Photovoltaic module and method of manufacturing the same

By distributing pigment particles in the front packaging layer of the photovoltaic module to form high and low density areas, the problem of unsightly appearance and manufacturing complexity when the photovoltaic module is installed during the exterior wall of the building is solved, color uniformity is achieved and manufacturing process is simplified.

CN112020776BActive Publication Date: 2024-12-06CSEM CENTRE SUISSE D ELECTRONIQUE ET DE MICROTECHNIQUE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980025311.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-16
Filing Date
2019-04-12
Publication Date
2024-12-06
Estimated Expiration
2039-04-12

AI Technical Summary

Technical Problem

Existing photovoltaic modules are not beautiful when installed in building exterior walls, and the existing technology is complex or requires additional layers, which increases the risk of module layering and manufacturing difficulty, and the unevenness of pigment particles and the flow of encapsulant lead to color. change.

Method used

Using pigment particles distributed in the front encapsulation layer of the photovoltaic module to form high-density and low-density areas, made by thermoplastic or partially crosslinked polymers, assembled using standard lamination devices, and a patterned film is provided on the light incident side to provide uniformity Background color.

Benefits of technology

The aesthetics and color uniformity of the photovoltaic module are achieved, the migration and aggregation of pigment particles is avoided, the manufacturing process is simplified, and the manufacturing process is suitable for standard lamination devices, and a good contrast effect with the pattern film is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112020776B_ABST
    Figure CN112020776B_ABST
Patent Text Reader

Abstract

A photovoltaic module (1) comprises: a front panel (11) arranged on the light incident side of the photovoltaic module (1); a back panel (19) arranged on the side of the photovoltaic module (1) opposite to the front panel (11); a photovoltaic conversion device (15) arranged between the front panel (11) and the back panel (19); and at least one front encapsulation layer (13) arranged between the photovoltaic conversion device (15) and the front panel (11), the front encapsulation layer comprising pigment particles (21) distributed therein; the photovoltaic module is characterized in that the front encapsulation layer (13) comprises a first region (13a) and a second region (13b), the first region being located closer to the front panel (11) than the second region (13b), and the first region comprising a higher density of pigment particles (21) than the second region (13b).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic modules, and more particularly to a colored photovoltaic module particularly suitable for building-integrated applications and a method for manufacturing the same. Background Art

[0002] Photovoltaic (PV) devices (also known as solar cells or solar panels) tend to be close to black in natural color, often with a purple or indigo hue, with the well-defined pattern of the individual cells clearly visible. When such PV devices are mounted on buildings, they can be unaesthetic, and for this reason, their direct use as building facades is generally unacceptable.

[0003] To overcome this problem, colored photovoltaic devices have been proposed that can be integrated with building structures, particularly as external cladding.

[0004] Document US 9,281,186 discloses a film placed on the front sheet of a photovoltaic device to change the appearance of the module. However, such a film requires a specific profile (which must conform to the geometry of the individual PVs that make up the module) and relies on a complex design, including facets in the front sheet and embedded elements in the inactive parts of the module.

[0005] US 2014 / 326292 discloses a PV device comprising a graphic film placed inside a module. The film is printed with color or texture and requires a selective reflective layer to limit the film's impact on module efficiency.

[0006] US 9,276,141, WO 2016 / 118885 and US 8,513,517 disclose decorative film stacks placed on or within PV devices.

[0007] EP2793271 describes a white photovoltaic module in which an interference filter is formed on an intermediate layer arranged on the light incident side of the photovoltaic module in order to reflect a certain amount of light in the entire visible spectrum. The production of such an interference filter requires specialized equipment and technology.

[0008] US 2012 / 247541 describes printing on top of an encapsulation layer.

[0009] However, all of these prior art solutions are either complex or require additional layers to be applied to the module. Crucially, for each additional layer added to the module, the risk of module delamination increases as there are more inter-layer interfaces that can separate. Furthermore, special manufacturing techniques or apparatus may be required.

[0010] WO2009 / 089236 proposes a solution to this problem. Figure 7In an embodiment of the invention, the front encapsulation layer itself contains pigment particles randomly dispersed therein. Therefore, no additional color film layer is required in addition to the front encapsulation layer, but it brings a whole different set of problems. Since the encapsulant used in this document is conventional, this may lead to significant non-uniformity of coloration. Moreover, in extreme cases, excessive encapsulant flow can lead to significant thickness variations within the module, especially in areas where PV cells are present and areas where PV cells are not present. This in turn can lead to undesirable color variations throughout the module.

[0011] It is therefore an object of the present invention to at least partially overcome the above-mentioned disadvantages of the prior art. Summary of the invention

[0012] More specifically, the present invention relates to a photovoltaic module, comprising:

[0013] - a front plate arranged on the light incident side of the photovoltaic module, made of, for example, glass, transparent ceramic, polymer or other suitable transparent material;

[0014] - a back sheet arranged on the opposite side of the photovoltaic module from the front sheet, the back sheet being made of, for example, glass, metal, polymer ceramic or other materials;

[0015] - a photovoltaic conversion device arranged between said front sheet and said back sheet, the PV device being of any convenient type;

[0016] - at least one front encapsulation layer arranged between the photovoltaic converter and the front sheet, the front encapsulation layer comprising pigment particles distributed therein and made of a thermoplastic or at least partially cross-linked polymer such as EVA or polyolefin, etc. If desired, a rear encapsulation layer may also be provided between the PV converter and the back sheet.

[0017] According to the present invention, the front encapsulation layer comprises a first region and a second region, wherein the first region is located closer to the front panel than the second region and comprises a higher density of pigment particles than the second region. This particle distribution not only provides coloration to the module making it suitable for use as, for example, a building exterior, but also avoids migration and aggregation of pigment particles in the first region during lamination, preventing undesirable changes in color distribution. In addition, no special manufacturing technology is required, because the PV module can be assembled with a standard lamination device and using a standard front panel form (without special features, such as texture or structure, etc.).

[0018] Advantageously, at least a portion of the pigment particles have a diameter in the range of 100 nm to 1 μm, preferably 300 nm to 700 nm, more preferably 400 nm to 600 nm. The diameter of the particles can be optimized for the desired optical properties of the front encapsulation layer. Similarly, the pigment particles can be provided in the front encapsulation layer at a mass concentration of 0.01 to 10 parts per 100 parts of the resin for forming the front encapsulation layer, which can again be adjusted to optimize the desired properties.

[0019] The pigment may include at least one of a zinc-based pigment (such as zinc oxide or zinc chromate), a titanium-based pigment (such as titanium oxide or titanium yellow), an iron-based pigment (such as iron oxide or Prussian blue), a chromium-based pigment (such as chromium oxide), a bismuth-based pigment (such as bismuth vanadate), a cobalt-based pigment (such as cobalt blue or cobalt stannate or cobalt / lithium / titanium oxide), an aluminum-based pigment (such as complex sulfur-containing sodium silicate), a tin-based pigment (such as tin sulfide) or a copper-based pigment.

[0020] Advantageously, the photovoltaic module may further comprise an internal front sheet and an internal front encapsulant layer located between the front encapsulant and the photovoltaic conversion device. Thus, the module of the present invention may be manufactured simply by laminating the front encapsulant layer and the front sheet onto a pre-existing prefabricated PV module. Thus, the module of the present invention may be custom manufactured based on existing, commercially available modules.

[0021] Advantageously, a graphic film printed with an image or pattern etc. may be arranged on the light incident side of the front plate. Therefore, the colored front encapsulation layer provides a uniform background color (which may be white, for example) to provide a good contrast with the graphic film.

[0022] The present invention also relates to a method for manufacturing a photovoltaic module, said method comprising the following steps:

[0023] - providing a laminating device, such as a heated vacuum bag laminator or other suitable device;

[0024] - arranging in the laminating device a layer stack, the layer stack comprising:

[0025] - a front sheet intended to be arranged on the light incident side of said photovoltaic module, the front sheet being made for example of glass, transparent ceramic, polymer or other suitable transparent material;

[0026] - a backsheet intended to be arranged on the opposite side of the photovoltaic module from the frontsheet, the backsheet being made for example of glass, transparent ceramic, polymer or other suitable transparent material;

[0027] - any convenient form of photovoltaic conversion device disposed between said front sheet and said back sheet;

[0028] - at least one front encapsulation layer (made of a suitable thermoplastic polymer or at least partially cross-linked polymer) arranged between the photovoltaic conversion device and the front sheet, the front encapsulation layer comprising pigment particles distributed therein. It is worth noting that, if necessary, a rear encapsulation layer can also be provided between the PV conversion device and the back sheet;

[0029] - applying heat and pressure to the layer stack in order to assemble the layer stack into the photovoltaic module by fusing and / or cross-linking one or more encapsulation layers.

[0030] According to the present invention, the front encapsulation layer includes a first film and a second film, wherein the first film is located closer to the front plate than the second film and contains a higher concentration of pigment particles than the second film. In other words, the second film substantially does not contain pigment particles, or at least contains fewer particles than the first film.

[0031] The particles provide the module with a color, making it suitable for use as, for example, a building facade, and further scatter a certain amount of incident light, which helps to hide the structure of the photovoltaic conversion device. The dual film structure that produces the above-mentioned two regions limits or even completely eliminates the migration and aggregation of the pigment particles in the first film during lamination, so that the finished module obtains the desired color distribution (usually uniform), but can be patterned. If the second film also contains pigment particles, any migration of the lower concentration of pigment therein will be masked by the more densely colored first film. In addition, no special manufacturing technology is required, because the PV module can be assembled with standard lamination processes and using a standard front sheet (without special features such as texture or structure, etc.).

[0032] In another approach, a method of manufacturing a photovoltaic module comprises the steps of:

[0033] - providing a laminating device, such as a heated vacuum bag laminator or other suitable device;

[0034] - arranging in the laminating device a layer stack, the layer stack comprising:

[0035] - Prefabricated photovoltaic modules;

[0036] - at least one front encapsulation layer arranged on a side of the prefabricated photovoltaic module for receiving incident light, the front encapsulation layer comprising pigment particles distributed therein;

[0037] - a front plate arranged on the light incident side of the at least one front encapsulation layer;

[0038] - applying heat and pressure to the layer stack in order to assemble the layer stack into the photovoltaic module by fusing and / or cross-linking the encapsulation material.

[0039] Likewise, the front encapsulation layer includes a first film and a second film, the first film being located closer to the front plate than the second film and containing a higher concentration of pigment particles than the second film.

[0040] Thus, the advantages of the present invention can be applied to pre-existing prefabricated PV modules. Thus, the modules of the present invention can be custom manufactured based on existing, commercially available modules. This is particularly effective because colored modules can be easily custom manufactured based on standard, commercially available modules.

[0041] Advantageously, during the application of heat and pressure, ie during lamination, the first film always has a higher viscosity than the second film. As a result, the migration and aggregation of the pigment particles distributed therein can be more strongly prevented.

[0042] Advantageously, during said application of heat and pressure, the first film has a tan delta value of less than 0.8 and the second film has a tan delta value of at least 0.9, preferably at least 1.2. Furthermore, at least at the lamination temperature, the viscosity of the second film is at most 80%, preferably at most 50%, of the viscosity of the first film. This is also the case close to the lamination temperature. This ensures that the first film behaves like a solid during the lamination process, preventing migration of pigment particles and maintaining a substantially constant thickness of the layer containing the pigment, while the second film behaves like a liquid.

[0043] Advantageously, the first film is non-crosslinkable and has a complex viscosity of greater than 400,000 Pa.s at 85°C, greater than 50,000 Pa.s at 105°C, and greater than 1,000 Pa.s at 165°C; and wherein the complex viscosity of the second film is less than 100,000 Pa.s at 85°C, less than 20,000 Pa.s at 105°C, and less than 10,000 Pa.s at 165°C. If the maximum lamination temperature is less than 165°C, the condition at 165°C is optional. Although these ranges overlap, this does not contradict the statement in the previous paragraph regarding the viscosity relationship, which is an important criterion to be met at the lamination temperature.

[0044] Advantageously, the first film is at least partially crosslinked and has a complex viscosity of greater than 20,000 Pa.s at 85°C, greater than 15,000 Pa.s at 105°C, and greater than 5,000 Pa.s at 165°C; and wherein the second film has a complex viscosity of less than 100,000 Pa.s at 85°C, less than 20,000 Pa.s at 105°C, and less than 10,000 Pa.s at 165°C. Again, if the lamination temperature is less than 165°C, the 165°C condition is optional. Again, these overlapping ranges do not contradict the statements in the previous paragraphs regarding the viscosity criteria that should be met at the lamination temperature.

[0045] Advantageously, the layer stack further comprises a graphic film arranged on the light incident side of the front plate. Thus, the graphic film can be incorporated directly into the module during lamination. Alternatively, it can also be applied later after lamination.

[0046] Advantageously, at least a portion, preferably at least 50%, or even at least 75%, of the pigment particles have a diameter in the range of 100 nm to 1 μm, preferably 300 to 700 nm, more preferably 400 to 600 nm. The diameter of the particles can be optimized for the desired optical properties of the front encapsulation layer. Likewise, the pigment particles can be provided in the front encapsulation layer at a mass concentration of 0.01 to 10 parts per 100 parts of resin, which can still be adjusted to optimize the desired properties.

[0047] Advantageously, the pigment comprises at least one of the following: a zinc-based pigment (such as zinc oxide or zinc chromate), a titanium-based pigment (such as titanium oxide or titanium yellow), an iron-based pigment (such as iron oxide or Prussian blue), a chromium-based pigment (such as chromium oxide), a bismuth-based pigment (such as bismuth vanadate), a cobalt-based pigment (such as cobalt blue or cobalt stannate or cobalt / lithium / titanium oxide), an aluminum-based pigment (such as complex sulfur-containing sodium silicate), a tin-based pigment (such as tin sulfide) or a copper-based pigment.

[0048] Advantageously, the front encapsulation layer is manufactured by mixing the pigment particles with a base resin and extruding the front encapsulation layer into a film. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Further details of the present invention will become more apparent upon reading the following description in conjunction with the following drawings, which illustrate:

[0050] - Figure 1 : A schematic cross-sectional view of a photovoltaic module according to the present invention;

[0051] - Figure 2 : A schematic cross-sectional view of another photovoltaic module according to the present invention;

[0052] - Figure 3 : A schematic cross-sectional view of a portion of a photovoltaic module provided with a graphic film according to the present invention;

[0053] - Figure 4 : A schematic diagram of manufacturing a photovoltaic module according to the present invention using a lamination device;

[0054] - Figures 5 to 8 : A graph showing experimental results obtained using a photovoltaic module similar to the present invention;

[0055] - Fig. 9 : A schematic diagram of a building structure provided with a photovoltaic module according to the present invention;

[0056] - Fig.10: A plot of complex viscosity versus temperature for an example front encapsulation layer film pair; and

[0057] - Fig.11 : Graph of Tan δ values ​​of the same films. DETAILED DESCRIPTION

[0058] It should be noted in the following that, unless it is explicitly stated that a particular layer is directly disposed on an adjacent layer, one or more intermediate layers may also exist between the layers. Therefore, "on..." should be interpreted as "directly or indirectly on..." by default. In addition, since the patterns, connectors, etc. of certain layers are well known to the skilled person, they are no longer indicated.

[0059] Figure 1 A first embodiment of a photovoltaic (PV) module 1 according to the invention is shown.

[0060] The module 1 comprises a front plate 11 at the light incident side of the module 1 for being illuminated when in use (indicated by the sun symbol in the figure), and a back plate 19 at the opposite side of the module 1 from the front plate 11. The front plate may be glass, transparent ceramic, polymer or any other convenient substantially transparent material, while the back plate may be metal, glass, ceramic, polymer or any other convenient material. The front plate 11 may be structured and may be provided with a coating.

[0061] Located between the front sheet and the back sheet is a photovoltaic conversion device 15, which includes one or more PV cells (including NIP, PIN, NP or PN junctions) patterned and interconnected as is generally known. The PV cells may be based on thin film silicon, crystalline silicon, germanium, perovskite, dye-sensitized cells or any other type of photovoltaic technology suitable for generating electrical energy from light incident on the light-incident side of the PV module 1.

[0062] The PV conversion device 15 is encapsulated on its front side by a front encapsulation layer 13 (sealing it to the front sheet 11) and on its rear side by a rear encapsulation layer 17. The latter seals the PV conversion device 15 to the back sheet 19, although it can indeed form the back sheet itself. The encapsulant can be a standard substance, such as polyolefins, EVA (ethylene-vinyl acetate), ionomers, polyvinyl butyral or modified fluoropolymers, etc. The thickness of each of the encapsulation layers 13, 17 is typically from 200 μm to 1 mm, or even up to 2 mm. In addition, multiple front encapsulation layers 13 can be stacked on top of each other. In the case of a transparent (e.g. glass) or non-dark back sheet, the rear encapsulation layer 17 can be tinted or colored with a dark color (e.g. black, dark brown, dark blue or similar colors) to help disguise the interconnections and structures present in the module. It should be noted that in the sense of the present invention, the encapsulation layer seals one layer to another. Therefore, the front encapsulation layer 13 is an internal layer and is therefore not an external layer of the module structure (e.g. front sheet or graphic film).

[0063] It should be noted that other intermediate layers may be provided between the layers shown, and that the layers need not be planar but may describe curved or more complex surfaces.

[0064] According to the present invention, the front encapsulant 13 contains pigment particles 21 incorporated therein. Specifically, the front encapsulant layer 13 includes a first region 13a and a second region 13b. The first region 13a is located closer to the front plate 11 (and thus toward the light incident side of the module 1) than the second region 13b, and the second region 13b is located closer to the PV conversion device 15 than the first region 13a. The first region 13a and the second region 13b are usually directly adjacent to each other and are therefore in contact with each other, but it is not excluded that there is an intermediate region of encapsulant between them.

[0065] The first region 13a contains a higher concentration of pigment particles 21 than the second region 13b, and the second region 13b may contain substantially no pigment particles 21, or only a lower concentration than the first region 13a. If the second region 13b contains pigment particles 21, it is provided at a concentration of at most 50%, preferably at most 30%, and further preferably at most 20% of the concentration in the first region 13a. In the case where pigment particles are present in each region 13a, 13b, these particles may be the same or different.

[0066] Other regions (not shown) of the front encapsulation layer 13 may be provided on either or both sides of its front sheet 11 side, or its PV device 15 side. These other regions are typically free of pigment particles 21, but it is not excluded that they contain low concentrations of pigment.

[0067] The pigment particles 21 are highly schematically represented, and at least a portion, preferably at least 50%, and further preferably at least 75% (or even substantially all) of the particles typically have a size range of 100nm to 1μm, most notably 300nm to 700nm, and particularly 400 to 600nm. It is worth noting that the pigment particles are discrete particles, which are different from colorants dispersed at the molecular level in an encapsulant or an encapsulant made of a colored material. The pigment particles 21 are distributed throughout the thickness of the first region 13a (so not just on its surface or near its surface); if any pigment particles are present in the second region 13b, they are also distributed throughout the thickness of that region. Below in Figure 4 The formation of the two regions 13a, 13b formed by the front encapsulation layer 13 is described in the context of FIG. The distribution of the pigment particles 21 can be random or can form a specific pattern formed when the film of the first region 13 is extruded. The pigment distribution is maintained by the method of the present invention (see below).

[0068] A wide variety of pigments can be used provided that they are chemically stable and stable under prolonged ultraviolet light exposure, either alone or in combination with suitable UV stabilizers, such as hindered amine light stabilizers (HALS), hydroxyphenylbenzotriazole, oxalyl anilide, benzophenone, benzotriazole, hydroxyphenyltriazine, etc. As examples of suitable pigments, titanium oxide or zinc oxide particles can be used to generate white. Yellow, orange, red and brown can be generated by using various iron oxides, such as Fe2O3 for red ochre, or FeO(OH) or yellow ochre for yellow. Yellow can also be generated by bismuth vanadate, or yellow titanium, or zinc chromate or tin sulfide. Green can be generated by chromium oxide or Co / Li / Ti oxide. Blue can be generated by, for example, composite sulfur-containing sodium silicate or Prussian blue, or cobalt stannate. Of course, the present invention is not limited to such pigments, and there are many other pigments on the market.

[0069] The pigment particles 21 may be provided in a concentration of 0.01 to 10 parts per hundred parts of resin (phr) used as the basis for the front encapsulation layer 13. More specifically, 0.1 to 5 phr, even more specifically 0.1 to 1 phr of pigment particles 21 may be used, depending on the thickness of the front encapsulation layer 13, with thinner encapsulation layers generally benefiting from higher concentrations of pigment particles 21.

[0070] The pigment particles 21 absorb a portion of the visible light incident on the PV device 1 to produce the desired color, and also scatter the light to provide a uniform color and help hide various features of the PV conversion device 15, such as its pattern, electrical interconnections between individual cells, edges of individual cells, color mismatches between individual cells and the rear encapsulation layer 17 and / or backsheet 19, and the like.

[0071] This scattering effect is particularly advantageous over simply providing a front encapsulant that is colored by a colorant dispersed therein at a molecular level, because such a colorant results in a greater degree of optical transparency due to the lack of light scattering, thereby failing to hide the various features of the PV conversion device 15 as described above.

[0072] Additionally, the scattering effect helps diffuse light that passes through the front encapsulant layer 13 and into the photovoltaically active portion of the PV conversion device 15, increasing the average path length of the light through the cell, in a manner similar to conventional diffusing elements incorporated into the PV module 1 on the light incident side of the PV conversion device 15. Of course, the overall efficiency decreases in proportion to the light that is reflected or scattered back onto the light incident side of the PV device.

[0073] The size of the pigment particles 21 can be adjusted to increase the transmittance of the infrared-sensitive PV conversion device 15 in the infrared range, and the pigment particles 21 can interfere with each other to produce a sparkling, glittering or rainbow effect by optimizing the pigment particle size and its density in the front encapsulation layer 13. More generally, the pigment particle size and concentration, the thickness of the front encapsulation layer 13, the thickness of the first region 13a, etc. can be adjusted within the above ranges by routine experimentation to achieve the desired color, optical effect, transmittance, reflectivity, etc., and for any given pigment, there is no specific a priori relationship between particle size and particle concentration - this relationship depends solely on the desired optical properties.

[0074] With regard to the manufacture of the front encapsulation layer 13, the required amount of pigment particles 21 can simply be mixed with the base resin or resin precursor that will form the first region 13a of the encapsulation layer 13, and optionally with the base resin or resin precursor of the second region 13b (if it is also pigmented). If necessary, a suitable UV stabilizer (as described above) can be added to the resin at the same time. This can then be extruded as normal without the need for any special equipment or techniques.

[0075] Due to this structure, a colored fritted front glass (or the like) is no longer required as the front sheet 11, so the invention can be carried out without special equipment and the PV module 1 can be assembled in a conventional lamination device (see below).

[0076] Figure 2 Another embodiment of a PV module according to the invention is shown. In this variant, the front encapsulation layer 13 and the front sheet 11 have been laminated to the front of a pre-existing prefabricated PV module 27. As a result, the final PV module 1 according to the invention also comprises an internal front sheet 25 and an internal front encapsulation layer 23, since these layers are already present in the pre-existing prefabricated PV module 27. The remaining layers 15, 17 and 19 are constituted by the prefabricated PV module, as described above, and need not be described again.

[0077] This arrangement allows the advantages of the present invention to be applied to any commercially available PV module by retrofitting the front encapsulant layer 13 and front sheet 11 to existing modules. This is also particularly advantageous because a variety of different modules 1 can be more easily produced according to the needs of the end user. In essence, the manufacturer can maintain a stock of pre-made standard PV modules 27 and then laminate the front encapsulant layer 13 and front sheet 11 thereon as required, or select the front encapsulant layer 13 of the appropriate color from stock, or manufacture it to order.

[0078] Figure 3Another variant of a PV module 1 according to the invention is partially shown, comprising a graphic film 29 applied to the light incident side of the front sheet 11. For example, the graphic film 29 may be a polymer film, such as a commercially available PET film, onto which an image, pattern or the like has been printed by any convenient technique. The graphic film 29 may be applied during lamination (see below), or after the manufacture of an otherwise finished PV module 1.

[0079] Graphic film 29 can be applied to Figure 1 or Figure 2 In the embodiment of FIG. 1 , the rest of the PV module 1 is therefore not in Figure 3 Indicated in.

[0080] Alternatively, in an unillustrated embodiment, a graphic film 29 may be laminated between the front encapsulation layer 13 and the front plate 11 .

[0081] As a further possibility that can be suitably applied in any of the above-mentioned embodiments, a polymer layer containing the above-mentioned pigment particles can be used as the front plate 11, for example directly in contact with the front encapsulation layer 13, or provided as an additional layer on top of the glass or polymer front plate. In these cases, the front encapsulation layer 13 can contain particles according to the present invention, or can be conventional. Particularly advantageous resins for such particle-containing layers are fluoroolefins, such as Lumiflon (from Asahi Glass Co. Ltd), however, other polymers are also possible.

[0082] Figure 4 The method for manufacturing a PV module 1 according to the invention is schematically represented.

[0083] The layer stack 31 comprising at least the layers 11, 13, 15, 17 and 19 and any other layers present is assembled in the laminating device 33. Figure 2 In the case of an embodiment of the present invention, the layer stack comprises a prefabricated PV module 27, to which the front encapsulation layer 13 and the front sheet 11 (and any other desired layers) have been applied. It should be noted that the layer stack 31 can be assembled in the lamination device 33 with the light incident side of the final PV module facing downwards or upwards.

[0084] Since the front encapsulation layer 13 has two regions 13a, 13b, it is formed by two separate films, a first film 13a which will be the first region (hence having the same reference numerals), and a second film 13b which will be the second region (hence also having the same reference numerals). Thus, the first film 13a contains the particles 21 as described above. These films are arranged in the correct order in the laminating device 33, as well as any additional films arranged on one side or the other thereof.

[0085] The laminating device may be a vacuum bag laminator, a drum laminator or any other convenient type. The laminating device 33 then applies heat and pressure, for example at a temperature of 140° C. to 180° C. and a pressure of up to 1 bar (typically 0.4 bar to 1 bar) for a suitable time, so that the various encapsulation layers fuse, thereby assembling the final PV module 1.

[0086] Thus, the PV module 1 according to the invention can be manufactured in conventional PV processing plants without the need for dedicated equipment.

[0087] The properties of the first and second films 13a, 13b may be optimized to better prevent pigment migration during lamination. As described above, in the prior art, when the pigmented encapsulant flows under heat and pressure, the pigment particles may migrate and aggregate. This often results in very uneven coloring, where the pigment migrates and the final thickness of the encapsulation layer varies, for example around a single cell making up the PV conversion device 15.

[0088] The solution to this particular problem consists in choosing the material for the first and second membranes 13a, 13b, each of which may for example have a thickness of 0.05 to 2 mm, preferably 0.1 to 1 mm.

[0089] Essentially, the material of the first film 13a is chosen to limit the migration of the pigment particles 21, while the material of the second film 13b is chosen for its encapsulation properties and its ability to flow, features such as the details of the underlying PV cells 15, if the intermediate layer is not present. To this end, the viscosity of the first film 13a during lamination is chosen to be higher than the viscosity of the second film 13b. This higher viscosity limits lateral flow (within the plane of the film 13a), preventing the migration of the pigment and thus avoiding uneven distribution of the pigment, while the lower viscosity of the second film 13b allows for proper flow and therefore proper sealing with the next layer. In addition, the second film 13b acts as a "buffer" layer, reducing the tendency of the thickness of the first film 13a to vary due to underlying features such as individual cells.

[0090] In addition, if the material of the first film 13a has viscoelastic properties, this further limits the change in thickness of the final first region, thereby avoiding the resulting change in light absorption.

[0091] There are several possibilities regarding the choice of the encapsulant material, depending on whether the first film 13a is made of a cross-linked polymer or not.

[0092] In the first case, the base resin of the first film 13a is not cross-linkable, such as polyethylene (PE), polypropylene, poly(ether ether ketone), polyethylene terephthalate, polyamide, nylon, poly(methylene oxide), POM, poly(4-methylpentene), poly(styrene), poly(vinyl alcohol), poly(vinyl chloride), poly(vinyl fluoride), poly(vinylidene chloride), polyurethane, polyimide, polycarbonate, acrylonitrile-butadiene-styrene, polyphenylene sulfide or styrene-acrylonitrile, in which case the desired viscosity is obtained by selecting and / or adjusting the composition of the encapsulant. It is a simple task for the skilled person based on the desired film properties during lamination (see below), in simple terms, the second film 13b generally has a lower melting temperature than the first film 13a, and the lamination temperature is selected so that the viscosity of the second film 13b remains much lower than the viscosity of the first film 13a. Ideally, the complex viscosity of the second film 13b during lamination remains at least 20% lower than the complex viscosity of the first film 13a, preferably at least 50% lower, and further preferably at least 10 times lower. Based on the required characteristics, the corresponding products can be selected from stock, or modified appropriately.

[0093] More specifically, the desired properties are preferably:

[0094] Complex viscosity: >400,000Pa.s at 85°C, >50,000Pa.s at 105°C, >1,000Pa.s at 165°C. Complex viscosity is irrelevant above the actual lamination temperature.

[0095] Tanδ<0.8 during the entire lamination process.

[0096] Addition of pigment particles within the above range may increase viscosity by up to 10%.

[0097] For reference, complex viscosity is the frequency-dependent viscosity function determined during forced harmonic oscillation of shear stress and is defined as the complex modulus divided by the angular frequency, where the complex modulus represents the material's overall resistance to deformation, whether that deformation is recoverable (i.e., elastic) or non-recoverable (i.e., viscous). This is measured using a dynamic moving die rheometer or similar tool, in the present case at a frequency of 1 Hz and a strain of 10%. Tan δ, also known as the "loss tangent," is the phase angle tangent that characterizes the ratio of the viscous modulus (G") to the elastic modulus (G'), quantifying the presence and extent of elasticity in the fluid. Tan δ values ​​less than 1.0 indicate elastically dominated (i.e., solid-like) behavior, while values ​​greater than 1 indicate viscous dominated (i.e., liquid-like) behavior, also measured at a frequency of 1 Hz and a strain of 10%.

[0098] Paired with the non-crosslinkable first film 13a is a second film 13b having the following properties:

[0099] Complex viscosity, <100,000 Pa.s at 85°C, <20,000 Pa.s at 105°C, <15,000 Pa.s at 165°C (provided that it is still sufficiently lower than the viscosity of the first film 13a as described above, the complex viscosity is also irrelevant above the actual lamination temperature);

[0100] Tanδ>0.9, preferably>1.2 at lamination temperature.

[0101] It should be noted that if the base resin of the second film 13b does not exhibit sufficient creep resistance, it may be at least partially cross-linked before and / or during and / or after lamination.

[0102] In the case where the first film 13a is cross-linked, the degree of pre-curing of the film helps determine its viscosity. The ideal parameters are as follows:

[0103] Complex viscosity: >20,000Pa.s at 85°C, >15,000Pa.s at 105°C, >5,000Pa.s at 165°C. Complex viscosity is irrelevant above the actual lamination temperature.

[0104] Tanδ<0.8 during the entire lamination process.

[0105] Note that the desired properties may be at least partially achieved by pre-crosslinking the first film 13a via different curing mechanisms, such as radiation curing, moisture curing, peroxide initiated curing.

[0106] The corresponding parameters of the second film 13b are as follows:

[0107] Complex viscosity: <100,000Pa.s at 85°C, <20,000Pa.s at 105°C, <10,000Pa.s at 165°C;

[0108] Tan δ>0.9, preferably>1.2 at least at lamination temperature.

[0109] When the encapsulant of the first film 13a is pre-crosslinked, the same base resin may be used for both layers, and only the first film 13a may be pre-cured.

[0110] It should be noted that if the viscosity of the first film 13a under lamination conditions is too high to ensure good wetting of and sufficient adhesion to the adjacent layers (e.g. the front panel 11), a supplementary encapsulation film may be placed between the first film 13a and the adjacent layers, which film is a conventional encapsulant material and acts in a similar manner to the second film 13b.

[0111] In any case, the general principles are as follows:

[0112] - tan δ of the first film 13a is < 0.8 during the entire lamination process, making it behave more like a solid;

[0113] - the second film 13b has a tan δ > 0.9, preferably > 1.2, at least at the lamination temperature, giving it a more liquid-like behavior; and

[0114] The viscosity of the second film 13b at least at the lamination temperature is not more than 80% of the viscosity of the first film 13a, preferably not more than 50% of the viscosity of the first film 13a, and further preferably not more than 10% of said viscosity.

[0115] Fig.10 shows a graph of complex viscosity (logarithmic vertical axis) versus temperature (linear horizontal axis), Fig.11 The values ​​of tan δ for material examples of the first film 13a and the second film 13b are illustrated (linear scale). More specifically, these materials are an XLPO encapsulant developed within CSEM, and an XLPO grade ASCE supplied by Mitsui Chemicals of Japan, respectively. Throughout the graph, to the right until about 165°C, the complex viscosity h* of the second film 13b does not even reach 50% of the complex viscosity of the first film 13a, and is therefore well within the acceptable range (maximum 80%). In this example, when the tan δ of the second film 13b is below 0.9, a lamination temperature of about 165°C can therefore be achieved. Ideally, the complex viscosity of the second film 13b should not exceed 10% of the complex viscosity of the first film 13a, and the tan δ of the second film 13b should be maintained at more than 1.2, but the maximum lamination temperature is shown to be about 160°C.

[0116] When the first film 13a is not cross-linkable, the viscosity decreases substantially with increasing temperature, so the material of the second film 13b should be carefully selected to withstand a sufficient viscosity difference during the entire lamination process, and the maximum temperature should also be carefully selected. If necessary, for example, for use in hot climates, the second film 13b may also be cross-linked to have sufficient creep resistance.

[0117] When the first film 13a is cross-linkable and not fully cross-linked after a previously performed pre-cross-linking step, it has a lower viscosity in the early stages of lamination, which helps fill voids, etc., and then cross-linking increases its viscosity and gives it greater mechanical strength. At any given moment in the lamination process, its viscosity and tanδ depend on the temperature and the degree of mesh (cross-linking) of the film, which may further develop as the lamination proceeds. Therefore, as the temperature increases, the inherent decrease in viscosity and the increase in Tanδ are compensated by increasing the mesh structure, thereby providing a wider range of material choices for the second film 13b, because it is relatively easy to select a material with a sufficiently low viscosity during the lamination process. In fact, in this case, it is easier to select a cross-linkable resin with good creep resistance for the second film 13b than in the case of the non-cross-linkable first film 13a.

[0118] In both cases, the interface between the two films 13a, 13b after lamination is perfect with no voids. In addition, cross diffusion of the pigment particles 21 at the interface is minimal.

[0119] The following table gives specific examples of pairs of materials for the first film 13a and the second film 13b. The commercial references given represent unchanged compositions, thus ensuring reproducibility.

[0120]

[0121] Figure 5 Shown according to Figure 2 1 is a graphical representation of experimental results of a PV module 1 manufactured according to an embodiment (but without the second region 13b) to illustrate the effect of certain combinations of encapsulants and pigments. In this case, the front encapsulant layer 13 is made of Dow Engage PV POE XUS 38660.00 polyolefin-based resin, 1 phr DuPont Ti Ti-Pure R-960 titanium dioxide-based pigment, and no other additives. The median particle size of the pigment is 500 nm.

[0122] The pigment particles were added and mixed manually with the base resin and extruded at 170° C. using a twin-screw extruder to obtain a white cross-linkable polyolefin film having a thickness of 0.85 mm.

[0123] The resulting white front encapsulant sheet was combined with a 50 μm thick ETFE front sheet and laminated onto a prefabricated PV module at a temperature of 165° C. and a pressure of about 1 bar (± 0.99 bar) for 720 seconds.

[0124] The metal connections of the PV modules are blackened and the backsheet 19 is also painted black to reduce the contrast.

[0125] Figure 5The diagram illustrates the external quantum efficiency (EQE) and reflectivity (R) of a PV module 1 according to the invention in the wavelength range from 350 nm to slightly above 1150 nm, as described above (W1), compared to a reference cell having the same structure but constructed using a transparent front encapsulation layer 13 (R1). It can be seen that the EQE decreases and the reflectivity increases over a wider bandwidth of light wavelengths.

[0126] Additionally, battery performance and color expressed in "Lab" color space coordinates were measured, and the results are shown in the table below:

[0127]

[0128] As can be seen from the table, the module 1 thus constructed is white and has a current loss of about 58%.

[0129] Figure 6 Shown according to Figure 2 1 is a graph of experimental results obtained by manufacturing another PV module 1 (also without the bottom layer area 13b) according to an embodiment of the present invention, wherein the front encapsulation layer 13 is made of ExxonMobil Escorene Ultra UL 00728CC EVA copolymer-based resin in which 0.05 wt.% of Scholz Red 110M pigment particles are dispersed.

[0130] The red pigment particles were manually mixed with the base resin and then extruded at 95°C to form a 0.9 mm thick film of the front encapsulant. Subsequently, it was combined with a 100 μm thick ETFE front sheet and laminated at 150°C and a pressure of substantially 1 bar for 720 seconds. As in the previous example, the metal connector was blackened and a black back sheet 19 was used.

[0131] The resulting PV modules have a terracotta color, making them particularly suitable for installation on roofs in areas where clay tiles are common. Figure 6 The graph of also shows the EQE and reflectivity results obtained for this PV module (T2) compared to a similarly constructed reference module (R2) using a conventional transparent front encapsulant. In this case, the EQE of the clay module T2 is only significantly reduced below a wavelength of about 650nm, and the reflectivity curve is only slightly increased above a wavelength of about 600nm.

[0132] Additionally, performance and color results are shown in the following table:

[0133]

[0134] Current losses are limited to 28.5%, which compares favorably to the 57.7% losses measured for the previous white module.

[0135] About the basis Figure 1The wavelength of light obtained by the constructed PV module (also without the bottom layer area 13b), Figure 7 A graph showing EQE, Figure 8 A graph showing reflectivity.

[0136] In this series of experiments, various PV modules according to the present invention were Figure 1 The structure is constructed of various front encapsulants consisting of one or more of the following layers:

[0137] ID Pigment concentration Thickness [mm] D_1 0.05 wt% 0.55 D_2 0.15 wt% 0.55 D_3 0.25 wt% 0.55

[0138] As mentioned before, the base resin was Polidiemme FE1252 EP modified polyolefin from Padanaplast and the pigment particles were Ti-Pure R-960 from DuPont. The base resin and pigment were first mixed and pelletized on a twin-screw extruder at 170°C. Subsequently, the pellets were extruded on a single-screw extruder at 170°C to form films with the stated thickness. The coloring of these films was adjusted to obtain a light diffusion effect and white color, and the following modules were constructed:

[0139] ID Pre-encapsulant R3 Transparent (reference) WD_1 D_1 WD_2 D_2 WD_3 D_3 WD_4 D_2+D_4 (stacked) WD_5 D_3+D_3 (stacked)

[0140] Considering Figure 7 and Figure 8 , PV module WD_3 represents a good compromise between performance and aesthetics.

[0141] The same PV modules were also tested for performance and reflectivity from 380nm to 780nm, and the results are shown below:

[0142] Current Relative performance Reflectivity ID <![CDATA[J SC [mA / cm 2 ]]> <![CDATA[ΔJ SC [%]]]> <![CDATA[R 380-780nm [%]]]> R3 36.2 - 6.3 WD_1 31.7 -12.4 15.6 WD_2 27.9 -22.9 23.7 WD_3 23.3 -35.6 29.8 WD_4 18.7 -48.3 46.1 WD_5 15.8 -56.3 48.8

[0143] As a final example, three Figure 3 The application image layer 29 is based on Figure 1 The reference module also includes a transparent front encapsulant 13, and then two other modules with front encapsulant layers 13 of WD_3 and WD_4 as described above are also manufactured. The image pattern on the reference module is almost invisible, while it is clearly visible on the other two modules.

[0144] The performance results of the three modules are shown below:

[0145]

[0146] Again, front encapsulant WD_3 represents a good compromise between aesthetics and power / current loss compared to the colorless reference.

[0147] at last, Fig. 9A PV module 1 according to the invention is shown mounted on the roof of a building structure 35. Alternatively, the PV module 1 can be mounted on an exterior wall, or integrated into the structure of the wall and / or roof, for example as cladding. In general, the PV module 1 can be mounted on or in the structure of a building 35.

[0148] Although the invention has been described with reference to specific embodiments, various modifications are possible without departing from the scope of the invention as defined in the appended claims.

Claims

1. A method for producing a photovoltaic module (1), the method comprising the following steps: - providing a laminating device (33); - Arranging a layer stack (31) in the laminating device (33), the layer stack comprising: - a front panel (11) intended to be arranged on the light incident side of said photovoltaic module (1); - a back sheet (19) intended to be arranged on the side of the photovoltaic module (1) opposite to the front sheet (11); - a photovoltaic conversion device (15) arranged between the front plate (13) and the back plate (19); - at least one front encapsulation layer (13) arranged between the photovoltaic conversion device (15) and the front panel (11), the front encapsulation layer (13) comprising pigment particles (21) distributed therein; - applying heat and pressure to the layer stack (31) to assemble it into the photovoltaic module (1), The front encapsulation layer (13) comprises a first film (13a) and a second film (13b), wherein the first film (13a) is located closer to the front plate (11) than the second film (13b) and contains a higher concentration of pigment particles than the second film (13b). Wherein, the first film (13a) is at least partially cross-linked and has a complex viscosity of greater than 20,000 Pa.s at 85°C, greater than 15,000 Pa.s at 105°C, and greater than 5,000 Pa.s at 165°C; and wherein the second film (13b) has a complex viscosity of less than 100,000 Pa.s at 85°C, less than 20,000 Pa.s at 105°C, and less than 10,000 Pa.s at 165°C; if the lamination temperature is less than 165°C, the 165°C condition is optional.

2. A method for manufacturing a photovoltaic module (1), the method comprising the following steps: - providing a laminating device (29); - arranging a layer stack in the laminating device (29), the layer stack comprising; - prefabricated photovoltaic modules (27); - at least one front encapsulation layer (13) arranged on the light incident side of the prefabricated photovoltaic module (27), the front encapsulation layer (13) comprising pigment particles (21) distributed therein; - a front plate (11) arranged on the light incident side of the at least one front encapsulation layer (13); - applying heat and pressure to the layer stack (31) to assemble it into the photovoltaic module (1); The front encapsulation layer (13) comprises a first film (13a) and a second film (13b), wherein the first film (13a) is located closer to the front plate (11) than the second film (13b) and contains a higher concentration of pigment particles than the second film (13b). Wherein, the first film (13a) is at least partially cross-linked and has a complex viscosity of greater than 20,000 Pa.s at 85°C, greater than 15,000 Pa.s at 105°C, and greater than 5,000 Pa.s at 165°C; and wherein the second film (13b) has a complex viscosity of less than 100,000 Pa.s at 85°C, less than 20,000 Pa.s at 105°C, and less than 10,000 Pa.s at 165°C; if the lamination temperature is less than 165°C, the 165°C condition is optional.

3. The method according to claim 1 or 2, wherein: The first film (13a) has a higher viscosity than the second film (13b) during the application of heat and pressure.

4. The method of claim 3, wherein: During the application of heat and pressure, the tan δ value of the first film (13a) is less than 0.8, the tan δ value of the second film (13b) is at least 0.9, and wherein, at the lamination temperature, the viscosity of the second film (13b) is at most 80% of the viscosity of the first film (13a).

5. The method of claim 4, wherein: The second film (13b) has a tan δ value of at least 1.

2.

6. The method of claim 4, wherein: At the lamination temperature, the viscosity of the second film (13b) is at most 50% of the viscosity of the first film (13a).

7. The method according to claim 1 or 2, wherein: At least a portion of the pigment particles (21) have a diameter ranging from 100 nm to 1 μm.

8. The method of claim 7, wherein: At least a portion of the pigment particles (21) have a diameter ranging from 300 nm to 700 nm.

9. The method of claim 7, wherein: At least a portion of the pigment particles (21) have a diameter ranging from 400 nm to 600 nm.

10. The method according to claim 1 or 2, wherein: The pigment particles (21) are provided in the front encapsulation layer (13) at a mass concentration of 0.01 to 10 parts per 100 parts of resin.

11. The method according to claim 1 or 2, wherein: The pigment comprises at least one of the following: Zinc-based pigments; Titanium-based pigments; Iron-based pigments; Chrome-based pigments; Bismuth-based pigments; Cobalt-based pigments; Aluminum-based pigments; Tin-based pigments; Copper-based pigments.

12. The method according to claim 1 or 2, wherein: The front encapsulation layer (13) is manufactured by mixing the pigment particles (21) with a base resin and extruding the front encapsulation layer (13) into a film.