A photosensitive resin composition
By using a photosensitive resin composition containing a cyclic anhydride structure in the manufacture of printed circuit boards, the problem of poor film removal performance of traditional photosensitive resin during the peeling of the anti-etching layer after etching or electroplating is solved, and high resolution is achieved. Adhesion and good film removal effect improve productivity.
Patent Information
- Application Number
- CN202110390496.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-04-12
AI Technical Summary
In the manufacturing of printed circuit boards, traditional photosensitive resin compositions have problems such as prolonging the film removal time, excessive film removal fragments, or impurity of film removal during the peeling process of the corrosion-resistant layer after etching or electroplating, which is difficult to meet the high level of film removal. Resolution and high adhesion requirements, especially when the line size reaches below 10μm.
A photosensitive resin composition is adopted, which includes an alkali-soluble resin, a photopolymerized monomer and a photoinitiator, and an auxiliary monomer containing a cyclic anhydride structure is added to the alkali-soluble resin. By controlling the proportion and molecular weight distribution of each raw material, the Its resolution, adhesion and film removal properties.
The photosensitive resin composition has good film decompression performance after etching or electroplating, ensuring the cleanliness and yield of the lines, while maintaining high adhesion and resolution, avoiding the problem of decreasing drug resistance.
Smart Images

Figure CN113204171B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of printed circuit board manufacturing, and in particular relates to a photosensitive resin composition. Background Art
[0002] In the manufacturing process of printed circuit boards, photosensitive resin compositions are widely used as resist materials for etching or electroplating. The pattern is transferred by photocuring and the following method is used to make circuit patterns: first, the photosensitive resin composition is pressed onto a copper plate; then a specific area of the photosensitive resin composition layer is exposed; then the supporting film PET is peeled off, and the unexposed area is removed with a liquid medicine; finally, the substrate with the resist pattern is etched and the resist layer is peeled off to form a circuit pattern, or electroplating is performed, and then the resist layer is peeled off and the metal surface covered by the resist layer is etched to form a circuit pattern.
[0003] As electronic devices develop towards being thinner, lighter, and smaller, the circuits on printed circuit boards are required to be more refined and denser, especially in the technical fields of semiconductor packaging substrates, where the circuit size required by the design has even reached less than 10μm. Traditional PCB manufacturing generally uses a subtractive process, but side etching is prone to occur during the copper etching process, and its application in the production of fine circuits with a line width / line spacing of less than 30um is limited. The additive process (SAP) directly forms an anti-etching pattern on thin copper, then thickens the copper through electroplating, removes the anti-etching pattern, and then quickly etches away the excess copper layer to form a circuit. Because the etching time is short, the side etching of the circuit is relatively small, and fine circuits with vertical side walls can be produced.
[0004] The miniaturization of circuits has put forward higher requirements on the resolution and adhesion of the photosensitive resist layer. In order to achieve higher resolution and adhesion, the commonly used method is to add benzyl (meth)acrylate, styrene or styrene derivatives with a benzene ring structure as a copolymer component to the alkali-soluble resin, one of the raw materials of the photosensitive resin composition, or to add multifunctional monomers to the photopolymerizable monomer to increase the crosslinking density. The disadvantages of these two methods are the problem of peeling off the resist layer after etching or electroplating, that is, the problem of extended film stripping time, excessive film stripping fragments, even film sandwiching and incomplete film stripping. Film stripping is a key process in the production of printed circuit boards. The cleanliness of the board surface film stripping, the film stripping time and the size of the film stripping fragments directly affect the production and product yield of the subsequent processes. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a photosensitive resin composition, which, when used as a dry film resist, has high resolution and adhesion as well as excellent film stripping performance and drug resistance.
[0006] In order to achieve the above object, the specific technical solution adopted by the present invention is as follows:
[0007] A photosensitive resin composition is made of at least the following raw materials in parts by mass: 45-65 parts of alkali-soluble resin, 30-50 parts of photopolymerizable monomers, and 0.5-5 parts of photoinitiators; the alkali-soluble resin is copolymerized by (meth)acrylic acid monomers, (meth)acrylate monomers, styrene derivative monomers, and auxiliary monomers; the auxiliary monomers are monomers containing cyclic anhydride structures. The (meth)acrylic acid monomers are one or more of acrylic acid monomers and methacrylic acid monomers, and the (meth)acrylate monomers are one or more of acrylic acid monomers and methacrylate monomers.
[0008] Conventional methods increase the rigidity by increasing the proportion of benzene ring-containing monomers in alkali-soluble resins, thereby improving resolution and adhesion, but this will result in extended stripping time, large film stripping fragments, and significantly poor film stripping performance. The prior art improves stripping performance by reducing the molecular weight of alkali-soluble resins or increasing the acid value of alkali-soluble resins, but this will cause a decrease in drug resistance and easily lead to lateral corrosion or plating of circuits; while the present invention adds monomers containing cyclic acid anhydride structures to alkali-soluble resins, which have the same resolution and adhesion as monomers containing benzene rings such as styrene and benzyl ester, and have good stripping performance, and will not cause a decrease in drug resistance like carboxylic acid groups. In addition, in the raw material formula of the above-mentioned photosensitive resin composition, the alkali-soluble resin is strictly controlled at 45-65 parts. When the weight is less than 45 parts, the photosensitive resin composition is prone to glue overflow and is not easy to preserve; when the weight is higher than 65 parts, there will be a risk of low sensitivity and poor resolution; the photopolymerizable monomer is strictly controlled at 30-50 parts. If the weight is lower than 30 parts, the photosensitive resin composition is prone to low photosensitivity and low resolution; if the weight is higher than 50 parts, the photosensitive layer will have glue overflow and a short shelf life.
[0009] Preferably, the side chain of the cyclic anhydride structure has an unsaturated bond. The unsaturated bond can ensure that the cyclic anhydride will not be destroyed by ring opening during copolymerization of the auxiliary monomer, and further ensure that it can play its role in the photosensitive resin composition in the future.
[0010] The auxiliary monomer is selected from one or more of the compounds represented by formula I-1 and I-2:
[0011]
[0012] Wherein, R1 is independently represented by a hydrogen atom or a straight-chain alkyl group having 1 to 15 carbon atoms, and R2 is represented by a hydrogen atom or a methyl group. The auxiliary monomers include (2-propylene) succinic anhydride, isobutylene succinic anhydride, 2-butene-1-yl succinic anhydride, n-octenyl succinic anhydride, 2-octenyl succinic anhydride, 2-nonenyl succinic anhydride, 2-decene succinic anhydride, 2-decyl-1-succinic anhydride, dodecenyl succinic anhydride, 2-dodecenyl-succinic anhydride, tetradecenyl succinic anhydride, pentadecenyl succinic anhydride, 2-hexene succinic anhydride, dodecenyl succinic anhydride, etc.
[0013] The (meth)acrylic acid monomer is selected from one or more compounds represented by formula II, and the (meth)acrylate monomer is selected from one or more compounds represented by formula III:
[0014]
[0015] Among them, R3 is a hydrogen atom or a methyl group, and R4 is a straight-chain alkyl group having 1 to 10 carbon atoms, a branched-chain alkyl group having 1 to 10 carbon atoms, a phenyl group, a benzyl group, a phenethyl group, or a phenylpropyl group. Preferably, R3 is a hydrogen atom or a methyl group, and R4 is a methyl group, an ethyl group, or a benzyl group. More preferably, R3 is a hydrogen atom or a methyl group, and R4 is an ethyl group.
[0016] The structural formula of the styrene derivative monomer is shown in Formula IV:
[0017]
[0018] Among them, R5 is an alkyl group with 1-3 carbon atoms, an alkoxy group with 1-3 carbon atoms, an amino group, a halogen atom or a hydrogen atom. The five substitution positions on the benzene ring can all be connected to the R5 group. The number of R5 is 1-5. When there are multiple R5 groups, the R5 groups at different substitution positions can be the same or different.
[0019] Preferably, the mass percentage of each monomer in the alkali-soluble resin is as follows: auxiliary monomer 1-10%, (meth) acrylic acid monomer 15-30%, (meth) acrylate monomer 10-65%, styrene derivative monomer 1-50%. The amount of auxiliary monomer must be strictly controlled. If the proportion is less than 1%, it will significantly affect the film stripping effect; if the proportion is higher than 10%, the film fragments are too small, which is easy to clog the nozzle and is not conducive to the collection and treatment of waste film scraps. Considering the film stripping effect, the mass percentage of the auxiliary monomer is further preferably 3-7%.
[0020] Preferably, the weight average molecular weight of the alkali-soluble resin is 30,000 to 150,000, and the acid value is 90 to 200 mg KOH / g; when the weight average molecular weight of the alkali-soluble resin is less than 30,000, there is a tendency that the developer resistance decreases and the dry film resist layer is easy to overflow; when it exceeds 150,000, there is a tendency that the developing time becomes longer and the resolution decreases. Further preferably, the weight average molecular weight of the alkali-soluble resin is 40,000 to 100,000, and the acid value is 110 to 170 mg KOH / g.
[0021] Preferably, the molecular weight distribution (i.e., the ratio of the number average molecular weight to the weight average molecular weight) of the alkali-soluble resin is 1.0 to 3.0; when the molecular weight distribution of the alkali-soluble resin exceeds 3.0, there is a risk of decreased adhesion and resolution. Further preferably, the molecular weight distribution of the alkali-soluble resin is 1.0 to 2.0.
[0022] Preferably, the photopolymerizable monomer is an ethylenically unsaturated double-bond monomer selected from nonylphenol acrylate, ethoxylated (propoxylated) nonylphenol acrylate, bisphenol A di(meth)acrylate, ethoxylated (propoxylated) bisphenol A di(meth)acrylate, polyethylene glycol (propylene glycol) di(meth)acrylate, ethoxylated (propoxylated) neopentyl glycol diacrylate, trimethylolpropane tri(meth)acrylate, ethoxylated (propoxylated) trimethylolpropane tri(meth)acrylate. To improve the resolution, the photopolymerizable monomer is further preferably ethoxylated bisphenol A di(meth)acrylate and / or ethoxylated trimethylolpropane tri(meth)acrylate.
[0023] Preferably, the photopolymerization initiator is selected from one or more of hexaarylbiimidazole series compounds and 9-phenylacridine.
[0024] The photosensitive resin composition further comprises 0.5 to 5.0 parts by weight of additives, and the raw materials comprise one or more of dyes, colorants, plasticizers, defoamers, and polymerization inhibitors.
[0025] Preferably, the photosensitive resin composition is prepared by dissolving the raw material in an organic solvent, the mass ratio of the raw material to the organic solvent is 1:(0.3-0.5), and the organic solvent is acetone.
[0026] The present invention has the following beneficial effects:
[0027] 1. The present invention introduces a monomer containing a cyclic anhydride structure as an auxiliary monomer into the alkali-soluble resin of the photosensitive resin composition, which significantly improves the film stripping performance of the photosensitive resin composition when used as a dry film resist (fast film stripping speed, no excessive film stripping fragments, and clean film stripping), so that the alkali-soluble resin will not have the problem of reduced film stripping performance even under the premise of adding styrene derivatives, effectively overcoming the defects of the prior art and improving the production yield.
[0028] 2. The alkali-soluble resin of the present invention is composed of a matrix of (meth) acrylic acid monomers, (meth) acrylic ester monomers and styrene derivative monomers. The matrix, in combination with a photopolymerizable monomer, can impart good adhesion and resolution to the photosensitive resin composition. Moreover, the adhesion and resolution of the matrix are not affected after adding a monomer containing a cyclic anhydride structure, and the stability is good.
[0029] 3. The present invention also ensures high adhesion and resolution of the photosensitive resin composition by strictly controlling parameters, specifically, by controlling the amount, weight average molecular weight, molecular weight distribution and amount of photopolymerizable monomer of the alkali-soluble resin to ensure resolution, and by controlling the molecular weight distribution of the alkali-soluble resin to ensure adhesion.
[0030] 4. The prior art improves the stripping performance by reducing the molecular weight of the alkali-soluble resin or increasing the acid value of the alkali-soluble resin, which will cause a decrease in chemical resistance and easily lead to lateral corrosion or plating of the circuit; while the monomer containing a cyclic acid anhydride structure of the present invention will not react with the developer and the electroplating solution, and will only undergo a hydrolysis reaction with the stripping solution such as sodium hydroxide, potassium hydroxide and other strong alkalis during the stripping stage, thereby accelerating the peeling and decomposition of the corrosion-resistant layer, thereby ensuring good plating resistance while improving the stripping performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 : Performance information and raw material composition of the alkali-soluble resin in the photosensitive resin composition of Examples 1-6 and Comparative Examples 1-3;
[0032] Figure 2 : Formula table of photosensitive resin compositions of Examples 1-6 and Comparative Examples 1-3;
[0033] Figure 3 : Performance test data of the photosensitive resin compositions of Examples 1-6 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0035] The present invention specifically modifies the alkali-soluble resin, that is, introduces a monomer containing a cyclic acid anhydride structure into the alkali-soluble resin, which can significantly improve the film removal performance of the photosensitive resin composition, thereby obtaining a photosensitive resin composition with good resolution, adhesion, film removal speed, anti-plating and other properties.
[0036] The performance information and raw material composition of the alkali-soluble resin used in Examples 1-6 and Comparative Examples 1-3 are as follows: Figure 1 As shown, pentadecenyl succinic anhydride, (2-propylene) succinic anhydride, 2-decyl-1-succinic anhydride, and 2-hexene succinic anhydride are auxiliary monomers, the alkali-soluble resin used is prepared by a conventional solution polymerization method, the solvent is butanone, and the raw materials used are conventional products purchased on the market.
[0037] Example 1
[0038] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1 A-1) 55 parts, photopolymerizable monomer 40 parts, photoinitiator 3.15 parts, additive 1.85 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 20 parts, (6) ethoxylated (12) propoxylated dimethacrylate 12 parts and (3) ethoxylated trimethylolpropane triacrylate 8 parts; the photoinitiator is 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole 3.1 parts and N-phenylglycine 0.05 parts; the additive includes brilliant green pigment 0.05 parts, leuco crystal violet 0.8 parts and p-toluenesulfonamide 1 part.
[0039] Example 2
[0040] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1 A-2) 45 parts, photopolymerizable monomer 50 parts, photoinitiator 2.95 parts, additive 2.05 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 30 parts, (6) ethoxylated (12) propoxylated dimethacrylate 8 parts and (3) ethoxylated trimethylolpropane triacrylate 12 parts; the photoinitiator is 2.9 parts of 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole and 0.05 parts of N-phenylglycine; the additive includes 0.05 parts of brilliant green pigment, 1 part of leuco crystal violet and 1 part of p-toluenesulfonamide.
[0041] Example 3
[0042] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1A-3) 65 parts, photopolymerizable monomer 30 parts, photoinitiator 0.5 parts, additives 4.5 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 15 parts and (6) ethoxylated (12) propoxylated dimethacrylate 15 parts; the photoinitiator is 9-phenylacridine 0.45 parts, N-phenylglycine 0.05 parts; the additive includes brilliant green pigment 0.05 parts, leuco crystal violet 1.45 parts and p-toluenesulfonamide 3 parts.
[0043] Example 4
[0044] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1 A-4) 50 parts, photopolymerizable monomer 44.5 parts, photoinitiator 5 parts, additive 0.5 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 29.5 parts and (6) ethoxylated (12) propoxylated dimethacrylate 15 parts; the photoinitiator is 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole 4.95 parts and N-phenylglycine 0.05 parts; the additive includes brilliant green pigment 0.05 parts and leuco crystal violet 0.45 parts.
[0045] Example 5
[0046] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1 The invention discloses a novel nanostructured carbon foam comprising: a nanostructured carbon foam comprising: 53 parts of (A-5), 38.6 parts of a photopolymerizable monomer, 3.4 parts of a photoinitiator, and 5 parts of an additive; the photopolymerizable monomer comprises: 22.6 parts of (10) ethoxylated bisphenol A dimethacrylate, 8 parts of (6) ethoxylated (12) propoxylated dimethacrylate, and 8 parts of (3) ethoxylated trimethylolpropane triacrylate; the photoinitiator comprises 3 parts of 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole, 0.35 parts of 9-phenylacridine, and 0.05 parts of N-phenylglycine; the additive comprises 0.05 parts of brilliant green pigment, 1.45 parts of leuco crystal violet, and 3.5 parts of p-toluenesulfonamide.
[0047] Example 6
[0048] A photosensitive resin composition, the raw materials of which include, by weight: an alkali-soluble resin ( Figure 1A-6) 58 parts, photopolymerizable monomer 36 parts, photoinitiator 2.95 parts, additive 3.05 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 24 parts, (6) ethoxylated (12) propoxylated dimethacrylate 8 parts and (3) ethoxylated trimethylolpropane triacrylate 4 parts; the photoinitiator is 2.9 parts of 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole and 0.05 parts of N-phenylglycine; the additive includes 0.05 parts of brilliant green pigment, 1 part of leuco crystal violet and 2 parts of p-toluenesulfonamide.
[0049] Comparative Example 1
[0050] This comparative example provides a photosensitive resin composition. Compared with the above embodiment, the main difference is that the alkali-soluble resin raw material does not contain auxiliary monomers. The raw materials of the photosensitive resin composition include, by weight: alkali-soluble resin ( Figure 1 A-7) 58 parts, photopolymerizable monomer 36 parts, photoinitiator 2.95 parts, additives 3.05 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 28 parts and (6) ethoxylated (12) propoxylated dimethacrylate 8 parts; the photoinitiator is 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole 2.9 parts and N-phenylglycine 0.05 parts; the additive includes 0.05 parts of brilliant green pigment, 1 part of leuco crystal violet and 2 parts of p-toluenesulfonamide.
[0051] Comparative Example 2
[0052] This comparative example provides a photosensitive resin composition. Compared with the above embodiment, the main difference is that the amount of auxiliary monomer (2-propylene) succinic anhydride in the alkali-soluble resin raw material is 0.5%wt, which is lower than the required range of 1-10%. The raw materials of the photosensitive resin composition include, by weight: alkali-soluble resin ( Figure 1 A-8) 58 parts, photopolymerizable monomer 36 parts, photoinitiator 2.95 parts, additives 3.05 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 28 parts and (6) ethoxylated (12) propoxylated dimethacrylate 8 parts; the photoinitiator is 2.9 parts of 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole and 0.05 parts of N-phenylglycine; the additive includes 0.05 parts of brilliant green pigment, 1 part of leuco crystal violet and 2 parts of p-toluenesulfonamide.
[0053] Comparative Example 3
[0054] This comparative example provides a photosensitive resin composition. Compared with the above embodiment, the main difference is that the amount of the auxiliary monomer pentadecene succinic anhydride in the alkali-soluble resin raw material is 13%wt, which exceeds the required range of 1-10%. The raw materials of the photosensitive resin composition include, by weight: alkali-soluble resin ( Figure 1 A-9) 58 parts, photopolymerizable monomer 36 parts, photoinitiator 2.95 parts, additives 3.05 parts; the photopolymerizable monomer includes (10) ethoxylated bisphenol A dimethacrylate 28 parts and (6) ethoxylated (12) propoxylated dimethacrylate 8 parts; the photoinitiator is 2.9 parts of 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole and 0.05 parts of N-phenylglycine; the additive includes 0.05 parts of brilliant green pigment, 1 part of leuco crystal violet and 2 parts of p-toluenesulfonamide.
[0055] The formulations of the photosensitive resin compositions of Examples 1-6 and Comparative Examples 1-3 are as follows: Figure 2 As shown, when the photosensitive resin composition is prepared, Figure 2 The components are mixed in proportion according to the formula, 60 parts by weight of acetone are added to 100 parts by weight of the mixture, and then stirred thoroughly until completely dissolved to prepare a resin composition solution with a solid content of 40%. When used, the resin composition solution is evenly coated on the surface of a 15um thick PET support film with a coating machine, and placed in a 90℃ oven for 10 minutes to form a 30um thick dry film resist layer, which appears blue-green under a yellow light; then, a 20um thick polyethylene film protective layer is attached to its surface to obtain a three-layer structure photosensitive dry film.
[0056] The photosensitive dry films prepared from the photosensitive resin compositions of Examples 1-6 and Comparative Examples 1-3 were subjected to the following operations to evaluate the performance of the photosensitive resin compositions:
[0057] 1. Laminating: Take the copper clad laminate, polish its copper surface with a grinder, wash with water, and dry it to get a bright and fresh copper surface; set the laminating machine roller temperature to 110°C, the conveying speed to 1.5m / min, and thermally laminate the photosensitive dry film to the copper clad laminate under standard pressure;
[0058] 2. Exposure: After film application, let the sample stand for more than 15 minutes, and then use the M-552 exposure machine of Zhisheng Technology for exposure, with the exposure grid number of 16-20 grids;
[0059] 3. Development: After exposure, the sample is left to stand for more than 15 minutes, the development temperature is 30°C, and the pressure is 1.2Kg / cm 2The developer is a 1%wt sodium carbonate aqueous solution, the developing time is 1.5-2.0 times the minimum developing time, and the developer is washed with water and dried after developing;
[0060] 4. Stripping: The stripping solution is NaOH, the concentration is 3.0wt%, the temperature is 50℃, and the developing pressure is 1.2Kg / cm 2 .
[0061] Based on the above operation, the photosensitive resin composition was evaluated for the following properties, and the evaluation items and methods were as follows:
[0062] 1. Evaluation of film stripping speed: Take a substrate after film pasting, exposure and development, cut it into a 4*5cm square, put it into a beaker containing 100mL of film stripping solution (concentration 3wt%, temperature 50℃), stir it with magnetic force for 1min, and record the time when the dry film is completely detached; evaluate the film stripping speed by testing the film stripping time. The shorter the film stripping time, the faster the film stripping speed.
[0063] 2. Evaluation of the size of film stripping fragments: Take a substrate after film application, exposure and development, cut it into a 4*5cm square, put it into a beaker containing 100mL of film stripping solution (concentration 3wt%, temperature 50℃), stir it with a magnetic stirrer for 1min, observe the size of the film stripping fragments, and evaluate the results according to the following criteria:
[0064] ○ / Excellent: fragment size 10-20 mm; △ / Fair: fragment size 25-30 mm; × / Poor: fragment size greater than 30 mm or less than 5 mm.
[0065] 3. Resolution evaluation: Exposure is performed using a mask having a wiring pattern with an exposure portion and an unexposed portion having a width of n:n (n is 10 to 100 μm). After development for 1.5 times the minimum development time, the minimum mask width at which a cured resist line is normally formed is taken as the resolution value and observed using a magnifying glass.
[0066] 4. Evaluation of adhesion: A photosensitive dry film resist is laminated on a copper plate by hot pressing, and exposed using a mask having a wiring pattern with a width of n:400 (n is 10 to 100 μm) between the exposed and unexposed parts. After development for 1.5 times the minimum development time, the minimum mask width at which a cured resist line is normally formed is taken as the adhesion value and observed using a magnifying glass.
[0067] 5. Evaluation of electroplating resistance: At 40°C, soak the developed substrate in 10% acidic degreasing solution for 10 min, then rinse with water for 5 min. After micro-etching with sodium sulfate, soak it in 10% sulfuric acid aqueous solution at room temperature for 2 min. Then immerse the substrate in a pre-prepared copper plating solution with a current density of 2ASD and electroplate for 70 min. Then soak it in 10% sulfuric acid aqueous solution at room temperature for 2 min. Then immerse the substrate in a pre-prepared tin plating solution with a current density of 1ASD and electroplate for 10 min. After washing with water, remove the cured resist and observe the sample with a 500x high-resolution scanning electron microscope to see if any penetration plating occurs.
[0068] The performance test data of Examples 1-6 and Comparative Examples 1-3 are as follows Figure 3 As shown, it can be seen that Examples 1-6 use different monomers containing cyclic anhydride structures as auxiliary monomers in the alkali-soluble resin, and have good resolution, adhesion, and anti-plating properties, can effectively shorten the film stripping time and reduce the size of film stripping fragments, and the film stripping is clean and has good comprehensive performance. In Comparative Example 1, although the resolution and adhesion are good, the film stripping time is long, the size of the film stripping fragments is large, and it is easy to cause film stripping residues and wrap around the roller; in Comparative Example 2, there is still room for improvement in the film stripping time and the size of the film stripping fragments; in Comparative Example 3, the adhesion and resolution are good, but the size of the film stripping fragments is too small, which is easy to cause nozzle clogging.
[0069] This specific implementation is only an explanation of the present invention, not a limitation of the present invention. Any changes made by those skilled in the art after reading the specification of the present invention will be protected by the patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A photosensitive resin composition, characterized in that: The invention is prepared from at least the following raw materials in parts by weight: 45 to 65 parts of alkali-soluble resin, 30 to 50 parts of photopolymerizable monomers, and 0.5 to 5 parts of photoinitiators; the alkali-soluble resin is copolymerized by (meth) acrylic acid monomers, (meth) acrylic ester monomers, styrene derivative monomers, and auxiliary monomers; the auxiliary monomers are monomers containing cyclic anhydride structures; the side chains of the cyclic anhydride structures have unsaturated bonds; the cyclic anhydride will not be destroyed by ring opening during copolymerization; the weight percentage of the auxiliary monomers in the alkali-soluble resin is 1 to 10%.
2. The photosensitive resin composition according to claim 1, characterized in that: The auxiliary monomer is selected from one or more of the compounds represented by formula I-1 and I-2: Here, R1 is independently a hydrogen atom or a linear alkyl group having 1 to 15 carbon atoms, and R2 is a hydrogen atom or a methyl group.
3. The photosensitive resin composition according to claim 1, characterized in that: The (meth)acrylic acid monomer is selected from one or more compounds represented by formula II, and the (meth)acrylate monomer is selected from one or more compounds represented by formula III: Among them, R3 is a hydrogen atom or a methyl group, and R4 is a straight-chain alkyl group having 1 to 10 carbon atoms, a branched-chain alkyl group having 1 to 10 carbon atoms, a phenyl group, a benzyl group, a phenethyl group, or a phenylpropyl group.
4. The photosensitive resin composition according to claim 1, characterized in that: The structural formula of the styrene derivative monomer is shown in Formula IV: Here, R5 is an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, an amino group, a halogen atom or a hydrogen atom.
5. The photosensitive resin composition according to claim 1, characterized in that: The mass percentages of the monomers in the alkali-soluble resin are as follows: 1-10% of auxiliary monomers, 15-30% of (meth)acrylic acid monomers, 10-65% of (meth)acrylate monomers, and 1-50% of styrene derivative monomers.
6. The photosensitive resin composition according to claim 1, characterized in that: The weight average molecular weight of the alkali-soluble resin is 30,000 to 150,000, and the acid value is 90 to 200 mg KOH / g.
7. The photosensitive resin composition according to claim 1, characterized in that: The molecular weight distribution of the alkali-soluble resin is 1.0 to 3.
0.
8. The photosensitive resin composition according to claim 1, characterized in that: The photopolymerizable monomer is an ethylenically unsaturated double-bond monomer selected from one or more of nonylphenol acrylate, ethoxylated (propoxylated) nonylphenol acrylate, bisphenol A di(meth)acrylate, ethoxylated (propoxylated) bisphenol A di(meth)acrylate, polyethylene glycol (propylene glycol) di(meth)acrylate, ethoxylated (propoxylated) neopentyl glycol diacrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated (propoxylated) trimethylolpropane tri(meth)acrylate.
9. The photosensitive resin composition according to claim 1, characterized in that: The photopolymerization initiator is selected from one or more of hexaarylbiimidazole series compounds and 9-phenylacridine.
10. The photosensitive resin composition according to claim 1, characterized in that: The raw material also includes 0.5 to 5.0 parts by weight of additives, and the raw material also includes one or more of a dye, a coloring agent, a plasticizer, a defoaming agent, and an inhibitor.