Pipe threaded joints
By forming a coating with high friction coefficient and low friction coefficient on the surface of the pipe threaded joint, adjusting the torque relationship, the problem of tightening efficiency and insufficient Delta torque under high tightening torque is solved, and more efficient tightening and airtightness is achieved .
Patent Information
- Application Number
- CN202080013530.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-12
- Filing Date
- 2020-02-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-02-07
AI Technical Summary
The existing pipe threaded joints are difficult to maintain tightening efficiency under high tightening torque conditions, and the Delta torque is insufficient, which affects the adjustment of the tightening torque and airtightness.
The surfaces of the male and female buckles are respectively formed with high friction coefficient and low friction coefficient. The shoulder plating is high friction coefficient and the non-shoulder plating is low friction coefficient. The shoulder torque is adjusted by adjusting the friction coefficient. and yield torque to increase Delta torque.
It realizes efficient thread tightening under the same or higher tightening torque conditions, increases Delta torque, and improves the ease of adjustment and airtightness of tightening torque.
Smart Images

Figure CN113454271B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a threaded joint for a pipe. Background Art
[0002] Oil well pipes are used to exploit oil and gas fields. Oil well pipes are formed by connecting multiple steel pipes according to the depth of the well. The steel pipes are connected by tightening the pipe threaded joints formed at the ends of the steel pipes. Oil well pipes are pulled up for inspection and loosened, and after inspection, they are tightened again and reused.
[0003] The pipe threaded joint has a pin and a box. The pin includes an external thread formed on the outer circumference of the end of the steel pipe and a non-threaded metal contact portion. The box includes an internal thread formed on the inner circumference of the end of the steel pipe and a non-threaded metal contact portion. The non-threaded metal contact portion includes a metal sealing portion and a shoulder portion. When the steel pipes are threaded together, the external thread and the internal thread, the metal sealing portions, and the shoulders come into contact.
[0004] The threaded parts of the pin and box parts and the unthreaded metal contact parts are repeatedly subjected to strong friction when tightening and loosening the steel pipe. If these parts do not have sufficient anti-friction durability, galling (irreparable seizure) will occur when tightening and loosening the threads repeatedly. Therefore, pipe threaded joints require sufficient anti-friction durability, that is, excellent seizure resistance.
[0005] In the past, compound grease containing heavy metals was used to improve the seizure resistance. The seizure resistance of the pipe threaded joint can be improved by applying the compound grease on the surface of the pipe threaded joint. However, heavy metals such as Pb contained in the compound grease may have an impact on the environment. Therefore, it is desired to develop a pipe threaded joint that does not use compound grease.
[0006] International Publication No. 2016 / 170031 (Patent Document 1) proposes a technique for improving the seizure resistance of a threaded joint for pipes by using a plating layer instead of compound grease.
[0007] The pipe threaded joint disclosed in Patent Document 1 includes: a threaded portion extending on the outer circumference or inner circumference thereof, a first sealing surface on the circumference, and a second sealing surface capable of forming metal-metal interference with the first sealing surface. The threaded portion and the first sealing surface of the pipe threaded joint are covered with a metal corrosion-resistant and seizure-resistant layer mainly composed of zinc by weight.
[0008] Furthermore, Japanese Patent Application Laid-Open No. 63-130986 (Patent Document 2) proposes a technique for improving the airtightness of a threaded joint for pipes by forming a plating layer on the surface of the threaded joint for pipes.
[0009] The pipe threaded joint disclosed in Patent Document 2 is a tapered thread and includes an external thread and an internal thread. The thread surface of the 1.0 to 2.0 pitch portion of the external thread or internal thread of the pipe threaded joint is subjected to a partial surface treatment process such as metal plating or spraying with a thickness of 30 to 200 μm, forming a phosphate film, etc. for maintaining airtightness.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: International Publication No. 2016 / 170031
[0013] Patent Document 2: Japanese Patent Application Laid-Open No. 63-130986 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] However, the torque (hereinafter referred to as tightening torque) of the pipe threaded joint when completing the tightening of the threads is predetermined. The tightening of the threads is performed to obtain the determined tightening torque when completing the tightening of the threads. In recent years, due to the deepening of oil wells, it is sometimes necessary to tighten the threads with a higher tightening torque than before.
[0016] The thread tightening operation of pipe threaded joints is performed on marine equipment and oil drilling. In the actual site where the thread tightening is performed, it is preferred that the thread tightening operation efficiency is high. If the tightening torque of each pipe threaded joint varies greatly, it is necessary to fine-tune the torque of the thread tightening equipment each time, which reduces the operation efficiency. Therefore, a pipe threaded joint is sought that can tighten the thread with the same tightening torque as before, and can tighten the thread even at a higher tightening torque than before.
[0017] On the other hand, it is preferred that the pipe threaded joint has an easy adjustment of the tightening torque. Specifically, when a pipe threaded joint having a shoulder portion is threaded, the shoulder portions of the pin and box come into contact with each other. The torque generated at this time is called the shoulder torque. When the pipe threaded joint is threaded, the thread is further tightened after the shoulder torque is reached until the tightening is completed. As a result, the airtightness of the pipe threaded joint is improved. If the thread is tightened excessively, the metal constituting at least one of the pin and box begins to undergo plastic deformation. The torque generated at this time is called the yield torque.
[0018] When the delta torque, which is defined by the difference between the yield torque and the shoulder torque, is large, the adjustment of the tightening torque becomes easy. Therefore, it is preferable that the delta torque of the threaded joint for pipes is large.
[0019] The seizure resistance and airtightness of a threaded joint for pipes can be improved by the techniques disclosed in Patent Document 1 or Patent Document 2. However, these documents do not mention increasing delta torque or tightening threads with a higher tightening torque than before.
[0020] An object of the present invention is to provide a threaded joint for pipes which has a large delta torque and can be threaded with a tightening torque equal to that of the related art or with a tightening torque higher than that of the related art.
[0021] Solutions for solving problems
[0022] The pipe threaded joint of the present invention includes a pin and a box. The pin includes: a pin side threaded portion, a pin side metal seal portion and a pin side shoulder portion. The box includes: a box side threaded portion, a box side metal seal portion and a box side shoulder portion. The pipe threaded joint further includes a shoulder plating and a non-shoulder plating. The shoulder plating is arranged on the pin side shoulder portion and / or the box side shoulder portion. The shoulder plating includes one or more layers. The outermost layer of the shoulder plating is a high friction coefficient plating. The non-shoulder plating is arranged on at least a portion of the pin side threaded portion, the pin side metal seal portion, the box side threaded portion and the box side metal seal portion. The non-shoulder plating includes one or more layers. The outermost layer of the non-shoulder plating is a low friction coefficient plating having a lower friction coefficient than the high friction coefficient plating.
[0023] Effects of the Invention
[0024] The threaded joint for pipes of the present invention has a large delta torque and can be threaded with a tightening torque equal to that of the related art or with a tightening torque higher than that of the related art. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a graph (torque graph) showing the relationship between the number of rotations of a steel pipe and the torque when tightening a threaded joint for pipes having a shoulder portion.
[0026] Figure 2 This is a torque diagram when both the shoulder torque and the yield torque are high.
[0027] Figure 3 This is a torque diagram when both the shoulder torque and the yield torque are low.
[0028] Figure 4 Torque diagram for low shoulder torque and high yield torque.
[0029] Figure 5 It is a figure which shows the structure of the coupling type pipe threaded joint of this embodiment.
[0030] Figure 6A cross-sectional view of a pipe threaded joint at the beginning of the tightening thread.
[0031] Figure 7 It is a cross-sectional view of the pipe threaded joint after the upper shoulder.
[0032] Figure 8 It is a figure which shows the structure of the integral type threaded joint for pipes of this embodiment.
[0033] Fig. 9 A cross-sectional view of a pipe threaded joint.
[0034] Fig.10 It is a cross-sectional view of the threaded joint for pipes according to the present embodiment.
[0035] Fig.11 For Fig.10 Cross-sectional views of threaded pipe joints according to various other embodiments.
[0036] Fig.12 For Fig.10 and Fig.11 Cross-sectional views of threaded pipe joints according to various other embodiments.
[0037] Fig.13 For Figure 10 to Figure 12 Cross-sectional views of threaded pipe joints according to various other embodiments.
[0038] Fig.14 This is an enlarged view of the shoulder plating layer of this embodiment.
[0039] Fig.15 For Fig.14 Enlarged views of the shoulder plating according to various other embodiments.
[0040] Fig.16 For Fig.14 and Fig.15 Enlarged views of the shoulder plating according to various other embodiments.
[0041] Fig.17 This is an enlarged view of the non-shoulder plating layer of this embodiment.
[0042] Fig.18 For Fig.17 Enlarged views of the non-shoulder plating according to various other embodiments.
[0043] Fig.19 For Fig.17 and Fig.18 Enlarged views of the non-shoulder plating according to various other embodiments. DETAILED DESCRIPTION
[0044] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. The same or corresponding parts in the drawings are denoted by the same reference numerals, and their description will not be repeated.
[0045] The present inventors have conducted various studies on the relationship between the plating layer on the surface of a threaded joint for pipes and the tightening torque and delta torque. As a result, the present inventors have obtained the following findings.
[0046] When steel pipes are threaded together, the optimum torque for completing the threading (called tightening torque) is predetermined. Figure 1 This is a graph (torque graph) showing the relationship between the number of revolutions of a steel pipe and the torque when tightening a threaded joint for a pipe having a shoulder. Hereinafter, the graph showing the relationship between the number of revolutions of a steel pipe and the torque is referred to as a torque graph. Figure 1 When tightening the thread of a pipe threaded joint, the torque initially increases in proportion to the number of revolutions. The rate of increase of the torque at this time is low. If the thread is tightened further, the shoulders come into contact with each other. The torque at this time is called the shoulder torque Ts. If the thread is tightened further after reaching the shoulder torque Ts, the torque increases again in proportion to the number of revolutions. The rate of increase of the torque at this time is high. When the torque reaches the specified value (tightening torque To), the thread is tightened.
[0047] When the torque when tightening the threads reaches the tightening torque To, the metal seals interfere with each other with an appropriate surface pressure. In this case, the airtightness of the pipe threaded joint is high. In addition, high compressive stress and high bending stress are applied to the threaded joint in the oil well. In order to prevent the tightening of the pipe threaded joint from loosening under such stress, it is necessary to tighten the pipe threaded joint with a sufficiently high torque (appropriate tightening torque To).
[0048] If the thread is further tightened after the tightening torque To is reached, the torque becomes too high. If the torque becomes too high, part of the male and female parts will undergo plastic deformation. The torque at this time is called the yield torque Ty. If the delta torque ΔT defined by the difference between the shoulder torque Ts and the yield torque Ty is large, the adjustment of the tightening torque To becomes easy. Therefore, it is preferred that the delta torque ΔT is large.
[0049] In order to increase the delta torque ΔT, it is effective to reduce the shoulder torque Ts or increase the yield torque Ty. The inventors of the present invention believe that the shoulder torque Ts and the yield torque Ty may be adjusted by changing the friction coefficient of the surface of the pin buckle part and the box buckle part. However, even if the surface of the pin buckle part and the box buckle part is changed simply by increasing or decreasing the friction coefficient, the shoulder torque Ts and the yield torque Ty generally behave in the same way.
[0050] Figure 2 This is a torque diagram when both the shoulder torque Ts and the yield torque Ty are high. Figure 2In the figure, the previous torque graph is shown by the dotted line. Figure 2 When the friction coefficient between the male and female parts increases, although the yield torque Ty increases, the shoulder torque Ts also increases (called high shoulder). As a result, even if the previous tightening torque To is reached, sometimes the shoulders will not contact each other and tightening cannot be completed (called no shoulder).
[0051] Figure 3 This is a torque diagram when both the shoulder torque Ts and the yield torque Ty are low. Figure 3 In the figure, the previous torque graph is shown by the dotted line. Figure 3 When the friction coefficient between the male and female parts decreases, the shoulder torque Ts decreases, but the yield torque Ty also decreases. As a result, the yield torque Ty is reached before the specified tightening torque To is reached, causing the shoulder part or the metal seal part to yield. In this case, it is impossible to obtain a sufficient tightening torque To.
[0052] If the yield torque Ty can be increased while the shoulder torque Ts is suppressed to a low level, not only the delta torque ΔT becomes larger, but also thread tightening can be performed with the same tightening torque To as before, or even with a tightening torque Toh higher than before. Figure 4 This is a torque diagram when the shoulder torque Ts is low and the yield torque Ty is high. Figure 4 In the figure, the previous torque graph is shown by the dotted line. Figure 4 In the torque diagram of increasing the yield torque Ty while maintaining the shoulder torque Ts at a low level, the delta torque ΔT becomes larger than the conventional delta torque ΔT'. In addition, even if the thread is tightened with the conventional tightening torque To, since it is greater than the shoulder torque Ts, sufficient airtightness can be ensured. Furthermore, even if the thread is tightened with a tightening torque Toh higher than the conventional tightening torque To, since it is less than the yield torque Ty, the thread can still be tightened without causing the pipe threaded joint to yield.
[0053] As a result of intensive studies, the present inventors found that, on the surfaces of the pin and box parts, the portion that has a greater influence on the generation of the shoulder torque Ts is different from the portion that has a greater influence on the generation of the yield torque Ty.
[0054] Figure 5 2 is a diagram showing the structure of a coupling type pipe threaded joint according to the present embodiment. Figure 5 The pipe threaded joint includes a steel pipe 1 and a coupling 2. The steel pipe 1 has a male buckle 3 having an external threaded portion on the outer surface formed at both ends. The coupling 2 has a female buckle 4 having an internal threaded portion on the inner surface formed at both ends. The coupling 2 is installed on the end of the steel pipe 1 by threading the male buckle 3 and the female buckle 4.
[0055] Figure 6 Cross-sectional view of a pipe threaded joint with the initial tightening of the threads. Figure 6 , the pin buckle part 3 comprises: a pin buckle part side shoulder part 33, a pin buckle part side metal sealing part 32 and a pin buckle part side threaded part 31. The box buckle part 4 comprises: a box buckle part side shoulder part 43, a box buckle part side metal sealing part 42 and a box buckle part side threaded part 41. At the beginning of thread tightening, the pin buckle part side threaded part 31 contacts and slides with the box buckle part side threaded part 41. When thread tightening continues, the pin buckle part side metal sealing part 32 contacts and slides with the box buckle part side metal sealing part 42. Then, the pin buckle part side shoulder part 33 contacts with the box buckle part side shoulder part 43. The torque at this time is the shoulder torque Ts.
[0056] Before the pin-side shoulder 33 and the box-side shoulder 43 come into contact, the pin-side threaded portion 31 and the box-side threaded portion 41, and the pin-side metal seal 32 and the box-side metal seal 42 come into contact and slide. That is, it can be considered that the portion that has a greater influence on the shoulder torque Ts is the portion other than the pin-side shoulder 33 and the box-side shoulder 43. That is, it can be considered that the pin-side threaded portion 31, the box-side threaded portion 41, the pin-side metal seal 32, and the box-side metal seal 42 have a greater influence on the shoulder torque Ts.
[0057] Figure 7 This is a cross-sectional view of a pipe threaded joint after the upper shoulder. Figure 7 After the pin side shoulder 33 and the box side shoulder 43 come into contact, the pin side shoulder 33 and the box side shoulder 43 slide frictionally while receiving a strong force in the axial direction of the steel pipe 1. Therefore, it can be expected that the pressure on the pin side shoulder 33 and the box side shoulder 43 is greater than the pressure on the pin side threaded portion 31, the box side threaded portion 41, the pin side metal seal portion 32, and the box side metal seal portion 42. In other words, it can be considered that the pin side shoulder 33 and the box side shoulder 43 have a greater influence on the yield torque Ty.
[0058] Based on the above research, the inventors have obtained the following insights. A low-friction-coefficient plating is formed on at least a portion of the pin-side threaded portion 31, the box-side threaded portion 41, the pin-side metal seal portion 32, and the box-side metal seal portion 42, which have a greater impact on the shoulder torque Ts, and a high-friction-coefficient plating is formed on the pin-side shoulder portion 33 and / or the box-side shoulder portion 43, which have a greater impact on the yield torque Ty. According to this structure, the yield torque Ty can be increased while maintaining the low shoulder torque Ts. As a result, a pipe threaded joint can be obtained that has a large delta torque ΔT and can be tightened with a tightening torque To that is equal to the previous one and a tightening torque Toh that is higher than the previous one.
[0059] The pipe threaded joint of the present embodiment completed based on the above insights includes a pin and a box. The pin includes: a pin side threaded portion, a pin side metal seal, and a pin side shoulder. The box includes: a box side threaded portion, a box side metal seal, and a box side shoulder. The pipe threaded joint further includes a shoulder plating and a non-shoulder plating. The shoulder plating is arranged on the pin side shoulder and / or the box side shoulder. The shoulder plating includes one or more layers. The outermost layer of the shoulder plating is a high friction coefficient plating. The non-shoulder plating is arranged on at least a portion of the pin side threaded portion, the pin side metal seal, the box side threaded portion, and the box side metal seal. The non-shoulder plating includes one or more layers. The outermost layer of the non-shoulder plating is a low friction coefficient plating having a lower friction coefficient than the high friction coefficient plating.
[0060] The threaded joint for pipes of the present embodiment has a large delta torque, and can be threaded with a tightening torque equal to that of the related art or with a tightening torque higher than that of the related art.
[0061] The shoulder portion plating layer may be disposed on the shoulder portion on the pin side, and the non-shoulder portion plating layer may be disposed on the threaded portion on the pin side and on the metal seal portion on the pin side.
[0062] The shoulder portion plating layer may be disposed on the shoulder portion on the box portion side, and the non-shoulder portion plating layer may be disposed on the threaded portion on the box portion side and on the metal seal portion on the box portion side.
[0063] The thickness of the shoulder portion plating layer may be 1 to 50 μm, and the thickness of the non-shoulder portion plating layer may be 1 to 50 μm.
[0064] When the thickness of each plating layer is within the above range, the effect of suppressing the shoulder torque to be low and improving the yield torque can be obtained more stably.
[0065] The pipe threaded joint may further include a lubricating coating. The lubricating coating is in a liquid or semi-solid state and is disposed as an outermost layer on at least a portion of the pin side threaded portion, the pin side metal seal portion, the pin side shoulder portion, the box side threaded portion, the box side metal seal portion, and the box side shoulder portion.
[0066] When a threaded joint for pipes includes a lubricating film as the outermost layer, the lubricity of the threaded joint for pipes is improved.
[0067] The high friction coefficient coating can be selected from the group consisting of Ni-P alloy coating, Zn-Ni alloy coating, Cu coating, Cr coating and Cu-Sn-Zn alloy coating, and the low friction coefficient coating can be selected from the group consisting of Zn-Ni alloy coating, Cu coating, Cr coating, Cu-Sn-Zn alloy coating and Zn coating.
[0068] When the composition of each plating layer is the above-mentioned composition, the effect of increasing the yield torque while maintaining the shoulder torque low can be more stably obtained.
[0069] The high friction coefficient plating layer may also be selected from the group consisting of Ni-P alloy plating layer and Zn-Ni alloy plating layer, and the low friction coefficient plating layer may also be selected from the group consisting of Cu plating layer, Cr plating layer, Cu-Sn-Zn alloy plating layer and Zn plating layer.
[0070] When the composition of each plating layer is the above-mentioned composition, the effect of improving the yield torque while maintaining the shoulder torque at a low level can be more stably obtained.
[0071] Hereinafter, the threaded joint for pipes according to the present embodiment will be described in detail.
[0072] [Pipe threaded joints]
[0073] The threaded joint for pipes according to the present embodiment includes a pin portion and a box portion. Figure 5 2 is a diagram showing the structure of a coupling type pipe threaded joint according to the present embodiment. Figure 5 , a coupling type pipe threaded joint comprises a steel pipe 1 and a coupling 2. A pin buckle 3 having an external threaded portion on the outer surface is formed at both ends of the steel pipe 1. A box buckle 4 having an internal threaded portion on the inner surface is formed at both ends of the coupling 2. The coupling 2 is mounted on the end of the steel pipe 1 by threading the pin buckle 3 and the box buckle 4. Although not shown in the figure, in order to protect each threaded portion, a protective device is sometimes installed on the pin buckle 3 of the steel pipe 1 and the box buckle 4 of the coupling 2 where the corresponding member is not installed.
[0074] On the other hand, it is also possible to use an integral pipe threaded joint in which one end of the steel pipe 1 is a pin portion 3 and the other end is a box portion 4 without using the coupling 2 . Figure 8 1 is a diagram showing the structure of an integral type pipe threaded joint according to the present embodiment. Figure 8 The integral pipe threaded joint includes a steel pipe 1. A male buckle 3 having an external threaded portion is formed on the outer surface of one end of the steel pipe 1. A female buckle 4 having an internal threaded portion is formed on the inner surface of the other end of the steel pipe 1. The male buckle 3 and the female buckle 4 are screwed together, so that a plurality of steel pipes 1 can be connected to each other. The pipe threaded joint of this embodiment can be used in both the coupling type and the integral type.
[0075] Fig. 9 This is a cross-sectional view of a pipe threaded joint. Fig. 9 The pin part 3 includes: a pin part side threaded portion 31, a pin part side metal seal portion 32 and a pin part side shoulder portion 33. The box part 4 includes: a box part side threaded portion 41, a box part side metal seal portion 42 and a box part side shoulder portion 43.
[0076] Fig. 9 In the embodiment, the pin part 3 is provided with a pin part side shoulder part 33, a pin part side metal seal part 32 and a pin part side threaded part 31 in order from the end of the steel pipe 1. In addition, the box part 4 is provided with a box part side threaded part 41, a box part side metal seal part 42 and a box part side shoulder part 43 in order from the end of the steel pipe 1 or the coupling 2. However, the arrangement of the pin part side threaded part 31 and the box part side threaded part 41, the pin part side metal seal part 32 and the box part side metal seal part 42, and the pin part side shoulder part 33 and the box part side shoulder part 43 is not limited to Fig. 9 The configuration can be changed appropriately. For example, Figure 8 As shown in , the pin part 3 may be sequentially configured with a pin part side metal seal, a pin part side threaded part, a pin part side metal seal, a pin part side shoulder, a pin part side metal seal, and a pin part side threaded part from the end of the steel pipe 1. The box part 4 may be sequentially configured with a box part side metal seal, a box part side threaded part, a box part side metal seal, a box part side shoulder, a box part side metal seal, and a box part side threaded part from the end of the steel pipe 1 or the coupling 2.
[0077] Fig.10 This is a cross-sectional view of a threaded joint for pipes according to this embodiment. Fig.10 The threaded joint for pipes of the present embodiment further includes a shoulder portion plating layer 5 and a non-shoulder portion plating layer 6 .
[0078] [Shoulder plating]
[0079] The shoulder plating layer 5 of this embodiment is disposed on the pin side shoulder 33 and / or the box side shoulder 43. Fig.10 The shoulder plating layer 5 may be disposed on both the pin-side shoulder 33 and the box-side shoulder 43 .
[0080] The shoulder plating layer 5 of the present embodiment may be disposed only on one of the pin-side shoulder 33 or the box-side shoulder 43 . Fig.11 For Fig.10 Cross-sectional views of threaded pipe joints according to various other embodiments. Fig.12 For Fig.10 and Fig.11 Cross-sectional views of threaded pipe joints according to various other embodiments. Fig.13 For Figure 10 to Figure 12 Cross-sectional views of various other embodiments of threaded pipe joints. Fig.11 and Fig.13 , the shoulder plating layer 5 can be arranged only on the male buckle side shoulder 33. Fig.12 The shoulder plating layer 5 may also be disposed only on the shoulder portion 43 on the female buckle side.
[0081] The shoulder plating layer 5 of this embodiment includes one layer or multiple layers. Fig.14 This is an enlarged view of the shoulder plating layer 5 of this embodiment. Fig.14 , the shoulder plating layer 5 may be composed of one layer. In this case, the shoulder plating layer 5 is a high friction coefficient plating layer 50 . Fig.15 For Fig.14 An enlarged view of the shoulder plating layer 5 of another embodiment. Fig.15 The shoulder coating 5 may also be composed of multiple layers. In this case, the shoulder coating 5 is provided with a high friction coefficient coating 50 on its outermost layer. Fig.15 As shown, the shoulder portion plating layer 5 may include an optional plating layer 70 below the high friction coefficient plating layer 50. The optional plating layer 70 may be a laminate of a plurality of plating layers.
[0082] [High friction coefficient coating]
[0083] The friction coefficient of the high friction coefficient coating 50 is higher than the friction coefficient of the low friction coefficient coating 60 described later. The pin buckle side shoulder 33 and the female buckle side shoulder 43 are subjected to high surface pressure and friction sliding at the same time in the final stage of the thread tightening. Therefore, if the outermost layer of the shoulder coating 5 on the pin buckle side shoulder 33 and / or the female buckle side shoulder 43 is a high friction coefficient coating 50, a high torque can be obtained in the final stage of the thread tightening. As a result, the yield torque Ty is high. The friction coefficient of the high friction coefficient coating 50 is not particularly limited as long as it is higher than the friction coefficient of the low friction coefficient coating 60. The lower limit of the friction coefficient of the preferably high friction coefficient coating 50 is 0.10, more preferably 0.11, further preferably 0.12, and further preferably 0.13. The upper limit of the friction coefficient of the preferably high friction coefficient coating 50 is 0.40, more preferably 0.30, and further preferably 0.20. The friction coefficient of the high friction coefficient plating layer 50 can be adjusted by, for example, changing the composition of the high friction coefficient plating layer 50 .
[0084] In the present embodiment, the high friction coefficient coating 50 can be either a single metal coating or an alloy coating. Furthermore, in the present embodiment, the chemical composition of the high friction coefficient coating 50 is not particularly limited. The chemical composition of the high friction coefficient coating 50 can be appropriately selected according to the chemical composition of the known coating. The high friction coefficient coating 50 can be selected, for example, from the group consisting of Cu coating, Cr coating, Zn coating, Ni coating, Cu-Sn alloy coating, Zn-Co alloy coating, Zn-Ni alloy coating, Ni-P alloy coating and Cu-Sn-Zn alloy coating. The high friction coefficient coating 50 can also be selected from the group consisting of Ni-P alloy coating, Zn-Ni alloy coating, Cu coating and Cr coating. The high friction coefficient coating 50 can also be selected from the group consisting of Ni-P alloy coating and Zn-Ni alloy coating.
[0085] As described above, when the shoulder plating layer 5 includes multiple layers, the high friction coefficient plating layer 50 is disposed on the outermost layer of the shoulder plating layer 5. However, the high friction coefficient plating layer 50 may not be disposed on the outermost layer of the pin side shoulder 33 and / or the box side shoulder 43. Fig.16 For Fig.14 and Fig.15 An enlarged view of the shoulder plating layer 5 of another embodiment. Fig.16 A lubricating film 80 may be provided on the shoulder portion plating layer 5. The lubricating film 80 will be described later.
[0086] [Non-shoulder plating]
[0087] The non-shoulder plating layer 6 of the present embodiment is disposed on at least a portion of the pin-side threaded portion 31, the pin-side metal seal portion 32, the box-side threaded portion 41, and the box-side metal seal portion 42. Fig.10 The non-shoulder plating layer 6 can be disposed on all the pin-side threaded portions 31 , the pin-side metal sealing portions 32 , the box-side threaded portions 41 , and the box-side metal sealing portions 42 .
[0088] The non-shoulder plating layer 6 of the present embodiment may also be disposed on a portion of the pin-side threaded portion 31, the pin-side metal seal portion 32, the box-side threaded portion 41, and the box-side metal seal portion 42. Fig.11 The non-shoulder plating layer 6 may be disposed only on the pin-side threaded portion 31 and the pin-side metal seal portion 32. Fig.12 and Fig.13 The non-shoulder portion plating layer 6 may be disposed only on the box-side threaded portion 41 and the box-side metal seal portion 42 .
[0089] The non-shoulder plating 6 may also be disposed only on the pin-side threaded portion 31 and the box-side threaded portion 41. The non-shoulder plating 6 may be disposed only on the pin-side metal seal 32 and the box-side metal seal 42. It can be seen that the non-shoulder plating 6 only needs to be disposed on at least a portion of the pin-side threaded portion 31, the pin-side metal seal 32, the box-side threaded portion 41, and the box-side metal seal 42.
[0090] The non-shoulder portion plating layer 6 of the present embodiment includes one layer or a plurality of layers. Fig.17 This is an enlarged view of the non-shoulder plating layer 6 of this embodiment. Fig.17 , the non-shoulder portion plating layer 6 may be composed of one layer. In this case, the non-shoulder portion plating layer 6 is a low friction coefficient plating layer 60 . Fig.18 For Fig.17 An enlarged view of the non-shoulder plating layer 6 of another embodiment. Fig.18 , the non-shoulder coating 6 may be composed of multiple layers. In this case, the non-shoulder coating 6 is provided with a low friction coefficient coating 60 on its outermost layer. Fig.18 As shown, the optional plating layer 70 may be provided below the low friction coefficient plating layer 60. The optional plating layer 70 may be a stack of a plurality of plating layers.
[0091] [Low friction coefficient coating]
[0092] The friction coefficient of the low friction coefficient coating 60 of the present embodiment is lower than that of the high friction coefficient coating 50. The pin threaded portion 31, the pin metal seal portion 32, the female threaded portion 41 and the female metal seal portion 42 slide against each other before the upper shoulder of the tight thread. Therefore, if the outermost layer of the non-shoulder coating 6 on at least one of the pin threaded portion 31, the pin metal seal portion 32, the female threaded portion 41 and the female metal seal portion 42 is a low friction coefficient coating 60, low torque can be obtained in the initial stage of the tight thread. As a result, the shoulder torque Ts is suppressed to a lower level. The friction coefficient of the low friction coefficient coating 60 is not particularly limited as long as it is lower than the friction coefficient of the high friction coefficient coating 50. However, the lower limit of the friction coefficient of the low friction coefficient coating 60 is preferably 0.01, more preferably 0.05, further preferably 0.08, and further preferably 0.10. The upper limit of the friction coefficient of the low friction coefficient plating layer 60 is preferably less than 0.13, more preferably 0.12, and further preferably 0.11. The friction coefficient of the low friction coefficient plating layer 60 can be adjusted by changing the composition of the low friction coefficient plating layer 60, for example.
[0093] In the present embodiment, the low friction coefficient coating 60 can be either a single metal coating or an alloy coating. Moreover, in the present embodiment, the chemical composition of the low friction coefficient coating 60 is not particularly limited. The chemical composition of the low friction coefficient coating 60 can be appropriately selected according to the chemical composition of the known coating. The low friction coefficient coating 60 can be selected from the group consisting of, for example, Cu coating, Cr coating, Zn coating, Ni coating, Cu-Sn alloy coating, Zn-Co alloy coating, Zn-Ni alloy coating, Ni-P alloy coating and Cu-Sn-Zn alloy coating. The low friction coefficient coating 60 can also be selected from the group consisting of Zn-Ni alloy coating, Cu coating, Cr coating and Zn coating. The low friction coefficient coating 60 can also be selected from the group consisting of Cu coating, Cr coating and Zn coating.
[0094] As described above, when the non-shoulder portion plating layer 6 includes multiple layers, the low friction coefficient plating layer 60 is arranged on the outermost layer of the non-shoulder portion plating layer 6. However, the low friction coefficient plating layer 60 may not be arranged on the outermost layer of the pin-side threaded portion 31, the pin-side metal seal portion 32, the box-side threaded portion 41, or the box-side metal seal portion 42. Fig.19 For Fig.17 and Fig.18 An enlarged view of the non-shoulder plating layer 6 of another embodiment. Fig.19 A lubricating film 80 may be provided on the non-shoulder portion plating layer 6. The lubricating film 80 will be described later.
[0095] [Friction coefficient of high friction coefficient coating and low friction coefficient coating]
[0096] In the present embodiment, the friction coefficient of the high friction coefficient coating 50 and the low friction coefficient coating 60 can be measured by the following method. Prepare a sample formed with a high friction coefficient coating 50 or a low friction coefficient coating 60. Perform a Bowden sliding test on the high friction coefficient coating 50 or the low friction coefficient coating 60. The Bowden sliding test is performed under the following conditions. Sliding pressure head: 3 / 16" (diameter 4.7625mm) steel ball (Fe, steel type SUJ2), pressing load: 3kgf, sliding form: linear reciprocating sliding, sliding amplitude: 30mm, number of sliding reciprocating times: 5 times, sliding speed: 4mm / second, test temperature: 25°C, lubricating oil: SEAL-GUARD ECF manufactured by JET-LUBE Co., Ltd. (trade name), lubricating oil coating amount: 40g / m 2 The arithmetic mean of the friction coefficients obtained by sliding back and forth five times was defined as the friction coefficient of each coating layer.
[0097] [Any plating]
[0098] In the present embodiment, any plating layer 70 may be formed or not. Furthermore, any plating layer 70 may be one layer or may be composed of multiple layers. In the present embodiment, any plating layer 70 may be a plating layer of a single metal or an alloy plating layer. That is, in the present embodiment, there is no particular limitation on the chemical composition of any plating layer 70. The chemical composition of any plating layer 70 may be appropriately selected according to the chemical composition of the known plating layer. For example, any plating layer 70 may be selected from the group consisting of a Cu plating layer, a Cr plating layer, a Zn plating layer, a Ni plating layer, a Cu-Sn alloy plating layer, a Zn-Co alloy plating layer, a Zn-Ni alloy plating layer, a Ni-P alloy plating layer and a Cu-Sn-Zn alloy plating layer.
[0099] The structure of the arbitrary plating layer 70 may be the same or different on the male buckle part 3 side and the female buckle part 4 side. The structure of the arbitrary plating layer 70 may be the same or different under the high friction coefficient plating layer 50 and under the low friction coefficient plating layer 60. The chemical composition of the arbitrary plating layer 70 may be the same or different on the male buckle part 3 side and the female buckle part 4 side. The chemical composition of the arbitrary plating layer 70 may be the same or different under the high friction coefficient plating layer 50 and under the low friction coefficient plating layer 60.
[0100] [Configuration of shoulder plating and non-shoulder plating]
[0101] In this embodiment, the arrangement of the shoulder portion plating layer 5 and the non-shoulder portion plating layer 6 is not limited to Fig.10 For example, refer to Fig.11 , the shoulder plating layer 5 can be arranged on the pin side shoulder 33, and the non-shoulder plating layer 6 can be arranged on the pin side threaded portion 31 and the pin side metal seal 32. In this case, the box side shoulder 43, the box side metal seal 42 and the box side threaded portion 41 may not be arranged with any structure, may be arranged with the lubricating film 80 described later, and may be arranged with a chemical conversion treatment film such as a phosphate film.
[0102] In addition, refer to Fig.12 , the shoulder plating layer 5 may also be arranged on the female buckle side shoulder 43, and the non-shoulder plating layer 6 may also be arranged on the female buckle side threaded portion 41 and the female buckle side metal seal 42. In this case, the male buckle side shoulder 33, the male buckle side metal seal 32 and the male buckle side threaded portion 31 may not be arranged with any structure, may be arranged with the lubricating film 80 described later, and may also be arranged with a chemical conversion treatment film such as a phosphate film. In addition, referring to Fig.13 The shoulder plating layer 5 may also be disposed on the shoulder portion 33 on the pin side, and the non-shoulder plating layer 6 may also be disposed on the threaded portion 41 on the box side and on the metal sealing portion 42 on the box side.
[0103] [Thickness of shoulder plating and non-shoulder plating]
[0104] In the present embodiment, the thickness of the shoulder plating layer 5 is not particularly limited. The thickness of the shoulder plating layer 5 is preferably 1 to 50 μm. In this case, the effect of improving the yield torque Ty can be obtained more stably. The more preferred lower limit of the thickness of the shoulder plating layer 5 is 3 μm, and more preferably 5 μm. The more preferred upper limit of the thickness of the shoulder plating layer 5 is 40 μm, and more preferably 25 μm.
[0105] In the present embodiment, the thickness of the non-shoulder plating layer 6 is not particularly limited. The thickness of the non-shoulder plating layer 6 is preferably 1 to 50 μm. In this case, the effect of maintaining a low shoulder torque Ts can be obtained more stably. The more preferred lower limit of the thickness of the non-shoulder plating layer 6 is 3 μm, and more preferably 5 μm. The more preferred upper limit of the thickness of the non-shoulder plating layer 6 is 40 μm, and more preferably 25 μm.
[0106] [Combination of high friction coefficient coating and low friction coefficient coating]
[0107] In the present embodiment, as long as the friction coefficient of the high friction coefficient coating 50 is higher than the friction coefficient of the low friction coefficient coating 60, there is no particular limitation on the combination of its composition. The combination of the composition of the high friction coefficient coating 50 and the low friction coefficient coating 60 is, for example, as follows. When the high friction coefficient coating 50 is a Ni-P alloy coating, the low friction coefficient coating 60 can be selected from the group consisting of a Cu coating, a Cr coating, a Zn coating, a Ni coating, a Cu-Sn alloy coating, a Zn-Co alloy coating, a Zn-Ni alloy coating and a Cu-Sn-Zn alloy coating. When the high friction coefficient coating 50 is a Zn-Ni alloy coating, the low friction coefficient coating 60 can be selected from the group consisting of a Cu coating, a Cr coating, a Zn coating, a Ni coating, a Cu-Sn alloy coating, a Zn-Co alloy coating and a Cu-Sn-Zn alloy coating.
[0108] When the low friction coefficient coating 60 is a Cu coating, the high friction coefficient coating 50 can be selected from the group consisting of a Ni coating, a Cu-Sn alloy coating, a Zn-Co alloy coating, a Zn-Ni alloy coating, a Ni-P alloy coating, and a Cu-Sn-Zn alloy coating. When the low friction coefficient coating 60 is a Cr coating, the high friction coefficient coating 50 can be selected from the group consisting of a Cu coating, a Ni coating, a Cu-Sn alloy coating, a Zn-Co alloy coating, a Zn-Ni alloy coating, a Ni-P alloy coating, and a Cu-Sn-Zn alloy coating. When the low friction coefficient coating 60 is a Zn coating, the high friction coefficient coating 50 can be selected from the group consisting of a Cr coating, a Cu coating, a Ni coating, a Cu-Sn alloy coating, a Zn-Co alloy coating, a Zn-Ni alloy coating, a Ni-P alloy coating, and a Cu-Sn-Zn alloy coating.
[0109] Preferably, the high friction coefficient plating layer 50 is selected from the group consisting of Ni-P alloy plating, Zn-Ni alloy plating, Cu plating, Cr plating and Cu-Sn-Zn alloy plating. Preferably, the low friction coefficient plating layer 60 is selected from the group consisting of Zn-Ni alloy plating, Cu plating, Cr plating, Cu-Sn-Zn alloy plating and Zn plating. That is, the high friction coefficient plating layer 50 and the low friction coefficient plating layer 60 are preferably a combination as described in (1) to (5) below.
[0110] (1) When the high friction coefficient plating layer 50 is a Ni-P alloy plating layer, the low friction coefficient plating layer 60 is selected from the group consisting of a Zn-Ni alloy plating layer, a Cu plating layer, a Cr plating layer, a Cu-Sn-Zn alloy plating layer and a Zn plating layer,
[0111] (2) When the high friction coefficient plating layer 50 is a Zn-Ni alloy plating layer, the low friction coefficient plating layer 60 is selected from the group consisting of a Cu plating layer, a Cr plating layer, a Cu-Sn-Zn alloy plating layer and a Zn plating layer,
[0112] (3) When the high friction coefficient plating layer 50 is a Cu plating layer, the low friction coefficient plating layer 60 is selected from the group consisting of a Cr plating layer, a Cu-Sn-Zn alloy plating layer and a Zn plating layer,
[0113] (4) When the high friction coefficient coating 50 is a Cr coating, the low friction coefficient coating 60 is selected from the group consisting of a Cu-Sn-Zn alloy coating and a Zn coating,
[0114] (5) When the high friction coefficient plating layer 50 is a Cu-Sn-Zn alloy plating layer, the low friction coefficient plating layer 60 is a Zn plating layer.
[0115] [Chemical composition of the coating]
[0116] The chemical composition of each of the above-mentioned plating layers is, for example, as follows. The Cu plating layer is a plating layer having a chemical composition including Cu and impurities. The Cr plating layer is a plating layer having a chemical composition including Cr and impurities. The Zn plating layer is a plating layer having a chemical composition including Zn and impurities. The Ni plating layer is a plating layer having a chemical composition including Ni and impurities. The Cu-Sn alloy plating layer is a plating layer having a chemical composition including Sn: 10-75%, the balance: Cu and impurities. The Zn-Co alloy plating layer is a plating layer having a chemical composition including Co: 5-25%, the balance: Zn and impurities. The Zn-Ni alloy plating layer is a plating layer having a chemical composition including Ni: 5-25%, the balance: Zn and impurities. The Ni-P alloy plating layer is a plating layer having a chemical composition including P: 0.1-20%, the balance: Ni and impurities. The Cu-Sn-Zn alloy plating layer is a plating layer having a chemical composition including Sn: 20-60%, Zn: 3-30%, the balance: Cu and impurities.
[0117] In this embodiment, the chemical composition of the coating can be measured by the following method. Specifically, a handheld fluorescent X-ray analyzer (DP2000 (trade name DELTA Premium) manufactured by JEOL Ltd.) is used to measure the chemical composition of the coating to be measured. During the measurement, the composition analysis is performed on four locations on the surface of the high friction coefficient coating 50, the low friction coefficient coating 60 or the arbitrary coating 70 (the four locations of 0°, 90°, 180°, and 270° in the pipe circumferential direction of the pipe threaded joint). It should be noted that the handheld fluorescent X-ray analyzer can use the Alloy Plus mode to analyze the chemical composition.
[0118] [Lubricating coating]
[0119] The threaded joint for pipes of this embodiment may further include a lubricating coating 80. Fig.16 The lubricating coating 80 can be disposed on the shoulder plating layer 5. Fig.19 The lubricating film 80 may also be disposed on the non-shoulder portion plating layer 6. However, the configuration of the lubricating film 80 is not limited to Fig.16 and Fig.19 . In the case where the pipe threaded joint of the present embodiment is provided with a lubricating coating 80, it is sufficient to be arranged as the outermost layer on at least a portion of the pin-side threaded portion 31, the pin-side metal seal portion 32, the pin-side shoulder portion 33, the box-side threaded portion 41, the box-side metal seal portion 42, and the box-side shoulder portion 43. That is, in the case where the shoulder plating layer 5 is not formed, the lubricating coating 80 can be directly arranged on the pin-side shoulder portion 33 or the box-side shoulder portion 43. In the case where the non-shoulder plating layer 6 is not formed, the lubricating coating 80 can be directly arranged on at least a portion of the pin-side threaded portion 31, the pin-side metal seal portion 32, the box-side threaded portion 41, and the box-side metal seal portion 42. The lubricating coating 80 can also be arranged as the outermost layer on all of the pin-side threaded portion 31, the pin-side metal seal portion 32, and the pin-side shoulder portion 33. The lubricating coating 80 may be disposed as the outermost layer on all of the box-side threaded portions 41, the box-side metal seal portion 42, and the box-side shoulder portion 43. When the pipe threaded joint includes the lubricating coating 80 as the outermost layer, the lubricity of the pipe threaded joint is improved.
[0120] The lubricating coating 80 is in a liquid or semi-solid state. Liquid refers to a state having a certain volume but not a certain shape. Semi-solid refers to a state that loses fluidity in a static state but can gain fluidity when subjected to external forces (pressure and heat, etc.). Liquid or semi-solid states include highly viscous bodies such as grease. The lubricating coating 80 can use a known lubricant. The lubricating coating 80 contains, for example, lubricating particles, alkaline aromatic organic acid metal salts, rosin, metal soaps and waxes. The lubricating coating 80 may also contain solvents and other components as needed.
[0121] The lubricating particles are not particularly limited as long as they are particles having lubricity. The lubricating particles are selected, for example, from graphite, MoS2 (molybdenum disulfide), WS2 (tungsten disulfide), BN (boron nitride), PTFE (polytetrafluoroethylene), CF x One or more of the group consisting of graphite fluoride and CaCO 3 (calcium carbonate). The content of the lubricating particles is, for example, 1 to 20% when the sum of all components of the lubricating film 80 excluding the solvent is 100%.
[0122] The basic aromatic organic acid metal salt is a salt composed of an aromatic organic acid and an excess of a base (alkali metal or alkaline earth metal). The content of the basic aromatic organic acid metal salt is, for example, 40 to 90% when the sum of all components of the lubricating coating 80 excluding the solvent is 100%.
[0123] Rosin is made from C 20 H 30 The natural resin mainly composed of rosin acid represented by O2. The content of rosin is, for example, 5 to 30% when the sum of all components of the lubricating film 80 excluding the solvent is set to 100%. Metal soap is a metal salt of a fatty acid. The content of metal soap is, for example, 2 to 30% when the sum of all components of the lubricating film 80 excluding the solvent is set to 100%. Wax is an organic substance that is solid at room temperature and becomes liquid when heated. The content of wax is, for example, 2 to 30% when the sum of all components of the lubricating film 80 excluding the solvent is set to 100%.
[0124] Lubricating film 80 may contain a solvent such as water or an organic solvent. Lubricating film 80 may contain a known rust-proofing additive, corrosion inhibitor, coloring pigment, etc. in a total amount of 10% or less.
[0125] A commercially available lubricant may be used for the lubricating coating 80. An example of a commercially available lubricant is SEAL-GUARD ECF manufactured by JET-LUBE Co., Ltd. The chemical composition of the lubricating coating 80 formed on the male buckle portion 3 may be the same as or different from the chemical composition of the lubricating coating 80 formed on the female buckle portion 4.
[0126] The thickness of the lubricating film 80 is not particularly limited. The thickness of the lubricating film 80 is, for example, 10 to 300 μm. When the thickness of the lubricating film 80 is 10 μm or more, the lubricity of the pipe threaded joint is stably improved. Even if the thickness of the lubricating film 80 exceeds 300 μm, the excess lubricating film 80 is removed when tightening the thread, so the above effect is saturated.
[0127] The thickness of the lubricating coating 80 can be measured by the following method. Prepare a male buckle portion 3 or a female buckle portion 4 having a lubricating coating 80. Wipe any measuring position (area: 5 mm×20 mm) of the lubricating coating 80 with cotton wool soaked in ethanol. Calculate the amount (g) of the lubricating coating 80 based on the difference between the weight of the cotton wool before wiping and the weight of the cotton wool after wiping. Calculate the amount (g) of the lubricating coating 80 based on the amount (g) of the lubricating coating 80 and the density (g / cm 3 ) and the area of the measurement position, the average thickness of the lubricating film 80 is calculated and taken as the thickness (μm) of the lubricating film 80.
[0128] [Base material of pipe threaded joints]
[0129] The chemical composition of the base material of the pipe threaded joint of the present embodiment is not particularly limited. The base material is, for example, carbon steel, stainless steel, and alloy steel. Among alloy steels, high alloy steels such as duplex stainless steel and Ni alloy containing alloy elements such as Cr, Ni, and Mo have high corrosion resistance. Therefore, when these high alloy steels are used in the base material, the corrosion resistance of the pipe threaded joint is improved.
[0130] [Manufacturing method]
[0131] The pipe threaded joint of the present embodiment can be manufactured, for example, by the following method. The manufacturing method includes a coating forming step. In the coating forming step, a high friction coefficient coating 50 and a low friction coefficient coating 60 are formed. The high friction coefficient coating 50 and the low friction coefficient coating 60 can be manufactured, for example, by a masking method or a brush plating method. Hereinafter, as an example, a manufacturing method for forming a Zn-Ni alloy coating as the high friction coefficient coating 50 and a Cu coating as the low friction coefficient coating 60 will be described.
[0132] [Plating layer forming process]
[0133] When the threaded joint for pipes of the present embodiment is manufactured by the masking method, the manufacturing can be carried out in the following order. Below, in order to specifically explain the plating formation process, the Cu plating is formed on the pin side threaded portion 31, the pin side metal seal portion 32, the box side threaded portion 41 and the box side metal seal portion 42, and the Zn-Ni alloy plating is formed on the pin side shoulder portion 33 and the box side shoulder portion 43. First, two plating solutions are prepared. The two plating solutions are, for example, a plating solution for forming a Zn-Ni alloy plating layer and a plating solution for forming a Cu plating layer. The plating solution for forming a Zn-Ni alloy plating layer contains zinc ions and nickel ions. The concentration of the metal ions is, for example, zinc ions: 1 to 100 g / L, nickel ions: 1 to 150 g / L. For example, a commercially available plating bath can be used for the plating solution for forming a Cu plating layer. For example, the plating solution for forming a Cu plating layer is DAIN COPPER LS-001 manufactured by Yamato Chemical Industry Co., Ltd. (trade name).
[0134] Then, the pin part 3 and / or the female part 4 are immersed in a plating solution for forming a Cu plating layer. Specifically, the pin part 3 and the female part 4 are energized to form a Cu plating layer on the pin side shoulder 33, the pin side metal seal 32, the pin side thread 31, the female side shoulder 43, the female side metal seal 42 and the female side thread 41. The conditions for electroplating can be set appropriately. The conditions for electroplating are, for example, a plating solution pH of 1 to 10, a plating solution temperature of 10 to 60°C, and a current density of 1 to 100 A / dm 2 , and treatment time: 0.1 to 250 minutes. Thus, a Cu plating layer corresponding to the low friction coefficient plating layer 60 is formed on the entire surface of the male buckle part 3 and / or the entire surface of the female buckle part 4 .
[0135] Next, masking is performed on the pin buckle side metal seal 32 and the pin buckle side threaded portion 31, and / or the box buckle side metal seal 42 and the box buckle side threaded portion 41, which are formed with a Cu plating layer equivalent to the low friction coefficient plating layer 60. Masking can be implemented by a known method. Specifically, masking can be performed by attaching an aluminum tape to the pin buckle side metal seal 32, the pin buckle side threaded portion 31, the box buckle side metal seal 42 and the box buckle side threaded portion 41, or by covering with a caulking agent.
[0136] The masked pin part 3 and / or the masked female part 4 are immersed in a plating solution for forming a Zn-Ni alloy plating layer. Specifically, the pin part 3 and / or the female part 4 are energized to form a Zn-Ni alloy plating layer. The metal sealing part 32 on the pin part side, the threaded part 31 on the pin part side, the metal sealing part 42 on the female part side and the threaded part 41 on the female part side have been masked, so the Zn-Ni alloy plating layer is formed only on the unmasked pin part side shoulder part 33 and the female part side shoulder part 43. The conditions for electroplating can be set appropriately. The conditions for electroplating are, for example, a plating solution pH of 1 to 10, a plating solution temperature of 10 to 60°C, and a current density of 1 to 100 A / dm 2 , and treatment time: 0.1 to 250 minutes. Thus, a Zn-Ni alloy plating layer equivalent to the high friction coefficient plating layer 50 is formed on the pin side shoulder portion 33 and / or the box side shoulder portion 43. Finally, the masking is removed from the pin side metal seal portion 32 and the pin side thread portion 31, and / or the box side metal seal portion 42 and the box side thread portion 41.
[0137] When the threaded joint for pipes of the present embodiment is manufactured by the brush method, the manufacturing process can be performed in the following order. First, two plating solutions are prepared in the same manner as in the above-mentioned masking method. The two plating solutions are, for example, a plating solution for forming a Cu plating layer and a plating solution for forming a Zn-Ni alloy plating layer.
[0138] Then, in the same manner as the above-mentioned masking method, a Cu plating layer is formed on the pin buckle side shoulder portion 33, the pin buckle side metal sealing portion 32 and the pin buckle side threaded portion 31, and / or the box buckle side shoulder portion 43, the box buckle side metal sealing portion 42 and the box buckle side threaded portion 41.
[0139] Next, prepare a brush with absorbent cotton wound around the electrode. Immerse the absorbent cotton in the plating solution for forming the Zn-Ni alloy plating layer so that the absorbent cotton contains the plating solution. Make the absorbent cotton containing the plating solution contact the male buckle side shoulder 33 and / or the female buckle side shoulder 43 and pass electricity. Thereby, a Zn-Ni alloy plating layer can be formed on the male buckle side shoulder 33 and / or the female buckle side shoulder 43. The conditions for electroplating can be set appropriately. The conditions for electroplating are, for example, plating solution pH: 1 to 10, plating solution temperature: 10 to 60°C, current density: 1 to 100 A / dm 2 , and treatment time: 0.1 to 200 minutes. Thus, a Zn—Ni alloy plating layer corresponding to the high friction coefficient plating layer 50 is formed on the pin side shoulder portion 33 and / or the box side shoulder portion 43 .
[0140] After forming each plating layer, it can also be washed with water and dried as needed. In the case of forming the optional plating layer 70, before forming the Cu plating layer, the male buckle part 3 or the female buckle part 4 is immersed in a plating solution for forming the optional plating layer 70, thereby forming the optional plating layer 70. The conditions for forming the optional plating layer 70 can be appropriately set.
[0141] Through the above steps, the threaded joint for pipes of the present embodiment can be manufactured. It should be noted that, in the description of the above manufacturing method, the case where a Zn-Ni alloy plating layer is formed as the high friction coefficient plating layer 50 and a Cu plating layer is formed as the low friction coefficient plating layer 60 is described, but different plating layers may be formed as the high friction coefficient plating layer 50 and the low friction coefficient plating layer 60. In this case, the manufacturing method may be performed in the same manner as the above manufacturing method using a plating bath containing metal ions contained in the plating layer to be formed.
[0142] [Lubricating film forming process]
[0143] A lubricating film forming step may be performed after forming the above-mentioned plating layer. In the lubricating film forming step, a lubricating film 80 is formed as an outermost layer on at least a portion of the pin side shoulder portion 33, the pin side metal seal portion 32, the pin side thread portion 31, the box side shoulder portion 43, the box side metal seal portion 42, and the box side thread portion 41.
[0144] By applying a composition containing the above-mentioned components on at least a portion of the above-mentioned pin buckle side shoulder portion 33, the pin buckle side metal seal portion 32, the pin buckle side threaded portion 31, the female buckle side shoulder portion 43, the female buckle side metal seal portion 42 and the female buckle side threaded portion 41, a lubricating coating 80 can be formed. The coating method is not particularly limited. The coating method is, for example, spraying, brushing and dipping. In the case of spraying, the composition containing the above-mentioned components can be heated and sprayed in a state where fluidity is improved. The lubricating coating forming process can be implemented on both the pin buckle portion 3 and the female buckle portion 4, or it can be implemented on only one of them.
[0145] [Substrate treatment process]
[0146] The above-mentioned manufacturing method can also be provided with a substrate treatment process before the coating forming process as required. The substrate treatment process is, for example, pickling and alkali degreasing. In the substrate treatment process, the oil content attached to the contact surface is cleaned. The substrate treatment process can further include grinding processes such as sandblasting and mechanical fine grinding. These substrate treatments can be implemented only one, or multiple substrate treatments can be implemented in combination.
[0147] Example
[0148] The following is an explanation of Examples. % in the Examples represents mass %.
[0149] [Plating layer forming process]
[0150] Various coatings were formed on the surface of a carbon steel plate, and the friction coefficient was measured. The steel plate used was SPCC (JIS G3141 (2017)) manufactured by PALTEK Co., Ltd. The composition of the steel plate was C ≤ 0.15%, Mn ≤ 0.60%, P ≤ 0.100%, and S ≤ 0.050%. The coating was formed on the surface of the steel plate under the following conditions.
[0151] Ni-P alloy plating
[0152] A Ni-P alloy plating layer with a thickness of 10 μm was formed on the surface of the steel sheet using SEK797 plating solution manufactured by Japan Kanigen Co., Ltd. (trade name). The plating conditions were plating solution temperature: 90°C, treatment time: 40 minutes (chemical plating). The Ni-P alloy plating layer had a chemical composition of P: 5-15 mass %, and the balance: Ni and impurities.
[0153] Zn-Ni alloy coating
[0154] A Zn-Ni alloy plating layer with a thickness of 10 μm was formed on the surface of the steel sheet using a plating solution DAIN ZINALLOY N-PL manufactured by Yamato Kasei Co., Ltd. (trade name). The plating conditions were a plating solution temperature of 35°C and a current density of 4 A / dm 2 , and treatment time: 15 minutes. The Zn-Ni alloy plating layer has a chemical composition of Ni: 10-20 mass %, and the balance: Zn and impurities.
[0155] Cu plating
[0156] A plating solution prepared with commercially available reagents was used to form a 10 μm thick Cu plating layer on the surface of the steel sheet. The plating solution contained 200 g / L of copper sulfate pentahydrate and 50 g / L of sulfuric acid. The plating conditions were a plating solution temperature of 35°C and a current density of 10 A / dm 2 , and treatment time: 5 minutes. The Cu plating layer has a chemical composition of Cu: 99 mass % or more, and the balance: impurities.
[0157] Zn coating
[0158] A plating solution prepared with commercially available reagents was used to form a Zn coating with a thickness of 10 μm on the surface of the steel sheet. The plating solution contained 350 g / L zinc sulfate heptahydrate and 75 g / L sodium sulfate, with a pH of 2. The plating conditions were a plating solution temperature of 50°C and a current density of 10 A / dm 2 , and treatment time: 4 minutes. The Zn plating layer has a chemical composition of Zn: 99 mass % or more, and the balance: impurities.
[0159] Cu-Sn-Zn alloy coating
[0160] A Cu-Sn-Zn alloy plating layer with a thickness of 10 μm was formed on the surface of the steel sheet using a plating bath manufactured by Nippon Chemical Industry Co., Ltd. The plating conditions were as follows: plating bath pH: 14, plating bath temperature: 45°C, current density: 2 A / dm 2 And the treatment time: 40 minutes. The Cu-Sn-Zn alloy plating layer has a chemical composition of Sn: 40 mass %, Zn: 7 mass %, and the balance: Cu and impurities.
[0161] Cr coating
[0162] A 10 μm thick Cr plating layer was formed on the steel sheet surface using a Chromium plating solution manufactured by SIFCO Industries. The plating conditions were as follows: plating solution temperature: 40°C, current density: 30 A / dm 2 , and treatment time: 30 minutes. The Cr plating layer has a chemical composition of Cr: 95 mass % or more, and the balance: impurities.
[0163] [Friction coefficient measurement test]
[0164] A Bowden sliding test was performed on the steel plates formed with each coating, and the friction coefficient of each coating was measured. The Bowden sliding test was performed under the following conditions. Sliding pressure head: 3 / 16" (diameter 4.7625mm) steel ball (Fe, steel type SUJ2), pressing load: 3kgf, sliding form: linear reciprocating sliding, sliding amplitude: 30mm, number of sliding reciprocating times: 5 times, sliding speed: 4mm / second, test temperature: 25°C, lubricating oil: SEAL-GUARD ECF manufactured by JET-LUBE Co., Ltd. (trade name), lubricating oil coating amount: 40g / m 2 The arithmetic mean of the friction coefficients obtained by sliding back and forth five times was taken as the friction coefficient of each plating layer. The friction coefficients of each plating layer are shown in Table 1.
[0165] [Table 1]
[0166] Table 1
[0167] Types of plating Friction coefficient Ni-P alloy plating 0.135 Zn-Ni alloy coating 0.134 Cu plating 0.121 Cr coating 0.116 Cu-Sn-Zn alloy coating 0.115 Zn coating 0.105
[0168] [FEM analysis]
[0169] According to the results in Table 1, the shoulder torque, yield torque, and delta torque when each plating layer is formed in the pipe threaded joint are subjected to FEM analysis. The pipe threaded joint uses VAM21HT (trade name) manufactured by Nippon Steel Corporation, size: 9-5 / 8" 53.5#. FEM analysis was performed under the conditions that no plating is formed on the box side (the box side is ground, and the surface of the box side is Fe) and only the plating is formed on the pin side. Test No. 7 is an example in which a Cu plating layer is formed on the entire surface, which is equivalent to the existing example. The results are shown in Table 2.
[0170] [Table 2]
[0171] Table 2
[0172]
[0173] In Table 2, the column "Analysis Value" shows the torque values (ft.lbs) obtained by FEM analysis. In Table 2, the column "Increase / Decrease Rate" shows the increase / decrease rate (%) based on the value of the conventional example (Cu plating is formed on the entire surface of the pin side) of test number 7. In Table 2, Ts represents shoulder torque, Ty represents yield torque, and ΔT represents delta torque.
[0174] [Evaluation results]
[0175] Referring to Tables 1 and 2, in Test No. 1 and Test No. 2, in which a high friction coefficient plating layer is formed on the shoulder portion and a low friction coefficient plating layer is formed on the thread portion and the metal seal portion, each torque value is improved. Specifically, in Test No. 1 and Test No. 2, although the shoulder torque does not change compared with Test No. 7 (conventional example), the yield torque is higher than that of Test No. 7. In addition, the delta torque is also increased compared with Test No. 7 (conventional example).
[0176] On the other hand, in test numbers 3 and 4 in which a high-friction-coefficient plating is formed not only on the shoulder portion but also on the metal sealing portion, although the yield torque is higher than that of test number 7 (existing example), the shoulder torque is also higher than that of test number 7 (existing example).
[0177] In Test No. 5 and Test No. 6, in which a plating layer with a high friction coefficient is formed on the threaded portion and a plating layer with a low friction coefficient is formed on the metal seal portion and the shoulder portion, the shoulder torque is lower than that of Test No. 7 (conventional example), but the yield torque is also lower than that of Test No. 7 (conventional example). In addition, in Test No. 5 and Test No. 6, the delta torque is also lower than that of Test No. 7 (conventional example).
[0178] In test numbers 8 and 9, in which the threaded portion, metal seal portion, and shoulder portion were plated with a higher friction coefficient than conventional Cu plating, the yield torque was higher than that of test number 7 (conventional example), but the shoulder torque was also higher than that of test number 7 (conventional example).
[0179] The embodiments of the present invention have been described above. However, the above embodiments are merely examples for implementing the present invention. Therefore, the present invention is not limited to the above embodiments, and the above embodiments may be appropriately modified and implemented without departing from the gist thereof.
[0180] Description of Reference Numerals
[0181] 1 Steel pipe
[0182] 2 Coupling
[0183] 3. Male buckle
[0184] 31 Pin side thread
[0185] 32 Metal seal on the male side
[0186] 33 Male side shoulder
[0187] 4 Female buckle
[0188] 41 Threaded part on the box side
[0189] 42 Metal seal part on the female buckle side
[0190] 43 Female buckle side shoulder
[0191] 5 Shoulder plating
[0192] 50 High friction coefficient coating
[0193] 6 Non-shoulder coating
[0194] 60 Low friction coating
[0195] 70 Any coating
[0196] 80 Lubricating film
Claims
1. A pipe threaded joint, comprising: A pin buckle portion, comprising a pin buckle side threaded portion, a pin buckle side metal sealing portion and a pin buckle side shoulder portion; A box portion, comprising a box portion side threaded portion, a box portion side metal sealing portion and a box portion side shoulder portion; The shoulder coating comprises one or more layers, the outermost layer being a high friction coefficient coating; and The non-shoulder coating comprises one or more layers, the outermost layer being a low friction coefficient coating having a lower friction coefficient than the high friction coefficient coating, The shoulder plating layer is arranged on the shoulder of the male buckle side. The non-shoulder plating layer is arranged on the threaded portion on the pin side and on the metal sealing portion on the pin side, and / or, The shoulder plating layer is arranged on the shoulder of the female buckle part. The non-shoulder portion plating layer is disposed on the box portion side threaded portion and on the box portion side metal seal portion.
2. The threaded joint for pipes according to claim 1, wherein: The thickness of the shoulder coating is 1 to 50 μm. The thickness of the non-shoulder coating is 1-50 μm.
3. The threaded joint for pipes according to claim 1, wherein: The pipe threaded joint further comprises a liquid or semi-solid lubricating coating as an outermost layer on at least a portion of the pin-side threaded portion, the pin-side metal sealing portion, the pin-side shoulder portion, the box-side threaded portion, the box-side metal sealing portion, and the box-side shoulder portion.
4. The threaded joint for pipes according to claim 2, wherein: The pipe threaded joint further comprises a liquid or semi-solid lubricating coating as an outermost layer on at least a portion of the pin-side threaded portion, the pin-side metal sealing portion, the pin-side shoulder portion, the box-side threaded portion, the box-side metal sealing portion, and the box-side shoulder portion.
5. The threaded joint for pipes according to any one of claims 1 to 4, wherein: The high friction coefficient coating is selected from the group consisting of a Ni-P alloy coating, a Zn-Ni alloy coating, a Cu coating, a Cr coating and a Cu-Sn-Zn alloy coating, The low friction coefficient plating layer is selected from the group consisting of a Zn-Ni alloy plating layer, a Cu plating layer, a Cr plating layer, a Cu-Sn-Zn alloy plating layer and a Zn plating layer.
6. The threaded joint for pipes according to claim 5, wherein: The high friction coefficient coating is selected from the group consisting of a Ni-P alloy coating and a Zn-Ni alloy coating, The low friction coefficient plating layer is selected from the group consisting of a Cu plating layer, a Cr plating layer, a Cu-Sn-Zn alloy plating layer and a Zn plating layer.