Light emitting device, electronic device using the same, and inspection method
By using a phosphor with a long luminous life in the light emitting device and adjusting the energy matching of the excitation light and the phosphor, the problem of fluorescence output saturation is solved, and efficient light output is achieved.
Patent Information
- Application Number
- CN202080035446.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-27
- Filing Date
- 2020-04-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-04-21
AI Technical Summary
The conventional light emitting device is prone to output saturation when the phosphor has a long luminous life, which leads to the problem of difficulty in increasing the light intensity.
Using a phosphor with a long luminescence life, and adjusting the energy matching of the excitation light and the phosphor, the sum of the energy E1 of the excitation light and the fluorescent energy E2 of the fluorescent light is smaller than the bandgap energy Eg of the fluorescent body's parent crystal, thereby inhibiting the absorption of the excited state. , thereby reducing the saturation of the fluorescence output.
It effectively suppresses the saturation of the fluorescence output, improves the intensity and brightness of the fluorescence, and maintains high output even under the excitation light of high energy density.
Smart Images

Figure CN113826226B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light emitting device, and an electronic device and an inspection method using the light emitting device. Background Art
[0002] Conventionally, there are known light-emitting devices that combine an excitation light source that emits laser light and a wavelength converter that includes a plurality of phosphors. As such light-emitting devices that have a light source that emits laser light, for example, laser lighting devices and laser projectors are known. Moreover, light-emitting devices that have a light source that emits laser light generally perform high-light-density excitation of the phosphors.
[0003] For such a light-emitting device, the intensity (brightness) of the light emitted by the phosphor generally tends to increase as the energy density of the laser from the excitation light source increases. However, when the energy density of the laser is higher than a specified value, it becomes difficult to increase the intensity of the light emitted by the phosphor. In other words, a phenomenon of saturation of the light output emitted by the phosphor occurs. In the past, it was believed that such saturation of the fluorescence output depends on the luminescence lifetime of the phosphor. Therefore, it was previously believed that a phosphor with a longer luminescence lifetime is less likely to emit high-intensity fluorescence than a phosphor with a short luminescence lifetime.
[0004] Therefore, Patent Document 1 discloses a light source device that can obtain output light with high brightness and excellent color rendering by using a phosphor with a short luminous lifetime. Specifically, the light source device is provided with an excitation light source and a phosphor layer that receives excitation light from the excitation light source and emits fluorescence, wherein the phosphor layer includes a predetermined first phosphor and / or a second phosphor, and the luminous lifetime of the first phosphor and the second phosphor is 0.1 nanosecond to 250 nanoseconds.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2018 / 163830 Summary of the invention
[0008] However, in a light emitting device using laser, in order to improve the degree of freedom in wavelength selection of fluorescence emitted by the phosphor and the afterglow property of the fluorescence, it is desirable to use not only phosphors with short emission lifetime but also phosphors with long emission lifetime.
[0009] The present invention is made in view of the problems of the prior art. Furthermore, the present invention aims to provide a light-emitting device capable of suppressing saturation of the fluorescence output emitted by a phosphor even when a phosphor with a long luminous lifetime is used, and an electronic device and an inspection method using the light-emitting device.
[0010] In order to solve the above-mentioned problems, a light emitting device according to a first aspect of the present invention comprises a light source and a first phosphor. The light source radiates light with an energy density exceeding 0.5 W / mm 2 The first phosphor absorbs the primary light and converts it into a first wavelength converted light with a longer wavelength than the primary light. The compound that becomes the matrix of the first phosphor is a simple oxide with one metal element or a composite oxide with multiple simple oxides of different types as end components. Moreover, when the energy conversion value of the peak wavelength of the primary light is E1 electron volts and the energy conversion value of the fluorescence peak wavelength of the first wavelength converted light is E2 electron volts, the band gap energy of the simple oxide crystal is greater than the sum of E1 and E2.
[0011] An electronic device according to a second aspect of the present invention includes the light emitting device according to the first aspect.
[0012] The inspection method according to the third aspect of the present invention utilizes the light emitting device according to the first aspect.
[0013] The phosphor according to the fourth aspect of the present invention is a phosphor having a composition formula represented by the following general formula (I).
[0014] (Gd 1-x La x )3(Ga 1-y-z Sc y Cr z )2Ga3O 12 (I)
[0015] (Wherein, x, y and z satisfy 0<x<1, 0<y≤0.60, 0<z<0.2.) BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 Yes means Ce 3+ Activate phosphor and Eu 2+ A graph showing the relationship between the fluorescence saturation characteristics (external quantum efficiency maintenance rate) and the emission lifetime (1 / e decay time) in an activated phosphor.
[0017] Figure 2 This is a diagram showing energy levels for explaining the output saturation characteristics of a phosphor.
[0018] Figure 3 (a) is used for Y3Al5O 12 :Ce 3+ A diagram of energy levels illustrating the output saturation characteristics of a phosphor. Figure 3 (b) is used for Y3Al5O 12 :Cr 3+ A diagram of energy levels illustrating the output saturation characteristics of a phosphor.
[0019] Figure 4 This is a diagram showing energy levels for explaining the output saturation characteristics of the first phosphor used in the light-emitting device of the present embodiment.
[0020] Figure 5 It is a schematic cross-sectional view showing an example of the light emitting device according to this embodiment.
[0021] Figure 6 It is a schematic cross-sectional view showing another example of the light emitting device according to the present embodiment.
[0022] Figure 7 It is a schematic cross-sectional view showing another example of the light emitting device according to the present embodiment.
[0023] Figure 8 It is a schematic cross-sectional view showing another example of the light emitting device according to the present embodiment.
[0024] Fig. 9 It is a diagram schematically showing the structure of the endoscope according to the present embodiment.
[0025] Fig.10 It is a diagram schematically showing the configuration of an endoscope system according to the present embodiment.
[0026] Fig.11 This is a graph showing the emission lifetime (1 / e decay time) of the phosphors of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2.
[0027] Fig.12 This is a schematic diagram showing a wavelength conversion device used for evaluating the fluorescence output saturation characteristics in Example 1. Fig.12 (a) shows a top view of the wavelength conversion device, Fig.12 (b) is a side view of the wavelength conversion device.
[0028] Fig.13 This is a schematic diagram showing an apparatus used in Example 1 to measure the emission intensity of each phosphor of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2.
[0029] Fig.14 This is a graph for explaining the duty ratio of the blue laser light used for evaluating the fluorescence output saturation characteristics in Example 1.
[0030] Fig.15 This is a graph showing the relationship between the relative emission intensity and the light energy density of the excitation light in the phosphors of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2.
[0031] Fig.16The X-ray diffraction patterns of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 and the garnet compound Gd3Ga2Ga3O registered in ICSD (Inorganic Crystal Structure Database) are shown. 12 Graph of the X-ray diffraction pattern.
[0032] Fig.17 It is a graph showing the emission spectra of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2.
[0033] Fig.18 This is a graph showing relative values of ICG absorption efficiency of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2.
[0034] Fig.19 Graph showing the excitation spectrum and fluorescence spectrum of indocyanine green (ICG) fluorescent dye. Fig.19 This is a graph for explaining the relative value of the intensity of the excitation spectrum of ICG at the fluorescence peak wavelength of the phosphor when obtaining the relative value of the ICG absorption efficiency. DETAILED DESCRIPTION
[0035] Hereinafter, the light emitting device of the present embodiment, the electronic device using the light emitting device, and the inspection method will be described with reference to the drawings. In addition, for the convenience of description, the dimensional ratios of the drawings are exaggerated and may be different from the actual ratios.
[0036] [Light-emitting device]
[0037] A light-emitting device that combines a light source that emits excitation light with a wavelength converter that includes a phosphor generally increases the intensity (brightness) of the fluorescence emitted by the phosphor as the energy of the excitation light increases. However, when the energy of the excitation light is higher than a specified value, the fluorescence output emitted by the phosphor is saturated and the intensity of the fluorescence becomes difficult to increase. It can be considered that the saturation of the fluorescence output emitted by the phosphor depends on the luminescence lifetime of the phosphor.
[0038] Figure 1 Shows Ce 3+ Activate phosphor and Eu 2+ The relationship between the external quantum efficiency maintenance rate and the luminescence lifetime (1 / e decay time) in the activated phosphor. In addition, the external quantum efficiency maintenance rate refers to the energy density of 15W / mm 2 The external quantum efficiency of the excitation light is 0.5W / mm 2 The ratio of the external quantum efficiency when the excitation light is high. It can be said that the higher the external quantum efficiency maintenance rate of the phosphor, the smaller the fluorescence output saturation. Figure 1As shown in FIG. 1 , it is known that as the 1 / e decay time, i.e., the luminescence lifetime, becomes shorter, the external quantum efficiency maintenance rate of the phosphor increases and the fluorescence output saturation decreases. Therefore, it has been believed that a phosphor with a longer luminescence lifetime has a larger luminescence output saturation and is less likely to emit high-intensity light than a phosphor with a short luminescence lifetime.
[0039] The mechanism of the occurrence of such fluorescence output saturation is considered to be as follows. First, if the fluorescent body is irradiated with excitation light of a wavelength corresponding to the absorption band inherent to the luminescent ion, Figure 2 The electrons in the ground state of the luminescent ion shown in (a) are Figure 2 (b) When the electron is excited by the high excited state energy level, it usually undergoes non-radiative relaxation to the lowest excited singlet state through internal conversion, and then returns to the ground state, emitting fluorescence. Here, when the electron with a low transition probability further absorbs the excitation light before relaxing from the excited state energy level to the ground state energy level, as shown in Figure 2 As shown in (c), excited state absorption (ESA) occurs when the electron transitions from the excited state energy level to the conduction band (CB) and photoionization is performed. In this way, when the transition probability of the electron is low, excited state absorption occurs, and the relaxation from the lowest excited singlet state to the ground state is reduced, so the intensity (brightness) of the fluorescence emitted by the phosphor is difficult to increase (refer to OBShchekin et al., Phys. Status Solidi, RRL10 (2016) and A. Lenef et al., Proc. SPIE 8841, Current Developments in Lens Design and Optical Engineering XIV, 884107 (2013).)
[0040] Here, Figure 3 (a) shows the activation of Ce with short luminescence lifetime 3+ The Y3Al5O phosphor after ionization 12 :Ce 3+ energy level. Figure 3 (b) shows the activation of Cr with a long luminescence lifetime. 3+ The Y3Al5O phosphor after ionization 12 :Cr 3+ In addition, Ce 3+ The luminescence lifetime (1 / e decay time) of an ion is usually 10 -9 ~10 -8 sec, Cr 3+ The luminescence lifetime of an ion is usually 10 -4 ~10 -3 Second.
[0041] like Figure 3 As shown in (a), in the Y3Al5O 12 :Ce 3+ When the fluorescent substance is irradiated with excitation light, Ce 3+ The electrons in the ion rise from the ground state to the excited state (refer to Figure 3 (a) (1)). The excited electrons relax non-radiatively to the lowest excited singlet state via internal conversion (refer to Figure 3 (a) (2)). Then, the electron undergoes a Stokes shift and relaxes from the excited state energy level to the ground state energy level, emitting fluorescence (refer to Figure 3 (a) (3)). Here, Ce 3+ The probability of electrons in ions transitioning from the excited state energy level to the ground state energy level is high, and energy relaxation is easy to occur. Therefore, since excited state absorption (ESA) is difficult to occur before relaxation from the excited state energy level to the ground state energy level, Y3Al5O 12 :Ce 3+ The fluorescence output of the phosphor is saturated and reduced.
[0042] Similarly, in the case of Y3Al5O 12 :Cr 3+ When the fluorescent substance is irradiated with excitation light, Figure 3 As shown in (b), Cr 3+ The electrons in the ion rise from the ground state to the excited state (refer to Figure 3 (b) (1)). The excited electrons relax non-radiatively to the lowest excited singlet state via internal conversion (refer to Figure 3 (b) (2)). Then, the electron relaxes from the excited state energy level to the ground state energy level, and emits fluorescence (refer to Figure 3 (b) (3)). Here, Cr 3+ The probability of electrons in ions transitioning from the excited state energy level to the ground state energy level is low, and energy relaxation is difficult to perform. Therefore, before the excited state energy level relaxes to the ground state energy level, the excitation light is further absorbed, and excited state absorption is likely to occur. As a result, since the relaxation from the lowest excited singlet state to the ground state is reduced, Y3Al5O 12 :Cr 3+ The fluorescence output of the phosphor becomes saturated and increases.
[0043] Here, if Figure 3 As shown in (b) (3), the energy conversion value of the peak wavelength of the excitation light further absorbed by the lowest excited singlet electron is E1 electron volt, and the energy conversion value of the fluorescence peak wavelength is E2 electron volt. The light energy can be calculated by the following mathematical formula 1.
[0044] [Mathematical formula 1]
[0045] E=hν=h×c / λ
[0046] h: Planck's constant, E: light energy, ν: frequency of light, c: speed of light, λ: wavelength of light
[0047] Furthermore, it can be considered that when the energy E1 of the excitation light further absorbed by the electrons in the lowest excited singlet state is smaller, the possibility of transition from the excited state energy level to the conduction band (CB) becomes smaller. In other words, it can be considered that when the sum (E1+E2) of the energy E1 of the peak wavelength of the excitation light and the energy E2 of the peak wavelength of the luminescence (fluorescence) is smaller than the band gap energy (Eg) of the crystal constituting the matrix of the phosphor, the possibility of excited state absorption becomes smaller.
[0048] Specifically, if Figure 4 As shown in FIG. 1 , when the peak wavelength of the fluorescence of the phosphor is 700 nm, the energy E2 of the fluorescence becomes 1.77 eV. In addition, when the peak wavelength of the excitation light that excites the phosphor is 450 nm, the energy E1 of the excitation light becomes 2.76 eV. Therefore, the sum of the energy E1 of the excitation light and the energy E2 of the fluorescence (E1+E2) becomes 4.53 eV. Moreover, when the band gap energy Eg of the mother crystal constituting the phosphor exceeds 4.53 eV, even if the electrons in the lowest excited singlet absorb the excitation light, it is difficult to transition to the conduction band (CB), thereby reducing the possibility of excited state absorption.
[0049] The light emitting device of this embodiment includes a light source that emits primary light as excitation light and a first phosphor that absorbs the primary light and converts it into first wavelength-converted light (fluorescence) having a wavelength longer than the primary light. Furthermore, the excitation light and the phosphor are appropriately selected so that the sum of the energy E1 of the excitation light and the energy E2 of the fluorescence (E1+E2) is smaller than the band gap energy Eg of the mother crystal constituting the first phosphor.
[0050] like Figures 5 to 8 As shown, the light emitting device 1, 1A, 1B, 1C of the present embodiment includes at least a light source 2 and a wavelength converter 3, 3A, the light source 2 emits primary light 6, and the wavelength converter 3, 3A includes a first phosphor 4 that emits first converted wavelength light 7. In the light emitting device 1, 1A, 1B, 1C, when the primary light 6 emitted by the light source 2 enters the wavelength converter 3, 3A, the wavelength converter 3, 3A emits the first converted wavelength light 7 as fluorescence.
[0051] (light source)
[0052] The light source 2 is a light emitting element that emits primary light 6. The primary light 6 is preferably laser light. This allows a design that irradiates high-density concentrated light onto the first phosphor 4, making it easy to manufacture a high-output point light source, thereby becoming a light emitting device that broadens the industrial application range of solid-state lighting.
[0053] As such a light source 2, for example, a laser element such as a surface emitting laser diode can be used. The output energy of the laser light emitted by one laser element is preferably 0.1 W or more, more preferably 1 W or more, and further preferably 5 W or more. In addition, the light energy density of the laser light emitted by the light source 2 is preferably more than 0.5 W / mm 2 , more preferably 2W / mm 2 More preferably, 10W / mm 2 As described later, the phosphor in the wavelength converter 3, 3A can convert the wavelength of high-output laser light with high efficiency. Therefore, by making the light energy density of the laser light emitted by the light source 2 exceed 0.5 W / mm 2 , the light-emitting device is capable of radiating high-output near-infrared light.
[0054] The light source 2 included in the light emitting device 1, 1A, 1B, 1C may be a light emitting diode (LED). For example, by using an LED that emits light with an energy of 100 mW or more as the light source 2, the phosphor in the wavelength converter 3, 3A can be excited with high-output light. As a result, the light emitting device 1, 1A, 1B, 1C can emit high-output near-infrared light, and can achieve the same effect as when using a laser element.
[0055] As described above, in the light emitting devices 1, 1A, 1B, and 1C, the light source 2 is preferably at least one of a laser element and a light emitting diode. However, the light source 2 is not limited thereto, and any light emitting element can be used as long as it can emit primary light 6 having a high energy density. Specifically, the light source 2 preferably emits light with an energy density exceeding 0.5 W / mm 2 In this case, since the light emitting devices 1, 1A, 1B, and 1C emit high-output near-infrared light, the phosphors in the wavelength converters 3 and 3A can be excited by the high-output light. In addition, the energy density of the primary light 6 emitted by the light source 2 is more preferably 2 W / mm 2 More preferably, 10W / mm 2 The upper limit of the light energy density of the primary light 6 emitted by the light source 2 is not particularly limited, and can be set to 50 W / mm 2 .
[0056] The primary light 6 emitted by the light source 2 is preferably purple light having a luminescence peak in a wavelength range of 380 nm to less than 435 nm or blue light having a luminescence peak in a wavelength range of 435 nm to less than 470 nm. Thus, since semiconductor light-emitting elements (light-emitting diodes, laser diodes) that are easy to obtain and relatively inexpensive can be used as the light source 2, it becomes a light-emitting device that is advantageous in industrial production. In addition, since the phosphor in the wavelength converter 3, 3A is excited with high efficiency, the light-emitting device can radiate high-output near-infrared light.
[0057] The light source 2 can emit primary light 6 having a luminescence peak in the wavelength range of 500 nm to 560 nm. Thus, since the high-power primary light 6 can excite the phosphor in the wavelength converter 3 or 3A, the light emitting device can emit high-power near-infrared light.
[0058] The light source 2 can emit primary light 6 having a luminescence peak in the wavelength range of 600 nm to 700 nm. Thus, the phosphor in the wavelength converter 3, 3A can be excited by red light with relatively low energy, thereby obtaining a light-emitting device that emits near-infrared light with low heat generation due to Stokes loss of the phosphor and high output.
[0059] As described above, the type of light source 2 provided in the light emitting device 1, 1A, 1B, 1C is not particularly limited. However, the type of light source 2 provided in the light emitting device 1, 1A, 1B, 1C is preferably three or less, more preferably two or less, and even more preferably one. By setting such a configuration, a simple configuration with a small number of light sources 2 is achieved, so that a compact light emitting device 1, 1A, 1B, 1C can be obtained.
[0060] The light sources included in the light emitting devices 1, 1A, 1B, 1C preferably include a plurality of light sources of the same type. With such a configuration, the wavelength converters 3, 3A can be excited with light having a higher energy, thereby obtaining a light emitting device that emits near-infrared light with a higher output.
[0061] (Wavelength Converter)
[0062] like Figures 5 to 8 As shown, the wavelength converters 3 and 3A emit fluorescence having a longer wavelength than the primary light 6 by receiving the primary light 6 . Figure 5 and Figure 6 The wavelength converter 3, 3A shown in the figure is configured to receive the primary light 6 at the front surface 3a and emit fluorescence from the back surface 3b. Figure 7 and Figure 8 The wavelength converter 3, 3A shown in the figure has a structure that receives the primary light 6 at the front surface 3a and emits fluorescence at the same front surface 3a.
[0063] The wavelength converter 3, 3A includes a first phosphor 4 that absorbs the primary light 6 and converts it into a first wavelength converted light 7 having a longer wavelength than the primary light 6. The compound that serves as the matrix of the first phosphor 4 is preferably a simple oxide having a metal element as one type or a composite oxide having a plurality of such simple oxides of different types as terminal components. Thus, it is easy to make the sum (E1+E2) of the energy E1 of the primary light 6 as the excitation light and the energy E2 of the first wavelength converted light 7 emitted by the first phosphor 4 smaller than the band gap energy Eg of the matrix crystal constituting the first phosphor 4.
[0064] The simple oxide constituting the matrix of the first phosphor 4 is not particularly limited as long as E1+E2 is smaller than Eg. The simple oxide is preferably Al2O3, Ga2O3, Sc2O3, Y2O3, La2O3, Gd2O3, Lu2O3, Eu2O3, Ho2O3, Er2O3, Tm2O3, ZrO2 or HfO2 as shown in Table 1. In addition, Table 1 also shows the band gap energy of the crystal of the simple oxide and the literature on the band gap energy.
[0065] Table 1
[0066]
[0067] The composite oxide constituting the matrix of the first phosphor 4 is not particularly limited as long as E1+E2 is smaller than Eg. The composite oxide is preferably an oxide formed by arbitrarily compounding at least two simple oxides selected from Al2O3, Ga2O3, Sc2O3, Y2O3, La2O3, Gd2O3, Lu2O3, Eu2O3, Ho2O3, Er2O3, Tm2O3, ZrO2 and HfO2. In addition, Table 2 shows the literature recording the band gap energy and band gap energy of the crystal of the composite oxide. According to the investigation of the inventors, the composite oxides formed by the simple oxide with large band gap energy of the crystal as the end component all tend to have higher band gap energy. For example, the composite oxide formed by the simple oxide with a band gap energy of more than 4.6eV as the end component tends to have a band gap energy of more than 4.6eV. Therefore, the composite oxide constituting the matrix of the first phosphor 4 is preferably formed by the simple oxide with large band gap energy as the end component.
[0068] Table 2
[0069]
[0070] The band gap energy Eg of the simple oxide crystal that is the matrix of the first phosphor 4 is preferably 4.6 eV or more. 3+In the case of being an activator of the first phosphor 4, the peak wavelength of the emission of the first phosphor 4 becomes about 690 nm or more. In addition, the excitation light (primary light 6) emitted by the light source 2 is usually composed of blue light with a peak wavelength of 450 nm. Therefore, the energy E1 of the peak wavelength of the excitation light becomes 2.756 eV, the energy E2 of the peak wavelength of the emission (fluorescence) becomes 1.797 eV or less, and the sum of E1 and E2 becomes 4.553 eV or less. Therefore, by using a compound having a crystal band gap energy Eg of 4.6 eV or more as the matrix of the first phosphor 4, it is easy to become a phosphor that is not prone to fluorescence saturation.
[0071] The first phosphor 4 preferably contains at least one element selected from aluminum (Al), gallium (Ga), and scandium (Sc) in the crystal of the compound serving as the matrix. 3+ , Ga 3+ Sc 3+ With Cr as an activator 3+ That is, Al 3+ The ionic radius of the hexa-coordinated Ga 3+ The ionic radius of the hexa-coordinated Sc 3+ The ionic radius of the hexa-coordinated Cr 3+ The ionic radius of the hexa-coordinated Therefore, in the crystal of the parent compound, Al 3+ , Ga 3+ Sc 3+ More likely to be Cr 3+ In addition, due to the Cr 3+ The ionic radius is larger than that of Al 3+ , Ga 3+ Sc 3+ The ionic radius of Cr is small, so in the partially replaced crystal, it acts on 3+ Therefore, since a wide fluorescence spectrum can be easily obtained, a light-emitting device that is advantageous for medical illumination using fluorescence imaging or photodynamic therapy (PDT) can be obtained.
[0072] The activator included in the first phosphor 4 may use an element with a long luminescence lifetime. As described above, by making the sum of the energy E1 of the primary light 6 and the energy E2 of the first wavelength converted light 7 smaller than the band gap energy Eg of the mother crystal of the first phosphor 4, it is possible to suppress the saturation of the fluorescence output and increase the intensity of the fluorescence emitted by the phosphor. Therefore, not only elements with a short luminescence lifetime but also elements with a long luminescence lifetime can be appropriately used as the activator. The activator included in the first phosphor 4 may use an element with a 1 / e decay time of 10-4 As such an activator, for example, it is preferably selected from Cr 3+ 、V 2+ , Mn 4+ and Fe 5+ At least one of .
[0073] In addition, the activator included in the first phosphor 4 may also use an element with a short luminescence lifetime. Specifically, the activator included in the first phosphor 4 may be an element with a 1 / e decay time of 10 -9 ~10 -8 Ce of seconds 3+ and a 1 / e decay time of 10 -7 ~10 -6 Eu 2+ At least one of .
[0074] The first wavelength converted light 7 emitted by the first phosphor 4 includes fluorescence based on the electron energy transition of transition metal ions, and the transition metal ions are preferably Cr. 3+ That is, the first phosphor 4 is preferably Cr 3+ Activate phosphor. Cr 3+ The absorption and emission mechanism of Cr is based on dd transition. Therefore, the wavelength of absorption and emission increases with the excitation of Cr. 3+ Therefore, by using Cr 3+ By selecting an appropriate mother crystal for the luminescent center, a light-emitting device can be made that can easily customize the spectral distribution in the red to near-infrared wavelength region according to the application. 3+ Activated phosphors can convert high energy density laser light into near-infrared light with high efficiency. 3+ By activating the phosphor, a light-emitting device that emits near-infrared light with higher output can be obtained.
[0075] In the first phosphor 4, the cationic element in the crystal of the compound serving as the matrix is preferably formed only of an element taking a trivalent valence. Cr as an activator may take not only Cr 3+ , you can also take Cr 2+ Cr 4+ Furthermore, if the first phosphor 4 is mixed with Cr, the Cr 3+ Therefore, by setting the cationic elements in the matrix crystal to only elements with a trivalent valence, Cr can be prevented from becoming Cr. 2+ Cr 4+The trivalent cation element has a wide band gap energy Eg, so that a light-emitting device that is less likely to cause fluorescence output saturation can be obtained.
[0076] The first phosphor 4 preferably contains two or more types of Cr 3+ The fluorescent substance is activated. Thus, the spectral distribution of the output light component in the near-infrared wavelength region can be controlled at least. Therefore, a light-emitting device can be obtained that can easily adjust the spectral distribution according to the application of the near-infrared fluorescent component.
[0077] The first phosphor 4 preferably has a garnet crystal structure. In addition, the first phosphor 4 is also preferably an oxide phosphor having a garnet crystal structure. Phosphors having a garnet structure, especially oxide phosphors, have a polyhedral particle shape close to a sphere, and the dispersibility of the phosphor particle group is excellent. Therefore, in the case where the phosphor included in the wavelength converter 3, 3A has a garnet structure, it is possible to easily manufacture a wavelength converter with excellent light transmittance and realize high output of the light-emitting device. In addition, phosphors having a garnet crystal structure have a track record as phosphors for LEDs, so by making the first phosphor 4 have a garnet crystal structure, a light-emitting device with high reliability can be obtained.
[0078] The first phosphor 4 is preferably a phosphor having a composition formula represented by the following general formula (I).
[0079] (Gd 1-x La x )3(Ga 1-y-z Sc y Cr z )2Ga3O 12 (I)
[0080] In addition, in the formula (I), x, y and z satisfy 0<x<1, 0<y≤0.60, and 0<z<0.2.
[0081] The phosphor represented by the general formula (I) is (Gd 1-x La x )3(Ga 1-y-z Sc y )2Ga3O 12 Cr 3+ The phosphor is an activator. 1-x La x )3(Ga 1-y-z Sc y )2Ga3O 12It is a composite oxide formed by using Gd2O3, La2O3, Ga2O3 and Sc2O3, which are simple oxides of metal elements, as terminal components. Here, according to Table 1, the band gap energy of Gd2O3 is 5.6eV, the band gap energy of La2O3 is 6.1eV, the band gap energy of Ga2O3 is 4.8eV, and the band gap energy of Sc2O3 is 6.0eV. In addition, according to the investigation of the inventors, composite oxides formed by using simple oxides with large crystal band gap energy as terminal components tend to have higher band gap energy. Therefore, it is speculated that: (Gd 1-x La x )3(Ga 1-y-z Sc y )2Ga3O 12 The band gap energy of the crystal becomes 4.8 eV or more.
[0082] The phosphor represented by the general formula (I) uses Cr 3+ As an activator, it is possible to convert high energy density laser light into near infrared light with high efficiency, and further, when using laser light, the fluorescence output is not easily saturated. Therefore, a light-emitting device that emits high output near infrared light can be obtained. 1-x La x )3(Ga 1-y-z Sc y )2Ga3O 12 As a parent compound, it can emit fluorescence with a large light component near 770 nm.
[0083] In the general formula (I) of the first phosphor 4, x more preferably satisfies 0.05≤x≤0.25. In addition, in the general formula (I), y more preferably satisfies 0.06≤y≤0.60, further preferably satisfies 0.20≤y≤0.60, and particularly preferably satisfies 0.20≤y≤0.50. By making x and y in the general formula (I) within this range, the absorption efficiency of near-infrared light for fluorescent agents used in fluorescence imaging can be improved. Therefore, by using the phosphor represented by the general formula (I) as the first phosphor 4, a light-emitting device suitable for fluorescence imaging can be obtained.
[0084] The first wavelength converted light 7 emitted by the first phosphor 4 is preferably near-infrared light having a fluorescence peak in a wavelength range of 700 nm to less than 1000 nm. Light in a wavelength range of 650 nm to less than 1400 nm is particularly easy to pass through a living body, and this wavelength range is generally referred to as a "biological window". Moreover, by making the first wavelength converted light 7 near-infrared light, a light-emitting device that is easy to introduce light from outside the body into the body and is beneficial for medical applications can be provided. In addition, such first wavelength converted light 7 becomes low-energy light with an energy conversion value E2 of 1.77 eV and less than 1.24 eV. Therefore, even if the primary light 6 is set to high-energy purple light (380 nm to less than 435 nm: less than 3.26 eV and 2.85 eV), the sum of E1 and E2 becomes less than 5.03 eV and greater than 4.09. Therefore, it is easy to use phosphors based on conventional oxides and complex oxides with high industrial performance, and the selection range of phosphors is also widened, thereby achieving a light-emitting device that is advantageous for industrial production.
[0085] The first wavelength converted light 7 preferably has a fluorescence peak in a wavelength region exceeding 750 nm, and further preferably has a fluorescence peak in a wavelength region exceeding 770 nm. Thus, the near-infrared light emitted by the light-emitting devices 1, 1A, 1B, and 1C becomes near-infrared light that is more easily transmitted through a living body, thereby providing a near-infrared light-emitting device suitable for medical lighting applications.
[0086] The first wavelength converted light 7 preferably has a light component at least in the entire wavelength range of 700 nm to 800 nm. As a result, as described later, the drug used in fluorescence imaging and photodynamic therapy has a structure that can efficiently absorb the light component of the first wavelength converted light 7. In addition, it has a structure that can cope with various drugs with different light absorption characteristics.
[0087] The first wavelength converted light 7 more preferably has a light component in at least the entire wavelength range of 750 nm to 800 nm. In addition, the first wavelength converted light 7 also preferably has a light component in the entire wavelength range of 600 nm to 800 nm. Thus, the drug used in fluorescence imaging and photodynamic therapy becomes a structure that can efficiently absorb the light component of the first wavelength converted light 7. In addition, it becomes a structure that can correspond to various drugs with different light absorption characteristics.
[0088] like Figure 5As shown, the wavelength converter 3 preferably has a sealing material 5 in which the first phosphor 4 is dispersed in addition to the first phosphor 4. Moreover, in the wavelength converter 3, the first phosphor 4 is preferably dispersed in the sealing material 5. By dispersing the first phosphor 4 in the sealing material 5, the primary light 6 emitted by the light source 2 can be efficiently absorbed and wavelength-converted into near-infrared light. In addition, the wavelength converter 3 can be easily formed into a sheet or film.
[0089] The sealing material 5 is preferably at least one of an organic material and an inorganic material, in particular at least one of a transparent (light-transmitting) organic material and a transparent (light-transmitting) inorganic material. As the sealing material of the organic material, for example, a transparent organic material such as silicone resin can be listed. As the sealing material of the inorganic material, for example, a transparent inorganic material such as low-melting-point glass can be listed.
[0090] like Figure 5 As shown in FIG. 1 , the wavelength converter 3 includes a first phosphor 4 that emits a first wavelength converted light 7. Figure 6 and Figure 8 As shown, the wavelength converter preferably further includes a second phosphor 8, and the second phosphor 8 absorbs the primary light 6 emitted by the light source 2 and emits the second wavelength converted light 9 as visible light. In other words, the light emitting device 1A, 1C preferably further includes a second phosphor 8 that absorbs the primary light 6 and converts it into the second wavelength converted light 9 having a longer wavelength than the primary light 6 and different from the first wavelength converted light 7. By appropriately combining a plurality of arbitrary phosphors, the shape of the fluorescence spectrum and the excitation characteristics can be controlled, so that the light emitting device 1A, 1C can be obtained in which the spectral distribution of the output light can be easily adjusted according to the application. In addition, by making the wavelength converter 3A include the second phosphor 8, the primary light 6 emitted by the light source 2, such as blue laser light, and the second wavelength converted light 9 can be emitted as white output light by additive color mixing.
[0091] The second phosphor 8 included in the wavelength converter 3A is not particularly limited as long as it can absorb the primary light 6 emitted by the light source 2 and emit the second wavelength converted light 9 as visible light. The second phosphor 8 is preferably a crystalline structure selected from a garnet type, a calcium ferrite type, and a lanthanum silicon nitride (La3Si6N 11 Ce 3+ Alternatively, the second phosphor 8 is preferably Ce, which is composed of at least one compound selected from the group consisting of a garnet-type crystal structure, a calcium ferrite-type crystal structure, and a lanthanum silicon nitrogen-type crystal structure. 3+ Activating the phosphor. By using such a second phosphor 8, it is possible to obtain output light having a large amount of green to yellow light components.
[0092] Specifically, the second phosphor 8 is preferably selected from M3RE2(SiO4)3, RE3Al2(AlO4)3, MRE2O4 and RE3Si6N 11 Ce having at least one compound (B) as a main component as a matrix 3+ Alternatively, the second phosphor 8 is preferably selected from M3RE2(SiO4)3, RE3Al2(AlO4)3, MRE2O4 and RE3Si6N 11 Ce as a matrix of at least one 3+ Alternatively, the second phosphor 8 is preferably Ce, which is a solid solution having the compound (B) as a terminal component as a matrix. 3+ Activate the phosphor. In addition, M is an alkaline earth metal and RE is a rare earth element.
[0093] Such a second phosphor 8 fully absorbs light in the wavelength range of 430nm to 480nm and efficiently converts it into green to yellow light having an intensity maximum in the wavelength range of 540nm to 590nm. Therefore, by using such a phosphor as the second phosphor 8, it is possible to easily obtain a visible light component.
[0094] The wavelength converter 3, 3A is preferably formed of an inorganic material. Here, the inorganic material refers to a material other than an organic material, and is a concept including ceramics and metals. By forming the wavelength converter 3, 3A from an inorganic material, the thermal conductivity thereof is higher than that of a wavelength converter including an organic material such as a sealing resin, so that the heat dissipation design becomes easy. Therefore, even when the primary light 6 emitted by the light source 2 photoexcites the phosphor at a high density, the temperature rise of the wavelength converter 3, 3A can be effectively suppressed. As a result, the temperature quenching of the phosphor in the wavelength converter 3, 3A can be suppressed to achieve high output of light emission.
[0095] As described above, the wavelength converters 3 and 3A are preferably formed of an inorganic material, and therefore the sealing material 5 is preferably formed of an inorganic material. In addition, zinc oxide (ZnO) is preferably used as the inorganic material of the sealing material 5. As a result, the heat dissipation of the phosphor is further improved, so that the output reduction of the phosphor caused by temperature quenching can be suppressed, and a light-emitting device emitting high-output near-infrared light can be obtained.
[0096] The wavelength converter 3, 3A may also be set as a wavelength converter without using the sealing material 5. In this case, the wavelength converter 3, 3A may also be composed of only a phosphor, and the phosphors may be fixed to each other using an organic or inorganic binder. As the binder, a commonly used resin-based adhesive or ceramic particles, low-melting-point glass, etc. may be used. The wavelength converter without using the sealing material 5 can be thinned, so it can be applied to a light-emitting device.
[0097] Next, the function of the light emitting device of this embodiment will be described. Figure 5 For the light emitting device 1 shown, first, the primary light 6 emitted by the light source 2 is irradiated to the front surface 3a of the wavelength converter 3. The irradiated primary light 6 is transmitted from the wavelength converter 3. Moreover, when the primary light 6 is transmitted from the wavelength converter 3, the first phosphor 4 included in the wavelength converter 3 absorbs a part of the primary light 6 and emits the first wavelength converted light 7. In this way, the light including the primary light 6 and the first wavelength converted light 7 is emitted from the back surface 3b of the wavelength converter 3 as output light.
[0098] At once Figure 6 For the light emitting device 1A shown, first, the primary light 6 emitted by the light source 2 is irradiated toward the front surface 3a of the wavelength converter 3A. The irradiated primary light 6 is transmitted through the wavelength converter 3A. Moreover, when the primary light 6 is transmitted through the wavelength converter 3A, the second phosphor 8 included in the wavelength converter 3A absorbs a part of the primary light 6 and emits the second wavelength converted light 9. Furthermore, the first phosphor 4 included in the wavelength converter 3A absorbs a part of the primary light 6 and emits the first wavelength converted light 7. In this way, light including the primary light 6, the first wavelength converted light 7, and the second wavelength converted light 9 is emitted as output light from the back surface 3b of the wavelength converter 3A.
[0099] At once Figure 7 In the light emitting device 1B shown, first, the primary light 6 emitted by the light source 2 is irradiated toward the front surface 3a of the wavelength converter 3. A large amount of the primary light 6 enters the wavelength converter 3 from the front surface 3a of the wavelength converter 3, and the other part is reflected from the front surface 3a. With respect to the wavelength converter 3, the first phosphor 4 excited by the primary light 6 emits the first wavelength converted light 7, and the first wavelength converted light 7 is emitted from the front surface 3a.
[0100] At once Figure 8In the light emitting device 1C shown, first, the primary light 6 emitted by the light source 2 is irradiated to the front surface 3a of the wavelength converter 3A. A large amount of the primary light 6 enters the wavelength converter 3A from the front surface 3a of the wavelength converter 3A, and the other part is reflected from the front surface 3a. In the wavelength converter 3A, the second phosphor 8 excited by the primary light 6 emits the second wavelength converted light 9, and the first phosphor 4 excited by the primary light 6 emits the first wavelength converted light 7. Then, the first wavelength converted light 7 and the second wavelength converted light 9 are emitted from the front surface 3a.
[0101] In the light-emitting device of this embodiment, the sum of the energy E1 of the excitation light emitted by the light source 2 and the energy E2 of the fluorescence emitted by the first phosphor 4 is smaller than the band gap energy Eg of the mother crystal constituting the first phosphor 4. Therefore, even if the excitation light with high light energy density is irradiated, the possibility of the electrons of the activator transitioning from the excited state to the conduction band (CB) becomes smaller. Therefore, even if a phosphor with a long luminescence lifetime is used as the first phosphor 4, the saturation of the fluorescence output emitted by the phosphor can be suppressed and the intensity (brightness) of the light emitted by the phosphor can be increased.
[0102] Thus, the light emitting devices 1, 1A, 1B, and 1C of the present embodiment include a light source 2 and a first phosphor 4, and the light source 2 radiates light with an energy density exceeding 0.5 W / mm 2 The primary light 6 of the first phosphor 4 is absorbed by the first phosphor 4 and converted into the first wavelength converted light 7 having a longer wavelength than the primary light 6. The compound that becomes the matrix of the first phosphor 4 is a simple oxide having a metal element as one kind or a composite oxide having a plurality of such simple oxides of different kinds as terminal components. Moreover, when the energy conversion value of the peak wavelength of the primary light 6 is E1 electron volt and the energy conversion value of the fluorescence peak wavelength of the first wavelength converted light 7 is E2 electron volt, the band gap energy Eg of the crystal of the simple oxide is larger than the sum of E1 and E2. In the light-emitting device, as the matrix compound of the first phosphor 4, a compound is used in which the phenomenon that the excited electrons are not easily excited to the conduction band of the matrix compound and deactivated even when the energy of the primary light 6 is applied to the electrons in the excited state in the activator at a high density is used. Therefore, even in the case of using a long afterglow phosphor having the property of not easily relaxing energy from the excited state to the ground state, the light-emitting device becomes a light-emitting device with small fluorescence output saturation (a phenomenon in which the fluorescence intensity of the phosphor is saturated when the light density irradiated to the phosphor is increased).
[0103] The light emitting device 1, 1A, 1B, 1C of the present embodiment is preferably a medical light source or a medical lighting device. The light emitting device 1, 1A, 1B, 1C can emit a wide near-infrared light with high output, and pass through the "biological window" to excite the fluorescent drug or photosensitizer taken into the body. Therefore, by using the light emitting device 1, 1A, 1B, 1C as a medical light source or a medical lighting device, the fluorescent drug or photosensitizer can fully function and a great therapeutic effect can be obtained.
[0104] The light emitting devices 1, 1A, 1B, 1C of this embodiment can also be used for optical coherence tomography (OCT) and the like. In addition, the light emitting devices 1, 1A, 1B, 1C are preferably medical light emitting devices for fluorescence imaging or photodynamic therapy. Fluorescence imaging and photodynamic therapy are medical technologies that are expected to be widely used and are highly practical. Moreover, the light emitting devices 1, 1A, 1B, 1C pass through the "biological window" and irradiate the interior of the organism with high-output light with a wide near-infrared range, which can enable the fluorescent agents and photosensitizers taken into the organism to fully function, so a large therapeutic effect can be expected.
[0105] Fluorescence imaging is a method described as follows: a fluorescent agent that selectively binds to a lesion such as a tumor is administered to a subject, and then the fluorescent agent is excited by specific light, and the fluorescence emitted by the fluorescent agent is detected and imaged by an image sensor, thereby observing the lesion. According to the fluorescence imaging method, lesions that are difficult to observe can be observed only with normal lighting. As a fluorescent agent, an agent that absorbs excitation light in the near-infrared light region and further emits fluorescence in the near-infrared light region with a wavelength longer than that of the excitation light can be used. As a fluorescent agent, for example, at least one selected from indocyanine green (ICG), phthalocyanine compounds, sodium talaporfin compounds, and dipicolylcyanine (DIPCY) compounds can be used.
[0106] Photodynamic therapy is a treatment method as follows: a photosensitive agent that selectively binds to a target biological tissue is administered to a subject, and then near-infrared rays are irradiated to the photosensitive agent. If near-infrared rays are irradiated to the photosensitive agent, active oxygen is generated by the photosensitive agent, thereby being able to treat lesions such as tumors and infections. As the photosensitive agent, for example, at least one selected from phthalocyanine compounds, porphyrin compounds, chlorin compounds, bacteriochlorin compounds, psoralen compounds, porfimer sodium compounds, and talaporfin sodium compounds can be used.
[0107] The light emitting device 1, 1A, 1B, 1C of this embodiment can also be made into a light source for a sensing system or a lighting system for a sensing system. In the light emitting device 1, 1A, 1B, 1C, a conventional light receiving element having light receiving sensitivity in the near-infrared wavelength region can be used to form a highly sensitive sensing system. Therefore, a light emitting device that can easily miniaturize the sensing system and expand the sensing range can be obtained.
[0108] In addition, in the present embodiment, the phosphor (first phosphor) is preferably a phosphor having a composition formula represented by the following general formula (I).
[0109] (Gd 1-x La x )3(Ga 1-y-z Sc y Cr z )2Ga3O 12 (I)
[0110] (Wherein, x, y and z satisfy 0<x<1, 0<y≤0.60, 0<z<0.2.)
[0111] Such phosphor uses Cr 3+ As an activator, it is possible to efficiently convert high energy density laser light into near infrared light, and even when using laser light, the fluorescence output is not easily saturated. In addition, the phosphor can emit fluorescence with a large light component near 770nm, so that, for example, a light-emitting device suitable for fluorescence imaging can be obtained.
[0112] In addition, the phosphor represented by the general formula (I) can be applied to the light-emitting devices 1, 1A, 1B, and 1C, but the light-emitting devices are not limited thereto. That is, the phosphor represented by the general formula (I) can be used in any light-emitting device that converts the wavelength of primary light and emits near-infrared light. In other words, the light-emitting device can include the phosphor represented by the general formula (I). In addition, such a light-emitting device can be used in any medical device that radiates near-infrared light. In other words, the medical device can include a light-emitting device having the phosphor represented by the general formula (I).
[0113] [Electronic equipment]
[0114] Next, the electronic device of this embodiment is described. The electronic device of this embodiment includes any of the light emitting devices 1, 1A, 1B, and 1C of this embodiment. As described above, the light emitting devices 1, 1A, 1B, and 1C can be expected to have a large therapeutic effect, and it is easy to achieve miniaturization of the sensing system. The electronic device of this embodiment includes the above-mentioned light emitting device, so if it is used for medical equipment or sensing equipment, it can be expected to have a large therapeutic effect and miniaturization of the sensing system.
[0115] The electronic device, for example, includes a light emitting device 1, 1A, 1B, 1C and a light receiving element. The light receiving element is, for example, a sensor such as an infrared sensor that detects light in the near-infrared wavelength region. Furthermore, the electronic device is preferably any device among an information recognition device, a discrimination device, a detection device, or a testing device. As described above, these devices can also easily realize the miniaturization of the sensing system and the expansion of the sensing range.
[0116] The information recognition device is, for example, a driving support system that detects a reflected component of emitted infrared light and recognizes surrounding conditions.
[0117] The distinguishing device is, for example, a device that distinguishes a predetermined irradiated object by utilizing the difference in infrared light components between the irradiating light and the reflected light reflected by the irradiated object.
[0118] The detection device is, for example, a device for detecting liquids. Examples of liquids include water and flammable liquids that are prohibited from being transported by aircraft. Specifically, the detection device may be a device for detecting water attached to glass and water absorbed by objects such as sponges and micropowders. The detection device may visualize the detected liquid. Specifically, the detection device may visualize the distribution information of the detected liquid.
[0119] The inspection device may be any of a medical inspection device, an agricultural and animal husbandry inspection device, a fishery inspection device, or an industrial inspection device, and these devices are useful for inspecting inspection objects in various industries.
[0120] Medical testing devices are, for example, testing devices for testing the health status of humans or animals other than humans. Animals other than humans are, for example, livestock. Medical testing devices are, for example, devices for testing organisms such as fundus examination and blood oxygen saturation examination, and devices for testing organs such as blood vessels and internal organs. Medical testing devices can be devices for testing the inside of a living body, or devices for testing the outside of a living body.
[0121] The inspection device for agriculture and animal husbandry is, for example, a device for inspecting agricultural and animal husbandry products including agricultural products and livestock products. Agricultural products may be, for example, products used as food such as fruits and vegetables and cereals, or may be used as fuel such as oil. Livestock products may be, for example, edible meat and dairy products. The inspection device for agriculture and animal husbandry may be a device for non-destructively inspecting the inside or outside of agricultural and animal husbandry products. The inspection device for agriculture and animal husbandry is, for example, a device for inspecting the sugar content of fruits and vegetables, a device for inspecting the sourness of fruits and vegetables, a device for inspecting the freshness of fruits and vegetables by visualizing leaf veins, a device for inspecting the quality of fruits and vegetables by visualizing scars and internal defects, a device for inspecting the quality of edible meat, a device for inspecting the quality of processed foods obtained by processing milk and edible meat as raw materials, etc.
[0122] The inspection device for fisheries is, for example, a device for inspecting the meat quality of fish such as tuna, or a device for inspecting the presence or absence of shellfish meat in the shell of a shellfish.
[0123] Examples of industrial inspection devices include foreign matter inspection devices, content inspection devices, state inspection devices, and structure inspection devices.
[0124] Examples of foreign matter inspection devices include devices for inspecting foreign matter in liquids placed in containers such as beverages and liquid medicines, devices for inspecting foreign matter in packaging materials, devices for inspecting foreign matter in printed images, devices for inspecting foreign matter in semiconductors and electronic components, devices for inspecting foreign matter such as bone residues, garbage and engine oil in foods, devices for inspecting foreign matter in processed foods in containers, and devices for inspecting foreign matter inside medical devices such as plasters, drugs and quasi-drugs.
[0125] Examples of content inspection devices include devices for inspecting the content of liquid in containers for beverages and liquid medicines, devices for inspecting the content of processed foods in containers, and devices for inspecting the asbestos content in building materials.
[0126] The state inspection device is, for example, a device that inspects the packaging state of the packaging material and a device that inspects the printing state of the packaging material.
[0127] The inspection device for the structure is, for example, an internal non-destructive inspection device and an external non-destructive inspection device for composite members or composite components such as resin products. As a specific example of a resin product, for example, a metal brush having a portion of a metal wire buried in a resin can be used to inspect the bonding state of the resin and the metal.
[0128] The electronic device of this embodiment can use color night vision technology. Color night vision technology is a technology that uses the correlation between the reflection intensity of visible light and infrared light to assign RGB signals to each wavelength of infrared light to colorize the image. According to color night vision technology, a color image can be obtained only with infrared light, so it is particularly suitable for crime prevention devices, etc.
[0129] As described above, the electronic device includes the light emitting devices 1, 1A, 1B, and 1C. In addition, when the light emitting devices 1, 1A, 1B, and 1C include a power source, a light source 2, and a wavelength converter 3, 3A, it is not necessary to accommodate all of them in one housing. Therefore, the electronic device of this embodiment can also provide an inspection method with excellent operability, high precision, and compactness.
[0130] [Test method]
[0131] Next, the inspection method of this embodiment is described. As described above, the electronic device having the light emitting device 1, 1A, 1B, 1C can be used as an inspection device. That is, the inspection method of this embodiment can use the light emitting device 1, 1A, 1B, 1C. Thus, it is possible to provide an inspection method with excellent operability, high precision, and compactness.
[0132] [Medical Devices]
[0133] Next, a medical device according to the present embodiment will be described. Specifically, as an example of the medical device, an endoscope including a light emitting device and an endoscope system using the endoscope will be described.
[0134] The endoscope of this embodiment includes the above-mentioned light emitting devices 1, 1A, 1B, and 1C. Fig. 9 As shown, the endoscope 11 includes a scope 110 , a light source connector 111 , a mounting adapter 112 , a relay lens 113 , a camera head 114 , and an operation switch 115 .
[0135] The mirror 110 is a thin and long light-guiding member that can guide light from the end to the front end, and is inserted into the body when used. The mirror 110 has an imaging window 110z at the front end, and an optical material such as optical glass or optical plastic is used in the imaging window 110z. The mirror 110 further has an optical fiber that guides the light introduced by the light source connector 111 to the front end and an optical fiber that transmits the optical image injected from the imaging window 110z.
[0136] The mount adapter 112 is a member for mounting the mirror 110 on the camera 114. Various mirrors 110 are detachably mounted on the mount adapter 112.
[0137] The light source connector 111 introduces illumination light from the light emitting device to illuminate the affected part in the body. In this embodiment, the illumination light includes visible light and near infrared light. The light introduced into the light source connector 111 is guided to the front end of the mirror 110 via the optical fiber and illuminates the affected part in the body through the imaging window 110z. Fig. 9 As shown, a transmission cable 111z for guiding illumination light from the light emitting device to the mirror 110 is connected to the light source connector 111. The transmission cable 111z may also include an optical fiber.
[0138] The relay lens 113 focuses the optical image transmitted from the mirror 110 onto the imaging surface of the image sensor. In addition, the relay lens 113 can move the lens according to the operation amount of the operation switch 115 to adjust the focus and magnification.
[0139] The camera head 114 has a dichroic prism inside. The dichroic prism decomposes the light focused by the relay lens 113 into R light (red light), G light (green light), and B light (blue light). In addition, the dichroic prism can further decompose IR light (near infrared light). Thus, the endoscope 11 that can identify the lesion part by using the fluorescence imaging method using near infrared light is obtained.
[0140] Furthermore, the camera head 114 has an image sensor as a detector inside. The image sensor converts the optical image formed on each imaging surface into an electrical signal. The image sensor is not particularly limited, and at least one of CCD (Charge Coupled Device) and CMOS (Complementary Metal Oxide Semiconductor) can be used. The image sensor is, for example, a dedicated sensor that receives light of B component (blue component), R component (red component) and G component (green component), respectively. In addition, the camera head 114 may further have a dedicated sensor that receives IR component (near infrared light component). Thus, the endoscope 11 that can identify a specific lesion site by using a fluorescence imaging method using near infrared light is obtained.
[0141] The camera head 114 may have a color filter inside to replace the dichroic prism. A color filter is provided on the imaging surface of the image sensor. For example, three color filters are provided, and the three color filters receive the light focused by the relay lens 113 and selectively transmit R light (red light), G light (green light), and B light (blue light). In addition, by further providing a color filter that selectively transmits IR light (near infrared light), the endoscope 11 that can identify a lesion using a fluorescence imaging method using near infrared light is obtained.
[0142] In the case of using a fluorescence imaging method using near-infrared light, the color filter that selectively transmits IR light preferably has a blocking film that cuts off the reflected component of near-infrared light (IR light) contained in the illumination light. As a result, only the fluorescence formed by IR light emitted by the fluorescent agent used in the fluorescence imaging method is imaged on the imaging surface of the image sensor for IR light. Therefore, it becomes easy to clearly observe the affected part that is illuminated by the fluorescent agent.
[0143] In addition, if Fig. 9 As shown, the camera 114 is connected to a signal cable 114 z for transmitting an electrical signal from the image sensor to the CCU 12 described later.
[0144] In the endoscope 11 having such a configuration, light from the subject passes through the mirror 110 and is guided to the relay lens 113 , and then passes through the dichroic prism in the camera head 114 to form an image on the image sensor.
[0145] like Fig.10 As shown, an endoscope system 100 of the present embodiment includes an endoscope 11 for capturing images inside a subject, a CCU (Camera Control Unit) 12, light emitting devices 1, 1A, 1B, 1C, and a display device 13 such as a monitor.
[0146] The CCU 12 includes at least an RGB signal processing unit, an IR signal processing unit, and an output unit. The CCU 12 implements the functions of the RGB signal processing unit, the IR signal processing unit, and the output unit by executing a program stored in a memory inside or outside the CCU 12 .
[0147] The RGB signal processing unit converts the electrical signals of the B component, R component, and G component from the image sensor into image signals that can be displayed on the display device 13 and outputs them to the output unit. In addition, the IR signal processing unit converts the electrical signals of the IR component from the image sensor into image signals and outputs them to the output unit.
[0148] The output unit outputs at least one of the image signals of the RGB color components and the image signal of the IR component to the display device 13. For example, the output unit outputs the image signal based on any one of the synchronous output mode and the superimposed output mode.
[0149] In the synchronous output mode, the output unit synchronously outputs the RGB image and the IR image through different screens. In the synchronous output mode, the RGB image and the IR image can be compared on different screens to observe the affected part. In the overlapped output mode, the output unit outputs a composite image formed by overlapping the RGB image and the IR image. In the overlapped output mode, for example, the affected part luminesced by the fluorescent agent used in the fluorescence imaging method can be clearly observed in the RGB image.
[0150] The display device 13 displays an image of an object such as an affected part on a screen based on an image signal from the CCU 12. In the case of the synchronous output mode, the display device 13 divides the screen into a plurality of screens, and displays the RGB image and the IR image in parallel on each screen. In the case of the overlap output mode, the display device 13 displays a composite image formed by overlapping the RGB image and the IR image on one screen.
[0151] As described above, the endoscope 11 of this embodiment includes the light emitting devices 1, 1A, 1B, and 1C, and radiates the first wavelength converted light 7 from the imaging window 110z of the endoscope 110. Therefore, by using the endoscope 11, the fluorescent agent and the photosensitizing agent taken into the body can be efficiently excited and the fluorescent agent and the photosensitizing agent can fully function.
[0152] In addition, when the endoscope 11 includes the light emitting device 1A or 1C including the second phosphor 8, the endoscope 11 radiates the second wavelength converted light 9 as visible light in addition to the first wavelength converted light 7. Therefore, by using the endoscope system 100, the position of the affected part can be identified and the first wavelength converted light 7 can be irradiated to the affected part.
[0153] The endoscope 11 of this embodiment preferably further includes a detector for detecting the fluorescence emitted by the fluorescent agent that absorbs the first wavelength converted light 7. By providing the endoscope 11 with a detector for detecting the fluorescence emitted by the fluorescent agent in addition to the light emitting devices 1, 1A, 1B, 1C, the affected part can be identified only by the endoscope. Therefore, it is not necessary to open the abdomen as in the past to identify the affected part, so that the patient can be diagnosed and treated with less burden. In addition, the doctor using the endoscope 11 can accurately grasp the affected part, so the treatment efficiency can be improved.
[0154] The medical device of this embodiment is preferably used in any method of fluorescence imaging or photodynamic therapy. The medical device can irradiate the inside of a living body with high output light with a wide near-infrared range to make the fluorescent agent and photosensitivity agent taken into the living body fully function, so a large therapeutic effect can be expected. In addition, such a medical device is conducive to miniaturization and cheapness because it uses a relatively simple light-emitting device 1, 1A, 1B, 1C.
[0155] Example 1
[0156] Next, the light emitting device of this embodiment will be described in further detail with reference to Example 1, but this embodiment is not limited thereto.
[0157] [Preparation of phosphor]
[0158] (Example 1-1)
[0159] The oxide phosphor used in Example 1-1 was synthesized using a preparation method utilizing a solid phase reaction. The phosphor of Example 1-1 is composed of (Al 0.99 ,Cr 0.01 )2O3 is an oxide phosphor. In addition, the phosphor of Example 1-1 is Cr 3+ Activate the phosphor.
[0160] When synthesizing the oxide phosphor of Example 1-1, the following compound powders were used as main raw materials.
[0161] Alumina hydroxide (AlOOH): Purity 2N5, manufactured by Kawai Lime Industry Co., Ltd.
[0162] Chromium oxide (Cr2O3): Purity is 3N, made by High Purity Chemical Research Institute Co., Ltd.
[0163] First, a compound (Al 0.99 ,Cr 0.01 )2O3 was used to weigh the above raw materials. Next, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, a slurry-like mixed raw material containing pure water and raw materials was obtained. After that, the slurry-like mixed raw material was dried in full using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0164] Next, the sintered raw material was transferred to a small alumina crucible and sintered in a box-type electric furnace at 1500°C in the atmosphere for 4 hours. The heating and cooling rate during sintering was set at 400°C / hour. 0.99 ,Cr 0.01 )2O3 is a composition formula representing the phosphor of Example 1-1.
[0165] (Example 1-2)
[0166] The oxide phosphor used in Example 1-2 was synthesized using a preparation method utilizing a solid phase reaction. The phosphor of Example 1-2 is composed of Gd3(Ga 0.97 ,Cr 0.03 )5O 12 The phosphor of Example 1-2 is Cr 3+ Activate the phosphor.
[0167] When synthesizing the oxide phosphor of Example 1-2, the following compound powders were used as main raw materials.
[0168] Gadolinium oxide (Gd2O3): Purity 3N, manufactured by Wako Pure Chemical Industries, Ltd.
[0169] Gallium oxide (Ga2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0170] Chromium oxide (Cr2O3): Purity is 3N, made by High Purity Chemical Research Institute Co., Ltd.
[0171] First, a compound Gd3(Ga 0.97 ,Cr 0.03 )5O 12 The raw materials were weighed in a manner. Then, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, a slurry-like mixed raw material containing pure water and the raw materials was obtained. After that, the slurry-like mixed raw material was completely dried using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0172] Next, the sintered raw material was transferred to a small alumina crucible and sintered in a box-type electric furnace at 1500°C in the atmosphere for 4 hours. The heating and cooling rate during sintering was set at 400°C / hour. 0.97 ,Cr 0.03 )5O 12 The phosphor of Example 1-2 is represented by the composition formula.
[0173] (Example 1-3)
[0174] The oxide phosphor used in Examples 1-3 was synthesized using a solid phase reaction preparation method. The phosphors in Examples 1-3 were composed of (Ga 0.99 ,Cr 0.01 )2O3. In addition, the phosphor of Example 1-3 is Cr 3+ Activate the phosphor.
[0175] When synthesizing the oxide phosphors of Examples 1-3, the following compound powders were used as main raw materials.
[0176] Gallium oxide (Ga2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0177] Chromium oxide (Cr2O3): Purity is 3N, made by High Purity Chemical Research Institute Co., Ltd.
[0178] First, a compound (Ga 0.99 ,Cr 0.01)2O3 was used to weigh the above raw materials. Next, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, a slurry-like mixed raw material containing pure water and raw materials was obtained. After that, the slurry-like mixed raw material was dried in full using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0179] Next, the sintered raw material was transferred to a small alumina crucible and sintered in a box-type electric furnace at 1500°C in the atmosphere for 4 hours. In addition, the heating and cooling rate during sintering was set to 400°C / hour. 0.99 ,Cr 0.01 )2O3 is a composition formula representing the phosphor of Examples 1-3.
[0180] (Reference Example 1-1)
[0181] As the oxide phosphor of Reference Example 1-1, (Y,Ce)3Al5O 12 The phosphor of Reference Example 1-1 is Ce 3+ Activate the phosphor. As the phosphor, model Y996 manufactured by Nemoto Specialty Chemical Co., Ltd. was used.
[0182] (Reference Example 1-2)
[0183] As the oxide phosphor of Reference Example 1-2, a phosphor represented by the composition formula of (Sr, Ca, Eu)AlSiN3 was used. 2+ Activated phosphor: The phosphor used was BR-102C manufactured by Mitsubishi Chemical Corporation.
[0184] [evaluate]
[0185] (Luminescence lifetime measurement)
[0186] The luminescence lifetime (1 / e decay time) of the phosphors of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2 was measured using a luminescence lifetime measuring device (Quantaurus-Tau compact luminescence lifetime measuring device manufactured by Hamamatsu Photonics Co., Ltd.). The luminescence lifetime measurement results are shown in Tables 3 and Fig.11 .
[0187] Table 3
[0188] Composition Abbreviation 1 / e decay time (μs) Example 1-1 <![CDATA[(Al 0.99 ,Cr 0.01 )2O3]]> <![CDATA[Al2O3:Cr 3+ ]]> 1895 Example 1-2 <![CDATA[Gd3(Ga 0.97 ,Cr 0.03 )5O 12 ]]> <![CDATA[GGG:Cr 3+ ]]> 104 Examples 1-3 <![CDATA[(Ga 0.99 ,Cr 0.01 )2O3]]> <![CDATA[Ga2O3:Cr 3+ ]]> 77 Reference Example 1-1 <![CDATA[(Y,Ce)3Al5O 12 ]]> <![CDATA[YAG:Ce 3+ ]]> 0.06 Reference Example 1-2 <![CDATA[(Sr,Ca,Eu)AlSiN3]]> <![CDATA[S-CASN:Eu 2+ ]]> 0.676
[0189] As shown in Table 3 and Fig.11As shown in the figure, the luminescence lifetime (1 / e decay time) of the phosphors of Examples 1-1 to 1-3 is 77 μs or more, which is similar to that of Ce in Reference Example 1-1. 3+ Activated phosphor and Eu of Reference Example 1-2 2+ The luminescence lifetime is more than 100 times longer than that of activated phosphors.
[0190] (Spectral characteristics)
[0191] Next, the fluorescence spectra of the phosphors of Examples 1-1 to 1-3 were measured using a quantum yield measuring device (absolute PL quantum yield measuring device C9920-02, manufactured by Hamamatsu Photonics Co., Ltd.) to determine the fluorescence peak wavelength. In addition, the excitation wavelength during the fluorescence spectrum measurement was set to 450 nm (E1 = 2.76 eV). The fluorescence peak wavelengths of the phosphors of Examples 1-1 to 1-3 and the energy conversion values (E2) of the fluorescence peak wavelengths are shown in Table 4. Table 4 further shows the sum (E1+E2) of the energy conversion value (E1) of the excitation light with a peak wavelength of 450 nm and the energy conversion value (E2) of the fluorescence peak wavelength in the phosphors of Examples 1-1 to 1-3. In addition, Table 4 also shows the band gap energy (Eg) of the parent crystals constituting the phosphors of Examples 1-1 to 1-3.
[0192] Table 4
[0193]
[0194] (Fluorescence output saturation characteristics)
[0195] Next, wavelength conversion devices were prepared using the phosphors of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2, and the fluorescence output saturation characteristics of each phosphor were evaluated. Specifically, first, using a mortar and pestle, the phosphor powders of each Example and Reference Example were mixed with a sealing material so that the filling rate of the phosphor was 40% by volume, thereby preparing a phosphor paste. In addition, the sealing material used was polysilsesquioxane (RSiO) manufactured by Konishi Chemical Industry Co., Ltd. 1.5 ), Grade: SR-13.
[0196] Next, if Fig.12As shown in the figure, a sapphire substrate 203 (9 mm in length, 9 mm in width, and 0.5 mm in thickness) is prepared, in which a dichroic mirror 201 is provided on one side and an anti-reflection coating (AR coating) 202 is provided on the other side. Then, the above-mentioned phosphor paste is applied to the surface of the dichroic mirror 201 in the sapphire substrate by screen printing. The screen printing plate used for screen printing is a circular screen printing plate with a mesh size of 74 μm (200 mesh) and a diameter of 7.8 mm. Then, the sapphire substrate 203 coated with the phosphor paste is heat-treated at 200° C. for 2 hours to cure the sealing material, thereby obtaining a wavelength conversion device 200 having a phosphor layer 204 containing a phosphor according to each embodiment and reference example.
[0197] Next, use Fig.13 The evaluation device shown measures the luminous intensity of each phosphor. Specifically, first, the wavelength conversion device 200 of each embodiment and reference example obtained as described above is placed in the center of the integrating sphere 300. Next, the blue laser (peak wavelength: 450 nm) emitted by the blue laser diode element 301 disposed outside the integrating sphere 300 is guided to the center of the integrating sphere 300 by the optical fiber 302 and irradiated to the wavelength conversion device 200. Then, the luminous characteristics of the fluorescence emitted by the wavelength conversion device 200 are measured by the multi-channel spectrometer 304 connected to the integrating sphere 300 via the optical fiber 303. In addition, as Fig.13 As shown, a collimator lens 305 is sandwiched between the blue laser diode element 301 and the light incident end of the optical fiber 302 .
[0198] Here, the blue laser diode element is usually CW driven (Continuous Wave). Therefore, as the power density of the excitation light increases, the heat generated by the phosphor increases, and the phosphor undergoes temperature quenching. Therefore, in order to separate the temperature quenching of the phosphor from the light output saturation, the function generator 306 and the current amplifier 307 are used to convert the blue laser emitted by the blue laser diode element 301 into pulse light with a frequency of 100 Hz and a duty cycle of 1%. That is, Fig.14 As shown, in a cycle of 10 msec, the time for irradiating the phosphor with the blue laser light is set to 100 μsec, and the remaining time is set to the cooling time of the phosphor.
[0199] Furthermore, by setting the irradiation area of the blue laser to the wavelength conversion device 200 to 0.6 mm Φ and increasing the rated output of the blue laser from 0.16 W / mm 2 Change to 4.00W / mm 2 , the fluorescence output saturation of the phosphors of each embodiment and reference example was evaluated.
[0200] Fig.15It shows that the laser energy is increased from 0.16W / mm 2 Change to 4.00W / mm 2 The relative intensity of the fluorescence emitted by the fluorescent body at the time. Fig.15 As shown, for the phosphors of Examples 1-1 to 1-3 and Reference Examples 1-1 to 1-2, even if the energy density of the laser is increased from 0.16 W / mm 2 Increased to 4.00W / mm 2 That is, it is known that not only the phosphors of Reference Examples 1-1 to 1-2 with short luminescence lifetimes but also the phosphors of Examples 1-1 to 1-3 with long luminescence lifetimes can emit high-energy fluorescence without causing fluorescence output saturation.
[0201] In addition, as shown in Table 4, the sum of E1 and E2 in the phosphors of Examples 1-1 to 1-3 is smaller than the band gap energy Eg of the parent crystal. Therefore, by appropriately adjusting the wavelength of the excitation light and the band gap energy and emission wavelength of the phosphor, even when a high-energy laser is used as the excitation light, the occurrence of excited state absorption (ESA) can be reduced and the fluorescence output saturation can be suppressed.
[0202] Example 2
[0203] Next, the phosphor represented by the general formula (I) that can be used in the light-emitting device of this embodiment will be described in further detail through Example 2, but this embodiment is not limited thereto.
[0204] [Preparation of phosphor]
[0205] (Reference Example 2-1)
[0206] The oxide phosphor used in Reference Example 2-1 was synthesized using a preparation method utilizing a solid phase reaction. The phosphor in Reference Example 2-1 is composed of (Gd 0.75 La 0.25 )3(Ga 0.97 Cr 0.03 )2Ga3O 12 The phosphor of Reference Example 2-1 is Cr 3+ Activate the phosphor.
[0207] When synthesizing the oxide phosphor of Reference Example 2-1, the following compound powders were used as main raw materials.
[0208] Gadolinium oxide (Gd2O3): Purity 3N, manufactured by Wako Pure Chemical Industries, Ltd.
[0209] Lanthanum oxide (La2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0210] Gallium oxide (Ga2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0211] Chromium oxide (Cr2O3): Purity is 3N, made by High Purity Chemical Research Institute Co., Ltd.
[0212] First, a compound (Gd 0.75 La 0.25 )3(Ga 0.97 Cr 0.03 )2Ga3O 12 The raw materials were weighed in a manner. Next, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, a slurry-like mixed raw material containing pure water and the raw materials was obtained. Afterwards, the slurry-like mixed raw material was dried in its entirety using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0213] Next, the calcined raw material was transferred to a small alumina crucible and calcined in an atmosphere at 1450°C for 1 hour using a box-type electric furnace. The temperature rise and fall rate during calcination was set to 400°C / hour. Thus, the phosphor of Reference Example 2-1 was obtained. The body color of the obtained phosphor was dark green.
[0214] (Example 2-1)
[0215] The oxide phosphor used in Example 2-1 was synthesized using a preparation method utilizing a solid phase reaction. The phosphor of Example 2-1 is composed of (Gd 0.75 La 0.25 )3(Ga 0.90 Sc 0.07 Cr 0.03 )2Ga3O 12 The phosphor of Example 2-1 is Cr 3+ Activate the phosphor.
[0216] When synthesizing the oxide phosphor of Example 2-1, the following compound powders were used as main raw materials.
[0217] Gadolinium oxide (Gd2O3): Purity 3N, manufactured by Wako Pure Chemical Industries, Ltd.
[0218] Lanthanum oxide (La2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0219] Gallium oxide (Ga2O3): Purity 4N, manufactured by Wako Pure Chemical Industries, Ltd.
[0220] Scandium oxide (Sc2O3): Purity 4N, manufactured by Shin-Etsu Chemical Co., Ltd.
[0221] Chromium oxide (Cr2O3): Purity is 3N, made by High Purity Chemical Research Institute Co., Ltd.
[0222] First, for the phosphor of Example 2-1, (Gd 0.75 La 0.25 )3(Ga 0.90 Sc 0.07 Cr 0.03 )2Ga3O 12 The raw materials were weighed in the form of a compound having a stoichiometric composition. Next, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, a slurry-like mixed raw material containing pure water and the raw materials was obtained. Afterwards, the slurry-like mixed raw material was dried in full using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0223] Next, the calcined raw material was transferred to a small alumina crucible and calcined in an atmosphere at 1450°C for 1 hour using a box-type electric furnace. The temperature rise and fall rate during calcination was set to 400°C / hour. Thus, the phosphor of Example 2-1 was obtained. The body color of the obtained phosphor was dark green.
[0224] (Example 2-2, Example 2-3, Example 2-4 and Reference Example 2-2)
[0225] The oxide phosphors used in Examples 2-2, 2-3, 2-4 and Reference Example 2-2 were synthesized using a solid phase reaction preparation method. The phosphors in Examples 2-2, 2-3 and 2-4 were respectively composed of (Gd 0.75 La 0.25 )3(Ga 0.75 Sc 0.22 Cr 0.03 )2Ga3O 12 , (Gd 0.75 La 0.25 )3(Ga 0.50 Sc 0.47 Cr 0.03 )2Ga3O 12 , (Gd 0.75 La 0.25 )3(Ga 0.38 Sc 0.59 Cr 0.03 )2Ga3O 12 The phosphor of Reference Example 2-2 is composed of (Gd 0.75 La0.25 )3(Ga 0.25 Sc 0.72 Cr 0.03 )2Ga3O 12 In addition, the phosphors of Example 2-2, Example 2-3, Example 2-4 and Reference Example 2-2 are all Cr 3+ Activate the phosphor.
[0226] First, for the phosphors of Example 2-2, Example 2-3 and Example 2-4, respectively, 0.75 La 0.25 )3(Ga 0.75 Sc 0.22 Cr 0.03 )2Ga3O 12 , (Gd 0.75 La 0.25 )3(Ga 0.50 Sc 0.47 Cr 0.03 )2Ga3O 12 , (Gd 0.75 La 0.25 )3(Ga 0.38 Sc 0.59 Cr 0.03 )2Ga3O 12 The above raw materials were weighed in a manner to form a compound with a stoichiometric composition. Further, for the phosphor of Reference Example 2-2, (Gd 0.75 La 0.25 )3(Ga 0.25 Sc 0.72 Cr 0.03 )2Ga3O 12 The raw materials were weighed in the form of a compound of a stoichiometric composition. Next, the weighed raw materials were added to a beaker filled with pure water and stirred for 1 hour using a magnetic stirrer. Thus, slurry-like mixed raw materials containing pure water and raw materials were obtained. Then, each slurry-like mixed raw material was fully dried using a dryer. Then, the dried mixed raw material was crushed using a mortar and pestle to obtain a calcined raw material.
[0227] Next, the calcined raw material was transferred to a small alumina crucible and calcined in an atmosphere at 1550°C for 1 hour using a box-type electric furnace. In addition, the temperature rise and fall rate during calcination was set to 400°C / hour. Thus, the phosphors of Example 2-2, Example 2-3, Example 2-4 and Reference Example 2-2 were obtained. The body color of the obtained phosphors was dark green.
[0228] [evaluate]
[0229] (Crystal structure analysis)
[0230] The crystal structures of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 were evaluated using an X-ray diffractometer (desktop X-ray diffractometer MiniFlex (registered trademark), manufactured by Rigaku Corporation).
[0231] Fig.16 The X-ray diffraction (XRD) patterns of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are shown respectively. For reference, Fig.16 The garnet compound Gd3Ga2Ga3O registered in ICSD (Inorganic Crystal Structure Database) is also shown. 12 The pattern of Fig.16 It can be determined that the XRD patterns of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are similar to those of Gd3Ga2Ga3O 12 This indicates that the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are all made of materials having the same structure as Gd3Ga2Ga3O 12 It is mainly composed of compounds with the same crystal structure as garnet.
[0232] From the above results, it can be considered that the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are compounds represented by the composition formulas shown in Table 5. Table 5 also shows the scandium concentration (y value) in each phosphor.
[0233] Table 5
[0234]
[0235] (Spectral characteristics)
[0236] Next, the fluorescence spectra and internal quantum efficiencies of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 were evaluated using a quantum yield measurement device (absolute PL quantum yield measurement device C9920-02, manufactured by Hamamatsu Photonics Co., Ltd.). Fig.17 The fluorescence spectra of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are shown. In addition, the excitation wavelength during the fluorescence spectrum measurement was set to 450 nm. Fig.17 In the figures, the fluorescence spectra are all normalized by setting the emission peak to 1.
[0237] The fluorescence spectra of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are all considered to be caused by Cr 3+The wide spectrum of dd transition. Moreover, as shown in Table 5, the peak wavelengths of the fluorescence spectra of the phosphors of Examples 2-1 to 2-4 are 759nm, 760nm, 766nm and 770nm, respectively. In addition, the peak wavelengths of the fluorescence spectra of the phosphors of Reference Examples 2-1 and 2-2 are 750nm and 766nm, respectively. This means that the fluorescence spectra of the phosphors of Examples 2-1 to 2-4 and Reference Example 2-2 overlap more with the excitation spectrum of indocyanine green (ICG) (excitation peak wavelength: about 780nm) than the fluorescence spectrum of the phosphor of Reference Example 2-1.
[0238] As shown in Table 5, the internal quantum efficiencies of the phosphors of Examples 2-1 to 2-4 were 69%, 78%, 76% and 61%, respectively. The internal quantum efficiencies of the phosphors of Reference Examples 2-1 and 2-2 were 80% and 46%, respectively.
[0239] Next, the extent to which indocyanine green (ICG), a drug suitable for fluorescence imaging, can absorb the fluorescence of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 was calculated. Fig.18 The relative values of ICG absorption efficiency of the phosphors of Examples 2-1 to 2-4 and Reference Examples 2-1 to 2-2 are shown. Here, the "relative value of ICG absorption efficiency" refers to the value obtained by multiplying the relative value of the intensity of the ICG excitation spectrum at the fluorescence peak wavelength of each phosphor by the internal quantum efficiency (%) of each phosphor, when the excitation spectrum intensity of ICG at a wavelength of 780 nm is 100.
[0240] Specifically, if Fig.19 As shown, in the case of the phosphor of Example 2-1, the fluorescence peak wavelength is 759nm, so the relative value of the intensity of the excitation spectrum of ICG at the fluorescence peak wavelength is 80. Moreover, the internal quantum efficiency of the phosphor of Example 2-1 is 69%. Therefore, the relative value of the ICG absorption efficiency of the phosphor of Example 2-2 becomes 55.2. In the case of the phosphor of Example 2-2, the fluorescence peak wavelength is 760nm, so the relative value of the intensity of the excitation spectrum of ICG at the fluorescence peak wavelength is 80. Moreover, the internal quantum efficiency of the phosphor of Example 2-2 is 78%. Therefore, the relative value of the ICG absorption efficiency of the phosphor of Example 2-2 becomes 62.4. The relative values of the ICG absorption efficiency of the phosphors of Examples 2-3 and 2-4 were also calculated in the same way, and the results were 64.6 and 54.9, respectively. The relative values of the ICG absorption efficiency of the phosphors of Reference Examples 2-1 and 2-2 were also calculated in the same way, and the results were 48.0 and 39.1, respectively.
[0241] like Fig.18As shown, the relative values of ICG absorption efficiency of Examples 2-1 to 2-4 are higher than those of Reference Examples 2-1 and 2-2. This result shows that the phosphors of Examples 2-1 to 2-4, i.e., the phosphors represented by the general formula (I), have high ICG absorption efficiency and are preferred as light-emitting devices suitable for fluorescence imaging.
[0242] As mentioned above, although the content of this embodiment was demonstrated based on an Example, it is obvious to a person skilled in the art that this embodiment is not limited to these description contents, and various deformation|transformation and improvement are possible.
[0243] The entire contents of Tokugan 2019-098537 (filing date: May 27, 2019) are incorporated herein by reference.
[0244] Industrial Applicability
[0245] According to the present application, it is possible to provide a light-emitting device capable of suppressing saturation of fluorescence output emitted by a phosphor even when a phosphor with a long emission lifetime is used, and an electronic device and an inspection method using the light-emitting device.
[0246] Explanation of symbols
[0247] 1, 1A, 1B, 1C Light-emitting device
[0248] 2 Light Source
[0249] 3. 3A wavelength converter
[0250] 4. First phosphor
[0251] 6 Primary Light
[0252] 7 First wavelength converted light
[0253] 8 Second phosphor
[0254] 9 Second wavelength converted light
Claims
1. A light emitting device comprising a light source and a first phosphor, The light source radiates light with an energy density exceeding 0.5 W / mm 2 The primary light, The first phosphor absorbs the primary light and converts the primary light into first wavelength-converted light having a wavelength longer than that of the primary light. in, The compound that becomes the matrix of the first phosphor is a composite oxide composed of a plurality of simple oxides of different types as terminal components, wherein the simple oxide is an oxide containing a metal element as one type, The first phosphor is a phosphor having a composition formula represented by the following general formula (I), (Gd 1-x La x )3(Ga 1-y-z Sc y Cr z )2Ga3O 12 (I) Where x, y and z satisfy 0<x<1, 0<y≤0.60, 0<z<0.2, When the energy conversion value of the peak wavelength of the primary light is E1 electron volt and the energy conversion value of the fluorescence peak wavelength of the first wavelength converted light is E2 electron volt, the band gap energy of the simple oxide crystal is greater than the sum of E1 and E2.
2. The light emitting device according to claim 1, wherein: The band gap energy of the simple oxide crystal is 4.6 eV or more.
3. The light emitting device according to claim 1 or 2, wherein: The first phosphor contains at least one element selected from the group consisting of Al, Ga, and Sc in the crystal of the compound serving as a matrix.
4. The light emitting device according to claim 1 or 2, wherein: The first wavelength converted light includes fluorescence based on the electronic energy transition of the transition metal ion. The transition metal ion is Cr 3+ .
5. The light emitting device according to claim 4, wherein: In the first phosphor, the cationic element in the crystal of the compound serving as a matrix is formed only of an element taking a trivalent valence.
6. The light emitting device according to claim 1 or 2, wherein: The primary light is violet light having a luminescence peak within a wavelength range of 380 nm to less than 435 nm or blue light having a luminescence peak within a wavelength range of 435 nm to less than 470 nm.
7. The light emitting device according to claim 1 or 2, wherein: The primary light is laser.
8. The light emitting device according to claim 1 or 2, wherein: The first wavelength converted light is near-infrared light having a fluorescence peak in a wavelength range of 700 nm to less than 1000 nm.
9. The light emitting device according to claim 1 or 2, wherein: The first phosphor contains two or more Cr 3+ Activate the phosphor. 10 . The light emitting device according to claim 1 , further comprising a second phosphor that absorbs the primary light and converts the light into a second wavelength converted light having a wavelength longer than that of the primary light and different from the first wavelength converted light.
11. The light-emitting device according to claim 1 or 2, which is a medical light source or a medical lighting device. 12 . The light-emitting device according to claim 1 or 2 , which is a medical light-emitting device used for fluorescence imaging or photodynamic therapy. 13 . The light-emitting device according to claim 1 or 2 , which is a light source for a sensing system or a lighting system for a sensing system. 14 . An electronic device comprising the light emitting device according to claim 1 . 15 . The electronic device according to claim 14 , which is any one of an information recognition device, a discrimination device, a detection device or a testing device.
16. The electronic device according to claim 15, wherein: The inspection device is any of a medical inspection device, an agricultural and animal husbandry inspection device, a fishery inspection device or an industrial inspection device.
17. A testing method using the light emitting device according to any one of claims 1 to 10.
Citation Information
Patent Citations
Light source device
WO2018163830A1
Light-emitting device using fluorophore
CN108028304A
Wavelength converter, and light emitting device, medical system, electronic apparatus, and inspection method using same
CN113711449A
Method of manufacturing fluorescent-material-containing member
US20170241621A1
Endoscope apparatus and method of operating endoscope apparatus
US20180153386A1