A high-crystallization silver powder and low-cost heterojunction silver paste and preparation method and application thereof

By coating the silver layer on the surface of the inorganic powder and combining carriers such as epoxy resin to prepare low-cost heterogeneous silver paste, the problems of high cost and reduced conductivity of traditional silver paste are solved, and cost reduction and performance improvement are achieved.

CN114188066BActive Publication Date: 2024-11-26SUZHOU BETELY POLYMER MATERIALS CO LTD +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202111438558.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-11-26
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

The high cost and reduced conductivity of silver paste of traditional heterojunction solar cell electrodes is problematic, especially the production cost and performance problems caused by the high price of silver and the oxidation of copper.

Method used

The silver layer is coated on the surface of the inorganic powder by chemical reduction to form high crystal silver powder, and low-cost heterogeneous silver paste is prepared in combination with carriers such as epoxy resin. The high-coverage silver-packed inorganic powder is used to reduce the use of silver 2. Add sheet silver powder to enhance conductivity.

Benefits of technology

It effectively reduces the production cost of silver paste and heterojunction battery cells, while maintaining high conductivity and oxidation resistance, and improving the weather resistance and printing properties of silver paste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114188066B_ABST
    Figure CN114188066B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-crystallization silver powder and a low-cost heterojunction silver paste and a preparation method and application thereof. After the surface of an inorganic powder is smoothed, the inorganic powder is mixed with an anti-flocculant and a dispersant water to obtain an inorganic powder dispersion, and then mixed with a reducing agent, a particle size control agent, and a water-soluble silver salt. A silver layer is coated on the surface of the inorganic powder by a chemical reduction method, thereby synthesizing a silver-coated inorganic nanopowder type high-crystallization spherical silver powder. The silver paste formula of the present invention adds highly dispersible flaky silver powder and highly crystalline silver powder, which effectively improves the conductivity of the silver paste while retaining the fine printing property of the silver paste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technical invention is applied in the production of conductive silver paste and silver powder for heterojunction solar cells in the technical field of solar cell photovoltaic industry. Background Art

[0002] Photovoltaic power generation, as a clean energy source, has always been sought after by people. Among them, heterojunction solar cells have been rapidly developed due to their unique advantages. From the production perspective, heterojunction cells can make the cells thinner, thereby improving the utilization efficiency of crystalline silicon. In addition, from the perspective of energy consumption in the production process, the curing temperature of heterojunction silver paste is very low, and curing can be achieved within 200°C; from the performance perspective, heterojunction cells will not produce polarization, have high light stability, and have a higher opening voltage, so heterojunction cells have a higher photoelectric conversion efficiency. Traditional heterojunction solar cell electrode silver paste is made of high-purity (>99%) silver powder. The price of silver is relatively high, and traditional heterojunction silver paste has a very high silver content, so the production and use costs of silver paste are very high; some people also advocate the use of copper-silver alloy, but because the problem of copper oxidation cannot be solved, the conductivity is greatly reduced. Summary of the invention

[0003] The present invention provides a method for synthesizing silver-coated inorganic high-crystalline silver powder by fully coating the surface of inorganic powder with silver. The silver-coated inorganic powder produced by the present invention has a conductivity close to that of pure silver powder, and the inorganic substances used are all inert inorganic powders that are insoluble in water and non-corrosive, and there is no stability problem. The heterojunction silver paste produced by the present invention can effectively reduce the manufacturing cost of silver paste and heterojunction battery.

[0004] The present invention adopts the following technical solution:

[0005] A high-crystallization silver powder is obtained by coating a silver layer on the surface of an inorganic powder, wherein the particle size of the inorganic powder is 1nm to 500nm.

[0006] Preferably, the inorganic powder is water-insoluble and non-corrosive, including one or more of glass powder, ceramic powder, silicon dioxide powder, carbon powder, and graphite powder.

[0007] Preferably, the particle size of the inorganic powder is 1 nm to 300 nm.

[0008] Preferably, the surface of the inorganic powder is smooth.

[0009] The invention discloses a method for preparing the above-mentioned high-crystallization silver powder, comprising the following steps: after surface smoothing of inorganic powder, a silver layer is coated on the surface of the inorganic powder by chemical reduction method, and the silver layer has high crystallinity, thereby synthesizing a silver-coated inorganic nanopowder type high-crystallization spherical silver powder.

[0010] In the present invention, surface smoothing treatment refers to modifying and modifying the surface edges and corners of the inorganic powder by physical surface smoothing treatment or chemical surface smoothing treatment, so as to make the surface of the inorganic powder smooth, which is conducive to the formation of a more sufficient coating layer of silver on the surface of the inorganic powder, thereby further improving the conductivity of the high-crystalline silver powder. Physical surface smoothing treatment includes: high-temperature heat treatment, high-speed impact, water-phase low-speed sand grinding, etc.; chemical surface smoothing treatment includes: acid etching, alkali etching, etc.

[0011] In the above technical solution, the inorganic powder is subjected to surface smoothing treatment and then mixed with a reducing agent and a water-soluble silver salt, and a silver layer is coated on the surface of the inorganic powder by chemical reduction; the reducing agent can be one or more of ascorbic acid, formaldehyde, hydrazine hydrate, etc. Further, the inorganic powder is subjected to surface smoothing treatment and then mixed with an anti-flocculant and dispersant water to obtain an inorganic powder dispersion, which is then mixed with a reducing agent, a particle size control agent, and a water-soluble silver salt, and a silver layer is coated on the surface of the inorganic powder by chemical reduction.

[0012] The present invention discloses a low-cost heterojunction silver paste, comprising a carrier, the above-mentioned high-crystalline silver powder, and flaky silver powder; the carrier comprises epoxy resin, thermosetting oligomer, solvent, epoxy curing agent, and blocked isocyanate curing agent. Preferably, the low-cost heterojunction silver paste is composed of a carrier, high-crystalline silver powder, and flaky silver powder, the mass percentage of the high-crystalline silver powder is 60% to 95%, the mass percentage of the flaky silver powder is 5% to 30%, and the balance is the carrier; preferably, the mass percentage of the high-crystalline silver powder is 65% to 80%, the mass percentage of the flaky silver powder is 10% to 20%, and the balance is the carrier. Preferably, the carrier is composed of epoxy resin, thermosetting oligomer, solvent, epoxy curing agent, and blocked isocyanate curing agent, and by mass percentage, the epoxy resin is 1% to 10%, the thermosetting oligomer is 0.1% to 5%, the epoxy curing agent is 0.1% to 3%, the blocked isocyanate curing agent is 1% to 5%, and the solvent is the balance.

[0013] In the present invention, the tap density of the flaky silver powder is 4.0 to 6.0 g / cm 3 , high temperature heat loss is 0.1~0.5%, particle size D50 is 1.0~3.0μm, and the sheet diameter ratio is 1.5~5.

[0014] In the present invention, the epoxy resin type can be one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic epoxy resin, polyester modified epoxy, polyurethane modified epoxy, and acrylic modified epoxy. The thermosetting polymer can be a trivalent or higher polyol, such as polyester polyol, polyether polyol, acrylic polyol, polyurethane polyol, etc., to improve weather resistance. The solvent is an ester solvent, alcohol solvent, ether solvent, ketone solvent, etc. with a boiling point between 190°C and 250°C, such as pinene alcohol, butyl carbitol, butyl carbitol acetate, diethylene glycol dibutyl ether, dimethyl glutarate, dimethyl adipate, ethylene glycol butyl ether acetate, diacetone alcohol, and isophorone. One or more of.

[0015] The invention discloses a method for preparing the above-mentioned low-cost heterojunction silver paste. The above-mentioned high-crystalline silver powder and flaky silver powder are dispersed in a carrier to obtain the low-cost heterojunction silver paste. Specifically, epoxy resin, thermosetting polymer, solvent, epoxy curing agent and blocked isocyanate curing agent are mixed and dispersed to obtain a carrier, and then the high-crystalline silver powder and flaky silver powder are added, and then centrifugal dispersion, three-roll grinding dispersion, and filtration are performed to remove impurities to obtain the low-cost heterojunction silver paste. After conventional viscosity adjustment, the paste can be directly used for printing heterojunction solar cell electrodes.

[0016] In the present invention, the coated core is not metal but inert nano inorganic powder. Compared with metal powder, inert inorganic powder itself does not have the problem of oxidation and corrosion, so the conductive performance will not be affected by oxidation. Moreover, the particle size of the inorganic powder used in the present invention is nanometer level. Compared with micrometer level powder, nanometer level powder has stronger surface activity. Especially after smoothing treatment, silver atoms are easy to grow and crystallize on its surface, thereby forming a more complete silver coating layer.

[0017] In the present invention, the dripping method, reaction concentration, stirring method and stirring speed, and reaction time are optimized for the entire reaction process, so that silver forms a more sufficient and complete coating layer on the surface of the nano inorganic crystal core.

[0018] The preparation of low-cost heterojunction silver paste of the present invention has the advantage (1) that high-coverage silver-coated inorganic powder is used, so that the actual amount of precious metal silver used in the formula is reduced while ensuring the conductive and antioxidant properties of the silver paste, thereby greatly reducing the production cost of the silver paste and the production cost of the heterojunction battery cell.

[0019] The preparation of the low-cost heterojunction silver paste of the present invention has the advantage (2) that a trifunctional or higher polyol is added to the formula, combined with a blocked isocyanate, an epoxy resin and a curing agent to form a more compact cross-linked structure, thereby increasing the cross-linking density of the cured product and effectively improving the weather resistance of the silver wire after curing.

[0020] The low-cost heterojunction silver paste of the present invention has the advantage (3) that, in order to further improve the conductivity of the silver paste, a highly dispersible flaky silver powder and a highly crystalline silver powder are added to the silver paste formula, which effectively improves the conductivity of the silver paste while retaining the fine printability of the silver paste. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Printing circuit pattern with silver paste;

[0022] Figure 2 This is a scanning electron microscope image of the silver-coated glass powder synthesized in Example 1;

[0023] Figure 3 This is a scanning electron microscope image of the silver-coated ceramic powder synthesized in Example 2;

[0024] Figure 4 This is a scanning electron microscope image of the pure silver powder synthesized in Comparative Example 1;

[0025] Figure 5 This is the laser particle size test result of glass powder GF-01;

[0026] Figure 6 This is the laser particle size test result of ceramic powder TO-1;

[0027] Figure 7 The laser particle size test result of the silver-coated glass powder synthesized in Example 1 is shown;

[0028] Figure 8 The laser particle size test results of the silver-coated ceramic powder synthesized in Example 2;

[0029] Fig. 9 This is a laser particle size test diagram of the pure silver powder synthesized in Comparative Example 1; DETAILED DESCRIPTION

[0030] The raw materials involved in the present invention are all existing products, and the specific preparation operations and testing methods are all existing conventional methods. The particle size of the powder of the present invention is measured by D50.

[0031] The present invention discloses a method for preparing the above-mentioned high-crystalline silver powder, comprising the following steps: after the inorganic powder is subjected to surface smoothing treatment, a layer of silver is coated on the surface of the inorganic powder by chemical reduction method, and the silver powder has high crystallinity, thereby synthesizing a silver-coated inorganic nanopowder type high-crystalline spherical silver powder. Specifically, the method for preparing the high-crystalline silver powder of the present invention is as follows:

[0032] Step a. The inorganic nanopowder is subjected to surface smoothing treatment by air flow impact polishing equipment (air flow milling equipment). Dry nitrogen is used in the process to avoid the nanopowder from absorbing moisture and agglomerating, which results in the powder inside the agglomerate not being well smoothed. The air pressure is 0.05-0.5 MPa. If the air pressure is too low, the impact force between the powders is insufficient, and there is no obvious smoothing effect. If the air pressure is too high, the inorganic powder will be broken, resulting in a change in particle size.

[0033] Step b. Preparation of an inorganic nanopowder dispersion: 1 to 5 g of the smoothed nano-inorganic powder, 1 to 20 g of an anti-flocculant, 0.1 to 3 g of a dispersant, and 1000 g of deionized water were ultrasonically dispersed while stirring for 0.5 to 2 hours to obtain a nanocrystalline core dispersion for later use;

[0034] Step c. Prepare a reducing agent solution having a concentration of 0.2 to 0.5 mol / L with deionized water having a conductivity of <2 μs, and add 1.0 to 20% of a particle size control agent to the solution, and control the temperature to be constant within the range of 10 to 40 ° C; the original agent used may be one or more of ascorbic acid, formaldehyde, hydrazine hydrate, etc.;

[0035] Step d. Prepare a silver nitrate solution having a concentration of 0.5 to 2.0 mol / L with deionized water having a conductivity of <2 μs, and control the temperature in the range of 10 to 40 ° C;

[0036] Step e. Add the nanocrystalline core dispersion into the reducing agent solution at one time, control the stirring speed between 150 and 400 r / min, and then add the silver nitrate solution dropwise within 2 to 8 hours; silver slowly and orderly grows on the nanocrystalline core under the action of the reducing agent until the nanocrystalline core is fully wrapped by silver;

[0037] Step f. The synthesized powder is filtered, washed with deionized water, washed with ethanol, dried at 50-100° C., crushed and sieved before use.

[0038] Further, the preparation method of the low-cost heterojunction silver paste of the present invention is schematically shown as follows (by weight):

[0039] Step 1: Preparation of vector

[0040] Epoxy resin, isocyanate curing agent, polyol, epoxy curing agent, catalyst, and solvent were weighed and mixed, and then centrifuged and dispersed using a centrifugal disperser at a centrifugal speed of 800 r / min and a centrifugal dispersion time of 3 min to obtain a carrier; the preparation method of the following embodiments is consistent with this;

[0041] Step 2: Preparation of silver paste

[0042] Take a carrier and add silver-coated inorganic powder, stir evenly, then add flaky silver powder, stir evenly to obtain a slurry, and then use a centrifugal disperser to centrifuge and disperse the slurry. The centrifugal speed is 1200r / min, and the centrifugal time is 2min. After the centrifugal dispersion of the slurry is completed, use an Eckart three-roll grinder to further grind and disperse, and then use a mesh of 400 mesh or more to filter and remove impurities from the ground silver paste to obtain a finished silver paste; the preparation method of the following embodiments is consistent with this.

[0043] Test Method

[0044] ①Particle size test

[0045] The measurement was performed using a Malvern 3000 laser particle size analyzer. The measuring medium was deionized water, the sample size was 30 mg, 0.025 g Tween-80 and 10 g ethanol were added for ultrasonic dispersion for 5 minutes, and when the particle size analyzer was ready, the ultrasonically dispersed sample could be poured in for testing. After the measurement, the D50 average value could be directly read.

[0046] ②High temperature heat loss

[0047] Take a sample of 3 to 5 g, calcine it in a muffle furnace at 750°C for 15 minutes, cool it to room temperature, weigh it and calculate the weight loss. The result divided by the sample size is the high-temperature heat loss, expressed as a percentage. Multiple parallel measurements are required, and then the average value is taken.

[0048] ③Specific surface area

[0049] The automatic surface area analyzer of Micromeritic Company of the United States was used for measurement in accordance with the standard "GB / T19587-2017 Determination of the specific surface area of ​​solid substances by gas adsorption BET method", and the average value was taken after multiple measurements.

[0050] ④Tap density

[0051] The density was measured using a tap density meter with 2000 taps and the average value was taken after multiple measurements.

[0052] ⑤Viscosity measurement

[0053] Use Anton Paar rheometer to measure at 25°C. The data measured at 10 inverse seconds is the required viscosity value. The viscosity of the silver paste should be controlled between 80,000cp and 130,000cp. If the viscosity of the silver paste is too low, the silver paste printing will easily cause diffusion problems. If the viscosity of the silver paste is too high, the silver paste will block the screen and cannot be printed well.

[0054] ⑥Resistivity

[0055] Print the silver paste into Figure 1The graph shown (taking silver paste (1) as an example) was baked at 180°C for 30 min and then taken out. The thickness of the 1.5 mm wide line was tested using a Keyence 3D laser scanner. The resistance of the 1.5 mm wide line was measured using a resistance meter. The line length was 10 cm. The resistivity of the silver paste was then calculated using the resistivity calculation formula.

[0056] ⑦Environmental testing method

[0057] The substrate sample printed with silver paste was placed in an 85% HR / 85°C ring tester for 500 hours of ring test, then taken out and the resistivity increase of 1.5 mm wide lines was measured and expressed as a percentage.

[0058] Embodiment 1

[0059] Take glass powder with D50=183nm, named GF-01, and the laser particle size test results are as follows Figure 5 As shown, a jet mill is used for smoothing. The working process of the jet mill is conventional technology, such as using dry compressed gas to continuously blow the powder from the feed port of the jet mill into the cavity of the jet mill. The powder will be driven by the airflow to rub against the wall of the jet mill cavity, thereby achieving a polishing and smoothing effect. After the powder comes out of the jet mill cavity, it is separated from the airflow by a cyclone separator and a filter element. The equipment can control the smoothness of the powder by controlling the airflow pressure. The airflow pressure is set to 0.25MPa in this embodiment. Take 1.5g of smoothed GF-01 glass powder, 1.5g of anti-flocculant polyvinyl pyrrolidone PVP-K30, 0.3g of dispersant (Tween-80), and 1000g of deionized water with a conductivity of 1.01μs / cm. After mixing, conventional ultrasonic stirring and dispersion for 2 hours to obtain a glass powder dispersion as a seed crystal;

[0060] Take 30.0g of ascorbic acid as a reducing agent and 7.2g of a particle size control agent (concentrated ammonia with a mass concentration of 25%), dissolve them in 800ml of deionized water with a conductivity of 1.01μs / cm, pour them into a reactor and start stirring at a speed of 250r / min, set the constant temperature water at 20°C, and wait for the reaction;

[0061] Take 42.5g of silver nitrate and dissolve it in 250ml of deionized water with a conductivity of 1.01μs / cm. After dissolution, keep the temperature at 20℃;

[0062] Before starting the reaction, pour all the glass powder dispersion into the reactor containing the reducing agent solution, then drip the silver nitrate solution into the reactor within 4 hours under stirring. Continue stirring for 30 minutes after the dripping. After the reaction is over, filter and separate the synthesized powder, wash it with deionized water until the filtrate conductivity is less than 20μs / cm, and then use ethanol ultrasonic cleaning for 3 times. After washing, dry the powder at 60°C to obtain silver-coated glass powder; the obtained silver-coated glass powder has a D50 of 1.84μm, high temperature heat loss of 0.25%, and a specific surface area of ​​0.36m 2 / g, tap density = 5.96g / cm 3 , SEM images are shown in Figure 2 As shown, the laser particle size test results are as follows Figure 7 shown.

[0063] Embodiment 2

[0064] The inorganic nanocrystalline core used was changed to zirconium oxide ceramic powder with D50 = 153nm, named TO-01, and the laser particle size test results were Figure 6 As shown, the usage is 2.3g, and the other processes are the same as those in Example 1. The D50 of the obtained silver-coated ceramic powder is 1.98μm, the high temperature heat loss is 0.24%, and the specific surface area is 0.34m 2 / g, tap density = 6.02g / cm 3 , SEM images are shown in Figure 3 As shown, the laser particle size test results are Figure 8 shown.

[0065] Comparative Example 1

[0066] Compared with Example 1, in Comparative Example 1, no seed crystals were added, and 1000 ml of deionized water for preparing seed crystals was directly added to the reducing solution. The other processes remained unchanged, that is, when the reaction started, 1000 g of deionized water with a conductivity of 1.01 μs / cm was poured into the reactor containing the reducing agent solution, and the silver nitrate solution was dripped into the reactor within 4 hours under stirring, and the subsequent steps were the same as those in Example 1; the obtained silver powder had a D50 of 2.13 μm, a high temperature heat loss of 0.33%, and a specific surface area of ​​0.43 m 2 / g, tap density = 5.88g / cm 3 , SEM images are shown in Figure 4 As shown, the laser particle size test results are Fig. 9 shown.

[0067] Comparative Example 2

[0068] Compared with Example 1, the time for adding the seed crystal is changed to that when the silver nitrate is added dropwise for 2 hours, all of it is added at once, and then the silver nitrate is continued to be added dropwise until the end, that is, before starting the reaction, the silver nitrate solution is dropped into the reactor within 4 hours, but at 2 hours, all the glass powder dispersion is poured into the reactor containing the reducing agent solution, and then the silver nitrate is continued to be added dropwise, and the other steps are the same as Example 1.

[0069] Comparative Example 3

[0070] Compared with Example 1, the seed crystal addition time is changed to when the silver nitrate addition is finished, that is, 4 hours after the addition, all the seed crystals are added at once, and then stirring is continued for 30 minutes, and the reaction is completed. The other steps are the same.

[0071] Table (1) shows the powder parameters prepared in Example 1, Example 2, Comparative Examples 1, 2 and 3.

[0072] Table (1) Powder parameters

[0073]

[0074] Figure 5 and Figure 6 The laser particle size test results of glass powder GF-01 and ceramic powder TO-1 are respectively 183nm and 153nm. The laser particle size test results of the coated silver powder synthesized using them as seeds, that is, the silver-coated glass powder and silver-coated ceramic powder of Example 1 and Example 2 are Figure 7 and Figure 8 As shown in the figure, their D50 are 1.84μm and 1.98μm respectively, and there is no particle distribution peak in the range of 100nm to 300nm, indicating that silver atoms have been deposited on the surface of the seed crystal and grown into larger particles of powder. Combined with the test results of the silver paste below, it can be further explained that the synthesized powder particles are silver-coated inorganic powders. Figure 2 and Figure 3 It can be clearly seen that the synthesized silver-coated glass powder and silver-coated ceramic powder have extremely high crystallinity.

[0075] Silver Paste Example

[0076] According to the formulas in Table 2 and Table 4, silver paste was prepared as follows:

[0077] Step 1: Preparation of vector

[0078] Weighing epoxy resin, isocyanate curing agent, polyol, epoxy curing agent, catalyst, and solvent, mixing them, and then using a centrifugal disperser for centrifugal dispersion, the centrifugal speed is 800 r / min, the centrifugal dispersion time is 3 min, to obtain a carrier;

[0079] Step 2: Preparation of silver paste

[0080] Take a carrier and add silver-coated inorganic powder (or silver powder), stir evenly, then add flaky silver powder (or not add, or add glass powder), stir evenly to obtain a slurry, and then use a centrifugal disperser to centrifuge and disperse the slurry. The centrifugal speed is 1200r / min, and the centrifugal time is 2min. After the centrifugal dispersion of the slurry is completed, use an Eckart three-roll grinder to further grind and disperse, and then use a mesh of 400 mesh or more to filter and remove impurities from the ground silver paste to obtain a finished silver paste; the preparation method of the following embodiments is consistent with this.

[0081] The high temperature heat loss of Shandong Jianbang's flake silver powder F1 is 0.19%, and D50 = 2.77μm.

[0082] The prepared silver paste is printed with a steel screen with 360 mesh, latex film thickness of 15μm and tension of 21N. After printing a specific pattern, it is baked at 180℃ for 30min, and then the resistance of the specific line is measured with a resistance meter, the film thickness of the line is measured with a film thickness meter, and then the corresponding resistivity is calculated.

[0083] Example 4 Silver paste example (2)

[0084] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of Colloid polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, 0.10g of hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of silver-coated ceramic powder of Example 2, 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0085] Example 5 Silver paste example (3)

[0086] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of Colloid polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of hexahydrophthalic anhydride, and prepare according to the preparation method of the body recorded above. After completion, take 22.00g of the silver powder synthesized in Synthesis Comparative Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the silver paste preparation method recorded above. The test method is the same as that of silver paste example (1).

[0087] Example 6 Silver Paste Example (4)

[0088] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of Dow polyether polyol Voranol 230-112, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of the silver-coated glass powder synthesized in Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0089] Example 7 Silver Paste Example (5)

[0090] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of BASF polyol 750, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of the silver-coated glass powder synthesized in Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0091] Comparative Example 4

[0092] Take 0.60g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of the silver-coated glass powder synthesized in Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0093] Comparative Example 5

[0094] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the preparation method of the body recorded above. After completion, take 22.00g of the silver-coated glass powder synthesized in Comparative Example 2 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the silver paste preparation method recorded above. The test method is the same as that of silver paste example (1).

[0095] Comparative Example 6

[0096] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the preparation method of the body recorded above. After completion, take 22.00g of the silver-coated glass powder synthesized in Comparative Example 3 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the silver paste preparation method recorded above. The test method is the same as that of silver paste example (1).

[0097] Comparative Example 7

[0098] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the preparation method of the body recorded above. After completion, take 20.85g of the pure silver powder synthesized in Comparative Example 1, 1.15g of the smoothed glass powder GF-01 used in Example 1, and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the silver paste preparation method recorded above. The test method is the same as that of silver paste example (1).

[0099] Comparative Example 8

[0100] Take 0.80g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, without blocked isocyanate, 1.00g of solvent diethylene glycol butyl ether acetate, 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of the silver powder synthesized in Comparative Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0101] Comparative Example 9

[0102] Take 0.40g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, without adding epoxy curing agent hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 22.00g of the silver powder synthesized in Comparative Example 1 and 5.00g of Shandong Jianbang flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0103] Comparative Example 10

[0104] Take 0.30g of epoxy resin 240, 0.40g of epoxy resin JER 1007, 0.30g of polyester polyol F1010, 0.50g of blocked isocyanate 3175, 1.00g of solvent diethylene glycol butyl ether acetate, and 0.10g of epoxy curing agent hexahydrophthalic anhydride, and prepare according to the above-mentioned preparation method. After completion, take 27.00g of the silver powder synthesized in Comparative Example 1, do not add flaky silver powder F1, and prepare according to the above-mentioned silver paste preparation method. The test method is the same as that of silver paste example (1).

[0105] Table (2) Silver paste components and properties

[0106]

[0107]

[0108] Table (3) Silver paste properties

[0109] serial number Silver paste example (1) Silver paste example (2) Silver paste example (3) Silver Paste Example(4) Silver Paste Example(5) Comparative Example 4 Viscosity 92000cp 87500cp 93500cp 95500cp 87800cp 82500cp Resistivity / Ω·cm <![CDATA[5.81*10 -6 ]]> <![CDATA[5.92*10 -6 ]]> <![CDATA[5.74*10 -6 ]]> <![CDATA[6.51*10 -6 ]]> <![CDATA[6.72*10 -6 ]]> <![CDATA[6.03*10 -6 ]]> Ring test 500H resistivity change <5% <5% <5% <5% <5% 9.7%

[0110] Table (4) Comparative Example Silver Paste Composition and Performance

[0111] serial number Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Epoxy Resin 240 0.30g 0.30g 0.30g 0.80g 0.40g 0.30g Epoxy resin JER1007 0.40g 0.40g 0.40g 0.40g 0.40g 0.40g Polyester polyol F1010 0.30g 0.30g 0.30g 0.30g 0.30g 0.30g Curing agent 3175 0.50g 0.50g 0.50g — 0.50g 0.50g Hexahydrophthalic anhydride 0.10g 0.10g 0.10g 0.10g — 0.10g Diethylene glycol butyl ether acetate 1.00g 1.00g 1.00g 1.00g 1.00g 1.00g Comparative Example 1 Powder — — 20.85g 22.00g 22.00g 27.00g Comparative Example 2 Powder 22.00g — — — — — Comparative Example 3 Powder — 22.00g — — — — Smoothing GF-01 — — 1.15g — — — Flake silver powder F1 5.00g 5.00g 5.00g 5.00g 5.00g — Viscosity 95500cp 101500cp 12500cp 85500cp 92500cp 83000cp Resistivity / Ω·cm <![CDATA[6.92*10 -6 ]]> <![CDATA[8.12*10 -6 ]]> <![CDATA[11.21*10 -6 ]]> ∞ <![CDATA[7.34*10 -6 ]]> <![CDATA[8.17*10 -6 ]]> Ring test 500H resistivity change <5% <5% <5% — <5% <5%

[0112] It can be seen from Silver Paste Example (1), Silver Paste Example (2) and Silver Paste Example (3) that after adding inorganic crystal seeds before synthesizing the silver powder and allowing the crystal seeds to be fully coated with a silver layer, the resistivity of the silver paste prepared with the obtained silver powder and the resistivity of the silver paste prepared with pure silver powder are at the same level. The introduction of inorganic crystal nuclei does not affect the conductivity of the silver paste, but the cost of the embodiments is significantly reduced. By observing Comparative Examples 5 and 6, it is found that as the method of adding crystal seeds affects the formed coating layer, the conductivity of the prepared silver paste decreases, which is manifested as an increase in resistivity. Comparative Example 7 directly adds smoothed glass powder GF-01 in proportion to the pure silver powder synthesized in Comparative Example 1 without inorganic crystal seeds during the preparation of the silver paste. The resistivity of the resulting silver paste is as high as 11.21*10 -6 Ω·cm. In comparison, the silver-coated inorganic powder in Example 1 and Example 2 is coated with a silver layer, which does not affect the conductivity of the silver paste. After using the silver-coated inorganic powder, the actual silver content of the silver paste is significantly lower than that of the pure silver powder formula, thereby reducing the silver cost of HIT silver paste production.

[0113] Comparing silver paste example (3), silver paste example (4), silver paste example (5) and comparative example 4, after adding polyol to the silver paste, the crosslinking density of the silver paste after curing is improved, thereby improving the resistivity change rate of the silver paste after ring measurement, and the results show that the silver paste prepared with polyester polyol F1010 has a lower resistivity.

[0114] If the silver paste is made without adding isocyanate 3175, such as in Comparative Example 8, the liquid polyester polyol cannot be cured and cross-linked, resulting in the silver line being unable to dry after baking and being in a viscous state, causing infinite line resistance. If the silver paste is made without adding hexahydrophthalic anhydride, such as in Comparative Example 9, the silver paste can be cured under the action of curing agent 3175, but the resistivity is slightly too high. After adding hexahydrophthalic anhydride, the cross-linking and curing of the epoxy resin in the silver paste can be strengthened, thereby further reducing the resistivity of the silver paste.

[0115] If the silver paste is prepared without adding the flaky silver powder F1, as in Comparative Example 10, the resistivity of the prepared silver paste is significantly higher. However, if the amount of F1 is increased, the resistivity cannot be further reduced. When the amount of F1 is too large, its tap density is only 4.3 g / cm 3 The viscosity of the prepared silver paste seriously exceeds the upper limit of viscosity suitable for printing (130000cp), so too much amount cannot be added.

Claims

1. A high-crystalline silver powder obtained by coating a silver layer on the surface of an inorganic powder, characterized in that: The preparation method of high-crystalline silver powder comprises the following steps: mixing inorganic powder with an anti-flocculant and dispersant water after surface smoothing treatment to obtain an inorganic powder dispersion; adding the inorganic powder dispersion into a reducing agent solution containing a particle size control agent at one time; controlling the stirring speed to be between 150 and 400 r / min; then dropwise adding a silver nitrate solution within 2 to 8 hours; and coating the surface of the inorganic powder with a silver layer by a chemical reduction method to obtain the high-crystalline silver powder; the inorganic powder comprises one or more of glass powder, ceramic powder, silicon dioxide powder, carbon powder, and graphite powder; the particle size of the inorganic powder is 1 nm to 300 nm; and the concentration of the silver nitrate solution is 0.5 to 2.0 mol / L.

2. The method for preparing the high-crystalline silver powder according to claim 1, characterized in that: The method comprises the following steps: mixing inorganic powder with an anti-flocculant and dispersant water after surface smoothing treatment to obtain an inorganic powder dispersion; then mixing the inorganic powder with a reducing agent, a particle size control agent and silver nitrate; and coating the surface of the inorganic powder with a silver layer by a chemical reduction method to obtain high-crystalline silver powder.

3. The method for preparing high-crystalline silver powder according to claim 2, characterized in that: The surface smoothing treatment includes physical surface smoothing treatment or chemical surface smoothing treatment; the reducing agent is one or more of ascorbic acid, formaldehyde and hydrazine hydrate.

4. A low-cost heterojunction silver paste comprising a carrier, the high-crystalline silver powder according to claim 1, and flaky silver powder; the carrier comprising an epoxy resin, a thermosetting oligomer, a solvent, an epoxy curing agent, and a blocked isocyanate curing agent; the thermosetting oligomer is a polyol with a valence of three or more.

5. The low-cost heterojunction silver paste according to claim 4, characterized in that: The low-cost heterojunction silver paste is composed of a carrier, high-crystalline silver powder, and flaky silver powder. The mass percentage of the high-crystalline silver powder is 60% to 95%, the mass percentage of the flaky silver powder is 5% to 30%, and the balance is the carrier. The carrier is composed of an epoxy resin, a thermosetting oligomer, a solvent, an epoxy curing agent, and a blocked isocyanate curing agent. By mass percentage, the epoxy resin is 1% to 10%, the thermosetting oligomer is 0.1% to 5%, the epoxy curing agent is 0.1% to 3%, the blocked isocyanate curing agent is 1% to 5%, and the solvent is the balance.

6. The method for preparing the low-cost heterojunction silver paste according to claim 4, characterized in that The high-crystalline silver powder and flaky silver powder according to claim 1 are dispersed in a carrier to obtain a low-cost heterojunction silver paste.

7. Use of the highly crystalline silver powder according to claim 1 in preparing heterojunction solar cell electrodes.

Citation Information

Patent Citations

  • Method for preparing metal and dielectric composite grains of silicon dioxide coated by Nano silver

    CN101003907A

  • Lead-free and low-silver photosensitive silver paste and preparation method thereof

    CN101728001A

  • Conductive silver paste for front face of crystalline silicon solar battery

    CN104575666A

  • Heat-cured conductive paste composition

    CN105793931A

  • Low-temperature conductive silver slurry and preparation method thereof