Masterbatches with semi-crystalline polyolefin carrier resins
By using semi-crystalline polyolefin carrier resin to carry high-load alkenyl functional additives and perform electron beam curing, the problems of insufficient thermal creep performance and additive exudation are solved, and higher stability and performance improvement are achieved.
Patent Information
- Application Number
- CN201880085626.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-02-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2038-03-09
AI Technical Summary
The thermal creep performance of existing electron beam cured polyethylene is insufficient, and porous polymer pellets have problems with additive oozing and limited load capacity during storage and use, which affects its stability and performance at high temperatures.
Semi-crystalline polyolefins are used as carrier resins to carry high loading alkenyl functional additives, and cured polyolefin products are prepared by electron beam radiation to ensure that the additive does not exudate during storage and use, and to improve the intersection of polyolefins. Link density.
The thermal creep performance of electron beam cured polyethylene is significantly improved, ensuring that the additive does not exudate at high temperatures, extending storage time, reducing the radiation dose during the curing process, and improving the stability of the curing state.
Smart Images

Figure BDA0002572417410000291
Abstract
Description
Technical Field
[0001] Polyolefin compositions, electron beam curing, methods and articles. Background Art
[0002] Patent publications include CN103865420(A), DE102006017346A1, EP1433811A2, EP2889323A1, US5367030, US6187847B1, US6191230B1, US6936655B2, US20020198335A1, US20080176981A1, US8449801B1, US8691984B2, and US9147784B2.
[0003] CN103865420 (A) by G.-f. Chou et al. is about the encapsulation structure of solar panels. The composition of paragraph
[0074] is prepared by direct compounding and is directly used to prepare a film once it is made. The composition has 110.1 total parts by weight and is prepared from: 100 parts by weight of HDPE having a melt index (I2) of 0.04 g / 10 min, 2 parts by weight (1.82 wt%) of triallylpropyl isocyanurate, 6 parts by weight of TiO2, 2 parts by weight of vinyl tris(β-methoxyethoxy)silane and 0.1 parts by weight of 2-hydroxy-4-benzophenone.
[0004] DE 10 2006 017 346 A1 from Aa Nichtnennung relates to migration-stable masterbatches.
[0005] EP 2 889 323 A1 by S. Deveci et al. relates to a polymer composition comprising carbon black and a carrier polymer for the carbon black.
[0006] US9147784B2 by Y. Shirahige et al. is about a sealing material sheet for solar cell modules.
[0007] Masterbatch is a solid or liquid additive concentrate formulation for delivering additives to a host polymer in need. After solidification, the host polymer (sometimes referred to as a host resin, a matrix resin or a matrix polymer) forms a cured product (e.g., a thermosetting material) comprising a network polymer or a matrix. Additives can be used to improve the curing rate or degree of the host polymer or enhance the performance of the cured product. Typical masterbatches include additives and carrier resins, sometimes referred to as carrier polymers. Preparations are prepared by mixing or blending a smaller amount of masterbatch with a significantly larger amount of host polymer. The concentration of additives in the masterbatch is significantly higher than its concentration in the formulation.
[0008] Electron beam radiation can be used in a method for curing (crosslinking) polyolefins. The method comprises applying a dose of electron beam radiation to an (electron beam) curable (EBC) polyolefin compound to obtain a cured polyolefin product. The method directly forms covalent bonds between polyolefin macromolecules of the EBC polyolefin compound. The electron beam curing method can be used to cure various types of polyolefins, including low density polyethylene (LDPE), linear low density polyethylene (LLDPE) and high density polyethylene (HDPE).
[0009] We introduce the following problems: (a) how to improve the thermal creep (heat setting) properties of electron beam cured polyethylene, (b) how to increase the electron beam radiation curing of (electron beam) curable (EBC) polyolefin compounds, and (c) how to prepare a stable additive masterbatch.
[0010] Crosslinked low density polyethylene (XLDPE) and crosslinked linear low density polyethylene (XLLDPE) are used for various industrial applications, wherein they are exposed to high operating temperatures, such as the insulating layer of hot water pipes and power cables. For these applications, crosslinked polyethylene should have enough thermal creep (heat setting) properties (that is, keep its shape at operating temperatures). The thermal creep properties of (electron beam) crosslinked high density polyethylene are usually weaker than the thermal creep properties of (electron beam) crosslinked linear low density polyethylene. Therefore, relative to independent linear low density polyethylene, only high density polyethylene is blended into linear low density polyethylene, and then the blend described in electron beam curing is expected to not improve thermal creep properties.
[0011] If the dose of electron beam radiation is too high, undesirable side effects may occur. These include the generation of excessive heat, charge and / or H2 gas. Excessive heat may cause oxidation or degradation of the cured polyolefin product. Excessive H2 gas may cause bubbles to form in the cured polyolefin product. Excessive charge may cause discharge from the cured polyolefin product. If the dose applied is too low, the compound is not fully cured or reaches a sufficient state of cure (degree of cure or crosslink density), and the performance of the incompletely cured polyolefin product may not be suitable for the intended purpose of protecting such cables.
[0012] The severity of these problems can be mitigated by mixing a small amount of an adjuvant additive into an EBC polyolefin compound to obtain an (electron beam) curable (EBC) formulation comprising an EBC polyolefin compound and an adjuvant. The EBC formulation can be cured with an electron beam at a lower radiation dose than the dose used to cure the EBC polyolefin compound without an adjuvant. In addition, by virtue of the additional crosslinking effect of the multivalent crosslinking groups derived from the silicon-based adjuvant, the resulting cured polyolefin product can reach the same or higher cure state compared to the cure state of a comparatively cured polyolefin product prepared without an adjuvant at the same lower EB dose. With all other conditions being equal, the higher the loading of the adjuvant in the EBC formulation, the lower the dose of electron beam radiation that can be used to achieve a given cure state.
[0013] The EBC polyolefin compound used as the main polymer in the coating of wires and cables can be a polyethylene, such as low density polyethylene (LDPE) or linear low density polyethylene (LLDPE). Typical additives used for these coatings have a polar main chain or substructure bonded to two or more alkenyl groups, such as triallyl isocyanurate (TAIC). There may be problems with storing EBC formulations of LDPE and / or LLDPE (main polymer) and 0.5 wt% or more additives at room temperature without additive leaching. The rate and / or extent of leaching may vary with increasing storage time and / or temperature (elevated temperature above room temperature and below the melting temperature of LDPE and / or LLDPE). The more leaching occurs, the worse the electron beam curing effect of the EBC formulation.
[0014] For the goal of higher additive loading in EBC formulations, porous polymer pellets can be tried. Porous polymer pellets are commercially available. For example, Membrana GmbH, Obernburg, Germany supplies porous polymer pellets under the brands ACCUREL XP and ACCUREL MP. These porous polymer pellets are composed of polypropylene, HDPE, LDPE, LLDPE, EVA, EMA, PC, PMMA, PA6, PA12, PS, SBC, SAN, PET or biopolyester, PLA. These porous pellets are said to have an additive loading capacity of up to 50% to 70%, depending on the specific product and the additives loaded.
[0015] Problems with porous polymer pellets include limited polymer selection and leakage of additives from the pores of the loaded pellets. The problem is more severe when the additive is a liquid, especially one of low surface tension and low viscosity at room temperature (23 degrees Celsius (° C.). When the porous polymer pellets are squeezed or compressed, such as when they are loaded with additives or the loaded pellets are transferred or fed, the squeezing / compression can push the liquid additive out of the pores of the porous polymer pellets. Any porous polymer pellet containing a load or the resulting product prepared therefrom may have an insufficient amount of additive for its intended use. Summary of the invention
[0016] We envision a technical solution that introduces one, two or more of the following problems: (a) how to improve the thermal creep (heat setting) properties of electron beam cured polyethylene, (b) how to increase electron beam radiation curing of (electron beam) curable (EBC) polyolefin compounds, and (c) how to prepare a stable additive masterbatch. The technical solution provides an alternative to using porous polymer pellets to carry additives, and unlike porous polymer pellets, the technical solution is unpredictably capable of carrying high loads of additives including liquid additives (such as triallyl isocyanurate) without leaching during storage thereof. The technical solution comprises a carrier resin that is a semi-crystalline polyolefin. The semi-crystalline polyolefin can be substantially non-porous and is suitable for delivering additives to EBC polyolefin compounds (host polymers) such as LDPE and / or LLDPE. Surprisingly, despite its semicrystalline, nonporous nature, the semicrystalline polyolefin is able to carry high loadings of additives, such as up to 20 wt%, and possibly more TAIC, without it seeping out during storage at room temperature, or leaking out during handling involving compression or extrusion. Even at elevated temperatures (above room temperature and below the melting temperature of the semicrystalline polyolefin), the inventive carrier resin may be able to carry high loadings of liquid or solid additives without it seeping out or leaking out.
[0017] Without being bound by theory, we believe that the semi-crystalline polyolefin defines a tortuous path therein that captures the auxiliary agent, releasing the auxiliary agent only after the crystalline portion of the semi-crystalline polyolefin has melted. Without being bound by theory, we believe that this advantage prevents the auxiliary agent from prematurely flowing out of the heated semi-crystalline polyolefin (such as granules or pellets) before it can be fully mixed into the melt of the EBC polyolefin compound (host polymer).
[0018] The technical solution is achieved and includes the invention of an additive masterbatch, which includes a semi-crystalline polyolefin (carrier resin) containing an alkenyl functional additive. In addition, the present invention is an EBC formulation comprising the masterbatch of the present invention and an EBC polyolefin compound (host polymer); a cured polyolefin product prepared by electron beam irradiation of the EBC formulation; methods for preparing and using the masterbatch, formulation and product; and articles containing or prepared from the masterbatch, formulation and product. We believe that the cured polyolefin product has direct polyolefin-polyolefin bonds and polyolefins crosslinked via multivalent crosslinking groups derived from the alkenyl functional additive.
[0019] The formulator can use the masterbatch of the present invention to quickly prepare EBC formulations, and the manufacturer can use the EBC formulation to prepare a cured polyolefin product with fewer defects relative to a comparative EBC polyolefin compound (host polymer) without an additive and a cured polyolefin product prepared therefrom. Advantageously, the exudation / leakage stability of the additive masterbatch of the present invention enables formulators and manufacturers to reserve the additive masterbatch. This also enables manufacturers to use the additive masterbatch from the reserve to prepare EBC formulations just before electron beam curing in order to shorten or eliminate the storage of the EBC formulation, thereby avoiding any risk of additives exuding from the EBC formulation. DETAILED DESCRIPTION
[0020] The Summary and Abstract are incorporated herein by reference.Examples of embodiments include the following numbered aspects.
[0021] Aspect 1. An additive masterbatch comprising (A) a semi-crystalline polyolefin carrier resin and (B) an olefin functional additive disposed in the (A) semi-crystalline polyolefin carrier resin; wherein (A) is 80.0 wt% to 99.9 wt% (wt%), alternatively 80.0 wt% to 99.0 wt%, alternatively 80.0 wt% to 98.9 wt%, alternatively 84 wt% to 98.9 wt%, alternatively 84 wt% to 98.8 wt%, alternatively 85 wt% to 94 wt%, of the combined weight of components (A) and (B), and (B) is 20.0 wt% to 0. .1wt%, alternatively 20.0wt% to 1.0wt%, alternatively 20.0wt% to 1.1wt%, alternatively 16wt% to 1.1wt%, alternatively 16wt% to 1.2wt%, alternatively 15wt% to 6wt%; wherein (A) the semi-crystalline polyolefin carrier resin has a crystallinity of 55.0 weight % to less than 100 weight % (wt%), as measured by a crystallinity test method using differential scanning calorimetry (DSC); wherein when (A) the semi-crystalline polyolefin carrier resin is a semi-crystalline polyethylene, the density of the semi-crystalline polyethylene is greater than 0.935 grams per cubic centimeter (g / cm 3). (A) the semi-crystalline polyolefin carrier resin is in a dispersed solid form, such as powder, granules, pellets or any combination of two or more thereof. The term "when..." above refers to a non-limiting embodiment of (A) the semi-crystalline polyolefin carrier resin. When (A) the semi-crystalline polyolefin carrier resin is not a semi-crystalline polyethylene, the additive masterbatch includes additional embodiments.
[0022] Aspect 2. The additive masterbatch according to aspect 1 is characterized in that any one of (i) to (x) is limited: (i) the additive masterbatch does not contain (C) (electron beam) curable polyolefin compound (host polymer) other than component (A); (ii) the additive masterbatch further comprises at least one additive independently selected from optional additives (D) to (L): (D) flame retardant, (E) antioxidant, (F) processing aid, (G) colorant, (H) metal deactivator, (I) hydrolyzable silane without (unsaturated carbon-carbon bonds), (J) corrosion inhibitor, (K) hindered amine light stabilizer, and (L) different from components (A) and (C) and being ethylene / (C4-C 20 ) an ethylene copolymer of an α-olefin copolymer, an ethylene / unsaturated carboxylic acid ester copolymer or a propylene / ethylene copolymer; (iii) the additive masterbatch does not contain a porous resin containing an olefinic functional additive (e.g., a porous LDPE, EVA copolymer or EEA copolymer powder, granules or pellets having pores containing an olefinic functional additive); (iv) the additive masterbatch does not contain any porous resin; (v) the additive masterbatch consists of components (A) and (B) (i.e., the additive masterbatch does not contain any components other than (A) and (B) and the above-mentioned additive masterbatch for (A) ), the wt% values of (B) and (C) are the wt% values of the total weight of the additive masterbatch (100.00wt%)); (vi) both of (i) and (ii); (vii) both of (i) and (iii); (viii) both of (i) and (iv); (ix) the additive masterbatch is capable of being maintained at a temperature of 23°C for at least 20 days without leaching of the olefinic functional additive, as measured by the Leakage Test Method (quantitative, described subsequently); and (x) both of (ix) and any one of (i) to (viii).
[0023] Aspect 3. The additive masterbatch according to aspect 1 or 2, wherein (A) the semi-crystalline polyolefin carrier resin comprises, alternatively consists essentially of, alternatively consists of: any one of (i) to (viii): (i) semi-crystalline medium density polyethylene; (ii) semi-crystalline high density polyethylene; (iii) semi-crystalline polypropylene; (iv) semi-crystalline ethylene / propylene copolymer; (v) semi-crystalline poly(ethylene-co-α-olefin) copolymer; (vi) a combination (e.g., a mixture or blend) of any two or more of (i), (ii) and (v); (vii) the crystallinity of (A) the semi-crystalline polyolefin carrier resin is 57.5 wt% to <100 wt%, alternatively 60.0 wt% to <100 wt%, alternatively 65 wt% to <100 wt%, alternatively 70.0 wt% to <100 wt% (using the crystallinity test method of DSC); or (viii) any one of limitation (vii) and limitations (i) to (vi).
[0024] Aspect 4. The auxiliary agent masterbatch according to any one of aspects 1 to 3, wherein (A) the semi-crystalline polyolefin carrier resin satisfies any one of (i) to (viii): (i) a density greater than (0.936 g / cm 3 , alternatively at least 0.940 g / cm 3 and is polyethylene; (ii) has a density of 0.89 to 0.946 g / cm 3 , alternatively 0.900 to 0.940 g / cm 3and is polypropylene; (iii) a crystallinity of 60.0 wt% to <100 wt%, alternatively 65 wt% to <100 wt%, alternatively 70.0 wt% to <100 wt%, alternatively 75 wt% to <100 wt% (using the Crystallinity Test Method of DSC) and is polyethylene; (iv) a melt index (I2, 190°C / 2.16 kg load) of 0.1 to 20 grams per 10 minutes (g / 10 min), alternatively 0.2 to 20 g / 10 min, alternatively 0.5 to 10 g / 10 min, both measured according to the Melt Index Test Method (described later), and is polyethylene, or a melt flow rate (MFR) of 0.5 to 20 g / 10 min measured according to the Melt Flow Rate Test Method n (230°C / 2.16 kg load), measured according to the Melt Flow Rate Test Method (described subsequently), and is polypropylene; (v) the molecular weight distribution (MWD) is unimodal; (vi) the MWD is multimodal, alternatively bimodal; (vii) wherein the combined weight of ingredients (A) and (B) is 50 wt% to 100 wt%, alternatively 70 wt% to 100 wt%, alternatively 80 wt% to 100 wt%, alternatively 90 wt% to 100 wt%, alternatively 50 wt% to 99.9 wt%, alternatively 70 wt% to 99.9 wt%, alternatively 80 wt% to 99.9 wt%, alternatively 90 wt% to 99.9 wt% of the additive masterbatch; (viii) any two of (i) to (vii).
[0025] Aspect 5. The auxiliary agent masterbatch according to any one of aspects 1 to 4, wherein (B) the alkenyl functional auxiliary agent is as described by any one of limitations (i) to (viii): (i) (B) is 2-allylphenyl allyl ether; 4-isopropenyl-2,6-dimethylphenyl allyl ether; 2,6-dimethyl-4-allylphenyl allyl ether; 2-methoxy-4-allylphenyl allyl ether; 2,2'-diallyl bisphenol A; O,O'-diallyl bisphenol A; or tetramethyl diallyl bisphenol A; (ii) (B) is 2,4-diphenyl-4-methyl-1-pentene or 1,3-diisopropenylbenzene; (iii) (B) is triallyl isocyanurate; triallyl cyanurate; triallyl trimellitate; N,N,N' ,N',N",N"-hexaallyl-1,3,5-triazine-2,4,6-triamine; triallyl orthoformate; pentaerythritol triallyl ether; triallyl citrate; or triallyl aconitate; (iv) (B) is trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, tri(2-hydroxyethyl)isocyanurate triacrylate, or propoxylated glycerol triacrylate; (v) (B) is polybutadiene or trivinylcyclohexane having a 1,2-vinyl content of at least 50 wt%; (vi) (B) is an alkenyl-functional organosiloxane of formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), wherein the subscript n is an integer greater than or equal to 3; each R 1 are independently (C2-C4)alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C4) alkyl, phenyl or R 1 ; (vii) (B) is an alkenyl functional monocyclic organosiloxane of formula (II): (R 1 ) x Si(OR 2 ) (4-x) (II), where the subscript x is an integer from 0 to 4; each R 1 are independently (C2-C4)alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C4) alkyl, phenyl or R1 ; provided that the alkenyl functional monocyclic organosiloxane of formula (II) contains 2 to 4 R 1 group; (viii) a combination of (i) to (vii) or any two or more thereof.
[0026] Aspect 6. A method for storing an additive masterbatch, the method comprising maintaining the additive masterbatch according to any one of Aspects 1 to 5 at a temperature of 20°C to 25°C for at least 20 days to obtain a stored additive masterbatch without leaching of the olefinic functional additive, as measured by the Leakage Test Method (quantitative, described later).
[0027] Aspect 7. An electron beam curable formulation comprising the auxiliary agent masterbatch according to any one of aspects 1 to 5, or a stored auxiliary agent masterbatch prepared according to the method described in aspect 6, and (C) an (electron beam) curable (EBC) polyolefin compound.
[0028] Aspect 8. The electron beam curable formulation according to aspect 7, characterized in that any one of (i) to (xiii) is limited: (i) (C) the EBC polyolefin compound has a density of 0.910 to 0.925 g / cm 3 (ii) (C) EBC polyolefin compound having a density of 0.910 to 0.925 g / cm 3 (iii) (C) EBC polyolefin compound having a density of 0.926 to 0.940 g / cm 3 (iv) (C) EBC polyolefin compounds having a density of 0.941 to 0.990 g / cm 3 (v) (C) the EBC polyolefin compound is a polyethylene elastomer selected from elastomers based on ethylene copolymers, such as ethylene-propylene rubber (EPR), ethylene-1-butene rubber (EBR) and ethylene-1-octene rubber (EOR); (vi) (C) the EBC polyolefin compound is ethylene / (C3-C 20)α-olefin) copolymer; (vii) (C) the EBC polyolefin compound is an ethylene-propylene copolymer (EPP); (viii) (C) the EBC polyolefin compound is an ethylene-propylene-diene monomer (EPDM) copolymer; (ix) (C) the EBC polyolefin compound is a combination of any two or more of (i) to (viii); (x) the (electron beam) curable formulation further comprises at least one ingredient that is not an additive masterbatch and is independently selected from the optional additives (D) to (L): (D) flame retardant, (E) antioxidant, (F) processing aid, (G) colorant, (H) metal deactivator, (I) hydrolyzable silane free of (unsaturated carbon-carbon bonds), (J) corrosion inhibitor, (K) hindered amine light stabilizer, and (L) different from ingredients (A) and (C) and is ethylene / (C4-C 20 ) an ethylene copolymer additive of an α-olefin copolymer, an ethylene / unsaturated carboxylic acid ester copolymer or a propylene / ethylene copolymer; (xi) limitation (x) and any one of limitations (i) to (viii); (xii) (B) is 0.1 wt% to 20 wt%, alternatively 0.5 wt% to 15 wt%, alternatively 5 wt% to 15 wt%, alternatively 5 wt% to 14 wt%, based on the combined weight of components (A), (B) and (C); and (xiii) limitation (xii) and any one of limitations (i) to (xi).
[0029] Aspect 9. A method for preparing an (electron beam) curable formulation, the method comprising mixing together an auxiliary agent masterbatch according to any one of aspects 1 to 5 in dispersed solid form or a stored auxiliary agent masterbatch prepared by the method according to aspect 6 and a (C) EBC polyolefin compound in dispersed solid or melt form to obtain a mixture; and melt mixing or extruding the mixture to prepare an (electron beam) curable (EBC) formulation. In some aspects, the prepared EBC formulation is an EBC formulation according to aspect 8. The extruded EBC formulation can be granulated to obtain an EBC formulation in the form of solid pellets. Alternatively, the extruded EBC formulation can be cooled to obtain an EBC formulation in the form of a shaped solid, such as an insulation layer on a cable.
[0030] Aspect 10. A method of electron beam curing a formulation in need thereof, the method comprising irradiating an EBC formulation according to aspect 7 or 8 or an (electron beam) curable formulation prepared by the method according to aspect 9 with an effective dose of electron beam radiation to obtain an electron beam cured polyolefin product. In some aspects, the additive masterbatch is a stored additive masterbatch prepared by the method according to aspect 6. In some aspects, the method further comprises a preliminary step prior to the irradiation step, which maintains the additive masterbatch according to any one of aspects 1 to 5 at a temperature of 20° C. to 25° C. for 1 to 100 days, alternatively 5 to 50 days, alternatively 14 to 20 days, to obtain a stored additive masterbatch without leaching of olefinic functional additives, as measured by the Leakage Test Method (described later), wherein the additive masterbatch of the EBC formulation comprises a stored additive masterbatch. The EBC formulation in the form of a shaped solid can be cured by the method to obtain a shaped form of an electron beam cured polyolefin product.
[0031] Aspect 11. An electron beam cured polyolefin product prepared by the method according to aspect 10. The product may have a defined shape, such as a coating, a film, or a molded or extruded shape.
[0032] Aspect 12. An article comprising the electron beam cured polyolefin product according to aspect 11 and a component in operative contact therewith.
[0033] Aspect 13. A coated conductor comprising a conductive core and a polymeric layer at least partially surrounding the conductive core, wherein at least a portion of the polymeric layer comprises the electron beam cured polyolefin product of aspect 11.
[0034] Aspect 14. A method of conducting electricity, the method comprising applying a voltage across the conductive core of the coated conductor according to aspect 13 so as to generate an electric current through the conductive core.
[0035] Additive: A solid or liquid compound or substance that imparts desired properties to a host polymer, or to a formulation comprising a masterbatch and a host polymer, or to a reaction product prepared therefrom. The properties may be chemical, electrical, mechanical, optical, physical and / or thermal.
[0036] α-Olefin: Compound of formula (I): H2C=C(H)-R(I), wherein R is a linear alkyl group.
[0037] Carrier resin: A dispersed solid (particulate) polymer used to temporarily hold and later release additives.
[0038] Coagent: A multifunctional compound that enhances the crosslinking of (co)polymer macromolecules during the curing process. A single coagent molecule can react with two, three or more (co)polymer macromolecules to prepare a crosslinked (co)polymer macromolecule product, wherein two, three or more (co)polymer macromolecules have been covalently bonded to the same multivalent crosslinking group from which the coagent molecule is derived. Coagents are also called curing coagents or crosslinking coagents. Typical coagents are acyclic or cyclic compounds containing carbon atoms or silicon atoms in their respective main chain or ring substructure. Therefore, the main chain or ring substructure of the coagent is based on carbon (carbon-based substructure) or silicon (silicon-based substructure). The structure and function of the coagent are different from those of the curing agent.
[0039] Additive masterbatch: a masterbatch in which the additive comprises an additive. The additive masterbatch may contain at least 45 wt%, alternatively at least 50 wt%, alternatively at least 55 wt%, alternatively at least 70 wt%, alternatively at least 80 wt%, alternatively at least 90 wt% of (A) a semi-crystalline polyolefin carrier resin; all based on the total weight of the additive masterbatch. The additive masterbatch may contain 55 wt% to 1 wt%, alternatively 50 wt% to 1 wt%, alternatively 45 wt% to 1 wt%, alternatively 30 wt% to 1 wt%, alternatively 20 wt% to 1 wt%, alternatively 10 wt% to 1 wt% of (B) an olefinic functional additive. The additive masterbatch may not contain the following: (i) ethylene / silane copolymer, (ii) ethylene / vinyl acetate (EVA) copolymer, (iii) ethylene / alkyl acrylate copolymer (e.g., EEA copolymer), (iv) carbon black; (v) pigment or colorant; (vi) filler; (vii) any two of (i) to (vi), alternatively any six. The additive masterbatch may have >0 to 5 wt% of any other carrier resin, such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ethylene / α-olefin copolymer, EEA copolymer, polypropylene, nylon (e.g., nylon 6 or 66), BPA-PC, polycarbonate, BPA-PS, polysulfone, or polyphenylene ether; alternatively, the additive masterbatch may not contain any carrier resin other than (A) semi-crystalline polyolefin carrier resin, or any resin. The additive masterbatch further comprises a filler. The filler may be calcium carbonate, zinc borate, zinc molybdate, zinc sulfide, carbon black, talc, magnesium oxide, zinc oxide or clay. The additive masterbatch may not contain any additive that prevents electron beam curing of the host polymer.
[0040] Coated conductor: A material for conducting electricity that is at least partially covered by a layer of a protective material. An example is a power cable.
[0041] Comonomer composition distribution (CCD) or chemical composition distribution is the variation in the amount of comonomer units incorporated into copolymer macromolecules. When the amount of comonomer units incorporated varies over a wide range between copolymer macromolecules, CCD is referred to as "broad". When the amount of comonomer units incorporated into copolymer macromolecules is relatively constant between copolymer macromolecules, CCD is referred to as "narrow". The measurement of CCD is the comonomer distribution breadth index (CDBI).
[0042] The comonomer distribution breadth index (CDBI) is the weight percent (wt%) of copolymer molecules having a comonomer unit content within 50% (i.e., ±50%) of the median total molar comonomer unit content. Such relatively high CDBI values indicate that the comonomer unit content of the copolymer molecules is relatively uniform. The CDBI value of a linear polyethylene homopolymer containing no comonomer is defined as 100%. When the CDBI value of a first copolymer is higher than the CDBI value of a second copolymer, the higher CDBI value indicates that the comonomer distribution of the first copolymer is controlled or limited than the comonomer distribution of the second copolymer.
[0043] (Co)polymer: polymer (homopolymer) and / or copolymer. A homopolymer is a macromolecule composed of monomer units derived from only one monomer and without comonomer units. A copolymer is a macromolecule or a collection of macromolecules having monomer units and one or more different types of comonomer units, wherein the monomer units constitute the majority of the total units per molecule on average. The monomer units of a copolymer are prepared by polymerizing a first monomer, and one or more different types of comonomer units are prepared by polymerizing one or more different second or more monomers (referred to as comonomers). Monomers and comonomers are polymerizable molecules. A monomer unit, also referred to as a monomer unit or "mer", is the largest structural unit that is contributed to the structure of (one or more) macromolecules by a single monomer molecule (derived from a single monomer molecule). A comonomer unit, also referred to as a comonomer unit or "comer", is the largest structural unit that is contributed to the structure of (one or more) macromolecules by a single comonomer molecule (derived from a single comonomer molecule). Each unit is typically divalent (before any curing or crosslinking). "Dipolymers" are copolymers made from a monomer (e.g., ethylene) and one type of comonomer (e.g., 1-hexene). "Terpolymers" are copolymers made from a monomer (e.g., ethylene) and two different types of comonomers (e.g., propylene and 1,3-butadiene). Ethylene-based copolymers have 50 wt% to less than 100 wt% of monomer units derived from ethylene (CH2=CH2) and greater than 0 to 50 wt% of comonomer units derived from one or more comonomers. Propylene-based copolymers have 50 wt% to less than 100 wt% of monomer units derived from propylene (CH2=CH2CH3) and greater than 0 to 50 wt% of comonomer units derived from one or more comonomers (e.g., ethylene, butadiene).
[0044] Curing agent: A free radical generating compound (in situ) which, upon activation, forms free radicals and initiates or enhances reactions involving crosslinking of macromolecules. Activation of the curing agent can be achieved by subjecting the curing agent to heat or light. Examples of curing agents are peroxides, diazo-functional organic compounds and 2,3-dimethyl-2,3-diphenylbutane. Examples of peroxides are organic hydroperoxides of the formula HOOR and organic peroxides of the formula ROOR, wherein each R is independently a hydrocarbon group.
[0045] Curing: Cross-linking to form a cross-linked product (network polymer).
[0046] Day: Any consecutive 24-hour period.
[0047] Dispersed solid: Particulate material in a physical state characterized by relatively stable shape and volume. Examples are powders, granules and pellets.
[0048] Effective dose: An amount sufficient to cause the desired polyolefin to crosslink and receive the amount described.
[0049] Electron beam curable: Capable of being cured by irradiation (treatment) with high energy beta radiation (e.g. from a high energy electron beam accelerator). The radiation induces covalent bonding (crosslinking) between adjacent macromolecules, forming a network polymer.
[0050] High-density polyethylene (HDPE): density is 0.941 to 0.990 g / cm 3 , the α-olefin comonomer unit content is greater than 0wt%, and has short chain branches.
[0051] Linear low density polyethylene (LLDPE): density of 0.910 to 0.925 g / cm3, α-olefin comonomer unit content greater than 0 wt%, and short chain branching. The comonomer distribution breadth index (CDBI) of LLDPE can be 70 wt% to less than 100 wt%.
[0052] Low-density polyethylene (LDPE): density is 0.910 to 0.925 g / cm 3 LDPE can be prepared via a free radical polymerization mechanism in a catalyst-free high pressure polymerization process.
[0053] Medium density polyethylene (MDPE): density is 0.926 to 0.940 g / cm 3 .
[0054] Article: An object made by man (by hand or machine).
[0055] Masterbatch: See Background Technology.
[0056] Melt: A liquid formed by heating a solid material above its maximum melting temperature.
[0057] Polyolefin: A macromolecule or collection of macromolecules composed of structural units derived from polymerizable olefins.
[0058] Semi-crystalline: A solid material having a first region that is neither crystalline nor amorphous and a second region that is amorphous. The percent crystallinity is typically between 10% and 90% as measured by the Crystallinity Test Method described later.
[0059] Formed solid: A state of matter with relatively constant volume and shape that is artificially created (by hand or machine). For example, a fluid is extruded, molded, or coated into an external form, which is then cooled in place to produce a shaped solid.
[0060] Store: keep or maintain.
[0061] Exudation: The slow release of a liquid from a solid material that has the liquid contained within it.
[0062] The additive masterbatch, EBC formulation and cured polyolefin product may be referred to herein as the masterbatch, formulation and product of the present invention, respectively.
[0063] The masterbatch, formulation and / or product of the present invention may not contain an acid condensation catalyst. Examples of acid condensation catalysts are (i) organic sulfonic acids, organic phosphonic acids or hydrogen halides; (ii) organic sulfonic acids; (iii) alkyl substituted aryl sulfonic acids; (iv) alkyl substituted aryl sulfonic acids in which 1 or 2 (C5-C 20 ) alkyl substituent and 1 aryl which is phenyl or naphthyl; (v) (C1-C5) alkylphosphonic acid, wherein the (C1-C5) alkyl is unsubstituted or substituted with one -NH2 group; (vi) HF, HCl or HBr; (vii) Lewis acid; or (viii) a combination of any two or more of (i) to (vii).
[0064] The masterbatch, formulation and / or product of the present invention may be free of TiO2. The masterbatch and / or formulation of the present invention may have greater than or equal to 2.0 wt% of an additive, the MI may be greater than or equal to 0.1 g / 10 min, or a combination of any two or more thereof. The masterbatch, formulation and / or product of the present invention may be free of a curing agent, such as a peroxide, such as an organic hydroperoxide or an organic peroxide.
[0065] In some aspects, the additive masterbatch is a dispersed solid, such as a powder, granules and / or pellets.
[0066] Electron beam curable formulation. The total weight of all ingredients and additives in the masterbatch, formulation and product of the present invention is independently 100.00wt%. The electron beam curable formulation can be a single component formulation, alternatively a two-component formulation. The two-component formulation can include a first and a second part, wherein the first part is mainly composed of the auxiliary agent masterbatch and the second part is mainly composed of the (C) EBC polyolefin compound.
[0067] Ingredient (A) semi-crystalline polyolefin carrier resin. The semi-crystalline polyolefin carrier resin may be a semi-crystalline polyethylene, which is a semi-crystalline medium density polyethylene (MDPE), a semi-crystalline high density polyethylene (HDPE) or a combination thereof. Ingredient (A) semi-crystalline polyolefin carrier resin may be in any dispersed solid form, such as powder, granules, pellets or any combination of two or more thereof.
[0068] The maximum density of semi-crystalline HDPE can be 0.970g / cm 3 , alternatively up to 0.960 g / cm 3 , alternatively up to 0.950 g / cm 3 The density of semi-crystalline HDPE can be >0.935 to 0.970 g / cm 3 , alternatively 0.935 to 0.965 g / cm 3 The density of (A) can be measured by ASTM D-1505, "Test Method for Density of Plastics by the Density-Gradient Technique".
[0069] The crystallinity of the (A) semi-crystalline polyolefin carrier resin may be at least 55 wt%, alternatively at least 58 wt%, alternatively at least 59 wt%. In any of the immediately preceding aspects, the crystallinity may be up to 90 wt%, alternatively up to 80 wt%, alternatively up to 78 wt%. In some aspects, the crystallinity is 55 wt% to 80 wt%, alternatively 58 wt% to 78 wt%, alternatively 58 wt% to 76 wt%, alternatively 62 wt% to 78 wt%, alternatively any one of 59±1 wt%, 62±1 wt%, 76±1 wt%, and 77±1 wt%. The crystallinity of a semi-crystalline polyolefin resin, such as (A) a semi-crystalline polyolefin carrier resin, may be determined by differential scanning calorimetry (DSC) according to ASTM D3418-15 or the crystallinity test method using DSC described subsequently. For a semi-crystalline polyethylene resin, wt% crystallinity=(ΔH f *100%) / 292 J / g. For semi-crystalline polypropylene resin, wt% crystallinity = (ΔH f *100%) / 165 J / g. In each equation, ΔH f is the heat of fusion of the second heating curve of the polyethylene resin or the polypropylene resin, as the case may be, * indicates mathematical multiplication, / indicates mathematical division, 292 J / g is the heat of fusion of 100% crystalline polyethylene (ΔH f ) is the literature value, and 165 J / g is the heat of fusion (ΔH) of 100% crystalline polypropylene. f) is based on literature values. Preferably, the crystallinity is determined by DSC according to the Crystallinity Test Method described later.
[0070] (A) The melt index (I2, 190°C / 2.16 kg load) of the semi-crystalline polyolefin carrier resin may be 10 to 20 g / 10 min, alternatively 0.1 to 10 g / 10 min, alternatively 0.20 to 9 g / 10 min. I2 may be determined by ASTM D1238 as described later.
[0071] (A) The semi-crystalline polyolefin carrier resin may be characterized by a molecular weight distribution (MWD) that is unimodal, alternatively bimodal.
[0072] (A) The semi-crystalline polyolefin carrier resin may be a bimodal semi-crystalline HDPE and have a density of 0.950 to 0.958 g / cm 3 , and a melt index of 0.20 to 0.40 g / 10 min. (A) The semi-crystalline polyolefin carrier resin may be a unimodal semi-crystalline HDPE, and a density of 0.930 to 0.970 g / cm 3 , and a melt index of 0.65 to 9 g / 10 min, alternatively a density of 0.935 to 0.965 g / cm 3 , and the melt index is 0.7 to 8.5 g / 10 min.
[0073] Ingredient (B) alkenyl functional auxiliary agent. A molecule containing a main chain or ring substructure and two or more propenyl groups, acrylates and / or vinyl groups bonded thereto, or a collection of such molecules. In some aspects, the main chain or substructure is composed of carbon atoms and optionally nitrogen atoms and does not contain silicon atoms. In some aspects, the main chain or substructure is composed of silicon atoms and optionally oxygen atoms.
[0074] When the backbone or substructure of (B) an alkenyl functional auxiliary agent is composed of carbon atoms and optionally nitrogen atoms and does not contain silicon atoms, (B) may be an acryl functional auxiliary agent as described in any one of limitations (i) to (v), a vinyl functional auxiliary agent as described in any one of limitations (vi) to (vii), or a combination thereof as described in limitation (viii): (i) (B) is 2-allylphenyl allyl ether; 4-isopropenyl-2,6-dimethylphenyl allyl ether; 2,6-dimethyl-4-allylphenyl allyl ether; 2-methoxy-4-allylphenyl Phenyl allyl ether; 2,2'-diallyl bisphenol A; O,O'-diallyl bisphenol A; or tetramethyl diallyl bisphenol A; (ii) (B) is 2,4-diphenyl-4-methyl-1-pentene or 1,3-diisopropenylbenzene; (iii) (B) is triallyl isocyanurate ("TAIC"); triallyl cyanurate ("TAC"); triallyl trimellitate ("TATM"); N,N,N',N',N",N"-hexaallyl-1,3,5-triazine-2,4,6-triamine ("HATATA"; also known as N 2 ,N 2 ,N 4 ,N 4 ,N 6 ,N 6 -hexaallyl-1,3,5-triazine-2,4,6-triamine); triallyl orthoformate; pentaerythritol triallyl ether; triallyl citrate; or triallyl aconitate; (iv) (B) is a mixture of any two of the acryl functional adjuvants in (i). Alternatively, (B) may be an acrylate functional conventional adjuvant selected from the group consisting of trimethylolpropane triacrylate ("TMPTA"), trimethylolpropane trimethacrylate ("TMPTMA"), ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, and propoxylated glycerol triacrylate; (vi) polybutadiene having a 1,2-vinyl content of at least 50 wt%; (vii) trivinylcyclohexane ("TVCH") (viii) a combination of the foregoing adjuvants or any two or more thereof. Alternatively, (B) may be an adjuvant described in US 5,346,961 or US 4,018,852. In some aspects, (B) is an acryl-functional adjuvant as described by any one of limitations (i) to (v). In some aspects, (B) is an acryl-functional adjuvant selected from the group consisting of TAIC, TAC, TATM, HATATA, TMPTA, and TMPTMA; alternatively TAIC, TAC, and TMPTMA; alternatively TAIC; alternatively TAC; alternatively TATM; alternatively HATATA; alternatively TMPTA; alternatively TMPTMA.
[0075] When the main chain of the substructure of (B) the alkenyl functional auxiliary agent is composed of silicon atoms and optionally oxygen atoms, (B) may be an alkenyl functional organosiloxane of any of the restrictions (i) to (iv): (i) a monocyclic organosiloxane of formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), wherein the subscript n is an integer greater than or equal to 3; each R 1 are independently (C2-C4)alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R2 is independently H, (C1-C4) alkyl, phenyl or R 1 , wherein in some aspects, the additive masterbatch does not contain (i.e., lacks) a phosphazene base; (ii) an alkenyl-functional monocyclic organosiloxane of formula (II): (R 1 ) x Si(OR 2 ) (4-x) (II), where the subscript x is an integer from 0 to 4; each R 1 are independently (C2-C4)alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C4) alkyl, phenyl or R 1 ; provided that the alkenyl functional monocyclic organosiloxane of formula (II) contains 2 to 4, alternatively 2 or 3, alternatively 3 or 4, alternatively 2, alternatively 3, alternatively 4 R 1 In some aspects, (B) is a monocyclic organosiloxane of formula (I). In some aspects, (B) is a monocyclic organosiloxane of formula (I), wherein the subscript n is an integer of 3 or 4; each R 1 is independently (C2-C4)alkenyl; and each R 2 In some aspects, (B) is a monocyclic organosiloxane of formula (I), wherein the subscript n is an integer of 3 or 4; each R 1 is independently (C2-C4)alkenyl; and each R 2 In some aspects, (B) is a monocyclic organosiloxane of formula (I), wherein the subscript n is an integer of 3 or 4; each R 1 is independently (C2)alkenyl (ie, vinyl); and each R 2It is methyl.
[0076] In some aspects, (B) is an acryl functional coagent or a monocyclic organosiloxane of formula (I). In some aspects, the acryl functional coagent is selected from TAIC, TAC, TATM, HATATA, TMPTA and TMPTMA; alternatively TAIC, TAC and TMPTMA; alternatively TAIC; alternatively TAC; alternatively TATM; alternatively HATATA; alternatively TMPTA; alternatively TMPTMA; and the monocyclic organosiloxane of formula (I) is selected from the monocyclic organosiloxane of formula (I), wherein the subscript n is an integer of 3 or 4; each R 1 is independently (C2-C4)alkenyl; and each R 2 is (C1-C4) alkyl; alternatively a monocyclic organosiloxane of formula (I) wherein the subscript n is an integer of 3 or 4; each R 1 is independently (C2)alkenyl; and each R 2 It is methyl.
[0077] Ingredient (C) electron beam curable (EBC) polyolefin compound ("host polymer"). The (C) EBC polyolefin compound may be a low density polyethylene (LDPE, linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), polyolefin elastomer, ethylene / (C3-C40) α-olefin) copolymer or a combination (e.g., blend or melt mixture) of any two or more thereof. The density of LDPE may be 0.910 to 0.925 g / cm 3 The density of LLDPE can be from 0.910 to 0.925 g / cm 3 The density of MDPE can be from 0.926 to 0.940 g / cm 3 The density of HDPE can be from 0.941 to 0.990 g / cm 3 The ethylene copolymer based elastomer may be selected from EPR and EBR, alternatively EPR and EOR, alternatively EBR and EOR, alternatively EPR, alternatively EBR, alternatively EOR. Examples of such elastomers are ENGAGE TM 、AFFINITY TM and INFUSE TM Polyolefin elastomer. Ethylene / (C3-C 20 The )α-olefin) copolymer may be an ethylene / propylene copolymer or an ethylene / (C4-C 20The (C) EBC polyolefin compound may differ from the (A) semi-crystalline polyolefin carrier resin and the (L) ethylene-based polymer additive in at least one property selected from the group consisting of monomer composition, comonomer composition, density, crystallinity, melt index, melt flow rate, number average molecular weight (M n ), weight average molecular weight (M w ), molecular weight distribution (M w / M n ) and porosity.
[0078] Prior to the mixing step for preparing the EBC formulation, the (C) EBC polyolefin compound may be dispersed in a solid form, such as powder, granules and / or pellets.
[0079] Optional ingredients (additives) (D) flame retardant. (D) Flame retardant is a compound that inhibits or slows the spread of fire by inhibiting chemical reactions in the flame. In some aspects, (D) flame retardant is (D1) mineral, (D2) organic halogen compound, (D3) (organic) phosphite compound; (D4) halogenated silicone; or (D5) any two or more of (D1) to (D4) combination. In some aspects, (D) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (D) is present in the masterbatch, formulation and / or product of the present invention at a concentration of 0.1wt% to 20wt%, alternatively 1wt% to 10wt%, alternatively 5wt% to 20wt% based on its total weight.
[0080] Optional Ingredients (Additives) (E) Antioxidants: Compounds used to inhibit oxidation of polyolefins. Examples of suitable secondary antioxidants are polymeric 1,2-dihydro-2,2,4-trimethylquinoline (Agerite MA); tris(4-tert-butyl-3-hydroxy-2,6-xylylmethyl)-s-triazine-2,4,6-(1H,3H,5H)trione (Cyanox 1790); distearyl-3,3-thiodipropionate (DSTDP); tetramethylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)methane (Irganox 1010); 1,2-bis(3,5-di-tert-butyl-4-hydroxyhydrocinnamoyl)hydrazine (Irganox 1024); bis(4,6-dimethylphenyl)isobutylene (Lowinox 22IB46); and 4,4-thiobis(2-tert-butyl-5-methylphenol) (TBM6). In some aspects, (E) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (E) is present in the masterbatch, formulation and / or product of the present invention at a concentration of 0.01 wt% to 10 wt%, alternatively 0.05 wt% to 5 wt%, alternatively 0.1 wt% to 3 wt% based on its total weight.
[0081] Optional ingredients (additives) (F) processing aids. Ingredient (F) can improve the flow of the melt of the additive masterbatch by the machine. (F) can be an organic processing aid, such as a fluoropolymer or a silicone processing aid, such as a polyorganosiloxane or a fluorofunctional polyorganosiloxane. In some aspects, (F) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (F) is present in the masterbatch, formulation and / or product of the present invention at a concentration of 1 wt% to 20 wt%, alternatively 2 wt% to 18 wt%, alternatively 3 wt% to 15 wt%, based on its total weight.
[0082] Optional ingredients (additives) (G) colorant. For example, a pigment or dye. For example, carbon black or titanium dioxide. Carbon black can be provided as a carbon black masterbatch, which is a formulation of poly (1-butene-co-ethylene) copolymer (≥95wt% to <100wt% of the total weight of the masterbatch) and carbon black (>0wt% to ≤5wt% of the total weight of the carbon black masterbatch. In some aspects, (G) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (G) colorant is present in the masterbatch, formulation and / or product of the present invention at 0.1wt% to 35wt%, alternatively 1wt% to 10wt%, based on its total weight.
[0083] Optional ingredients (additives) (H) metal deactivator. For example, oxalyl bis (benzylidene hydrazide) (OABH). In some aspects, (H) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (H) is present in the masterbatch, formulation and / or product of the present invention at 0.001 wt% to 0.2 wt%, alternatively 0.01 wt% to 0.15 wt%, alternatively 0.01 wt% to 0.10 wt%, based on the total weight.
[0084] Optional ingredient (additive) (I) A hydrolyzable silane free of (unsaturated carbon-carbon bonds). Suitable for scavenging moisture. Ingredient (I) may be a silane containing at least 1, alternatively at least 2, alternatively at least 3, alternatively 4 hydrolyzable groups (e.g., R as defined above) 2 ); and up to 3, alternatively up to 2, alternatively up to 1, alternatively 0 non-hydrolyzable (unsaturated carbon-carbon bond)-free groups (such as alkyl or aryl) of any monosilane. Examples of (I) are acetoxytrimethylsilane, 4-phenylmethylphenylsulfonyloxytributylsilane, dimethylamino-methoxy-dioctylsilane, octyltrimethoxysilane and tetramethoxysilane. In some aspects, (I) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (I) is present in the masterbatch, formulation and / or product of the present invention at 0.1 wt% to 2 wt%, alternatively 0.1 wt% to 1.5 wt%, alternatively 0.1 wt% to 1.0 wt%, based on the total weight thereof.
[0085] Optional ingredients (additives) (J) corrosion inhibitors. For example, tin (II) sulfate. In some aspects, (J) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (J) is present in the masterbatch, formulation and / or product of the present invention at 0.00001 wt% to 0.1 wt%, alternatively 0.0001 wt% to 0.01 wt%, based on its total weight.
[0086] Optional ingredients (additives) (K) Hindered amine light stabilizer. (K) is a compound that inhibits oxidative degradation. Suitable examples of (K) are dimethyl succinate, polymers with 4-hydroxy-2,2,6,6-tetramethyl-1-piperidin-ethanol (CAS No. 65447-77-0, commercially available LOWILITE 62); and poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6 hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]])(CAS 71878-19-8 / 70624-18-9, Chimassorb 994LD, BASF). In some aspects, (K) is not present in the masterbatch, formulation and / or product of the present invention. In some aspects, (K) is present in the masterbatch, formulation and / or product of the present invention at 0.001 wt% to 0.2 wt%, alternatively 0.01 wt% to 0.15 wt%, alternatively 0.01 wt% to 0.10 wt%, based on the total weight thereof.
[0087] Optional ingredient (additive) (L) ethylene copolymer additive. Ingredient (L) is different from ingredients (A) and (C). (L) is LDPE, ethylene / α-olefin copolymer, ethylene / unsaturated carboxylic acid ester copolymer (e.g., ethylene / vinyl acetate (EVA) copolymer, ethylene / ethyl acrylate (EEA) copolymer, or ethylene / ethyl methacrylate (EEMA) copolymer). In some aspects, (L) is not present in the masterbatch, formulation, and / or product of the present invention. In some aspects, (L) is present in the masterbatch, formulation, and / or product of the present invention at a concentration of 0.1 wt% to 20 wt%, alternatively 1 wt% to 10 wt%, alternatively 5 wt% to 20 wt%, based on the total weight thereof.
[0088] Other optional ingredients. In some aspects, the masterbatch of the present invention, formulations and / or products do not contain any optional ingredients. In some aspects, the masterbatch of the present invention, formulations and / or products do not contain any optional ingredients except ingredients (D) to (L). In some aspects, the masterbatch of the present invention, formulations and / or products additionally contain at least one optional ingredient (additive) in addition to or in place of (D) to (L). For example, a lubricant or an antiblocking agent.
[0089] Any optional ingredients may be applicable to impart at least one characteristic or property to a desired masterbatch of the present invention, formulation and / or product. Said characteristic or property may be applicable to improve the performance of a masterbatch of the present invention, formulation and / or product in operation or application, wherein the masterbatch of the present invention, formulation and / or product is exposed to elevated warm operating temperatures. Such operations or applications include melt mixing, extrusion, molding, hot water pipes and insulation layers of power cables.
[0090] (C3-C 20 )α-olefins and (C3-C 20 )α-olefins. Compounds of formula (I): H2C=C(H)-R(I), wherein R is a straight chain (C1-C 18 ) alkyl or straight chain (C2-C 18 (C3) The α-olefin is 1-propylene and its R group in formula (I) is methyl. (C2-C 18 ) Alkyl is a monovalent unsubstituted saturated hydrocarbon having 2 to 18 carbon atoms. (C2-C 18 Examples of (C4-C4-C4-alkyl) groups are ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl. 20 ) the α-olefin is 1-butene, 1-hexene or 1-octene; alternatively 1-butene, 1-hexene or 1-octene; alternatively 1-butene or 1-hexene; alternatively 1-butene or 1-octene; alternatively 1-hexene or 1-octene; alternatively 1-butene; alternatively 1-hexene; alternatively 1-octene; alternatively a combination of any two of 1-butene, 1-hexene and 1-octene.
[0091] Any compound herein includes all isotopic forms thereof, including naturally abundant forms and / or isotopically enriched forms, which may have additional uses, such as medical or anti-counterfeiting applications.
[0092] Method for curing by electron beam radiation. The method may include irradiating an electron beam of an EBC formulation with an effective dose of electron beam radiation. The effective dose of the electron beam radiation may be 49 to 201 kilojoules of energy (kJ / kg) per kilogram of EBC formulation, alternatively 49 to 160 kJ / kg, alternatively 80 to 201 kJ / kg, alternatively 80 to 160 kJ / kg, alternatively 50 to 80 kJ / kg, alternatively 100 to 140 kJ / kg, alternatively 160 to 201 kJ / kg. Electron beam radiation can be generated using an electron beam accelerator machine, such as the Aibang AB5.0 machine available from Aibang Radiation Technology Company, Limited, Wuxi, China. The electron beam irradiation step may be carried out at any suitable temperature, such as 10° C. to 50° C. (e.g., 23° C. ± 1° C.), in any suitable atmosphere, such as air or molecular nitrogen, and for any suitable length of time, such as 0.1 to 20 minutes, alternatively 0.1 to 10 minutes, alternatively 0.1 to 5 minutes. The radiation may be dosed continuously or intermittently, alternatively continuously.
[0093] Unless otherwise indicated, the following applies. Alternatively, before different embodiments. ASTM means standards organization, ASTM International, West Conshohocken, Pennsylvania, USA. IEC means standards organization, International Electrotechnical Commission, Geneva, Switzerland. Any comparative example is used only for illustrative purposes and should not be prior art. Absence or lack thereof means that there is no such thing as a complete absence; alternatively undetectable. IUPAC is the International Union of Pure and Applied Chemistry (IUPAC Secretariat, Research Triangle Park, North Carolina, USA). "Can" gives the right to choose, not necessity. Operability means being functionally capable or effective. Optional (ground) means not existing (or excluding), alternatively existing (or including). PPM is based on weight. Properties are measured using standard test methods and conditions for measurement (e.g., viscosity: 23°C and 101.3 kPa). Ranges include endpoints, subranges, and whole and / or fractional values contained therein, except that integer ranges do not include fractional values. Room temperature is 23°C ± 1°C. Substituted when referring to a compound means having one or more substituents in place of hydrogen, up to and including full substitution. Comonomer composition distribution can be characterized by the CDBI method.
[0094] Comonomer Distribution Width Index (CDBI) Method: Methods for calculating the CDBI value of a copolymer are known in the art, such as in WO 93 / 03093. The CDBI value of a copolymer is easily calculated by data obtained from techniques known in the art, such as TREF (temperature rising elution fractionation), such as described in, for example, US 5,008,204 or Wild et al., Journal of Polymer Science: Polymer Physics Edition (J. Poly. Sci. Polv. Phys. Ed.), Vol. 20, p. 441 (1982). The CDBI method is described in paragraphs
[0054] to
[0061] of U.S. Provisional Patent Application No. 62 / 478,163 filed on March 29, 2017 and its corresponding PCT International Patent Application No. PCT / US2018 / _____ filed on March __, 2018.
[0095] Crystallinity Test Method. Used to determine the crystallinity in wt% of a semi-crystalline polyolefin resin, such as (A) a semi-crystalline polyolefin carrier resin. Use a DSC instrument, DSC Q1000 (TA Instruments), to determine the melting peak and weight % (wt%) crystallinity as follows. Procedure (A) Baseline calibrate the instrument. Use the software calibration wizard. First obtain a baseline by heating the cell from -80°C to 280°C without any sample in an aluminum DSC pan. Then use a sapphire standard as instructed by the calibration wizard. 1 to 2 milligrams (mg) of fresh indium sample is analyzed by heating the standard sample to 180°C, cooling to 120°C at a cooling rate of 10°C / min, then holding the standard sample isothermally at 120°C for 1 minute, and then heating the standard sample from 120°C to 180°C at a heating rate of 10°C / min. Determine the heat of fusion (H2O2) of the indium standard sample. f )=28.71±0.50 joules / gram (J / g) and melting onset=156.6℃±0.5℃. The DSC measurements were performed on the test samples using the same DSC instrument. For polyethylene test samples, see procedure (B) below. For polypropylene test samples, see procedure (C) below. The crystallinity wt% determined using DSC will be about 3wt% lower than the crystallinity wt% determined according to the method based on the density of semi-crystalline polyolefins.
[0096] Procedure (B) DSC of polyethylene test sample. A test sample of the polymer is pressed into a film at a temperature of 160°C. 5 to 8 mg of the test sample film is weighed in a DSC pan. A lid is pressed on the pan to seal the pan and ensure a closed atmosphere. The sealed pan is placed in a DSC unit, the unit is equilibrated at 30°C, and heated to 140°C at a rate of about 100°C / min, the sample is held at 140°C for 1 minute, the sample is cooled to 0°C or lower (e.g. -40°C) at a rate of 10°C / min to obtain a cooling curve heat of fusion (H f ), and isothermally maintained at 0°C or lower (e.g. -40°C) for 3 minutes. The sample is then heated again to 180°C at a rate of 10°C / min to obtain the second heating curve melting heat (ΔH f ). Using the resulting curve, calculate the cooling curve heat of fusion (J / g) by integrating from the start of crystallization to 10°C. Calculate the second heating curve heat of fusion (J / g) by integrating from 10°C to the end of melting. Calculate the heat of fusion (ΔH) of the second heat curve of the test sample from the f ) and its heat of fusion normalized to 100% crystalline polyethylene to measure the crystallinity of the polymer by weight (crystallinity wt%), where crystallinity wt% = ((ΔH f *100%) / 292 J / g, where ΔH fAs defined above, * indicates mathematical multiplication, / indicates mathematical division, and 292 J / g is the heat of fusion (ΔH f )’s literature value.
[0097] Procedure (C) DSC of polypropylene test sample. A test sample of polypropylene was pressed into a film at a temperature of 210°C. 5 to 8 mg of the test sample film was weighed in a DSC pan. A lid was pressed onto the pan to seal the pan and ensure a closed atmosphere. The sealed pan was placed in a DSC cell and heated to 230°C at a rate of about 100°C / min, the sample was held at 230°C for 5 minutes, the sample was cooled to -20°C at a rate of 10°C / min to obtain a cooling curve heat of fusion, and was held isothermally at -20°C for 5 minutes. The sample was then heated again at a rate of 10°C / min until melting was complete to obtain a second heating curve heat of fusion ((ΔH f )). Using the obtained curve, calculate the cooling curve melting heat (J / g) by integrating from the start of crystallization to 10°C. Calculate the second heating curve melting heat (J / g) by integrating from 10°C to the end of melting. Calculate the second heating curve melting heat (ΔH) from the test sample. f ) and its heat of fusion normalized to 100% crystalline polypropylene to measure the crystallinity of the polymer by weight (crystallinity wt%), where crystallinity wt% = ((ΔH f *100%) / 165 J / g, where ΔH f As defined above, * indicates mathematical multiplication, / indicates mathematical division, and 165 J / g is the heat of fusion (ΔH f )’s literature value.
[0098] Density Test Method: Measured according to ASTM D792-13, Standard Test Methods for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B (used to test solid plastics in liquids other than water, such as in liquid 2-propanol). Report results in grams per cubic centimeter (g / cm 3 ) as the unit.
[0099] Thermal creep (heat set) test method: The test specimen (dog bone shape of the dimensions specified in ASTM 638-34; thickness <2 millimeters (mm); marking lines 20 mm apart) was placed in an oven at 200°C and a weight equal to 20 Newtons per square centimeter (N / cm 2) force. The elongation of the test sample (the distance between the marking lines) is then measured under these conditions and expressed as a percentage of the initial 20mm distance. For illustration, if the distance between the marking lines widens to 40mm, the thermal creep is 100% (100*(40-20) / 20)=100%), and if it widens to 100mm, the thermal creep is 400%. Under all other conditions being the same, the lower the crosslinking level in the test sample, the greater its elongation in the thermal creep test method. On the contrary, the higher the crosslinking level of the test sample, the smaller its elongation. If the crosslinking level of the test sample is low enough, the test sample may fail due to fracture, which may occur within a few minutes or even seconds at the beginning of its test run. Although power cables may not be able to withstand operating temperatures as high as 200°C, this test is a reliable way for industrial evaluation of materials used for their insulation layers. The lower the thermal creep percentage, the better the performance of the material. In the power cable industry, after the test sample is kept at 200°C for 15 minutes, a thermal creep of less than 175% passes the thermal creep test. And a thermal creep of less than 100% after 15 minutes at 200°C is particularly desirable. If the test sample is intact after 15 minutes, remove the weight and then take the test sample out of the oven and allow it to cool to room temperature. Measure the residual elongation of the test sample after cooling. For power cables, the residual elongation at room temperature should be less than 15% of the thermal creep value measured at 200°C.
[0100] Melt Flow Rate (230°C, 2.16 kilograms (kg), "MFR") Test Method: For propylene (co)polymers, the 230°C / 2.16 kg condition, formerly known as "Condition E" and also referred to as MFR, is measured according to ASTM D1238-13. The results are reported in grams eluted per 10 minutes (g / 10 min) or equivalently in decigrams per 1.0 minute (dg / 1 min). 10.0 dg = 1.00 g.
[0101] Melt Index (190°C, 2.16 kilograms (kg), "I2") Test Method: For ethylene (co)polymers, measured according to ASTM D1238-13 using the 190°C / 2.16 kg condition (formerly known as "Condition E" and also referred to as I2). The results are reported in grams eluted per 10 minutes (g / 10 min) or equivalently decigrams per 1.0 minute (dg / 1 min). 10.0 dg = 1.00 g.
[0102] Exudation Test Method (Qualitative): Prepare HDPE pellets containing additives as described later for the masterbatch examples of the present invention (e.g., IE1 to IE4). Prepare LLDPE pellets containing additives as described later for comparative EBC formulations CE1 to CE5. Add each pellet sample to a separate, unused, press-sealed polyethylene plastic bag (also known as a zip lock or snap seal bag). Seal the bag. Press the pellets in the bag. Store the bag and contents at room temperature for 14 days. At 14 days, observe the oil stains left on the surface of the bag under light. Oil stains indicate surface migration and poor solubility. The more oil stains on the bag surface, the more TAIC exudes. The amount of exudation is progressively ranked by characterizing the oil stains as none, minimal, small amounts, or significant (more than a small amount).
[0103] Exudation Test Method (Quantitative): HDPE pellets or LLDPE pellets were prepared as described above for the qualitative test method. The initial loading of the adjuvant on the freshly prepared pellets was measured using thermogravimetric analysis (TGA). Each pellet weighed 20 to 30 mg and had a volumetric size of approximately 4 mm×2.5 mm. The pellets were stored at room temperature for 20 days. At 20 days, a sample of the stored pellets was washed with acetonitrile (ACN) according to the following procedure: (1) 3.000 g ± 0.001 g of the pellet sample was weighed into a 40 mL vial. (2) 14.5 mL of ACN was fed into a 40 mL vial. (3) The vial was sealed with a rubber-lined cap and the sealed vial was shaken on an oscillator for 5 minutes. After shaking, the washed pellet sample was analyzed again by TGA to obtain the adjuvant content of the washed pellets. The % reduction in adjuvant content of washed pellets was calculated by comparing the initial adjuvant loading in fresh pellets with the adjuvant content in washed pellets. The % adjuvant migration in HDPE or LLDPE compounds was quantified as equal to the % reduction in said adjuvant content of the pellets after storage.
[0104] Examples
[0105] Semi-crystalline polyolefin carrier resin (A1): HDPE, with a density of 0.965 g / cc 3 , melt index (I2) is 7.5 to 8.5 g / 10 min; and has a unimodal MWD. By the Crystallinity Test Methods Parts (A) and (B), the second heating curve melting heat (ΔHf) of resin (A1) is 223.7 J / g, and the corresponding crystallinity is 76.6 wt%. As a product AXELERON TM CX6944NT CPD is commercially available from The Dow Chemical Company.
[0106] Olefin functional auxiliary (B1): triallyl isocyanurate (TAIC).
[0107] Alkenyl functional auxiliary (B2): tetramethyl-tetravinyl-cyclotetrasiloxane (ViD4).
[0108] Alkenyl-functional coagent (B3): trimethylolpropane trimethacrylate ("TMPTMA").
[0109] Alkenyl functional auxiliary (B4): triallyl cyanurate (TAC).
[0110] EBC polyolefin compound (C1): ethylene / 1-butene LLDPE (C1), stabilized with metal deactivator (H1) oxalyl bis(benzylidene hydrazide) (OABH) and two antioxidants, and having a density of 0.921 g / cc 3 , a melt index (I2) of 0.7 g / 10 min, and a unimodal MWD. It is commercially available from The Dow Chemical Company as a pellet product DFDA-7540NT.
[0111] Comparative Examples 1 and 2 (CE1 and CE2): Two comparative EBC formulations were prepared by soaking LLDPE (C1) pellets with one of the additives (B1) in an 80°C oven for 6 hours to allow the additive to penetrate into the LLDPE pellets.
[0112] Comparative Examples 3 to 5 (CE3 to CE5): Three comparative EBC formulations were prepared by compounding, respectively. LLDPE (C1) was fed into a Brabender mixer at 120°C. The LLDPE (C1) was completely melted at a rotor speed of 35 revolutions per minute (rpm). Then, additives (B2) were gradually added to one of (B4) over 15 minutes, respectively, and the resulting mixture was melt-mixed at 35 rpm for 4 minutes. The rotation was then stopped and the mixed EBC formulation (one of CE3 to CE5) was taken out of the Brabender mixer. The formulation was quickly hot-pressed at 120°C to form formulation CE3, CE4 or CE5 into a 1 millimeter (mm) thick sheet.
[0113] Comparative Examples 6 and 7: Comparative cured polyolefin products were prepared by hot pressing formulation CE1 or CE2 at 120°C to form formulation CE1 or CE2 into 1-mm thick sheets, and then curing the sheets of EBC formulations of CE1 and CE2, respectively, with an electron beam at a radiation dose of 100 kilojoules per kilogram (kJ / kg).
[0114] Inventive Examples 1 to 4 (IE1 to IE4): additive masterbatches MB1 to MB4 of the present invention. (A1) and any one of the additives (B1) to (B4) were melt-mixed in a Banbury compounder using a compounding temperature of 155° C. and a rotor speed of 60 to 65 revolutions per minute (rpm), and then the melt of the additive masterbatch was extruded under air cooling to obtain an extruded additive masterbatch, and the extruded additive masterbatch was pelletized to obtain additive masterbatches of IE1 to IE4 in the form of pellets.
[0115] Inventive Examples 5 to 6: EBC formulations EBCF1 to EBCF2 of the present invention.
[0116] Inventive Examples 7 and 8: Inventive cured polyolefin products were prepared by electron beam curing EBC formulations EBCF1 and EBCF2 of IE5 and IE6, respectively, with a radiation dose of 100 kilojoules per kilogram (kJ / kg).
[0117] See Table 1 below for composition information on comparative EBC formulations CE1 to CE5. See Table 2 below for composition information on masterbatches MB1 to MB4 for IE1 to IE4. See Table 3 below for composition information on inventive EBC formulations EBCF1 to EBCF2 for IE5 to IE6. See Table 4 below for exudation results on CE1 to CE5. See Table 5 below for exudation results on IE1 to IE6. See Table 6 below for thermal creep on CE6 and CE7 and IE7 and IE8.
[0118] Table 1: Composition (wt%): Comparative EBC formulations CE1 to CE5.
[0119] Instance number CE1 CE2 CE3 CE4 CE5 HDPE(A1) 0 0 0 0 0 TAIC(B1) 0.5 0.8 0 0 0 ViD4(B2) 0 0 13 0 0 TMPTMA(B3) 0 0 0 13 0 TAC(B4) 0 0 0 0 13 LLDPE(C1) 99.5 99.2 87 87 87 total 100.00 100.00 100.00 100.00 100.00 Additives and loading (wt%) TAIC(0.5) TAIC(0.8) ViD4(13) TMPTMA(13) TAC(13)
[0120] Table 2: Composition (wt%): additive masterbatches MB1 to MB4 of the present invention of IE1 to IE4, respectively.
[0121] Instance number IE1 IE2 IE3 IE4 HDPE(A1) 85 87 87 87 TAIC(B1) 15 0 0 0 ViD4(B2) 0 13 0 0 TMPTMA(B3) 0 0 13 0 TAC(B4) 0 0 0 13 Total masterbatch wt% 100.00 100.00 100.00 100.00
[0122] Table 3: Composition (wt%): EBC formulations EBCF1 to EBCF2 according to the invention prepared with the additive masterbatch MB1 according to the invention.
[0123] Instance number IE5 IE6 MB1(IE1) 8 40 MB2(IE2) 0 0 MB3(IE3) 0 0 MB4(IE4) 0 0 LLDPE(C1) 92 60 Total EBC formulations 100.00 100.00 Additives and loading (wt%) TAIC(1.2) TAIC(6)
[0124] Table 4: Exudation results for comparative EBC formulations CE1 to CE5.
[0125] Instance number CE1 CE2 CE3 CE4 CE5 Test Materials EBC formulations EBC formulations EBC formulations EBC formulations EBC formulations Loss of additives through leakage Very rare Yes, obviously >5% >50% >10% Leakage test method Qualitative Qualitative Quantification Quantification Quantification
[0126] Table 5: Bleeding results for the inventive EBC formulations EBCF1 to EBCF2 and the inventive additive masterbatches MB2 to MB4.
[0127] Instance number IE2 IE3 IE4 IE5 IE6 Test Materials MB2 MB3 MB4 EBCF1 EBCF2 Loss of additives through leakage (during the test) 0% 0% 0% none none Leakage test method Quantification Quantification Quantification Qualitative Qualitative
[0128] The exudation data in Tables 4 and 5 show that the additive masterbatch of the present invention is significantly better at room temperature and prevents leaching of the ethylenically functional additive therefrom compared to the LLDPE / additive blends.
[0129] Table 6: Hot creep results for comparative cured polyolefin products CE6 and CE7 and inventive cured polyolefin products IE7 and IE8.
[0130]
[0131] *Cure = 100 kilojoules per kilogram (kJ / kg) of exposure dose of electron beam radiation; **Thermal creep: measured at 200°C on electron beam cured test material.
[0132] The hot creep data in Table 6 show that the inventive EBC formulations containing the inventive masterbatch cure significantly better to yield inventive cured polyolefin products with improved (reduced) hot creep at 200°C than comparative cured polyolefin products made from comparative EBC formulations containing the same olefin functional coagent but without the inventive masterbatch. Due to TAIC exudation limits, the TAIC loadings in the comparative EBC formulations are lower than the TAIC loadings in the inventive EBC formulations without such exudation limits. The higher TAIC loadings in the inventive EBC formulations show the beneficial effect of increasing the electron beam curing efficiency of the inventive curing process.
Claims
1. An additive masterbatch, comprising (A) a semi-crystalline polyolefin carrier resin and (B) an olefinic functional additive disposed in the (A) semi-crystalline polyolefin carrier resin, wherein the semi-crystalline polyolefin carrier resin is a semi-crystalline polyethylene, the semi-crystalline polyethylene is a semi-crystalline medium density polyethylene (MDPE), a semi-crystalline high density polyethylene (HDPE) or a combination thereof, and the olefinic functional additive is a molecule containing a main chain or a ring substructure and two or more propylene groups, acrylate groups and / or vinyl groups bonded thereto, or the A collection of molecules; wherein (A) is 80.0 wt% to 99.9 wt% (wt%) of the combined weight of components (A) and (B), and (B) is 20.0 wt% to 0.1 wt% of the combined weight; wherein the (A) semi-crystalline polyolefin carrier resin has a crystallinity of 55.0 wt% to less than 100 wt% (wt%), as measured by a crystallinity test method using differential scanning calorimetry (DSC); wherein the density of the semi-crystalline polyethylene is greater than 0.935 grams per cubic centimeter (g / cm 3 ), Wherein the (B) alkenyl functional auxiliary agent is described by any one of limitations (i) to (iv): (i)(B) is triallyl isocyanurate; triallyl cyanurate; triallyl trimellitate; N,N,N',N',N",N"-hexaallyl-1,3,5-triazine-2,4,6-triamine; triallyl orthoformate; pentaerythritol triallyl ether; triallyl citrate; or triallyl aconitate; (ii) (B) is trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, or propoxylated glycerol triacrylate; (iii) (B) is an alkenyl functional organosiloxane of formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), wherein the subscript n is an integer greater than or equal to 3; each R 1 Independently for C 2 -C 4 Alkenyl or H 2 C=C(R 1a )-C(=O)-O-(CH 2 ) m -, where R 1a is H or methyl and the subscript m is an integer from 1 to 4; and each R 2 Independently H, C 1 -C 4 Alkyl, phenyl or R 1 ;and (iv) A combination of (i) to (iii) or any two of them.
2. The additive masterbatch according to claim 1, Features Limitation to any one of (i) to (iv): (i) the additive masterbatch further comprises at least one additive independently selected from the optional following additives: (D) flame retardant, (E) antioxidant, (G) colorant, (H) metal deactivator, (I) hydrolyzable silane without unsaturated carbon-carbon bonds, (J) corrosion inhibitor, (K) hindered amine light stabilizer, and (L) ethylene-based copolymer, which is different from components (A) and (C) and is ethylene / C 4 -C 20 α-olefin copolymers, ethylene / unsaturated carboxylic acid ester copolymers or propylene / ethylene based copolymers, wherein (C) is an electron beam curable polyolefin compound; (ii) the additive masterbatch does not contain any porous resin; (iii) the additive masterbatch can be maintained at a temperature of 23°C for at least 20 days without the olefin functional additive leaching, as measured by the quantitative leaching test method; and (iv) (iii) and any one of (i) to (ii).
3. The additive masterbatch according to claim 1, Features Limiting any one of (i) to (iv): (i) the additive masterbatch further comprises at least one additive (F) processing aid; (ii) the additive masterbatch does not contain any porous resin; (iii) the additive masterbatch can be maintained at a temperature of 23°C for at least 20 days without the olefinic functional additive leaching, as measured by the quantitative leaching test method; and (iv) (iii) and any one of (i) to (ii) both. The additive masterbatch according to claim 2 , wherein the porous resin is a porous resin containing an olefinic functional additive. The additive masterbatch according to claim 3 , wherein the porous resin is a porous resin containing an olefinic functional additive.
6. The additive masterbatch according to claim 1, wherein the additive masterbatch consists of components (A) and (B).
7. The additive masterbatch according to any one of claims 1 to 6, wherein the (A) semi-crystalline polyolefin carrier resin comprises any one of (i) to (v): (i) semi-crystalline medium density polyethylene; (ii) semi-crystalline high density polyethylene; (iii) a combination of (i) and (ii); (iv) the (A) semi-crystalline polyolefin carrier resin has a crystallinity of 57.5 wt% to <100 wt%, as measured by the crystallinity test method using DSC; or (v) any one of limitation (iv) and limitations (i) to (iii).
8. The additive masterbatch according to any one of claims 1 to 6, wherein the (A) semi-crystalline polyolefin carrier resin satisfies any one of (i) to (vii): (i) a density greater than 0.936 g / cm 3 and is polyethylene; (ii) a crystallinity of 60.0 wt% to <100 wt%, measured by a crystallinity test method using DSC, and is polyethylene; (iii) a melt index I 2 0.1 to 20 grams per 10 minutes (g / 10min), measured according to the melt index test method at 190°C / 2.16kg load, and is polyethylene; (iv) the molecular weight distribution MWD is unimodal; (v) the MWD is multimodal; (vi) wherein the combined weight of components (A) and (B) is 50wt% to 100wt% of the additive masterbatch; (vii) any two of the limits (i) to (vi) are limited.
9. A method of storing an additive masterbatch, the method comprising maintaining the additive masterbatch according to any one of claims 1 to 8 at a temperature of 20°C to 25°C for at least 20 days to obtain a stored additive masterbatch without leaching of the olefinic functional additive as measured by the quantitative leaching test method.
10. An electron beam curable formulation comprising the auxiliary agent masterbatch according to any one of claims 1 to 8, or the stored auxiliary agent masterbatch prepared by the method according to claim 9, and (C) an electron beam curable EBC polyolefin compound.
11. The electron beam curable formulation according to claim 10, Features Limit any one of (i) to (x): (i) the (C) EBC polyolefin compound has a density of 0.910 to 0.925 g / cm 3 (ii) the (C) EBC polyolefin compound has a density of 0.910 to 0.925 g / cm 3 (iii) the (C) EBC polyolefin compound has a density of 0.926 to 0.940 g / cm 3 (iv) the (C) EBC polyolefin compound has a density of 0.941 to 0.990 g / cm 3 (v) the (C) EBC polyolefin compound is a polyethylene elastomer selected from ethylene-propylene rubber (EPR), ethylene-1-butene rubber (EBR) and ethylene-1-octene rubber (EOR); (vi) the (C) EBC polyolefin compound is a combination of any two or more of (i) to (v); (vii) the electron beam curable formulation further comprises at least one additive which is not a component of the auxiliary masterbatch and is independently selected from the optional following additives: (D) a flame retardant, (E) an antioxidant, (G) a colorant, (H) a metal deactivator, (I) a hydrolyzable silane free of unsaturated carbon-carbon bonds, (J) a corrosion inhibitor, (K) a hindered amine light stabilizer, and (L) an ethylene-based copolymer additive which is different from components (A) and (C) and is an ethylene / C 4 -C 20 α-olefin copolymers, ethylene / unsaturated carboxylic acid ester copolymers or propylene / ethylene-based copolymers; (viii) limitation (vii) and any one of limitations (i) to (v); (ix) (B) is 0.1 wt% to 20 wt% of the combined weight of components (A), (B) and (C); and (x) limitation (ix) and any one of limitations (i) to (viii).
12. The electron beam curable formulation according to claim 10, Features The following restrictions: The (C) EBC polyolefin compound is ethylene / C 3 -C 20 Alpha-olefin copolymers.
13. The electron beam curable formulation of claim 10, Features The following restrictions apply: the (C) EBC polyolefin compound is an ethylene-propylene copolymer.
14. The electron beam curable formulation of claim 10, Features The following restrictions apply: the (C) EBC polyolefin compound is an ethylene-propylene-diene monomer (EPDM) copolymer.
15. The electron beam curable formulation of claim 10, Features Limit any one of (i) to (xi): (i) the (C) EBC polyolefin compound has a density of 0.910 to 0.925 g / cm 3 (ii) the (C) EBC polyolefin compound has a density of 0.910 to 0.925 g / cm 3 (iii) the (C) EBC polyolefin compound has a density of 0.926 to 0.940 g / cm 3 (iv) the (C) EBC polyolefin compound has a density of 0.941 to 0.990 g / cm 3 (v) the (C) EBC polyolefin compound is ethylene / C 3 -C 20 α-olefin copolymer; (vi) the (C) EBC polyolefin compound is an ethylene-propylene-diene monomer (EPDM) copolymer; (vii) the (C) EBC polyolefin compound is a combination of any two or more of (i) to (vi); (viii) the electron beam curable formulation further comprises at least one ingredient that is not the additive masterbatch and is an additive (F) processing aid; (ix) limitation (viii) and any one of limitations (i) to (vi); (x) (B) is 0.1 wt% to 20 wt% of the combined weight of ingredients (A), (B) and (C); and (xi) limitation (x) and any one of limitations (i) to (ix).
16. The electron beam curable formulation of claim 15, wherein the ethylene / C 3 -C 20 The α-olefin copolymer is selected from the group consisting of ethylene-propylene rubber (EPR), ethylene-1-butene rubber (EBR) and ethylene-1-octene rubber (EOR).
17. The electron beam curable formulation of claim 15, wherein the ethylene / C 3 -C 20 The α-olefin copolymer is an ethylene-propylene copolymer.
18. A method for preparing an electron beam curable formulation, the method comprising mixing together an auxiliary masterbatch according to any one of claims 1 to 8 in dispersed solid form or the stored auxiliary masterbatch prepared by the method according to claim 9 and (C) an EBC polyolefin compound in dispersed solid or melt form to obtain a mixture; and melt mixing or extruding the mixture to prepare the electron beam curable EBC formulation.
19. A method of electron beam curing a formulation in need thereof, the method comprising irradiating the EBC formulation according to any one of claims 11 to 17 or the electron beam curable formulation prepared by the method according to claim 18 with an effective dose of electron beam radiation to obtain an electron beam cured polyolefin product.
20. An electron beam cured polyolefin product prepared by the method of claim 19.
21. An article comprising the electron beam cured polyolefin product of claim 20 and a component in operative contact therewith.
22. A coated conductor comprising a conductive core and a polymeric layer at least partially surrounding the conductive core, wherein at least a portion of the polymeric layer comprises the electron beam cured polyolefin product of claim 20.
23. A method of conducting electricity, the method comprising applying a voltage across the conductive core of the coated conductor of claim 22 so as to produce an electric current through the conductive core.