A kind of polyvinylidene fluoride hollow fiber membrane with mesh pore structure and preparation method thereof

By adding ultra-high molecular weight polymer to polyvinylidene fluoride and using thermal phase separation method, the problem of high temperature and dense structure in the preparation of porous polyvinylidene fluoride films in the prior art was solved, and excellent mechanical properties were successfully prepared and high water flux mesh pore structure membrane.

CN113648844BActive Publication Date: 2024-11-19GUIZHOU MATERIAL IND TECH INSTITUE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202110979026.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-25
Publication Date
2024-11-19
Estimated Expiration
2041-08-25

AI Technical Summary

Technical Problem

In the prior art, when preparing polyvinylidene fluoride porous membranes, it is difficult to obtain a membrane with a thin cortex and a support layer that penetrates the mesh pore structure at low temperatures, and the preparation conditions are harsh, which affects the flux and mechanical properties of the membrane.

Method used

By mixing a small amount of ultra-high molecular weight polyvinylidene fluoride with ordinary molecular weight polyvinylidene fluoride, and using the thermo-phase separation method, a thin cortex, good surface pore properties, and a mesh pore structure was prepared with a mesh pore structure using the S-L phase separation method. PVDF hollow fiber membrane avoids dense structures caused by diluent extraction and polymer crystallization under high temperature conditions.

Benefits of technology

It has achieved the preparation of a mesh pore structure polyvinylidene fluoride hollow fiber membrane with excellent chemical stability, excellent mechanical properties and high water flux at low temperatures, which simplifies the process flow and improves the mechanical strength and permeability of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113648844B_ABST
    Figure CN113648844B_ABST
Patent Text Reader

Abstract

The present invention discloses a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure and a preparation method thereof, the preparation method comprising: mixing ordinary molecular weight polyvinylidene fluoride, an additive, and a diluent under heating conditions to obtain a casting solution; after the casting solution is extruded through a spinneret, it is cooled, wound, extracted, dried, and then separated by solid-liquid phase to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure; wherein the additive is ultra-high molecular weight polyvinylidene fluoride. The present invention mixes a small amount of ultra-high molecular weight polyvinylidene fluoride as an additive with ordinary molecular weight polyvinylidene fluoride, and a microporous membrane with a thin and porous skin layer and a supporting layer with a through mesh pore structure can be obtained with a single diluent at a temperature lower than the melting temperature of the polymer, which has the characteristics of simple process, low temperature requirement, easy control of processing and molding, etc. The obtained hollow fiber membrane has excellent chemical stability, excellent mechanical properties, and high water flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of separation membrane preparation, and specifically relates to a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure and a preparation method thereof. Background Art

[0002] Polyvinylidene fluoride (PVDF) is a highly polar crystalline polymer material. Due to its excellent properties in weather resistance, heat resistance and mechanical properties, it is widely used as a separation membrane material in water treatment, membrane contactors and medical tissue engineering. Non-solvent-induced phase separation and thermal-induced phase separation are currently the most commonly used techniques for preparing porous membranes. Compared with non-solvent-induced phase separation technology, thermal-induced phase separation technology has the advantages of easy control of pore structure, high membrane mechanical properties, and membrane storage in a dry state. It is particularly suitable for the preparation of polymer porous membranes without solvents at room temperature. This method has been used to prepare polyvinylidene fluoride porous membranes for water treatment.

[0003] Thermally induced phase separation technology is a method for preparing microporous membranes by changing temperature to cause phase separation proposed by Castro in the 1980s (US Patent, 4247498, 1981). This technology is to form a homogeneous solution of a polymer and a specific diluent at high temperature. The diluent is a good solvent for the polymer at high temperature and a non-solvent for the polymer at low temperature. When the temperature is lowered, the solution undergoes solid-liquid (SL) or liquid-liquid (LL) phase separation. After the diluent is extracted from the membrane, the space occupied by the diluent in the system forms micropores, and a membrane material containing a microporous structure is obtained. The ideal structure of a separation membrane is a thin skin layer and a through-mesh pore structure of the support layer. In order to obtain a mesh pore structure when LL phase separation occurs, a binary mixed diluent system is usually required to make the interaction between the polymer and the mixed diluent moderate, form a bicontinuous polymer-poor phase and a polymer-rich phase during the cooling process, and form a relatively interconnected mesh pore structure after the diluent is extracted. However, the preparation conditions are very demanding, such as the need to strictly measure the mass ratio of the diluent to the non-diluent, the temperature for forming the solution is high (220°C, about 50°C higher than the melting temperature of the polymer), and the control is difficult. At this temperature, the polymer is prone to degradation. The SL phase separation has a low temperature requirement and is easy to operate. However, the direct crystallization of the polymer during the SL phase separation process will form a structure with a thick and dense cortex and a spherical support layer. The dense and thick cortex increases the filtration resistance of the membrane, and even makes the membrane almost have no flux, which cannot meet the requirements of industrial applications. Almost all the single diluents found so far can only form a SL phase separation system with PVDF.

[0004] Ultra-high molecular weight polyvinylidene fluoride has the characteristics of high molecular weight, long chain segment, high viscosity, slow molecular motion speed, etc., which can affect the crystallization process of the polymer and can be mixed with other polymers for final applications and products. At present, there is a film-making method of blending ultra-high molecular weight polyethylene and polyvinylidene fluoride (Li Nana et al., Enhanced ultra-high molecular weight polyethylene and polyvinylidene fluoride binary blend film and preparation method thereof, CN 106492645 A, 2016), but due to the incompatibility of the two polymers and the different cooling shrinkage rates, the blend film has solid-solid phase separation interface holes during the cooling process, which has a direct impact on the membrane pore structure and membrane strength. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] One of the purposes of the present invention is to provide a method for preparing a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure. A microporous membrane with a thin and porous skin and a supporting layer with a through mesh pore structure can be obtained by using a single diluent at a temperature lower than the melting temperature of the polymer. The method has the characteristics of simple process, low temperature requirement, and easy control of processing and molding. The prepared hollow fiber membrane has excellent chemical stability, excellent mechanical properties, and high water flux, thereby overcoming the shortcomings of the prior art.

[0008] The present invention mixes a small amount of ultra-high molecular weight polyvinylidene fluoride as an additive with polyvinylidene fluoride of ordinary molecular weight. The system prepares a PVDF hollow fiber membrane with a thin skin, good surface porosity and a support layer with a mesh pore structure through SL phase separation of a thermally induced phase separation method. The method avoids the thick skin and spherical particle structure formed by the SL phase separation membrane and the disadvantages of harsh preparation conditions and high temperature of LL phase separation. At the same time, the advantages of low temperature requirement for SL phase separation and through mesh pore structure formed by LL phase separation are achieved.

[0009] In order to achieve the above-mentioned object of the present invention, the present invention provides the following technical solution: a method for preparing a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure, characterized in that: comprising:

[0010] The casting solution is obtained by mixing polyvinylidene fluoride of normal molecular weight, additives, and diluent under heating conditions;

[0011] The casting solution is extruded through a spinneret, cooled, wound, extracted, dried, and then separated into solid and liquid phases to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure;

[0012] Wherein, the additive is ultra-high molecular weight polyvinylidene fluoride.

[0013] As a preferred solution of the method for preparing the PVDF hollow fiber membrane with a mesh pore structure of the present invention, the weight average molecular weight of the ultra-high molecular weight PVDF is not less than 1 million, and the weight average molecular weight of the ordinary molecular weight PVDF is 100,000 to 700,000.

[0014] As a preferred embodiment of the method for preparing the PVDF hollow fiber membrane with a mesh pore structure of the present invention, the casting solution comprises, by weight, 2 to 10 parts of ultrahigh molecular weight PVDF, 15 to 40 parts of ordinary molecular weight PVDF and 50 to 83 parts of diluent.

[0015] As a preferred embodiment of the method for preparing the reticular pore structure polyvinylidene fluoride hollow fiber membrane of the present invention, the diluent includes one or more of dibutyl phthalate, dibutyl sebacate, acetyl tributyl citrate, tributyl citrate, propylene carbonate, and γ-butyrolactone.

[0016] As a preferred solution of the method for preparing the hollow fiber membrane of polyvinylidene fluoride with a mesh pore structure of the present invention, wherein: the mixing is carried out under heating conditions, and the heating temperature is lower than the melting temperature of polyvinylidene fluoride with ordinary molecular weight.

[0017] As a preferred solution of the method for preparing the polyvinylidene fluoride hollow fiber membrane with a mesh pore structure of the present invention, the heating temperature is 150-170°C.

[0018] As a preferred solution of the method for preparing the PVDF hollow fiber membrane with a mesh pore structure of the present invention, the core liquid used in extruding the casting liquid through a spinneret to form the inner cavity of the hollow fiber is one of a diluent and nitrogen.

[0019] As a preferred solution of the method for preparing the PVDF hollow fiber membrane with a mesh pore structure of the present invention, wherein: the core liquid temperature is 60-100°C and / or the core liquid flow rate is 0.01-0.1 L / min during the extrusion through a spinneret.

[0020] As a preferred solution of the method for preparing the PVDF hollow fiber membrane with a mesh pore structure of the present invention, wherein: the cooling liquid is deionized water at 25°C; and / or the extraction agent is ethanol with a purity of not less than 99%.

[0021] Another object of the present invention is to provide a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure obtained by the preparation method as described above, wherein the obtained polyvinylidene fluoride hollow fiber membrane with a mesh pore structure has high strength, good membrane pore permeability and excellent permeability.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) Compared with other methods of adding complex multi-component mixed diluent systems, only a single diluent can be used at a relatively low temperature (not higher than the melting temperature of the polymer) to obtain an ideal thin skin layer with a high surface porosity and a support layer with mesh pores. The temperature control requirements are low and no antioxidant needs to be added. Therefore, the process is simple and convenient for actual production;

[0024] (2) Compared with the preparation of hollow fiber membranes composited with ultra-high molecular weight polyethylene and polyvinylidene fluoride, only the same polymer with different molecular weights needs to be added, so the compatibility of the system is better, avoiding the occurrence of macroscopic phase separation and interface defect holes during the cooling process due to the poor compatibility of the two polymers, and the membrane has higher retention accuracy and better mechanical properties;

[0025] (3) Compared with the thick and dense spherical particle structure hollow fiber membrane prepared by SL phase separation of simple ordinary molecular weight polyvinylidene fluoride, the membrane prepared by the present invention forms a structure with a thin skin layer and many openings and a support layer with through-mesh pores by significantly hindering polymer crystallization. Therefore, the mechanical strength of the membrane is higher, it is not easy to break the wire and cause leakage during use, and the permeability performance is better. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0027] Figure 1 The following are scanning electron microscope images of the hollow fiber membrane prepared in Example 1 of the present invention; wherein (a) is a SEM image of a cross section of the polyvinylidene fluoride microporous membrane close to the outer skin layer, and (b) is a SEM image of a cross section of the support layer of the polyvinylidene fluoride microporous membrane;

[0028] Figure 2 The figures are scanning electron microscope images of the hollow fiber membrane prepared in Comparative Example 1 of the present invention; wherein (a) is a SEM image of the cross section of the microporous membrane close to the outer skin layer, and (b) is a SEM image of the support layer of the cross section of the microporous membrane. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and those skilled in the art can make similar promotions without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below. If specific conditions are not indicated in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0031] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0032] In view of the problems of poor porosity, thick and dense skin and low flux in conventional solid-liquid phase separation membranes in the prior art, the present invention provides a method for preparing a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure to solve the technical problems existing in existing products.

[0033] Specifically, the present invention mixes a small amount of ultra-high molecular weight polyvinylidene fluoride as an additive with polyvinylidene fluoride of ordinary molecular weight, and the system is prepared by SL phase separation of thermally induced phase separation to obtain a PVDF hollow fiber membrane with a thin skin layer, good surface porosity, and a support layer with a mesh pore structure. It avoids the thick skin layer and spherical particle structure formed by the SL phase separation membrane, and also avoids the disadvantages of harsh preparation conditions and high temperature of LL phase separation. At the same time, it achieves the advantages of low SL phase separation temperature requirement and LL phase separation to form a through mesh pore structure. The preparation method thereof can be referred to as follows:

[0034] The casting solution is obtained by mixing polyvinylidene fluoride of normal molecular weight, additives, and diluent under heating conditions;

[0035] The casting solution is extruded through a spinneret, cooled, wound, extracted, dried, and then separated into solid and liquid phases to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure;

[0036] Wherein, the additive is ultra-high molecular weight polyvinylidene fluoride.

[0037] It should be noted that the weight average molecular weight of the ultra-high molecular weight polyvinylidene fluoride is not less than 1 million, for example, it can be, but not limited to, 1.2 million, 1.3 million, 1.5 million or 2 million, and the weight average molecular weight of the normal molecular weight polyvinylidene fluoride is 100,000 to 700,000, for example, it can be, but not limited to, 100,000, 300,000, 500,000 or 700,000.

[0038] Specifically, the casting solution contains 2 to 10 parts by mass of ultra-high molecular weight polyvinylidene fluoride, for example, but not limited to 2, 3, 4, 5, 6, 7, 8, 9 or 10 parts, etc.; 15 to 40 parts by mass of ordinary molecular weight polyvinylidene fluoride, for example, but not limited to 15, 20, 25, 30, 35 or 40 parts, etc.; and 50 to 83 parts of diluent, for example, but not limited to 50, 57, 63, 72, 78 or 83 parts, etc.

[0039] In the above reaction steps, the diluent includes one or more of dibutyl phthalate, dibutyl sebacate, acetyl tributyl citrate, tributyl citrate, propylene carbonate, and γ-butyrolactone.

[0040] In the above reaction steps, the mixing is carried out under heating conditions, and the heating temperature is lower than the melting point of ordinary molecular weight polyvinylidene fluoride; specifically, the heating temperature is 150-170°C, for example, it can be, but not limited to, 150, 155, 160, 165 or 170°C.

[0041] In the above reaction steps, the casting liquid is extruded through a spinneret, and the casting liquid and the heated core liquid are extruded through the spinneret, and the core liquid is one of a diluent or nitrogen; specifically, the core liquid temperature is 60 to 100°C, for example, it can be, but not limited to, 60, 70, 80, 90 or 100°C; and / or the core liquid flow rate is 0.01 to 0.1 L / min, for example, it can be, but not limited to, 0.01, 0.03, 0.05, 0.08 or 0.1 L / min, etc.

[0042] In the above reaction steps, the cooling liquid is deionized water at 25° C.; and / or, the extraction agent is ethanol with a purity of not less than 99%.

[0043] The polyvinylidene fluoride hollow fiber membrane with a mesh pore structure prepared by any of the above methods has the advantages of high strength, good membrane pore penetration, excellent permeability, etc.

[0044] Example 1

[0045] (1) ultra-high molecular weight polyvinylidene fluoride (molecular weight 1.3 million) / normal molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (dibutyl phthalate) were added into a reaction kettle at a mass ratio of 6 / 20 / 74, mixed and stirred at 170° C. for 3 h, and then vacuum degassed for 3 h to obtain a uniform casting solution;

[0046] (2) A diluent (dibutyl phthalate) was used as the core liquid, the core liquid temperature was 80°C, the core liquid flow rate was 0.03 L / min, and the casting liquid was measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it was immersed in a 25°C coagulation bath (deionized water) for cooling and forming. The membrane filaments were then immersed in anhydrous ethanol for 48 h to extract the residual diluent in the membrane, and then immersed in deionized water for 24 h to remove the residual ethanol. Finally, the membrane filaments were naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure.

[0047] The scanning electron microscope image of the hollow fiber membrane obtained in Example 1 is shown in Figure 1 As shown, it can be seen that the membrane structure has a thin outer skin layer, no inner skin layer, and a mesh pore structure of the supporting layer.

[0048] Water flux test: After the 300mm membrane wire is capped and cast, it is tested with 25℃ pure water at 0.1MPa pressure for 2h. Then the pure water flux per unit area and time is calculated. The average value is taken after five tests. The test results show that the pure water flux is 784L / (m 2 h).

[0049] Breaking strength test: Take a 100mm fiber membrane and perform a tensile test on a universal testing machine at a linear speed of 10mm / s. Record the maximum force when the membrane breaks and take the average value after five tests. The test results show that the breaking strength is 13.5MPa.

[0050] Example 2

[0051] (1) ultra-high molecular weight polyvinylidene fluoride (molecular weight 1.3 million) / normal molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (dibutyl phthalate) were added into a reaction kettle at a mass ratio of 4 / 22 / 74, mixed and stirred at 160° C. for 3 h, and then vacuum degassed for 3 h to obtain a uniform casting solution;

[0052] (2) A diluent (dibutyl phthalate) is used as the core liquid, the core liquid temperature is 80°C, the core liquid flow rate is 0.03 L / min, and the casting liquid is measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it is immersed in a 25°C coagulation bath (deionized water) for cooling and forming. The membrane filaments are then immersed in anhydrous ethanol for 48 hours, and the residual diluent in the membrane is extracted with 99% pure ethanol. The membrane is then immersed in deionized water for 24 hours to remove the residual ethanol. Finally, the membrane filaments are naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure.

[0053] It was determined that the membrane structure obtained in Example 2 had a thin outer skin layer, no inner skin layer, and a support layer with a mesh pore structure. The obtained mesh pore structure polyvinylidene fluoride hollow fiber membrane was subjected to the performance tests described in Example 1. The test results showed that the breaking strength was 11.2 MPa; at 0.1 MPa and 25°C, the pure water flux of the membrane was 836 L / (m 2 h).

[0054] Example 3

[0055] (1) Ultra-high molecular weight polyvinylidene fluoride (molecular weight 1.3 million) / normal molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (tributyl acetyl citrate) were added into a reaction kettle at a mass ratio of 8 / 18 / 74, mixed and stirred at 170° C. for 3 h, and then vacuum degassed for 3 h to obtain a uniform casting solution;

[0056] (2) A diluent (tributyl acetyl citrate) was used as the core liquid, the core liquid temperature was 80°C, the core liquid flow rate was 0.03 L / min, and the casting liquid was measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it was immersed in a 25°C coagulation bath (deionized water) to cool and form. The membrane filaments were then immersed in anhydrous ethanol for 48 h to extract the residual diluent in the membrane, and then immersed in deionized water for 24 h to remove the residual ethanol. Finally, the membrane filaments were naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure.

[0057] The membrane structure obtained in Example 3 was determined to have a thin outer skin layer, no inner skin layer, and a mesh-like pore structure for the support layer. The obtained mesh-like pore structure polyvinylidene fluoride hollow fiber membrane was subjected to the performance tests described in Example 1. The test results showed that the breaking strength was 14.6 MPa; at 0.1 MPa and 25°C, the pure water flux of the membrane was 757 L / (m 2 h).

[0058] Example 4

[0059] (1) Ultra-high molecular weight polyvinylidene fluoride (molecular weight 1.5 million) / normal molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (tributyl acetyl citrate) were added into a reaction kettle at a mass ratio of 4 / 22 / 74, mixed and stirred at 170° C. for 3 h, and then vacuum degassed for 3 h to obtain a uniform casting solution;

[0060] (2) A diluent (tributyl acetyl citrate) was used as the core liquid, the core liquid temperature was 80°C, the core liquid flow rate was 0.03 L / min, and the casting liquid was measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it was immersed in a 25°C coagulation bath (deionized water) to cool and form. The membrane filaments were then immersed in anhydrous ethanol for 48 h to extract the residual diluent in the membrane, and then immersed in deionized water for 24 h to remove the residual ethanol. Finally, the membrane filaments were naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure.

[0061] The membrane structure obtained in Example 4 was determined to have a thin outer skin layer, no inner skin layer, and a support layer with a mesh pore structure. The obtained mesh pore structure polyvinylidene fluoride hollow fiber membrane was subjected to the performance tests described in Example 1. The test results showed that the breaking strength was 12.2 MPa; at 0.1 MPa and 25°C, the pure water flux of the membrane was 824 L / (m 2 h).

[0062] Comparative Example 1

[0063] (1) Adding ordinary molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (dibutyl phthalate) into a reaction kettle at a mass ratio of 26 / 74, mixing and stirring at 160°C for 3 hours, and then vacuum degassing for 3 hours to obtain a uniform casting solution;

[0064] (2) A diluent (dibutyl phthalate) was used as the core liquid, the core liquid temperature was 80°C, the core liquid flow rate was 0.03 L / min, and the casting liquid was measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it was immersed in a 25°C coagulation bath (deionized water) to cool and form. The membrane filaments were then immersed in anhydrous ethanol for 48 h to extract the residual diluent in the membrane, and then immersed in deionized water for 24 h to remove the residual ethanol. Finally, the membrane filaments were naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane.

[0065] The scanning electron microscope image of the hollow fiber membrane obtained in Comparative Example 1 is shown in Figure 2 As shown, it can be seen that the membrane structure obtained in Comparative Example 1 is a thick outer skin layer, no inner skin layer, and a support layer with a spherical particle structure.

[0066] The obtained polyvinylidene fluoride hollow fiber membrane was subjected to the performance tests described in Example 1. The test results showed that the breaking strength was 8.9 MPa; the pure water flux of the membrane was 8 L / (m 2 h).

[0067] Comparative Example 2

[0068] (1) Adding ordinary molecular weight polyvinylidene fluoride (weight average molecular weight 330,000) / diluent (tributyl acetyl citrate) into a reaction kettle at a mass ratio of 26 / 74, mixing and stirring at 160°C for 3 hours, and then vacuum degassing for 3 hours to obtain a uniform casting solution;

[0069] (2) A diluent (tributyl acetyl citrate) was used as the core liquid, the core liquid temperature was 80°C, the core liquid flow rate was 0.03 L / min, and the casting liquid was measured by a spinning pump and continuously extruded from a hollow fiber spinneret at a flow rate of 0.05 L / min. After passing through an air gap of 0.5 cm, it was immersed in a 25°C coagulation bath (deionized water) to cool and form. The membrane filaments were then immersed in anhydrous ethanol for 48 h to extract the residual diluent in the membrane, and then immersed in deionized water for 24 h to remove the residual ethanol. Finally, the membrane filaments were naturally dried to obtain a polyvinylidene fluoride hollow fiber membrane.

[0070] The membrane structure obtained in Comparative Example 2 was determined to have a thick outer skin layer, no inner skin layer, and a spherical particle structure as the support layer. The obtained reticular pore structure polyvinylidene fluoride hollow fiber membrane was subjected to the performance tests described in Example 1. The test results showed that the breaking strength was 8.6 MPa; at 0.1 MPa and 25°C, the pure water flux of the membrane was 11 L / (m 2 h).

[0071] The principle of obtaining a thin skin layer and a mesh-like porous support layer in the present invention is that when only ordinary molecular weight polyvinylidene fluoride is used to prepare a membrane through a thermally induced phase separation method, SL phase separation occurs to form a dense thick skin layer and a spherical particle structure. The main reason is that the membrane preparation temperature is lower than the melting temperature of the polymer. When the casting liquid is reduced to a certain temperature, the polymer directly crystallizes. The molecular chain segments of ordinary molecular weight polyvinylidene fluoride move too fast and the crystallization rate is fast. When it contacts with a quenching agent (water) with strong thermal conductivity, the temperature of the polymer solution drops sharply to form a large temperature gradient, which causes the polymer to crystallize rapidly to form a very thick dense skin layer and a spherical particle structure, so that the membrane has almost no flux.

[0072] Adding a small amount of ultra-high molecular weight polyvinylidene fluoride into the system can increase the viscosity of the casting liquid system, slow down the heat transfer rate, and thus reduce the crystallization rate, and then reduce the skin thickness due to its large molecular weight, long chain segment, poor flexibility, and slow molecular movement speed. On the other hand, ultra-high molecular weight polyvinylidene fluoride and ordinary molecular weight polyvinylidene fluoride are the same substance, so they are very compatible, and the chain segments are entangled, which significantly slows down the chain segment movement speed of ordinary molecular weight polyvinylidene fluoride during the crystallization process, thereby slowing down the crystallization rate, hindering the crystallization process of polyvinylidene fluoride, thereby hindering the formation of spherical particle structure and thick and dense skin, and finally forming a through mesh pore structure surrounded by imperfectly crystallized string crystals or lamellar crystals. Because the molecular weight of ultra-high molecular weight polyvinylidene fluoride is too large, it is not only difficult to process when used alone, but also the polymer solid content cannot be too high, which makes the film shrink severely and almost has no compressive resistance. Therefore, ultra-high molecular weight polyvinylidene fluoride cannot be used alone to make films.

[0073] Compared with other methods of adding complex multi-component mixed diluent systems, the present invention can obtain an ideal thin skin layer and a membrane structure with a high surface porosity and a support layer with mesh holes by using only a single diluent at a relatively low temperature (not higher than the melting temperature of the polymer), and has low requirements for temperature control and no need to add antioxidants, so the process is simple and convenient for actual production; compared with the preparation of a hollow fiber membrane composite of ultra-high molecular weight polyethylene and polyvinylidene fluoride, only the same polymer with different molecular weights needs to be added, so the system has better compatibility, avoiding macroscopic phase separation and interface defect holes in the cooling process due to poor compatibility of the two polymers, and the membrane has higher retention accuracy and better mechanical properties; compared with a thick and dense spherical particle structure hollow fiber membrane prepared by simple ordinary molecular weight polyvinylidene fluoride through SL phase separation, the membrane prepared by the present invention forms a structure with a thin skin layer and many openings and a support layer with through mesh holes by significantly hindering polymer crystallization, so the membrane has higher mechanical strength, is not prone to broken wires and leakage during use, and has better permeability.

[0074] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure, characterized in that: include, By mass fraction, 20 parts of ordinary molecular weight polyvinylidene fluoride, 6 parts of additives, and 74 parts of diluents are mixed under heating conditions to obtain a casting solution; the heating temperature is 150-170° C.; The casting liquid is extruded through a spinneret, cooled, wound, extracted, dried, and then separated into a solid-liquid phase to obtain a polyvinylidene fluoride hollow fiber membrane with a mesh pore structure; after the casting liquid is extruded through the spinneret, the core liquid temperature is 60-100° C.; Among them, the additive is ultra-high molecular weight polyvinylidene fluoride; the weight average molecular weight of the ordinary molecular weight polyvinylidene fluoride is 100,000 to 700,000, and the weight average molecular weight of the ultra-high molecular weight polyvinylidene fluoride is not less than 1 million; the diluent is one of dibutyl phthalate, dibutyl sebacate, acetylcitrate tributyl citrate, tributyl citrate, and γ-butyrolactone; the polyvinylidene fluoride hollow fiber membrane is a polyvinylidene fluoride hollow fiber membrane with a thin skin, good surface porosity, and a support layer with a mesh pore structure.

2. The method for preparing the polyvinylidene fluoride hollow fiber membrane with a mesh pore structure as claimed in claim 1, characterized in that: The mixing is carried out under heating conditions, and the heating temperature is lower than the melting temperature of polyvinylidene fluoride with ordinary molecular weight.

3. The method for preparing the polyvinylidene fluoride hollow fiber membrane with a mesh pore structure as claimed in claim 1, characterized in that: The casting liquid is extruded through a spinneret, and the core liquid used is one of a diluent or nitrogen.

4. The method for preparing the polyvinylidene fluoride hollow fiber membrane with a mesh pore structure according to claim 3, characterized in that: The core liquid flow rate is 0.01-0.1 L / min during extrusion through the spinneret.

5. The method for preparing the polyvinylidene fluoride hollow fiber membrane with a mesh pore structure as claimed in claim 1, characterized in that: For the cooling, the coolant is deionized water at 25° C.; for the extraction, the extractant is ethanol with a purity of not less than 99%.

6. A polyvinylidene fluoride hollow fiber membrane with a mesh pore structure obtained by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Enhanced ultrahigh-molecular-weight polyethylene and polyvinylidene fluoride binary blend membrane and preparation method thereof

    CN106492645A

  • Methods for making microporous products

    US4247498A

  • Method for manufacturing polyvinylidene fluoride multi-core ultrafiltration membrane tube

    CN101543733A

  • Polyvinylidene fluoride hollow fiber microporous membrane and preparation method

    CN104043344A

  • Vinylidene fluoride type resin hollow filament porous membrane and method for manufacruring the same