methyl pentadecanoic acid, ethyl tetradecanoic acid, propyl tridecanoic acid, butyl dodecanoic acid, pentyl undecanoic acid, hexyl decanoic acid, heptyl nonanoic acid, methyl cyclohexanoic acid, ethyl cyclohexanoic acid, propyl cyclohexanoic acid, butyl cyclohexanoic acid, pentyl cyclohexanoic acid, hexyl cyclohexanoic acid, heptyl cyclohexanoic acid, octyl cyclohexanoic acid, nonyl cyclohexanoic acid; octenyl acid, nonenyl acid, methyl nonenyl acid, decenoic acid, undecenoic acid, dodecenoic acid, tridecenoic acid, tetradecenoic acid, myristic acid, pentadecenoic acid, hexadecenoic acid, palmitoleic acid, 6(Z)-hexadecenoic acid (sapienic acid The organic acid may be used alone or in combination of two or more. By combining such an organic acid with the submicron copper particles, there is a tendency to balance the dispersibility of the submicron copper particles with the separation of the organic acid during sintering.
[0060] The treatment amount of the surface treatment agent can be an amount of one to three molecular layers attached to the surface of the submicron copper particles. This amount can be determined by the number of molecular layers attached to the surface of the submicron copper particles (n), the specific surface area of the submicron copper particles (A p )(Unit: m 2 / g), molecular weight of the surface treatment agent (M s ) (unit: g / mol), minimum coating area of surface treatment agent (S S )(Unit: m 2 / ), Avogadro constant (N A )(6.02×10 23 Specifically, the treatment amount of the surface treatment agent is calculated as follows: the treatment amount of the surface treatment agent (mass %) = {(n·A p ·M s) / (S S ·N A +n·A p ·M s )}×100% formula is used to calculate.
[0061] The specific surface area of the submicron copper particles can be determined by measuring the dried submicron copper particles using the BET specific surface area measurement method. The minimum coating area of the surface treatment agent is 2.05×10 -19 m 2 / 1 molecule. In the case of a surface treatment agent other than these, it can be measured, for example, by calculation by a molecular model or by the method described in "Chemistry and Education" (Kamieda, Inafuku, Mori, 40 (2), 1992, p114-117). An example of a quantitative method for a surface treatment agent is shown below. The surface treatment agent can be identified by a heat-leaving gas-gas chromatograph mass spectrometer of a dry powder after the dispersion medium is removed from the copper paste for bonding, thereby determining the carbon number and molecular weight of the surface treatment agent. The carbon fraction ratio of the surface treatment agent can be analyzed by carbon fraction analysis. As a carbon fraction analysis method, for example, a high-frequency induction heating furnace combustion / infrared absorption method can be cited. The surface treatment amount can be calculated using the above formula from the carbon number, molecular weight and carbon fraction ratio of the identified surface treatment agent.
[0062] The treatment amount of the surface treatment agent may be 0.07% by mass or more and 2.1% by mass or less, 0.10% by mass or more and 1.6% by mass or less, or 0.2% by mass or more and 1.1% by mass or less.
[0063] Since the submicron copper particles have good sinterability, they can reduce problems such as high synthesis cost, poor dispersibility, and reduced volume shrinkage after sintering that are seen in bonding materials that mainly use copper nanoparticles.
[0064] As the submicron copper particles of the present embodiment, commercially available products can be used. As commercially available submicron particles, for example, CH-0200 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.36 μm), HT-14 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.41 μm), CT-500 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a volume average particle size of 0.72 μm), and Tn-Cu100 (manufactured by Taiyo Nippon Sanso Corporation, with a volume average particle size of 0.12 μm) can be cited.
[0065] (Micron copper particles)
[0066] As micron copper particles, particles containing copper particles having a particle size of 2 μm or more and 50 μm or less can be cited, for example, copper particles having a volume average particle size of 2 μm or more and 50 μm or less can be used. If the volume average particle size of the micron copper particles is within the above range, the volume shrinkage during sintering of the copper paste for bonding can be sufficiently reduced, and it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the bonding copper paste is used for bonding of semiconductor elements, if the volume average particle size of the micron copper particles is within the above range, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above effect, the volume average particle size of the micron copper particles can be 3 μm or more and 20 μm or less, or 3 μm or more and 10 μm or less.
[0067] The micron copper particles may contain 50% by mass of copper particles having a particle size of 2 μm or more and 50 μm or less. From the viewpoint of orientation in the joint body, reinforcement effect, and filling property of the joint paste, the micron copper particles may contain 70% by mass or more, 80% by mass or more, or 100% by mass of copper particles having a particle size of 2 μm or more and 50 μm or less. From the viewpoint of suppressing joint failure, the micron copper particles preferably do not contain particles having a size exceeding the joint thickness, such as particles having a maximum diameter exceeding 20 μm.
[0068] The content of the micron copper particles can be 10% by mass or more and 90% by mass or less, 15% by mass or more and 65% by mass or less, or 20% by mass or more and 60% by mass or less, based on the total mass of the metal particles. When the content of the micron copper particles is within the above range, it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, if the content of the micron copper particles is within the above range, the semiconductor device has a tendency to show good chip shear strength and connection reliability.
[0069] The content of submicron copper particles and the sum of the content of micron copper particles can be 80% by mass or more, based on the total mass of the metal particles. If the content of submicron copper particles and the sum of the content of micron copper particles are within the above range, the volume shrinkage during sintering of the copper paste for bonding can be fully reduced, and it is easy to ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above-mentioned effect, the content of submicron copper particles and the sum of the content of micron copper particles can be 90% by mass or more, 95% by mass or more, or 100% by mass, based on the total mass of the metal particles.
[0070] The shape of the micron copper particles is not particularly limited. As the shape of the micron copper particles, for example, spherical, blocky, needle-shaped, flaky, slightly spherical and their agglomerates can be cited. The shape of the micron copper particles is preferably flaky. By using flaky micron copper particles, the micron copper particles in the copper paste for bonding are oriented roughly parallel to the bonding surface, which can suppress the volume shrinkage during sintering of the copper paste for bonding and easily ensure the bonding strength of the bonded body manufactured by sintering the copper paste for bonding. When the copper paste for bonding is used for bonding of semiconductor elements, the semiconductor device has a tendency to show good chip shear strength and connection reliability. From the viewpoint of further exerting the above-mentioned effect, as flaky micron copper particles, the aspect ratio can be more than 4 or more than 6.
[0071] There is no particular limitation on the treatment of micron copper particles with or without a surface treatment agent. From the viewpoint of dispersion stability and oxidation resistance, micron copper particles can be treated with a surface treatment agent. The surface treatment agent can be removed during bonding. Examples of such surface treatment agents include aliphatic carboxylic acids such as palmitic acid, stearic acid, arachidic acid, and oleic acid; aromatic carboxylic acids such as terephthalic acid, pyromellitic acid, and o-phenoxybenzoic acid; aliphatic alcohols such as cetyl alcohol, stearyl alcohol, isobornyl cyclohexanol, and tetraethylene glycol; aromatic alcohols such as p-phenylphenol; alkylamines such as octylamine, dodecylamine, and stearylamine; aliphatic nitriles such as stearonitrile and decanoonitrile; silane coupling agents such as alkyl alkoxysilanes; polymer treatment agents such as polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, and silicone oligomers. The surface treatment agent can be used alone or in combination of two or more.
[0072] The treatment amount of the surface treatment agent can be an amount of more than one molecular layer on the particle surface. The treatment amount of this surface treatment agent varies with the specific surface area of the micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent. The treatment amount of the surface treatment agent is usually 0.001 mass % or more. For the specific surface area of the micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent, the above method can be used to obtain.
[0073] When the copper paste for bonding is prepared only from the above-mentioned submicron copper particles, the copper paste for bonding is easy to peel off from the bonded surface during sintering due to the large volume shrinkage and sintering shrinkage accompanying the drying of the dispersion medium, and it is difficult to obtain sufficient chip shear strength and connection reliability in the bonding of semiconductor elements, etc. By using submicron copper particles and micron copper particles in combination, the volume shrinkage during sintering of the copper paste for bonding can be suppressed, and the bonded body can have sufficient bonding strength. When the copper paste for bonding is used for bonding of semiconductor elements, the effect of showing good chip shear strength and connection reliability of the semiconductor device can be obtained.
[0074] As the micron copper particles of the present embodiment, commercially available products can be used. As commercially available micron particles, for example, MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd., with a volume average particle size of 7.5 μm), 3L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with a volume average particle size of 8.0 μm), 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd., with a volume average particle size of 3.8 μm), and Cu-HWQ3.0 μm (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with a volume average particle size of 3.0 μm) can be cited.
[0075] (Other metal particles except copper particles)
[0076] As metal particles, other metal particles other than submicron copper particles and micron copper particles may be contained, for example, particles such as nickel, silver, gold, palladium, and platinum may be contained. Other metal particles may have a volume average particle size of 0.01 μm or more and 10 μm or less, 0.01 μm or more and 5 μm or less, or 0.05 μm or more and 3 μm or less. When other metal particles are contained, their content may be less than 20% by mass or less than 10% by mass based on the total mass of the metal particles from the viewpoint of obtaining sufficient bonding. Other metal particles may also be contained. The shape of other metal particles is not particularly limited.
[0077] By containing metal particles other than copper particles, a sintered body formed by solid solution or dispersion of multiple metals can be obtained, thereby improving the mechanical properties of the sintered body such as yield stress and fatigue strength, and the connection reliability is easily improved. In addition, by adding multiple metal particles, the sintered body of the copper paste for bonding can have sufficient bonding strength relative to a specific bonded body. When the copper paste for bonding is used for bonding semiconductor elements, the chip shear strength and connection reliability of the semiconductor device are easily improved.
[0078] (Dispersion Medium)
[0079] The dispersion medium is not particularly limited and may be a volatile dispersion medium. Examples of the volatile dispersion medium include monohydric and polyhydric alcohols such as pentanol, hexanol, heptanol, octanol, decanol, ethylene glycol, diethylene glycol, propylene glycol, butanediol, α-terpineol, and isobornylcyclohexanol (MTPH); ethylene glycol butyl ether, ethylene glycol phenyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, triethylene glycol methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol propyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol Ethers such as propyl ether, dipropylene glycol butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol methyl ether, and tripropylene glycol dimethyl ether; esters such as ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate (DPMA), ethyl lactate, butyl lactate, γ-butyrolactone, and propylene carbonate; acid amides such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide; aliphatic hydrocarbons such as cyclohexanone, octane, nonane, decane, and undecane; aromatic hydrocarbons such as benzene, toluene, and xylene; mercaptans having an alkyl group with a carbon number of 1 to 18; mercaptans having a cycloalkyl group with a carbon number of 5 to 7. Examples of the mercaptans having an alkyl group having 1 to 18 carbon atoms include ethyl mercaptan, n-propyl mercaptan, isopropyl mercaptan, n-butyl mercaptan, isobutyl mercaptan, tert-butyl mercaptan, pentyl mercaptan, hexyl mercaptan, and dodecyl mercaptan. Examples of the mercaptans having a cycloalkyl group having 5 to 7 carbon atoms include cyclopentyl mercaptan, cyclohexyl mercaptan, and cycloheptyl mercaptan.
[0080] The content of the dispersion medium may be 5 to 50 parts by mass based on 100 parts by mass of the total mass of the metal particles. When the content of the dispersion medium is within the above range, the viscosity of the copper paste for bonding can be adjusted to be more appropriate, and the sintering of the copper particles is less likely to be inhibited.
[0081] (additive)
[0082] The copper paste for bonding may further contain, as required, a wettability enhancer such as a nonionic surfactant or a fluorine-based surfactant, a defoamer such as silicone oil, an ion scavenger such as an inorganic ion exchanger, or the like.
[0083] As one form of the copper paste for joining according to the present embodiment, the following copper paste for joining can be cited: the above-mentioned metal particles contain submicron copper particles with a volume average particle size of not less than 0.12 μm and not more than 0.8 μm, preferably not less than 0.15 μm and not more than 0.8 μm, and micron copper particles with a volume average particle size of not less than 2 μm and not more than 50 μm, the content of submicron copper particles and the sum of the content of micron copper particles is not less than 80 mass% based on the total mass of the metal particles, and the content of submicron copper particles is not less than 30 mass% and not more than 90 mass% based on the mass of the submicron copper particles and the sum of the mass of the micron copper particles.
[0084] As the copper paste for bonding, the following copper paste for bonding can be cited: submicron copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less, preferably 0.15 μm or more and 0.8 μm or less; micron copper particles having a volume average particle size of 2 μm or more and 50 μm or less; a dispersion medium; and other components as required, wherein the sum of the amount of submicron copper particles and the amount of micron copper particles is 80% by mass or more based on the total mass of the metal particles, and the amount of submicron copper particles is 30% by mass or more and 90% by mass or less based on the sum of the amount of submicron copper particles and the amount of micron copper particles.
[0085] In addition, as another embodiment of the copper paste for bonding of the present embodiment, the following copper paste for bonding can be cited: as submicron copper particles, based on the total mass of metal particles, 24 to 80% by mass of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less, preferably 0.15 μm or more and 0.8 μm or less are contained, as micron copper particles, based on the total mass of metal particles, 8 to 70% by mass of micron copper particles having a particle size of 2 μm or more and 50 μm or less are contained, and the content of submicron copper particles is based on the sum of the mass of submicron copper particles and the mass of micron copper particles, 30% or more and 90% or less by mass. The particle size here refers to the maximum particle size, which is calculated by observing the copper particles used as the raw material or the dried copper particles from which the volatile components are removed from the copper paste for bonding using a scanning electron microscope (SEM).
[0086] When the copper particles are not spherical, their particle size can be the maximum particle size obtained by the following method. The method for obtaining the maximum particle size of copper particles from SEM images is exemplified. The powder of copper particles is placed on a carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed at 5000 times using a SEM device. A rectangle of the copper particles circumscribed to the SEM image is plotted using image processing software, and the long side of the rectangle is used as the major diameter of the particle. The major diameter is used as the maximum particle size.
[0087] (Preparation of copper paste for bonding)
[0088] The copper paste for bonding can be prepared by mixing the above-mentioned submicron copper particles, micron copper particles, other metal particles and any additives in a dispersion medium. After mixing the components, stirring treatment can also be performed. The copper paste for bonding can also adjust the maximum particle size of the dispersion liquid by a classification operation. At this time, the maximum particle size of the dispersion liquid can be less than 20 μm, and can also be less than 10 μm.
[0089] The copper paste for bonding can also be prepared by mixing submicron copper particles, a surface treatment agent, and a dispersion medium in advance, performing a dispersion treatment to prepare a dispersion of submicron copper particles, and then mixing micron copper particles, other metal particles, and any additives. By adopting this sequence, the dispersibility of submicron copper particles is improved, the miscibility with micron copper particles is improved, and the performance of the copper paste for bonding is further improved. It is also possible to remove agglomerates from the dispersion of submicron copper particles by a classification operation.
[0090] The stirring treatment can be performed using a stirrer. Examples of the stirrer include a rotation-revolution type stirring device, a Raikai machine, a twin-screw kneader, a three-roll mill, a planetary mixer, and a thin-layer shear disperser.
[0091] The classification operation can be performed by, for example, filtration, natural sedimentation, or centrifugal separation. Examples of the filter for filtration include metal meshes, metal filters, and nylon meshes.
[0092] Examples of the dispersion treatment include a thin layer shear disperser, a bead mill, an ultrasonic homogenizer, a high shear stirrer, a narrow gap three-roll mill, a wet ultrafine particle device, a supersonic jet mill, and an ultrahigh pressure homogenizer.
[0093] The viscosity of the copper paste for bonding can be adjusted to be suitable for various printing and coating techniques during molding. The viscosity of the copper paste for bonding can be, for example, 0.05 Pa·s to 2.0 Pa·s as the Casson viscosity at 25°C, or 0.06 Pa·s to 1.0 Pa·s.
[0094] According to the copper paste for joining of the present embodiment, by using the above-mentioned submicron copper particles and micron copper particles in a fixed ratio, good sintering properties can be obtained, and then the volume shrinkage during sintering can be suppressed. Therefore, the copper paste for joining of the present embodiment can ensure the bonding force with the component without excessive pressure, and the joint body manufactured by sintering the copper paste for joining can have sufficient bonding strength. When the copper paste for joining is used for the joining of semiconductor elements, the semiconductor device shows good chip shear strength and connection reliability. That is, the copper paste for joining of the present embodiment can be used as a joining material for non-pressurized joining. In addition, according to the copper paste for joining of the present embodiment, by using relatively cheap copper particles, the manufacturing cost can be suppressed and mass production can be achieved. In particular, the copper paste for joining of the present embodiment can obtain the above-mentioned effect by submicron copper particles and micron copper particles, so compared with the joining material with expensive copper nanoparticles as the main component, it has the advantage of being able to be supplied more cheaply and stably. Thus, for example, when manufacturing a joint body such as a semiconductor device, production stability can be further improved.
[0095] <Joint body and semiconductor device>
[0096] The following is a reference to the attached Figure 1 The preferred embodiment will be described in detail. In addition, in the drawings, the same or corresponding parts are given the same symbols, and repeated descriptions are omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0097] Figure 1 1 is a schematic cross-sectional view showing an example of a bonded body manufactured using the bonding copper paste of the present embodiment. The bonded body 100 of the present embodiment includes a first member 2, a second member 3, and a sintered body 1 of the bonding copper paste bonding the first member and the second member.
[0098] As the first component 2 and the second component 3, for example, there can be cited semiconductor elements such as IGBT, diode, Schottky barrier diode, MOS-FET, thyristor, logic circuit, sensor, analog integrated circuit, LED, semiconductor laser, signal transmitter, etc., lead frame, ceramic substrate with metal plate (such as DBC), LED package and other semiconductor element mounting substrate, metal wiring such as copper tape and metal frame, blocks such as metal blocks, power supply components such as terminals, heat dissipation plates, water-cooling plates, etc.
[0099] The first component 2 and the second component 3 may contain metal in the surfaces 4a and 4b in contact with the sintered body of the copper paste for bonding. As metals, for example, copper, nickel, silver, gold, palladium, platinum, lead, tin, cobalt, etc. can be cited. One metal can be used alone, or two or more metals can be used in combination. In addition, the surface in contact with the sintered body can be an alloy containing the above metals. As metals used in alloys, in addition to the above metals, zinc, manganese, aluminum, beryllium, titanium, chromium, iron, molybdenum, etc. can also be cited. As components containing metal in the surface in contact with the sintered body, for example, components with various metal plating, wires, chips with metal plating, heat sinks, ceramic substrates with metal plates, lead frames with various metal plating or lead frames formed by various metals, copper plates, copper foils. In addition, when the second component 3 is a semiconductor element, the first component 2 can also be a block with thermal conductivity and electrical conductivity such as a metal wiring such as a metal frame, a metal block, etc.
[0100] The die shear strength of the bonded body may be 10 MPa or more, 15 MPa or more, 20 MPa or more, or 30 MPa or more, from the viewpoint of sufficiently bonding the first member and the second member. The die shear strength may be measured using a universal bond strength tester (4000 series, manufactured by DAGE).
[0101] The thermal conductivity of the sintered body of the copper paste for bonding may be 100 W / (m·K) or more, 120 W / (m·K) or more, or 150 W / (m·K) or more from the viewpoint of heat dissipation and connection reliability at high temperatures. The thermal conductivity can be obtained from the thermal diffusivity, specific heat capacity, and density of the sintered body of the copper paste for bonding.
[0102] Hereinafter, a method for producing a joint body using the copper paste for joining according to the present embodiment will be described.
[0103] The method for manufacturing a joint body using the copper paste for jointing of the present embodiment comprises the following steps: preparing a laminated body having a first member, the copper paste for jointing and a second member in sequence on one side of the first member in the direction in which the first member acts in its own weight, and sintering the copper paste for jointing under the weight of the first member or under the weight of the first member and a pressure of 0.01 MPa or less. The direction in which the first member acts in its own weight may also be referred to as the direction in which gravity acts.
[0104] The above-mentioned laminated body can be prepared, for example, by providing the copper paste for bonding of the present embodiment on a necessary portion of the second member and then placing the first member on the copper paste for bonding.
[0105] As a method of setting the copper paste for bonding of the present embodiment on the necessary part of the second member, a method of depositing the copper paste for bonding may be used. As such method, for example, screen printing, transfer printing, offset printing, inkjet printing, dispenser, jet dispenser, needle dispenser, comma coater, slit coater, die coater, gravure coater, slit coating, relief printing, gravure printing, gravure printing, steel screen printing, soft etching, rod coating, applicator, particle deposition method, spray coater, spin coater, dip coater, electrodeposition coating, etc. may be used. The thickness of the copper paste for bonding may be greater than 1 μm and less than 1000 μm, greater than 10 μm and less than 500 μm, greater than 50 μm and less than 200 μm, greater than 10 μm and less than 3000 μm, greater than 15 μm and less than 500 μm, greater than 20 μm and less than 300 μm, greater than 5 μm and less than 500 μm, greater than 10 μm and less than 250 μm, or greater than 15 μm and less than 150 μm.
[0106] The copper paste for bonding provided on the second member can also be properly dried from the viewpoint of suppressing the flow and occurrence of pores during sintering. The ambient gas during drying can be in the atmosphere, or in an oxygen-free ambient gas such as nitrogen or a rare gas, or in a reducing ambient gas such as hydrogen or formic acid. The drying method can be drying by placing at room temperature, or heating drying, or reduced pressure drying. For example, heating drying or reduced pressure drying can use a heating plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, a hot plate pressing device, etc. The drying temperature and time can be appropriately adjusted according to the type and amount of the dispersion medium used. As the drying temperature and time, for example, it can be above 50°C and below 180°C, and dried for more than 1 minute and less than 120 minutes.
[0107] Examples of a method for placing the first member on the copper paste for bonding include a chip mounter, a flip chip bonding machine, and a positioning jig made of carbon or ceramics.
[0108] The copper paste for bonding is sintered by heating the laminate. The heating treatment may be performed using, for example, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, etc.
[0109] The atmosphere during sintering may be an oxygen-free atmosphere from the viewpoint of suppressing oxidation of the sintered body, the first component, and the second component. The atmosphere during sintering may also be a reducing atmosphere from the viewpoint of removing the surface oxides of the copper particles of the copper paste for bonding. As an oxygen-free atmosphere, for example, nitrogen, a rare gas, or the like may be introduced or vacuum may be used. As a reducing atmosphere, for example, pure hydrogen, a mixed gas of hydrogen and nitrogen representing the composition gas, nitrogen containing formic acid gas, a mixed gas of hydrogen and a rare gas, a rare gas containing formic acid gas, etc. may be used.
[0110] The maximum temperature during the heat treatment may be 250° C. or higher and 450° C. or lower, 250° C. or higher and 400° C. or lower, or 250° C. or higher and 350° C. or lower, from the viewpoint of reducing thermal damage to the first member and the second member and improving the yield. When the maximum temperature is 200° C. or higher and the maximum temperature holding time is 60 minutes or less, sintering tends to proceed sufficiently.
[0111] The holding time at the maximum temperature may be 1 minute to 60 minutes, 1 minute to less than 40 minutes, or 1 minute to less than 30 minutes, from the viewpoint of completely volatilizing the dispersion medium and improving the yield.
[0112] By using the copper paste for bonding of the present embodiment, when the stack is sintered, the bonded body has sufficient bonding strength even when bonding is performed without pressure. That is, sufficient bonding strength can be obtained when subjected to the deadweight generated only by the first member stacked on the copper paste for bonding, or in addition to the deadweight of the first member, a pressure of less than 0.01MPa, preferably less than 0.005MPa. When the pressure received during sintering is within the above range, since no special pressurized connection is required, the porosity can be reduced without compromising the pass rate, and the chip shear strength and connection reliability can be further improved. As a method for subjecting the copper paste for bonding to a pressure of less than 0.01MPa, for example, a method of placing a heavy object on the first member can be cited.
[0113] In the above-mentioned joint body, at least one of the first component and the second component can be a semiconductor element. As semiconductor elements, for example, power modules, signal transmitters, amplifiers, LED modules, etc. formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, etc. can be cited. At this time, the above-mentioned joint body becomes a semiconductor device. The obtained semiconductor device can have sufficient chip shear strength and connection reliability.
[0114] Figure 2This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment. Figure 2 The semiconductor device 110 shown is formed by a semiconductor element 8 connected to a lead frame 5a via a sintered body 1 of a copper paste for bonding according to the present embodiment, and a molding resin 7 molding the semiconductor element 8. The semiconductor element 8 is connected to the lead frame 5b via a wire 6.
[0115] Examples of semiconductor devices manufactured using the copper paste for bonding according to this embodiment include power modules formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, and the like, signal transmitters, amplifiers, high-brightness LED modules, sensors, and the like.
[0116] The semiconductor device can be manufactured in the same manner as the manufacturing method of the above-mentioned joint body. That is, the manufacturing method of the semiconductor device comprises the following steps: at least one of the first component and the second component uses a semiconductor element, a laminated body having a first component, and the above-mentioned copper paste for bonding and a second component are sequentially prepared on one side of the direction in which the self-weight of the first component acts, and the copper paste for bonding is sintered under the self-weight of the first component, or under the self-weight of the first component and a pressure of less than 0.01 MPa. For example, a step of providing a copper paste for bonding on the lead frame 5a and configuring a semiconductor element 8 for heating can be cited. The obtained semiconductor device can have sufficient chip shear strength and connection reliability even when bonding is performed without pressure. The semiconductor device of this embodiment has a sintered body of copper having sufficient bonding force, thermal conductivity and high melting point, and has sufficient chip shear strength, excellent connection reliability, and excellent power cycle tolerance.
[0117] The above method can reduce the damage to the semiconductor element when the metal wiring or bulk as the first member is bonded to the semiconductor element when the second member is a semiconductor element. A semiconductor device in which a member such as a metal wiring or bulk is bonded to a semiconductor element is described below.
[0118] As an embodiment of such a semiconductor device, the following semiconductor device can be cited: a semiconductor device comprising a first electrode, a semiconductor element electrically connected to the first electrode, and a second electrode electrically connected to the semiconductor element via a metal wiring, and a sintered body having the above-mentioned copper paste for bonding between the semiconductor element and the metal wiring and between the metal wiring and the second electrode.
[0119] Figure 3 It is a schematic cross-sectional view showing an example of the above-mentioned semiconductor device. Figure 3The semiconductor device 200 shown in the figure includes: an insulating substrate 21 having a first electrode 22 and a second electrode 24, a semiconductor element 23 bonded to the first electrode 22 via a sintered body 1 of the above-mentioned copper paste for bonding, and a metal wiring 25 electrically connecting the semiconductor element 23 and the second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded respectively via the sintered body 1 of the copper paste for bonding. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The semiconductor device 200 includes a copper plate 28 on the side opposite to the surface of the insulating substrate 21 on which the above-mentioned electrodes and the like are mounted. The above-mentioned structure of the semiconductor device 200 is sealed with an insulator 29. The semiconductor device 200 has one semiconductor element 23 on the first electrode 22, but may also have two or more. In this case, the plurality of semiconductor elements 23 can be bonded to the metal wiring 25 via the sintered body 1 of the copper paste for bonding.
[0120] Figure 4 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 4 The semiconductor device 210 shown in the figure has a block 30 provided between the semiconductor element 23 and the metal wiring 25, and the semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered body 1 of a bonding copper paste, and has other Figure 3 The structure is the same as that of the semiconductor device 200 shown in FIG.
[0121] Figure 5 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 5 The semiconductor device 220 shown in the figure further includes a semiconductor element 23 and a block 30 on the first electrode 22, and a sintered body 1 of a copper paste for bonding them. Figure 4 The semiconductor device 220 has the same structure as the semiconductor device 210 shown in the figure. The semiconductor device 220 has two semiconductor elements on the first electrode 22, and may have three or more. In this case, the three or more semiconductor elements 23 may be respectively bonded to the metal wiring 25 via the block 30 and the sintered body 1 of the bonding copper paste. In addition, the position of the block 30 may be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0122] Examples of the insulating substrate 21 include ceramics such as alumina, aluminum nitride, and silicon nitride, highly thermally conductive particle / resin composites, polyimide resins, and polymaleimide resins.
[0123] As metals constituting the first electrode 22, the second electrode 24 and the third electrode 26, for example, copper, nickel, silver, gold, palladium, platinum, lead, tin, cobalt, etc. can be cited. One of these metals can be used alone, or two or more can be used in combination. In addition, the electrode can also have an alloy containing the above metals on the surface in contact with the copper paste for bonding and the sintered body 1. As metals used in the alloy, in addition to the above metals, zinc, manganese, aluminum, beryllium, titanium, chromium, iron, molybdenum, etc. can also be cited.
[0124] Examples of the metal wiring include metal frames having a strip, plate, cube, cylinder, L-shaped, U-shaped, or U-shaped shape. Examples of the material of the metal wiring include silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or alloys thereof. The metal wiring may have a width of 1 μm to 30 μm and a thickness of 20 μm to 5 mm.
[0125] As the block, preferably one with excellent thermal conductivity and electrical conductivity can be used, for example, silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or their alloys. By providing the block on the semiconductor element, the heat dissipation is further improved. The number of blocks can be appropriately changed.
[0126] Examples of the insulator 29 include silicone rubber, polymaleimide resin, polyimide resin, and polyamide-imide resin.
[0127] Figures 3 to 5 The semiconductor device shown can be used for a power module requiring a large capacity and high reliability.
[0128] Figures 3 to 5 The semiconductor device shown can be manufactured, for example, by a method comprising the following steps: preparing an insulating substrate comprising a first electrode and a second electrode, arranging a bonding copper paste, a semiconductor element, a bonding copper paste as required, a block, and a bonding copper paste on the first electrode in order from the first electrode side, arranging a bonding copper paste on the second electrode, and arranging metal wiring on the bonding copper paste on the semiconductor element or the block and the bonding copper paste on the second electrode in a manner such that the bonding copper pastes are cross-linked; and sintering the bonding copper paste under the self-weight of each component or under the self-weight of each component and a pressure of less than 0.01 MPa.
[0129] According to this manufacturing method, a semiconductor device can be manufactured without applying pressure, so bonding can be performed without deforming the metal wiring having a bridge portion, and even when a component having a smaller bonding area than the semiconductor element is bonded to the semiconductor element, damage to the semiconductor element can be further reduced.
[0130] Figure 6 It is a schematic cross-sectional view showing still another example of a semiconductor device. Figure 6The semiconductor device 300 shown includes a first electrode 22, a semiconductor element 23 bonded to the first electrode 22 via a sintered body 1 of a copper paste for bonding, and a metal wiring 25 electrically connecting the semiconductor element 23 to a second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded to each other via the sintered body 1 of the copper paste for bonding. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The above-mentioned structure of the semiconductor device 300 is sealed with a sealing material 31. The semiconductor device 300 has one semiconductor element 23 on the first electrode 22, and may have two or more. In this case, the plurality of semiconductor elements 23 can be bonded to the metal wiring 25 via the sintered body 1 of the copper paste for bonding.
[0131] Figure 7 It is a schematic cross-sectional view showing still another example of a semiconductor device. Figure 7 The semiconductor device 310 shown in the figure has a block 30 provided between the semiconductor element 23 and the metal wiring 25, and the semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered body 1 of a bonding copper paste. Figure 6 The structure is the same as that of the semiconductor device 300 shown in FIG.
[0132] Figure 8 It is a schematic cross-sectional view showing still another example of a semiconductor device. Figure 8 The semiconductor device 320 shown in the figure further includes a semiconductor element 23 and a bulk body 30 on the first electrode 22, and a sintered body 1 of a copper paste for bonding them. Figure 7 The semiconductor device 320 has the same structure as the semiconductor device 310 shown in the figure. The semiconductor device 320 has two semiconductor elements on the first electrode 22, and may also have three or more. In this case, the three or more semiconductor elements 23 can be respectively connected to the metal wiring 25 through the block 30 and the sintered body 1 of the bonding copper paste. In addition, the position of the block 30 can be appropriately changed, for example, it can also be set between the first electrode 22 and the semiconductor element 23.
[0133] Figures 6 to 8 The first electrode 22 and the second electrode 24 shown may also be a lead frame, a copper plate, a copper / molybdenum sintered body, etc.
[0134] Examples of the sealing material 31 include heat-resistant solid sealing materials and highly thermally conductive composite materials.
[0135] The sintered body 1 of the copper paste for bonding may be the same as that described in connection with the semiconductor devices 200 to 220 .
[0136] Figures 6 to 8 The semiconductor device of the embodiment shown can be used for a miniaturized power module by using a lead frame or the like as the first electrode and the second electrode. This semiconductor device can be manufactured in the same manner as the manufacturing method of the semiconductor device described above.
[0137] Furthermore, another embodiment of a semiconductor device having a structure in which a bulk body is bonded to a semiconductor element will be described.
[0138] The semiconductor device may include a first heat conducting member, a second heat conducting member, and a semiconductor element disposed between the first heat conducting member and the second heat conducting member, and a sintered body of the copper paste for bonding is provided between at least one of the first heat conducting member and the semiconductor element and between the semiconductor element and the second heat conducting member.
[0139] Fig. 9 It is a schematic cross-sectional view showing an example of this embodiment. Fig. 9 The semiconductor device 400 shown in the figure comprises a first heat-conducting member 32, a semiconductor element 23 joined to the first heat-conducting member 32 by a sintered body 1 of a copper paste for joining, a block 30 joined to the semiconductor element 23 by a sintered body 1 of a copper paste for joining, and a second heat-conducting member 33 joined to the block 30 by a sintered body 1 of a copper paste for joining. The semiconductor element 23 is connected to an electrode 34 via a wire 35. The first heat-conducting member 32 and the second heat-conducting member of the semiconductor device 400 are sealed with a sealing material 31. The semiconductor device 400 has two semiconductor elements, or may have one or more than three, and the number of blocks may be appropriately changed. In addition, the position of the block 30 may be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0140] The heat conducting member has both the function of releasing heat generated from the semiconductor element 23 to the outside and the function of serving as an electrode for electrically connecting the semiconductor element to the outside. For example, copper, aluminum, or an alloy thereof is used for such a heat conducting member.
[0141] Fig. 9 The semiconductor device shown can have a double-sided cooling structure with excellent heat dissipation by having heat-conducting components on both sides of the semiconductor element. This semiconductor device can be manufactured by a method having the following steps: preparing a stacked body in which a copper paste for bonding, a semiconductor element, a copper paste for bonding, a block, a copper paste for bonding, and a second heat-conducting component are stacked in order from the first heat-conducting component side on a first heat-conducting component, and sintering the copper paste for bonding under the weight of each component or under the weight of each component and a pressure of 0.01 MPa or less. In addition, the stacked body can also be stacked in the opposite order to the above.
[0142] Example
[0143] The present invention is described in more detail below by way of examples, but the present invention is not limited to the following examples.
[0144] (Preparation Example 1)
[0145] 0.35 g of α-terpineol (Wako Pure Chemical Industries, Ltd.) and 0.85 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 3.52 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 5.28 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. A rotation-revolution type stirring device (Planetary Vacuum Mixer ARV-310, manufactured by Shinkey Co., Ltd.) was used at 2000 min. -1 The capped plastic bottle was stirred at 2000 rpm for 2 minutes. Then, the mixture was treated with an ultrasonic homogenizer (US-600, manufactured by Nippon Seiki Co., Ltd.) at 19.6 kHz, 600 W, for 1 minute. Next, the mixture was treated with an auto-rotation-revolution type stirring device (Planetary Vacuum Mixer ARV-310, manufactured by Shinkey Co., Ltd.) at 2000 min. -1 The sealed plastic bottle was stirred at 2000 rpm for 2 minutes. The mixed solution was used as copper paste 1 for bonding.
[0146] (Preparation Example 2)
[0147] 0.44 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.76 g of isobornylcyclohexanol (MTPH, manufactured by Nippon Terpene Chemical Co., Ltd.) as dispersion media, 4.40 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 4.40 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 2 for bonding.
[0148] (Preparation Example 3)
[0149] 0.52 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.68 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 5.28 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 3.52 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 3 for bonding.
[0150] (Preparation Example 4)
[0151] 0.61 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.59 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 6.16 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 2.64 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 4 for bonding.
[0152] (Preparation Example 5)
[0153] 0.78 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.42 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 7.91 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 0.88 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 5 for bonding.
[0154] (Preparation Example 6)
[0155] 0.90 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium, 6.40 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 2.75 g of 3L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 6 for bonding.
[0156] (Preparation Example 7)
[0157] 0.90 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium, 4.58 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 4.58 g of 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 7 for bonding.
[0158] (Preparation Example 8)
[0159] 0.61 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.59 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 6.16 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 2.64 g of Cu-HWQ 3.0 μm (manufactured by Fukuda Metal Foil Powder Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 8 for bonding.
[0160] (Preparation Example 9)
[0161] 6.1 g of α-terpineol and 0.59 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as a dispersion medium, 6.16 g of HT-14 (containing no surface treatment agent, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 0.58 g of lauric acid (manufactured by Wako Pure Chemical Industries, Ltd.) as a surface treatment agent were mixed and mixed for 10 minutes using an automatic mortar to prepare a mixed solution. Thereafter, the mixed solution was treated with an ultrasonic homogenizer (US-600, manufactured by Nippon Seiki Co., Ltd.) at 19.6 kHz and 600 W for 2 minutes, and the resulting paste-like composition was passed through a nylon mesh (Bolding Cloth 355T, manufactured by AS ONE Co., Ltd.) to obtain a HT-14 paste-like composition. 7.36 g of the HT-14 paste composition and 2.64 g of MA-C025 (Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until the dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste for bonding 9.
[0162] (Preparation Example 10)
[0163] 0.94 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.26 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 2.64 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 6.16 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 10 for bonding.
[0164] (Preparation Example 11)
[0165] 0.78 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.42 g of isobornylcyclohexanol (MTPH, manufactured by Nippon Terpene Chemical Co., Ltd.) as dispersion media, 7.92 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 0.88 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 11 for bonding.
[0166] (Preparation Example 12)
[0167] 1.20 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium, 7.00 g of CT-500 (surface treatment agent: unknown, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 3.00 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 12 for bonding.
[0168] (Preparation Example 13)
[0169] 1.20 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium and 8.80 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 13 for bonding.
[0170] (Preparation Example 14)
[0171] 0.22 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 1.12 g of isobornylcyclohexanol (MTPH, manufactured by Terpene Chemical Co., Ltd.) as dispersion media, 0.88 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles, and 7.92 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as in Preparation Example 1 was carried out to prepare a copper paste 14 for bonding.
[0172] (Preparation Example 15)
[0173] 1.20 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium and 8.80 g of CH-0200 (surface treatment agent: lauric acid, manufactured by Mitsui Mining & Smelting Co., Ltd.) as submicron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. Except for using this mixed solution, the same method as Preparation Example 1 was carried out to prepare a copper paste 15 for bonding.
[0174] (Preparation Example 16)
[0175] 1.50 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium, 5.95 g of CS-10 (surface treatment agent: unknown, manufactured by Mitsui Mining & Smelting Co., Ltd., 50% volume average particle size: 1.1 μm, proportion of particles with a particle size of 0.12 to 0.8 μm (mass %): 18%) as copper particles, and 2.55 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. A copper paste 16 for bonding was prepared in the same manner as in Preparation Example 1 except that this mixed solution was used.
[0176] (Preparation Example 17)
[0177] 1.06 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium, 6.37 g of Cu-HWQ 1.5 μm (surface treatment agent: none, manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., 50% volume average particle size: 1.7 μm, proportion of particles with a particle size of 0.12 to 0.8 μm (mass %): 11%) as copper particles, and 2.73 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) as micron copper particles were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. A copper paste 17 for bonding was prepared in the same manner as in Preparation Example 1 except that this mixed solution was used.
[0178] (Preparation Example 18)
[0179] 0.67 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 0.60 g of isobornylcyclohexanol (MTPH, manufactured by Nippon Terpene Chemical Co., Ltd.) as dispersion media, 6.17 g of Cu-HWQ 3.0 μm (surface treatment agent: none, manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., 50% volume average particle size: 3 μm, proportion of particles with a particle size of 0.12 to 0.8 μm (mass %): 0.3%) as micron copper particles, and 2.64 g of MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd.) were kneaded in an agate mortar until dry powder disappeared, and the mixed solution was transferred to a plastic bottle. The same method as in Preparation Example 1 was carried out except that this mixed solution was used to prepare a copper paste 18 for bonding.
[0180] <Manufacturing of joint body>
[0181] (Examples 1 to 11, 16)
[0182] A bonded body was produced by the following method using the bonding copper pastes 1 to 12. The die shear strength of the bonded body was measured by the method described below.
[0183] A stainless steel metal mask (thickness: 100 μm) with 3 rows and 3 columns of 3 mm × 3 mm square openings is placed on a 19 mm × 25 mm copper plate (thickness: 3 mm), and the copper paste for bonding is applied by screen printing using a metal scraper. A 2 mm × 2 mm copper block (thickness: 250 μm) with a nickel-plated surface to be bonded is placed on the coated copper paste for bonding, and gently pressed with tweezers. It is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 3 L / min to replace the air with argon gas. After that, hydrogen gas is flowed in at 300 ml / min, and the temperature is raised for 10 minutes. After heating, sintering treatment is carried out under the conditions of a maximum temperature of 350°C and a maximum temperature holding time of 10 minutes to obtain a bonded body having a copper plate and a nickel-plated copper block bonded thereto. After sintering, the argon gas is replaced with 0.3 L / min for cooling, and the bonded body is taken out into the air at a temperature below 50°C.
[0184] (Example 12)
[0185] A bonded body was produced by the following method using the bonding copper paste 4. The die shear strength of the bonded body was measured by the method described later.
[0186] A stainless steel metal mask (thickness: 100 μm) with 3 rows and 3 columns of 3 mm × 3 mm square openings is placed on a 19 mm × 25 mm copper plate (thickness: 3 mm), and the copper paste for bonding is applied by screen printing using a metal scraper. A 2 mm × 2 mm copper block (thickness: 250 μm) with a gold-plated surface to be bonded is placed on the coated copper paste for bonding, and gently pressed with tweezers. It is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 3 L / min to replace the air with argon gas. After that, hydrogen gas is flowed in at 300 ml / min, and the temperature is raised for 10 minutes. After heating, sintering treatment is carried out under the conditions of a maximum temperature of 350°C and a maximum temperature holding time of 10 minutes to obtain a bonded body having a copper plate and a gold-plated copper block bonded thereto. After sintering, the argon gas is replaced with 0.3 L / min for cooling, and the bonded body is taken out into the air at a temperature below 50°C.
[0187] (Example 13)
[0188] A bonded body was produced by the following method using the bonding copper paste 4. The die shear strength of the bonded body was measured by the method described later.
[0189] A stainless steel metal mask (thickness: 100 μm) with 3 rows and 3 columns of 3 mm × 3 mm square openings is placed on a 19 mm × 25 mm copper plate (thickness: 3 mm), and the copper paste for bonding is applied by screen printing using a metal scraper. A 2 mm × 2 mm copper block (thickness: 250 μm) with a nickel-plated surface to be bonded is placed on the coated copper paste for bonding, and gently pressed with tweezers. A 15 mm × 15 mm SUS block (weight: 15 g) is placed on it in a manner overlapping 9 2 mm × 2 mm copper blocks (thickness: 250 μm) with a nickel-plated surface to be bonded, and it is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas is flowed in at 3 L / min to replace the air with argon gas. After that, hydrogen gas is flowed in at 300 ml / min, and the temperature is raised for 10 minutes. After heating, sintering was performed under the conditions of a maximum temperature of 350°C and a maximum temperature holding time of 10 minutes to obtain a joint body of a copper plate and a nickel-plated copper block. After sintering, the argon gas was replaced with 0.3 L / min for cooling, and the joint body was taken out into the air at a temperature below 50°C.
[0190] (Example 14)
[0191] A bonded body was produced by the following method using the bonding copper paste 4. The die shear strength of the bonded body was measured by the method described later.
[0192] A stainless steel metal mask (thickness: 100 μm) with 3 rows and 3 columns of 3 mm × 3 mm square openings is placed on a 19 mm × 25 mm copper plate (thickness: 3 mm), and the copper paste for bonding is applied by screen printing using a metal scraper. A 2 mm × 2 mm copper block (thickness: 250 μm) with a nickel-plated surface to be bonded is placed on the coated copper paste for bonding, and it is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 3 L / min to replace the air with argon gas. After that, hydrogen gas is flowed in at 300 ml / min, and the temperature is raised for 10 minutes. After heating, sintering treatment is carried out under the conditions of a maximum temperature of 250°C and a maximum temperature holding time of 60 minutes to obtain a bonded body having a copper plate and a nickel-plated copper block bonded thereto. After sintering, the argon gas is replaced with 0.3 L / min for cooling, and the bonded body is taken out into the air at a temperature below 50°C.
[0193] (Example 15)
[0194] A bonded body was produced by the following method using the bonding copper paste 4. The die shear strength of the bonded body was measured by the method described later.
[0195] A stainless steel metal mask (thickness: 100 μm) with 3 rows and 3 columns of 3 mm × 3 mm square openings is placed on a 19 mm × 25 mm copper plate (thickness: 3 mm), and the copper paste for bonding is applied by screen printing using a metal scraper. A 2 mm × 2 mm copper block (thickness: 250 μm) with a nickel-plated surface to be bonded is placed on the coated copper paste for bonding, and it is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 3 L / min to replace the air with argon gas. After that, hydrogen gas is flowed in at 300 ml / min, and the temperature is raised for 20 minutes. After heating, sintering treatment is carried out under the conditions of a maximum temperature of 450°C and a maximum temperature holding time of 10 minutes to obtain a bonded body having a copper plate and a nickel-plated copper block bonded thereto. After sintering, the argon gas is replaced with 0.3 L / min for cooling, and the bonded body is taken out into the air at a temperature below 50°C.
[0196] (Comparative Examples 1 to 6)
[0197] A bonded body was produced by the same method as in Example 1 except that the bonding copper pastes 13 to 18 were used. The die shear strength of the bonded body was measured by the method described below.
[0198] <Measurement method>
[0199] (Chip shear strength)
[0200] The bonding strength of the joint body was evaluated by die shear strength. A universal bonding strength tester (4000 series, manufactured by DAGE) equipped with a DS-100 force sensor was used to press the copper block in the horizontal direction at a measuring speed of 5 mm / min and a measuring height of 50 μm to measure the die shear strength of the joint body. The average value of the values measured for 8 joint bodies was taken as the die shear strength.
[0201] (50% volume average particle size)
[0202] The 50% volume average particle size was measured according to the following (1) to (5) using a Shimadzu nanoparticle size distribution measuring apparatus (SALD-7500nano, manufactured by Shimadzu Corporation) and accompanying software (WingSALDII-7500-for Japanese V3., manufactured by Shimadzu Corporation).
[0203] (1) Software settings
[0204] Start WingSALDII-7500-for Japanese V3.1 using the computer attached to the measuring device, press the manual control to initialize the device. After the initialization is completed, specify the save file name, click "Next", set the measurement conditions and particle size distribution calculation conditions as follows, and click "Next".
[0205] (Measurement conditions)
[0206] Detection of diffracted / scattered light
[0207] Average times (number of measurements: 1): 128, number of measurements: 1, measurement interval (seconds): 2
[0208] ·Measurement of absorbance range
[0209] Maximum value: 0.2, Minimum value: 0
[0210] Blank area / Measurement area
[0211] Maximum allowable variation of blank measurement: 150, optimal measurement range (MAX): 45000, optimal measurement range (MIN): 15000
[0212] (Particle size distribution calculation conditions)
[0213] Refractive index selection: reference sample / pure metal / semiconductor, etc. (solid value)
[0214] Sample material: 4Copper
[0215] Refractive index selection: 1.18-2.21, check "Evaluate side / rear sensors"
[0216] (2) Blank determination
[0217] The Shimadzu nanoparticle size distribution measuring device SALD-7500nano batch cell (SALD-BC75, manufactured by Shimadzu Corporation) was installed in the SALD-7500nano for measurement. α-Terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) was dripped into the batch cell with a funnel attached to the SALD-BC75 (component number S347-61030-41, manufactured by Shimadzu Corporation, hereinafter referred to as the "batch cell") using a glass pipette to reach between the two marking lines of the batch cell. Select "Diagnosis" and "Adjustment" on the screen of WingSALDII-7500-for Japanese V3. to confirm that the position sensor power is within the allowable range of the device. Click "Cancel" to return to the original screen and select blank measurement for measurement.
[0218] (3) Preparation of assay solution
[0219] 2 mg of the copper paste for bonding to be measured was placed on the stirring rod of the batch cell holder (part number S347-62301, manufactured by Shimadzu Corporation) attached to SALD-BC75, and installed in the batch cell with a funnel. Next, "Stirring" was selected on the screen of WingSALDII-7500-for Japanese V3., and stirring was performed for 15 minutes.
[0220] (4) Determination
[0221] After stirring, select "Measure" on the screen of WingSALDII-7500-for Japanese V3. to perform measurement. Repeat the steps (1) to (4) 4 times to perform 4 measurements.
[0222] (5) Statistics
[0223] Start WingSALDII-7500-for Japanese V3., click "Open", select the measured file, and display the measured data on the screen of WingSALDII-7500-for Japanese V3. Click "Overlay", and the 50.000% diameter will be displayed in the lower part of the screen, and the average value of the four times will be the 50% volume average particle diameter.
[0224] Tables 1 to 3 show the results of Examples and Comparative Examples.
[0225]
[0226] Table 2
[0227]
[0228] Table 3
[0229]
[0230] Comparison of the embodiments and the comparative examples shows that the mass ratio of submicron copper particles and micron copper particles affects the chip shear strength. It is believed that the reason is that when the micron copper particles are increased too much, the filling rate of the sintered copper layer is reduced, the sintered body is prone to produce a large number of voids, and the chip shear strength is reduced. On the other hand, it is believed that when the submicron copper particles are increased too much, a large number of voids are easily produced in the sintered body due to volume shrinkage, and the chip shear strength is reduced. In addition, it can be seen from the results of the embodiments that if the mass ratio of submicron copper particles and micron copper particles is appropriate, the sintered body of the copper paste for bonding is firmly bonded to any one of gold, nickel, and copper, showing good chip shear strength. In addition, in Example 13, the result of manufacturing the bonded body under the condition of applying a pressure of 0.0042MPa on the basis of applying the dead weight of the copper block to the copper paste for bonding is that the gap is crushed during bonding, the gap is reduced, and the bonding is more firmly bonded, thereby increasing the chip shear strength. In Example 15, the maximum temperature reached 450° C., and the sintering of the copper paste for bonding was further advanced compared with Example 4, so the die shear strength became better. In Comparative Examples 4 to 6, the volume average particle size of the submicron copper particles was too large, and the sintering property of the copper paste for bonding was reduced, so the die shear strength of the bonded body was reduced.
[0231] (Cross-sectional morphology observation)
[0232] The conjugate was fixed in a cup using a sample fixture (Samplklip I, Buehler), and epoxy injection resin (Epomaunto, Refinetec Co., Ltd.) was flowed around until the entire sample was embedded, and the sample was left to stand in a vacuum dryer and decompressed for 1 minute for degassing. After that, the epoxy injection resin was cured by placing it at room temperature (25°C) for 10 hours. A Refineso Lo (RCA-005, Refinetec Co., Ltd.) with a diamond shear wheel (11-304, Refinetec Co., Ltd.) was used to shear near the cross section of the conjugate to be observed after injection molding. The cross section was scraped using a polishing device (Refine Polisher Hv, manufactured by Refinetec Co., Ltd.) with water-resistant abrasive paper (Carbon Mac Paper, manufactured by Refinetec Co., Ltd.) to expose the cross section without cracks to the silicon chip, and then the excess injection resin was scraped to finish the size that can be placed on a CP (cross section polishing machine) processing machine. The CP processing machine (IM4000, manufactured by Hitachi High-Technologies Co., Ltd.) was used at an acceleration voltage of 6 kV and an argon gas flow rate of 0.07 to 0.1 cm3 The cross-section of the cut sample was polished under the conditions of 100 nm / min and 2 hours of treatment time. The cross-section was sputtered with platinum at a thickness of 10 nm using a sputtering device (ION SPUTTER, manufactured by Hitachi High-Technologies Co., Ltd.) to prepare a sample for SEM observation. The cross-section of the joint of the SEM sample was observed using a SEM device (ESEM XL30, manufactured by Philips) with an applied voltage of 10 kV.
[0233] Fig.10 This is a SEM image of a cross section of the bonded body of Example 1. Fig.11 This is a SEM image of a cross section of the bonded body of Example 12. Fig.12 This is a SEM image of a cross section of Example 13. Fig.13 This is a SEM image of a cross section of the bonded body of Comparative Example 2. Figures 10-12 It can be seen that the sintered body of the copper paste for bonding can be bonded to the copper plate 9, the gold-plated copper block 12, and the nickel-plated copper block 13 through the sintered body 10 of micron copper particles and the sintered body 11 of submicron copper particles. Figures 10-12 It is shown that when the mass ratio of submicron copper particles to micron copper particles is appropriate, the micron copper particles are oriented approximately parallel to the surface to be joined, and the submicron copper particles fill the gaps between them. Fig.13 This indicates that when the number of submicron copper particles is too small relative to the number of micron copper particles, the gaps between the micron copper particles cannot be sufficiently filled. It is believed that due to this structural difference, the bonded body of Comparative Example 2 failed to obtain sufficient die shear strength.
[0234] Explanation of symbols
[0235] 1 sintered body of copper paste for bonding, 2 first member, 3 second member, 5a, 5b lead frame, 6 electric wire, 7 injection resin, 8 semiconductor element, 9 copper plate, 10 sintered body of micrometer copper particles, 11 sintered body of submicrometer copper particles, 12 gold-plated copper block, 13 nickel-plated copper block, 100 bonded body, 110 semiconductor device, 21 insulating substrate, 22 first electrode, 23 semiconductor element, 24 second electrode, 25 metal wiring, 26 third electrode, 27 electric wire, 28 copper plate, 29 insulator, 30 block, 31 sealing material, 32 first heat-conducting member, 33 second heat-conducting member, 34 electrode, 35 electric wire, 200 semiconductor device, 210 semiconductor device, 220 semiconductor device, 300 semiconductor device, 310 semiconductor device, 320 semiconductor device, 400 semiconductor device
Claims
1. A copper paste for bonding, comprising metal particles and a dispersion medium, wherein: The metal particles contain submicron copper particles having a volume average particle size of 0.3 μm or more and 0.8 μm or less and micron copper particles having a volume average particle size of 2 μm or more and 50 μm or less, the content of the submicron copper particles and the sum of the contents of the micron copper particles being 80% by mass or more based on the total mass of the metal particles, the content of the submicron copper particles being 30% by mass or more and 90% by mass or less based on the sum of the mass of the submicron copper particles and the mass of the micron copper particles, and the content of the micron copper particles being 10% by mass or more and 90% by mass or less based on the total mass of the metal particles.
2. The copper paste for bonding according to claim 1, wherein The micron copper particles are in the form of thin flakes. The copper paste for bonding according to claim 1 or 2, which is for non-pressurized bonding.
4. A method for manufacturing a joint body, comprising the following steps: preparing a stacked body having a first component, and a copper paste for joining according to any one of claims 1 to 3 and a second component on one side of the first component in the direction of its own weight, and sintering the copper paste for joining under the condition of being subjected to the own weight of the first component, or under the condition of being subjected to the own weight of the first component and a pressure of 0.01 MPa or less.
5. A method for manufacturing a semiconductor device, comprising the following steps: preparing a stacked body having a first component, and on one side of the first component in a direction in which its own weight acts, the copper paste for bonding according to any one of claims 1 to 3 and a second component in sequence, sintering the copper paste for bonding under the own weight of the first component, or under the own weight of the first component and a pressure of 0.01 MPa or less, at least one of the first component and the second component being a semiconductor element. 6 . A joined body comprising a first member, a second member, and a sintered body of the joining copper paste according to claim 1 , which joins the first member and the second member.
7. The conjugate according to claim 6, wherein: At least one of the first member and the second member contains at least one metal selected from the group consisting of copper, nickel, silver, gold, and palladium on a surface in contact with the sintered body. 8 . A semiconductor device comprising a first member, a second member, and a sintered body of the copper paste for bonding according to claim 1 for bonding the first member and the second member, wherein at least one of the first member and the second member is a semiconductor element.