A processing method for metal-assisted photochemical etching of silicon carbide nanopore arrays
By plating precious metal layers and deposition of metal masks on silicon carbide wafers, combining polystyrene nanomicrospheres and plasma etching, metal-assisted photochemical etching is solved by using ultraviolet light to solve the slow processing speed of silicon carbide nanopore arrays and The problem of difficult size control has achieved efficient and controllable nanopore array processing.
Patent Information
- Application Number
- CN202111130234.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-26
AI Technical Summary
In the prior art, the processing speed of metal-assisted photochemical etching of silicon carbide nanopore arrays is slow and difficult to control in size, and the traditional wet etching method has low processing selectivity for silicon carbide, resulting in damage to the surface of the substrate material.
Nanopores are controlled by plating a noble metal layer on the bottom surface of the silicon carbide wafer as a catalytic layer and depositing a metal mask that does not react with the etchant on the top surface, combining self-assembled polystyrene nanomicrospheres and plasma etching to control the nanopores by controlling the nanopores by plating the bottom surface of the silicon carbide wafer as a catalytic layer and depositing a metal mask that does not react with the etchant on the top surface The spacing and pore size are used to perform metal-assisted photochemical etching using ultraviolet light to regulate the etching time to achieve controllable nanopore array processing.
The processing rate and size controllability of the silicon carbide nanopore array are significantly improved, and efficient metal-assisted photochemical etching is achieved, solving the problems of slow etching rates and difficult to control in the prior art.
Smart Images

Figure CN113871294B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of silicon carbide etching processing, and in particular to a processing method for metal-assisted photochemical etching of silicon carbide nanopore arrays. Background Art
[0002] As a third-generation semiconductor, silicon carbide is widely used in high-temperature, high-frequency and high-power electronic devices due to its excellent physical and chemical properties. Especially in the field of new energy vehicles, silicon carbide is the first choice for power chip materials. However, due to the good chemical stability of silicon carbide, it is difficult to effectively process it using traditional wet etching methods. Therefore, dry etching is mostly used in industry to process silicon carbide wafers, but due to its low etching selectivity, it is easy to cause damage to the surface of the substrate material. Moreover, dry etching requires vacuum and high temperature, making its equipment relatively expensive. Wet etching has the advantages of high etching selectivity, simple operation and low cost. Therefore, it is urgent to propose an effective and controllable new wet etching method to process silicon carbide.
[0003] At present, the more effective wet etching methods for etching silicon carbide are: anodic etching, metal-assisted anodic etching, photoelectrochemical etching and metal-assisted photochemical etching. Anodic etching, metal-assisted anodic etching and photoelectrochemical etching all require electrical contact with the substrate, with the substrate connected to the anode and the etching liquid connected to the cathode. By applying a certain external bias voltage, an external electric field is generated, so that the holes inside the substrate are gathered at the substrate / etching liquid interface under the action of the electric field, and the hole concentration at the interface is increased, thereby increasing the etching rate and achieving effective etching of silicon carbide. However, due to the uneven distribution of the electric field, the holes or nanowires etched are randomly distributed, and their structural dimensions cannot be precisely controlled.
[0004] Metal-assisted photochemical etching is achieved by depositing a layer of noble metal on the surface of the substrate, which serves as a catalyst layer and a mask, and irradiating the surface with ultraviolet light. The area not covered by the noble metal layer will be etched. Its etching mechanism is as follows: for n-type semiconductors, since the contact potential difference is generated at the contact interface between the noble metal / semiconductor and the etching solution / semiconductor, a positive space charge region will be formed on the semiconductor surface, and the contact barrier of the semiconductor surface in contact with the noble metal is higher than that of the semiconductor surface in contact with the etching solution. Therefore, holes will flow from high barriers to low barriers, that is, holes will gather on the semiconductor surface in contact with the etching solution. At the same time, ultraviolet light irradiation of the semiconductor can generate photogenerated holes on its surface, which further increases the hole concentration on the semiconductor surface in contact with the etching solution, thereby increasing the etching reaction rate.
[0005] Since metal-assisted photochemical etching does not require electrical contact and additional external bias, its processing flow is simpler. However, metal-assisted photochemical etching has the disadvantage of slow etching rate, and the distribution and size of the nanopore array obtained by metal-assisted photochemical etching in preparing silicon carbide nanopore arrays are difficult to control.
[0006] Therefore, it is urgent to propose an efficient and controllable metal-assisted photochemical etching method for processing silicon carbide nanohole arrays, so that the processing rate can be improved, and the distribution and size of the processed nanohole arrays can be controlled. Summary of the invention
[0007] In response to the problems raised by the background technology, the purpose of the present invention is to propose a processing method for metal-assisted photochemical etching of silicon carbide nanopore arrays, by coating a noble metal layer on the bottom surface of a silicon carbide wafer as a catalytic layer and depositing a metal mask that does not react with the etchant on the top surface of the silicon carbide wafer to achieve efficient metal-assisted photochemical etching, and by self-assembling polystyrene nanospheres of different diameters to control the spacing of silicon carbide nanopores, by controlling the time of plasma etching of polystyrene nanospheres to control the pore size of the silicon carbide nanopores, by controlling the metal-assisted photochemical etching time to control the pore depth, so as to achieve controllable preparation of silicon carbide nanopore arrays, solve the problem of slow etching rate of existing metal-assisted photochemical etching, and solve the problem that the size of silicon carbide nanopore arrays currently processed by metal-assisted photochemical etching is difficult to control.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] A method for processing a silicon carbide nanopore array by metal-assisted photochemical etching comprises the following steps:
[0010] Step (1): cleaning the silicon carbide wafer;
[0011] Step (2): self-assembling a monolayer of densely packed polystyrene nanospheres on the top surface of the cleaned silicon carbide wafer;
[0012] Step (3): a metal mask that does not react with the etchant is deposited on the top surface of the silicon carbide wafer, and a noble metal layer is deposited on the bottom surface of the silicon carbide wafer;
[0013] Step (4): soaking the silicon carbide wafer after step (3) in acetone and performing ultrasonic cleaning;
[0014] Step (5): immersing the silicon carbide wafer obtained in step (4) in an etching solution, and irradiating the top surface of the silicon carbide wafer with ultraviolet light to perform metal-assisted photochemical etching;
[0015] Step (6): Stop the etching reaction, clean the silicon carbide wafer, and obtain a silicon carbide nanopore array.
[0016] Furthermore, before performing the step (3), the single-layer densely packed polystyrene nanospheres self-assembled on the top surface of the silicon carbide wafer in step (2) are etched by plasma, and the single-layer densely packed polystyrene nanospheres are converted into a single-layer non-densely packed polystyrene nanospheres.
[0017] Furthermore, in step (3), the metal mask is one of a Ti mask, a Pt mask, an Au mask and an Ag mask;
[0018] The noble metal layer is a Pt metal layer or an Ag metal layer.
[0019] Furthermore, in step (3), the thickness of the metal mask is 7-14 nm, and the thickness of the noble metal layer is 20-100 nm.
[0020] Furthermore, in step (5), the raw materials of the etching solution include H 2 O, HF, and H 2 O 2 , the H 2 O, the HF and the H 2 O 2 The volume ratio is 21:6:5;
[0021] The mass fraction of HF is 45-52wt.%, and the H 2 O 2 The mass fraction is 25-35wt.%.
[0022] Furthermore, in the step (2), the polystyrene nanosphere colloid is spin-coated on the top surface of the silicon carbide wafer by a coating machine to form a single layer of densely packed polystyrene nanospheres;
[0023] The diameter of the single-layer densely packed polystyrene nano-microspheres is 50nm-1μm.
[0024] Furthermore, in step (5), the wavelength of the ultraviolet light is 365 nm and the power density is 2200 mW / cm 2 .
[0025] Furthermore, in the step (5), the metal-assisted photochemical etching is performed for 5-60 minutes to obtain a silicon carbide nanopore array with a pore depth of 50-642 nm.
[0026] Furthermore, in the step (1), the specific steps of cleaning the silicon carbide wafer are: ultrasonically cleaning the silicon carbide wafer with anhydrous ethanol and deionized water for 3-7 minutes respectively, blowing it dry with nitrogen, and then plasma cleaning it for 3-7 minutes.
[0027] Furthermore, in step (1), the silicon carbide wafer is a 5×5 mm N-type silicon carbide wafer.
[0028] The above technical solution has the following beneficial effects:
[0029] 1. This technical solution obtains a template with an array hole pattern by self-assembling a single layer of densely packed polystyrene nanospheres on the top surface of a silicon carbide wafer and reducing its diameter by plasma etching, and then depositing a metal layer that does not react with the etching solution on the top surface of the silicon carbide wafer by vapor deposition technology. A layer of precious metal is deposited on the bottom surface of the silicon carbide wafer as a catalytic layer, which can greatly increase the rate of metal-assisted photochemical etching. The silicon carbide wafer is immersed in the etching solution and irradiated with ultraviolet light. The metal-assisted photochemical etching transfers the template pattern to the silicon carbide wafer. The hole depth of the silicon carbide array can be controlled by controlling the metal-assisted photochemical etching time, thereby controllably processing the silicon carbide array hole structure.
[0030] 2. This technical solution etches a single layer of densely packed polystyrene nanospheres through plasma. The diameter of the obtained single layer of non-densely packed polystyrene nanospheres decreases with the increase of plasma etching time. The diameter of the non-densely packed polystyrene nanospheres can be controlled by adjusting the plasma etching time as needed, so that the pore size of the prepared silicon carbide nanopore array can be controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the presentation step (1) of Example 1 of the present invention.
[0032] Figure 2 This is a schematic diagram of the presentation step (2) of Example 1 of the present invention.
[0033] Figure 3 This is a schematic diagram of presenting step (3) of Example 1 of the present invention.
[0034] Figure 4 This is a schematic diagram of presenting step (4) of Example 1 of the present invention.
[0035] Figure 5 This is a schematic diagram of presenting step (5) of Example 1 of the present invention.
[0036] Figure 6 This is a schematic diagram of the presentation step (7) of Example 1 of the present invention.
[0037] Figure 7 This is a schematic diagram of the presentation step (8) of Example 1 of the present invention.
[0038] Figure 8 Schematic diagram of a triangular prism-shaped silicon carbide nanorod array prepared in Example 2 of the present invention.
[0039] Wherein: silicon carbide wafer 101, single layer of densely packed polystyrene nanospheres 201, single layer of non-densely packed polystyrene beads 301, metal mask 401, noble metal layer 402, etching solution 601, ultraviolet light 701, silicon carbide nanopore array 801, triangular prism-shaped silicon carbide nanocolumn array 802. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.
[0041] A method for processing a silicon carbide nanopore array by metal-assisted photochemical etching comprises the following steps:
[0042] Step (1): cleaning the silicon carbide wafer;
[0043] Step (2): self-assembling a monolayer of densely packed polystyrene nanospheres on the top surface of the cleaned silicon carbide wafer;
[0044] Step (3): a metal mask that does not react with the etchant is deposited on the top surface of the silicon carbide wafer, and a noble metal layer is deposited on the bottom surface of the silicon carbide wafer;
[0045] Step (4): soaking the silicon carbide wafer after step (3) in acetone and performing ultrasonic cleaning;
[0046] Step (5): immersing the silicon carbide wafer obtained in step (4) in an etching solution, and irradiating the top surface of the silicon carbide wafer with ultraviolet light to perform metal-assisted photochemical etching;
[0047] Step (6): Stop the etching reaction, clean the silicon carbide wafer, and obtain a silicon carbide nanopore array.
[0048] Since the prior art only deposits a noble metal layer on the top surface, the noble metal layer needs to be used as both a mask and a catalyst layer, which results in a limited catalytic effect. As the area of the etching pattern increases, the area of the noble metal layer will inevitably decrease, which will also reduce its catalytic effect, thereby slowing down the etching rate. When the noble metal layer is deposited on the bottom surface and the noble metal layer contacts the semiconductor, due to the need to balance the Fermi energy levels of the two, the electrons in the semiconductor flow to the noble metal, while the holes are injected into the semiconductor, forming a positive space charge region on the contact surface of the semiconductor. This space charge is composed of holes, which increases the hole concentration in the semiconductor, thereby increasing the etching reaction rate. This shows that the deposition of noble metals on the bottom surface of the semiconductor also has a catalytic effect and can increase the etching rate. Since the metal mask and the noble metal layer are deposited on two separate surfaces, the noble metal layer will not be affected by the metal mask; at the same time, because the metal mask needs to be patterned, the area of the noble metal layer is always larger than that of the mask, which shows that the method of depositing the metal mask and the noble metal layer on the top and bottom surfaces respectively is more efficient than depositing the noble metal layer only on the top surface.
[0049] The technical solution is to self-assemble a single layer of densely packed polystyrene nanospheres on the top surface of a silicon carbide wafer and reduce their diameter by plasma etching, and then deposit a metal layer that does not react with the etching solution on the top surface of the silicon carbide wafer by vapor deposition technology to obtain a template with an array hole pattern. A layer of precious metal is deposited on the bottom surface of the silicon carbide wafer as a catalytic layer, which can greatly improve the rate of metal-assisted photochemical etching. The silicon carbide wafer is immersed in the etching solution and irradiated with ultraviolet light. The metal-assisted photochemical etching transfers the template pattern to the silicon carbide wafer. The hole depth of the silicon carbide array can be controlled by controlling the metal-assisted photochemical etching time, thereby controllably processing the silicon carbide array hole structure.
[0050] Specifically, in step (4), the silicon carbide wafer is immersed in an acetone solution and placed in an ultrasonic cleaning tank for 5-6 minutes to dissolve the single layer of non-densely packed polystyrene nanospheres on the top surface of the silicon carbide wafer, and then rinsed with deionized water 2-3 times and blown dry with nitrogen. It is worth noting that other inert gases can also be used for drying, such as argon, neon and other inert gases.
[0051] In step (6), after the etching reaction is stopped, the carbide wafer is rinsed with deionized water for 2-3 times and blown dry with nitrogen to obtain a silicon carbide nanopore array.
[0052] Metal-assisted chemical etching generally involves plating metal on the top surface as an etching shield layer, and then etching in an etchant. Compared with metal-assisted chemical etching, the etching method of the present technical solution is metal-assisted photochemical etching, and a metal layer is plated on both the top and bottom surfaces of the silicon carbide wafer. Compared with the single-sided metal layer, the silicon carbide etching rate can be effectively improved. At the same time, ultraviolet light is irradiated during etching by the etchant to provide photogenerated holes, which can further effectively improve the silicon carbide etching rate. Moreover, it is currently difficult to control the pore size and pore depth of the columnar array structure when using metal-assisted chemical etching to prepare a nano-columnar array structure. The present technical solution can provide an efficient and controllable method for processing silicon carbide nanopore arrays, which controls the spacing of silicon carbide nanopores by self-assembling polystyrene nanospheres of different diameters, controls the pore size of silicon carbide nanopores by controlling the time of plasma etching of polystyrene nanospheres, and controls the pore depth by controlling the metal-assisted photochemical etching time, so as to achieve controllable preparation of silicon carbide nanopore arrays.
[0053] In this technical solution, if a metal mask is only plated on the top surface of the silicon carbide wafer without plating a metal layer on the bottom surface of the silicon carbide wafer, the silicon carbide etching rate will be greatly reduced.
[0054] Since silicon carbide is a wide-bandgap semiconductor, it can be effectively etched using metal-assisted photochemical etching.
[0055] As a further explanation, before performing step (3), the single-layer densely packed polystyrene nanospheres self-assembled on the top surface of the silicon carbide wafer in step (2) are etched using plasma to convert the single-layer densely packed polystyrene nanospheres into a single-layer non-densely packed polystyrene nanospheres.
[0056] It is worth explaining that the principle of plasma etching is: in the plasma cleaning system, the glow discharge reaction is used to activate the gas in the cavity into active particles such as ions and free radicals. These have active chemical properties and can react with polystyrene nanospheres to form volatile products, thereby achieving the etching of polystyrene nanospheres.
[0057] Specifically, a single layer of densely packed polystyrene nanospheres is etched by plasma, and the diameter of the obtained single layer of non-densely packed polystyrene nanospheres decreases with the increase of plasma etching time. The diameter of the non-densely packed polystyrene nanospheres can be controlled by adjusting the plasma etching time as needed, so that the pore size of the prepared silicon carbide nanopore array can be controlled.
[0058] Preferably, a silicon carbide wafer provided with a single layer of densely packed polystyrene nanospheres needs to be placed in a plasma cleaner, and the single layer of densely packed polystyrene nanospheres is etched by plasma. In one embodiment of the present technical solution, the parameters of the plasma cleaner are a power of 100 W and a vacuum degree of 0.2 mbar. The time for plasma etching the single layer of densely packed polystyrene nanospheres is 5-60 min.
[0059] Specifically, a single layer of densely packed polystyrene nanospheres is etched by plasma, and the diameter of the obtained single layer of non-densely packed polystyrene nanospheres decreases with the increase of plasma etching time. When the diameter of the single layer of densely packed polystyrene nanospheres is 480nm, if the etching time is 10min, polystyrene nanospheres with a diameter of about 318nm can be obtained; when the etching time is 15min, the diameter of the polystyrene nanospheres is about 176nm, and when the etching time is 20min, the diameter of the non-densely packed polystyrene nanospheres is about 150nm. Therefore, the diameter of the non-densely packed polystyrene nanospheres can be controlled by adjusting the plasma etching time as needed, so that the size of the prepared silicon carbide nanopore array can be controlled.
[0060] Further explanation, in the step (3), the metal mask is one of a Ti mask, a Pt mask, an Au mask and an Ag mask;
[0061] The noble metal layer is a Pt metal layer or an Ag metal layer.
[0062] It is worth noting that different metals have different catalytic effects, which will affect the etching rate of silicon carbide wafers. Pt has the strongest catalytic effect, followed by Au, Ag, and finally Ti. Pt, Au, Ag and Ti do not react with the etching solution and can all be used for the mask on the top surface and the metal layer on the bottom surface. Different metal combinations will affect the etching rate of silicon carbide, such as the metal of the metal mask is Ti and the metal of the precious metal layer is Pt, the metal of the metal mask is Ti and the metal of the precious metal layer is Au, or the metal of the metal mask is Au and the metal of the precious metal layer is Pt. However, the stronger the catalytic effect is, the better. Too strong a catalytic effect will result in too many holes, and the holes at the bottom of the nanopores will diffuse to the side walls, resulting in excessive etching of the side walls of the nanopores.
[0063] Preferably, in one embodiment of the present invention, the metal mask is a Ti mask, and the noble metal layer is a Pt metal layer. In this case, the prepared nanohole array is better. A Ti mask layer is deposited on the top surface of the silicon carbide wafer and a Pt metal layer is deposited on the bottom surface by magnetron sputtering.
[0064] Further explanation, in step (3), the thickness of the metal mask is 7-14 nm, and the thickness of the noble metal layer is 20-100 nm.
[0065] Further explanation, in step (5), the raw materials of the etching solution include H 2 O, HF, and H 2 O 2 , the H 2 O, the HF and the H 2 O 2 The volume ratio is 21:6:5;
[0066] The mass fraction of HF is 45-52wt.%, and the H 2 O 2 The mass fraction is 25-35wt.%.
[0067] H in the etching solution 2 O 2 As oxidant, H 2 O 2 The concentration of H will affect the etching rate of silicon carbide wafers. Within a certain range, 2 O 2 The higher the concentration, the higher the etching rate and the greater the etching depth of the nanopore. 2 O 2 A high concentration will affect the material transport process during the etching process, reducing the transport rate of reactants and products and leading to a decrease in the etching rate. 2 O:HF:H 2 O 2 The volume ratio is set to 21:6:5. At this time, the etching rate of the etching solution is better.
[0068] Preferably, in step (5), H 2 O 2 The volume is 1-10mL. 2 O 2 When the mass fraction of H in the etching solution is constant, 2 O 2 The higher the volume, the faster the etching rate.
[0069] Preferably, the mass fraction of HF is 49wt.%, H 2 O 2 The mass fraction of H 2 O is deionized water, HF and H 2 O 2 The mass fraction of HF and H in the prepared etching solution will affect 2 O 2 concentration.
[0070] Further explanation, in the step (2), the polystyrene nanosphere colloid is spin-coated on the top surface of the silicon carbide wafer by a coating machine to form a single layer of densely packed polystyrene nanospheres;
[0071] The diameter of the single-layer densely packed polystyrene nano-microspheres is 50nm-1μm.
[0072] Specifically, the operation of self-assembled monolayer densely packed polystyrene nanospheres is as follows: set the parameters of the glue spreader to 100 rpm / min, rotate for 10 minutes, so that the polystyrene nanospheres are evenly distributed on the top surface of the silicon carbide wafer; then set the parameters of the glue spreader to 1000 rpm / min, rotate for 1 minute, and finally set the parameters of the glue spreader to 2500 rpm / min, rotate for 2 minutes, shake off excess colloid, and make the water in the colloid evaporate quickly to form densely packed polystyrene nanospheres on the top surface of the silicon carbide wafer.
[0073] The pore size of silicon carbide nanopore arrays is related to the diameter of a single layer of non-close-packed polystyrene nanospheres.
[0074] In the step (2), the diameter of a single layer of densely packed polystyrene nanospheres is in the range of 50 nm to micrometer level. Since the self-assembled polystyrene nanospheres are densely packed, the diameter of the single layer of densely packed polystyrene nanospheres is also equal to the spacing between the microspheres. The spacing of the densely packed polystyrene nanospheres can be controlled by selecting densely packed polystyrene nanospheres of different diameters as required.
[0075] Further explanation: in step (5), the wavelength of ultraviolet light is 365nm and the power density is 2200mW / cm 2 .
[0076] Specifically, the silicon carbide wafer obtained in step (4) is immersed in an etching solution, and ultraviolet light is irradiated at a distance of 1 cm from the top surface of the silicon carbide wafer to perform metal-assisted photochemical etching. Since ultraviolet light irradiates the top surface of the silicon carbide wafer to generate photogenerated holes at its interface, and when the noble metal contacts the bottom surface of the N-type silicon carbide wafer, the energy band of the silicon carbide wafer is bent at the interface of the noble metal layer / silicon carbide wafer, generating an internal electric field directed from the silicon carbide wafer to the noble metal layer, a large number of holes are gathered at the bottom surface of the silicon carbide to form a high potential, and the internal holes are gathered at the top surface of the silicon carbide wafer under the action of the high potential, so the hole concentration on the top surface of the silicon carbide wafer is improved, which promotes the etching rate to accelerate and realize efficient etching of silicon carbide.
[0077] Further explanation: in the step (5), the metal-assisted photochemical etching is performed for 5-60 minutes to obtain a silicon carbide nanopore array with a pore depth of 50-642 nm.
[0078] The technical solution controls the hole depth by controlling the time of metal-assisted photochemical etching. As the time of metal-assisted photochemical etching increases, the hole depth of the obtained silicon carbide nanopore array becomes deeper.
[0079] To further illustrate, in step (1), the specific steps of cleaning the silicon carbide wafer are: ultrasonically cleaning the silicon carbide wafer with anhydrous ethanol and deionized water for 3-7 minutes respectively, drying it with nitrogen, and then plasma cleaning it for 3-7 minutes.
[0080] This technical solution uses nitrogen to dry, because nitrogen is chemically inactive, which can prevent the gas from chemically reacting with other substances dissolved in water to generate precipitation or other impurities.
[0081] As a further explanation, in step (1), the silicon carbide wafer is a 5×5 mm N-type silicon carbide wafer.
[0082] The present technical solution is further described below in conjunction with embodiments.
[0083] Example 1
[0084] like Figure 1-7 As shown, a method for processing a silicon carbide nanopore array by metal-assisted photochemical etching comprises the following steps:
[0085] Step (1): select a 5×5 mm N-type silicon carbide wafer 101, ultrasonically clean it with anhydrous ethanol and deionized water for 5 minutes respectively, blow dry it with nitrogen, and then perform plasma cleaning for 5 minutes;
[0086] Step (2): On the top surface of the silicon carbide wafer 101 in step (1), a self-assembled monolayer of densely packed polystyrene nanospheres 201 is formed. The specific operation is as follows: 7.5 μL of polystyrene nanosphere colloid 201 with a diameter of 480 nm is spin-coated on the top surface of the silicon carbide wafer using a coating machine, wherein first, the coating machine parameter is set to 100 rpm / min, and the coating machine is rotated for 10 minutes to make the polystyrene nanospheres evenly distributed; secondly, the coating machine parameter is set to 1000 rpm / min, and the coating machine is rotated for 1 minute; finally, the coating machine parameter is set to 2500 rpm / min, and the coating machine is rotated for 2 minutes to shake off the excess. The remaining colloid is removed, and the water in the colloid is evaporated quickly, so that a single-layer densely packed polystyrene nano-microsphere colloid with a diameter of 480nm is formed on the top surface of the silicon carbide wafer 101; the single-layer densely packed polystyrene nano-microsphere self-assembled on the top surface of the silicon carbide wafer in step (2) is etched by plasma, and the single-layer densely packed polystyrene nano-microsphere is converted into a single-layer non-densely packed polystyrene nano-microsphere 202, wherein the parameters of the plasma cleaning instrument are power 100W, vacuum degree 0.2mbar, no auxiliary gas is introduced, and the etching time is 10min, and polystyrene nano-microspheres with a diameter of about 318nm can be obtained;
[0087] Step (3): depositing a Ti mask 401 which does not react with the etchant on the top surface of the silicon carbide wafer in step (2) by magnetron sputtering, and at the same time, depositing a Pt metal layer 402 on the bottom surface;
[0088] Step (4): Soak the silicon carbide wafer obtained in step (3) in acetone and place it in an ultrasonic cleaning tank for about 5-6 minutes to accelerate the dissolution of the polystyrene nanospheres by ultrasonic cleaning, so as to dissolve the single layer of non-densely packed polystyrene nanospheres 202 on the top surface of the wafer, then rinse with deionized water 2-3 times and blow dry with nitrogen;
[0089] Step (5): Immerse the silicon carbide wafer in step (5) in the etching solution 601, and irradiate the top surface of the silicon carbide wafer with ultraviolet light 701 to perform metal-assisted photochemical etching, wherein the ultraviolet light 701 used in the metal-assisted photochemical etching has a wavelength of 365 nm and a power density of 2200 mW / cm 2 The silicon carbide wafer obtained in step (5) is immersed in the etching solution prepared in step (6), and irradiated with ultraviolet light at a distance of 1 cm from the top surface of the wafer, wherein the etching solution 601 is H 2 O:HF:H 2 O 2 =21:6:5 volume ratio mixed solution, its H 2 O is deionized water, HF is 49wt.%, H 2 O 2 30wt.%;
[0090] Step (6): Stop the etching reaction, rinse the silicon carbide wafer with deionized water 2-3 times, and blow dry with nitrogen to obtain a high-quality silicon carbide nanopore array 801.
[0091] Example 2
[0092] like Figure 8 As shown, the processing method of the metal-assisted photochemical etching of the silicon carbide nanopore array in this embodiment is similar to that in embodiment 1, but there is no need to reduce the self-assembled monolayer of densely packed polystyrene nanospheres. After the self-assembled monolayer of densely packed polystyrene nanospheres is completed, a Ti mask that does not react with the etching solution is directly deposited on the top surface of the silicon carbide wafer by vapor deposition technology, and a Pt metal layer is deposited on the bottom surface of the silicon carbide wafer, and the silicon carbide wafer is immersed in the etching solution and irradiated with ultraviolet light, so that a triangular prism-shaped silicon carbide nanocolumn array 802 can be processed.
[0093] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A method for processing a silicon carbide nanopore array by metal-assisted photochemical etching, characterized in that: The following steps are involved: Step (1): cleaning the silicon carbide wafer; Step (2): self-assembling a monolayer of densely packed polystyrene nanospheres on the top surface of the cleaned silicon carbide wafer; Step (3): a metal mask that does not react with the etchant is deposited on the top surface of the silicon carbide wafer, and a noble metal layer is deposited on the bottom surface of the silicon carbide wafer; Step (4): soaking the silicon carbide wafer after step (3) in acetone and performing ultrasonic cleaning; Step (5): immersing the silicon carbide wafer obtained in step (4) in an etching solution, and irradiating the top surface of the silicon carbide wafer with ultraviolet light to perform metal-assisted photochemical etching; Step (6): Stop the etching reaction, clean the silicon carbide wafer, and obtain a silicon carbide nanopore array.
2. The method for processing a silicon carbide nanopore array by metal-assisted photochemical etching according to claim 1, characterized in that: Before performing the step (3), the single-layer densely packed polystyrene nanospheres self-assembled on the top surface of the silicon carbide wafer in step (2) are etched by plasma, and the single-layer densely packed polystyrene nanospheres are converted into single-layer non-densely packed polystyrene nanospheres.
3. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (3), the metal mask is one of a Ti mask, a Pt mask, an Au mask and an Ag mask; The noble metal layer is a Pt metal layer or an Ag metal layer.
4. The method for processing a silicon carbide nanopore array by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (3), the thickness of the metal mask is 7-14 nm, and the thickness of the noble metal layer is 20-100 nm.
5. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (5), the raw materials of the etching solution include H2O, HF and H2O2, and the volume ratio of the H2O, the HF and the H2O2 is 21:6:5; The mass fraction of HF is 45-52 wt.%, and the mass fraction of H2O2 is 25-35 wt.%.
6. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (2), the polystyrene nanosphere colloid is spin-coated on the top surface of the silicon carbide wafer by a spin coater to form a single layer of densely packed polystyrene nanospheres; The diameter of the single-layer densely packed polystyrene nano-microspheres is 50nm-1μm.
7. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In step (5), the wavelength of the ultraviolet light is 365 nm and the power density is 2200 mW / cm 2 .
8. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 7, characterized in that: In the step (5), the metal-assisted photochemical etching is performed for 5-60 minutes to obtain a silicon carbide nanopore array with a pore depth of 50-642 nm.
9. The method for processing silicon carbide nanopore arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (1), the specific steps of cleaning the silicon carbide wafer are: ultrasonically cleaning the silicon carbide wafer with anhydrous ethanol and deionized water for 3-7 minutes respectively, blowing it dry with nitrogen, and then plasma cleaning it for 3-7 minutes.
10. The method for processing silicon carbide nanohole arrays by metal-assisted photochemical etching according to claim 1, characterized in that: In the step (1), the silicon carbide wafer is a 5×5 mm N-type silicon carbide wafer.