Method for manufacturing patterned single-layer phase difference material
By using a composition of specific polymers and additives in the manufacturing process of patterned single-layer phase difference material, combined with multiple UV irradiation and heating processes, the HAZE problem in patterned single-layer phase difference material is solved, and high phase is achieved The suppression of the difference value and low phase difference value regions improves the hardness and optical performance of the film.
Patent Information
- Application Number
- CN202080074674.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-05
- Filing Date
- 2020-11-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-04
AI Technical Summary
In the prior art, when manufacturing a patterned single-layer phase difference material, there is a problem of turbidity (HAZE) in the unexposed portion of ultraviolet light, and it is difficult to exhibit a high phase difference value in the anisotropic phase and suppress the phase difference value of the isotropic phase.
By using a composition containing a specific polymer and additive, multiple UV irradiation and heating processes are used to form high anisotropic and low anisotropic regions, and optical anisotropicity is controlled using different exposure amounts of polarized UV and all-light UV rays. Inhibits the whitening of the membrane.
The whitening of the film is suppressed in the high-phase difference region and the low-phase difference region, the hardness of the film is improved, and the emergence of HAZE is effectively suppressed.
Smart Images

Figure BDA0003609529630000031 
Figure BDA0003609529630000041 
Figure BDA0003609529630000051
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a patterned single-layer phase difference material and a single-layer phase difference material. Specifically, the present invention relates to a patterned single-layer phase difference material obtained from a composition containing a liquid crystal polymer, wherein the liquid crystal polymer has the property that the orientation increases with the exposure amount below the optimal exposure amount, and the orientation decreases with the exposure amount above the optimal exposure amount. The liquid crystal polymer can be preferably used for materials with optical properties suitable for display devices, recording materials, etc., and can be particularly preferably used for optical compensation films such as polarizing plates and phase difference plates for liquid crystal displays. Background Art
[0002] According to the requirements of improving the display quality and lightening of liquid crystal display devices, as optical compensation films such as polarizing plates and phase difference plates, the requirements for polymer films that control the internal molecular orientation structure are increased. In order to cope with this requirement, a film obtained by utilizing the optical anisotropy of polymerizable liquid crystal compounds has been developed. The polymerizable liquid crystal compound used here is usually a liquid crystal compound having a polymerizable group and a liquid crystal structural part (a structural part having a spacer part and a liquid crystal original part), and acryl is widely used as the polymerizable group.
[0003] The polymerizable liquid crystal compound is usually polymerized by irradiation with radiation such as ultraviolet rays to form a polymer (film). For example, it is known that a specific polymerizable liquid crystal compound having an acrylic group is loaded between supports obtained by an orientation treatment, and the compound is irradiated with radiation while being kept in a liquid crystal state to obtain a polymer (Patent Document 1); a photopolymerization initiator is added to a mixture of two polymerizable liquid crystal compounds having an acrylic group or a composition in which a chiral liquid crystal is mixed in the mixture, and ultraviolet rays are irradiated to obtain a polymer (Patent Document 2).
[0004] In addition, various single-layer coating type alignment films have been reported, such as polymerizable liquid crystal compounds that do not require a liquid crystal alignment film, alignment films using polymers (Patent Documents 3 and 4), and alignment films using polymers containing photo-crosslinking sites (Patent Documents 5 and 6).
[0005] On the other hand, it is known that in an alignment film using a polymer having a photo-crosslinking site, when a patterned single-layer retardation film based on the material is produced using an exposure mask, haze (HAZE) in the portion not exposed to ultraviolet rays becomes a problem.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 62-70407
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 9-208957
[0010] Patent Document 3: European Patent Application Publication No. 1090325
[0011] Patent Document 4: International Publication No. 2008 / 031243
[0012] Patent Document 5: Japanese Patent Application Publication No. 2008-164925
[0013] Patent Document 6: Japanese Patent Application Laid-Open No. 11-189665 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The present invention is completed in view of the above-mentioned problems, and its purpose is to provide a method for manufacturing a patterned single-layer phase difference material that exhibits a high phase difference value in the anisotropic phase, suppresses the phase difference value in the isotropic phase, and further suppresses haze (HAZE) through a simple process.
[0016] Means for solving problems
[0017] The present inventors have repeatedly conducted in-depth studies to solve the above-mentioned problems, and as a result, have found that by using a composition containing a specific polymer and a specific additive and applying the following method for manufacturing a patterned phase difference material, it is possible to manufacture a patterned single-layer phase difference material that exhibits a high phase difference value in the anisotropic phase, suppresses the phase difference value in the isotropic phase, and further suppresses turbidity (HAZE), thereby completing the present invention.
[0018] That is, the present invention provides the following method for producing a patterned single-layer phase difference material.
[0019] 1. A method for manufacturing a patterned single-layer phase difference material, comprising:
[0020] (I) a step of coating a polymer composition containing a liquid crystalline polymer on a substrate to form a coating film, wherein the liquid crystalline polymer has a property that the orientation property increases with the exposure amount at an exposure amount lower than an optimum exposure amount, and the orientation property decreases with the exposure amount at an exposure amount higher than the optimum exposure amount;
[0021] (II) a step of irradiating the coating film obtained in step (I) with ultraviolet rays twice to generate a high anisotropy region and a low anisotropy region, wherein at least one of the irradiations is performed through a mask and at least one of the irradiations is performed with polarized ultraviolet rays, wherein the high anisotropy region has high optical anisotropy due to the irradiation with polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy due to the amount of ultraviolet rays being insufficient in a region below an optimum exposure amount and being excessive in a region above an optimum exposure amount; and
[0022] (III) A step of heating the coating film obtained in the step (II) to obtain a phase difference material.
[0023] 2. The method for producing a patterned single-layer phase difference material according to 1, wherein:
[0024] The above polymer composition comprises:
[0025] (A) a side chain polymer having a side chain having a photoreactive site represented by the following formula (a);
[0026] (B) a silane coupling agent; and
[0027] (C) an organic solvent;
[0028] [Chemical formula 1]
[0029]
[0030] In the formula, R 1 is an alkylene group having 1 to 30 carbon atoms, wherein one or more hydrogen atoms in the alkylene group may be substituted by a fluorine atom or an organic group; in addition, R 1 -CH 2 CH 2 - may or may not be substituted by -CH=CH-, R 1 -CH 2 - is or is not substituted by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-; wherein the adjacent -CH 2 - will not be substituted by these groups at the same time; in addition, -CH 2 -For or not for R 1 The terminal -CH 2 -;
[0031] R 2 is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed cyclic group;
[0032] R 3is a single bond, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)-O-;
[0033] R is an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group or a nitro group, and when c ≥ 2, each R is the same or different;
[0034] a is 0, 1, or 2;
[0035] b is 0 or 1;
[0036] c is an integer satisfying 0≤c≤2b+4;
[0037] The dotted lines are the bonding sites.
[0038] 3. The method for producing a patterned single-layer phase difference material according to 2, wherein the side chain having a photoreactive site is represented by the following formula (a1):
[0039] [Chemical formula 2]
[0040]
[0041] In the formula, R 1 , R 2 and a are the same as above;
[0042] R 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-;
[0043] The benzene ring in formula (a1) may be substituted with a substituent selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group, and a nitro group;
[0044] The dotted lines are the bonding sites.
[0045] 4. The method for producing a patterned single-layer retardation material according to 2 or 3, wherein the side chain polymer (A) further has a side chain that exhibits only liquid crystallinity.
[0046] 5. The method for producing a patterned single-layer phase difference material according to 4, wherein the side chain that only exhibits liquid crystallinity is a liquid crystal side chain represented by any one of the following formulas (1) to (13);
[0047] [Chemical formula 3]
[0048]
[0049] [Chemical formula 4]
[0050]
[0051] In formula (1) to formula (13), A 1 , A 2 are each independently a single bond, -O-, -CH 2 -, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-C(=O)-, -CH=CH-C(=O)-O- or -OC(=O)-CH=CH-;
[0052] R 11 For-No 2 , -CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms;
[0053] R 12 is a group selected from the group consisting of phenyl, naphthyl, biphenyl, furyl, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, and a group obtained by combining them, and the hydrogen atom bonded to them is or is not replaced by -NO 2 , -CN, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms;
[0054] R 13 For hydrogen atoms, -NO 2 、-CN、-CH=C(CN) 2 , -CH=CH-CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms;
[0055] E is -C(=O)-O- or -OC(=O)-;
[0056] d is an integer from 1 to 12;
[0057] k1 to k5 are each independently an integer of 0 to 2, wherein the total of k1 to k5 is 2 or more;
[0058] k6 and k7 are each independently an integer of 0 to 2, wherein the sum of k6 and k7 is 1 or more;
[0059] m1, m2 and m3 are each independently an integer from 1 to 3;
[0060] n is 0 or 1;
[0061] Z 1 and Z 2are each independently a single bond, -C(=O)-, -CH 2 O-, -CH=N- or -CF 2 -;
[0062] The dotted lines are the bonding sites.
[0063] 6. The method for producing a patterned single-layer retardation material according to 5, wherein the side chain that exhibits only liquid crystallinity is a liquid crystal side chain represented by any one of formulae (1) to (11).
[0064] 7. A single-layer phase difference material, which is manufactured by any one of the methods 1 to 6.
[0065] Effects of the Invention
[0066] According to the present invention, it is possible to provide a patterned retardation material which has a region with a high retardation value and a region with a low retardation value and which can suppress whitening of a film in the region with a low retardation value. DETAILED DESCRIPTION
[0067] The method for producing a patterned single-layer phase difference material of the present invention comprises the following steps [I] to [III]:
[0068] (I) a step of coating a polymer composition containing a liquid crystalline polymer on a substrate to form a coating film, wherein the liquid crystalline polymer has a property that the orientation property increases with the exposure amount at an exposure amount lower than an optimum exposure amount, and the orientation property decreases with the exposure amount at an exposure amount higher than the optimum exposure amount;
[0069] (II) a step of irradiating the coating film obtained in step (I) with ultraviolet rays twice to generate a high anisotropy region and a low anisotropy region, wherein at least one of the irradiations is performed through a mask and at least one of the irradiations is performed with polarized ultraviolet rays, wherein the high anisotropy region has high optical anisotropy due to the irradiation with polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy due to the amount of ultraviolet rays being insufficient in a region below an optimum exposure amount and being excessive in a region above an optimum exposure amount; and
[0070] (III) A step of heating the coating film obtained in the step (II) to obtain a phase difference material.
[0071] The above-mentioned polymer composition includes a liquid crystalline polymer, which has a property that the more exposure the exposure is below the optimal exposure, the more the orientation increases, and the more exposure the exposure is above the optimal exposure, the less the orientation decreases (hereinafter, also referred to as a side chain polymer), and the coating obtained using the above-mentioned polymer composition is a film containing a photosensitive side chain polymer that can show liquid crystal properties. The coating is not subjected to friction treatment, and an orientation treatment is performed by polarized irradiation. In addition, after polarized irradiation, a film (hereinafter, also referred to as a single-layer phase difference material) is formed by heating the above-mentioned coating to impart optical anisotropy. At this time, the slight anisotropy expressed by polarized irradiation forms a driving force, and the liquid crystal side chain polymer itself is effectively reoriented by self-organization. As a result, a highly efficient orientation treatment is achieved, and a single-layer phase difference material imparting high optical anisotropy can be obtained.
[0072] In addition, the method for manufacturing the patterned single-layer phase difference material of the present invention has the following steps: in order to produce high anisotropy regions and low anisotropy regions, at least once through a mask, at least once using polarized ultraviolet rays, and irradiating ultraviolet rays twice, wherein the high anisotropy region has high optical anisotropy by irradiating polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy by making the amount of ultraviolet rays insufficient in the region below the optimal exposure amount and excessive in the region above the optimal exposure amount. By having the above-mentioned steps, ultraviolet rays are irradiated in both the region having anisotropy and the region having reduced anisotropy compared thereto, thereby increasing the hardness of the film, and as a result, in the patterned phase difference material, the turbidity of the film in the region with low anisotropy, that is, the so-called whitening phenomenon, can be suppressed. Thus, a patterned phase difference material with suppressed HAZE can be obtained.
[0073] Hereinafter, embodiments of the present invention will be described in detail.
[0074] [Polymer composition]
[0075] The polymer composition used in the production method of the present invention comprises: (A) a side chain type polymer having a side chain having a photoreactive site, (B) a silane coupling agent, and (C) an organic solvent.
[0076] [(A) Side chain polymer]
[0077] The component (A) is a photosensitive side chain polymer that exhibits liquid crystallinity in a predetermined temperature range and has a side chain having a photoreactive site represented by the following formula (a) (hereinafter also referred to as side chain a).
[0078] [Chemical formula 5]
[0079]
[0080] In formula (a), R 1 is an alkylene group having 1 to 30 carbon atoms, and one or more hydrogen atoms in the alkylene group may be substituted with a fluorine atom or an organic group. 1 -CH 2 CH 2 - may be substituted by -CH=CH-, R 1 -CH 2 - may be substituted by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-. 2 - will not be substituted by these groups at the same time. In addition, -CH 2 - can be R 1 The terminal -CH 2 -. R 2 is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed cyclic group. 3 is a single bond, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)-O-. R is an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group or a nitro group. When c ≥ 2, each R may be the same or different. a is 0, 1 or 2. b is 0 or 1. c is an integer satisfying 0≤c≤2b+4. The dotted line is a bonding site.
[0081] R 1 The alkylene group having 1 to 30 carbon atoms may be linear, branched or cyclic, and specific examples thereof include methylene, ethylene, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl and decane-1,10-diyl.
[0082] As R 2 The divalent aromatic group represented by may be phenylene, biphenylene, etc. 2 The divalent alicyclic group represented by is exemplified by cyclohexanediyl and the like. 2 The divalent heterocyclic group represented by is exemplified by furandiyl and the like. 2 Examples of the divalent fused cyclic group represented by include naphthylene and the like.
[0083] As the side chain a, a side chain represented by the following formula (a1) (hereinafter also referred to as side chain a1) is preferred.
[0084] [Chemical formula 6]
[0085]
[0086] In formula (a1), R 1 , R 2 and a are the same as above. 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-. The benzene ring in formula (a1) may be substituted with a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group and a nitro group. The dotted line is a bonding site.
[0087] As the side chain a1, for example, a side chain represented by the following formula (a1-1) is preferred.
[0088] [Chemical formula 7]
[0089]
[0090] In formula (a1-1), L is a linear or branched alkylene group having 1 to 16 carbon atoms. X is a single bond, -O-, -C(=O)-O-, or -OC(=O)-.
[0091] The side chain polymer (A) is preferably a polymer that reacts to light in the wavelength range of 250 to 400 nm and exhibits liquid crystallinity in the temperature range of 100 to 300° C. The side chain polymer (A) preferably has a photosensitive side chain that reacts to light in the wavelength range of 250 to 400 nm.
[0092] A photosensitive side chain is bonded to the main chain of the side chain polymer (A), which can be responsive to light and cause a crosslinking reaction or an isomerization reaction. The structure of the photosensitive side chain polymer that can exhibit liquid crystallinity is not particularly limited as long as it satisfies the above characteristics, and preferably has a rigid mesogen component in the side chain structure. When the side chain polymer is made into a single-layer phase difference material, stable optical anisotropy can be obtained.
[0093] As a more specific example of the structure of a photosensitive side chain polymer capable of exhibiting liquid crystal properties, it is preferably a structure having a main chain composed of at least one free radical polymerizable group selected from (meth)acrylate, itaconate, fumarate, maleate, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene and the like and siloxane, and a side chain a.
[0094] In addition, the side chain polymer (A) exhibits liquid crystallinity in the temperature range of 100 to 300° C., and therefore it is further preferred to have a side chain that exhibits only liquid crystallinity (hereinafter, also referred to as side chain b). It should be noted that “exhibiting only liquid crystallinity” here means that the polymer having only the side chain b does not exhibit photosensitivity in the production process of the phase difference material of the present invention (i.e., steps (I) to (III) described later), and only exhibits liquid crystallinity.
[0095] The side chain b is preferably any liquid crystalline side chain selected from the following formulae (1) to (13).
[0096] [Chemical formula 8]
[0097]
[0098] [Chemical formula 9]
[0099]
[0100] In formulas (1) to (13), A 1 , A 2 are each independently a single bond, -O-, -CH 2 -, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-C(=O)-, -CH=CH-C(=O)-O- or -OC(=O)-CH=CH-. R 11 For-No 2 , -CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. 12 is a group selected from the group consisting of a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, and a group obtained by combining them, and the hydrogen atom bonded to them may be -NO 2 , -CN, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. 13 For hydrogen atoms, -NO 2 、-CN、-CH=C(CN) 2, -CH=CH-CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. E is -C(=O)-O- or -OC(=O)-. d is an integer from 1 to 12; k1 to k5 are each independently an integer from 0 to 2, wherein the total of k1 to k5 is 2 or more. k6 and k7 are each independently an integer from 0 to 2, wherein the total of k6 and k7 is 1 or more. m1, m2 and m3 are each independently an integer from 1 to 3. n is 0 or 1. Z 1 and Z 2 are each independently a single bond, -C(=O)-, -CH 2 O-, -CH=N- or -CF 2 -. The dotted line is the bonding site.
[0101] Among them, the side chain b is preferably a side chain represented by any one of formulae (1) to (11).
[0102] The side chain polymer of the component (A) can be obtained by polymerizing a monomer having a structure represented by the formula (a) and a monomer having a structure that exhibits only liquid crystallinity, which is used as desired.
[0103] Examples of the monomer having a structure represented by formula (a) (hereinafter also referred to as monomer M1) include compounds represented by the following formula (M1).
[0104] [Chemical formula 10]
[0105]
[0106] (Where R 1 , R 2 , R 3 , R, a, m and n are the same as above)
[0107] As the monomer M1, a monomer represented by the following formula (M1A) is preferred.
[0108] [Chemical formula 11]
[0109]
[0110] (Where R 1 , R 2 , R 3A , R and a are the same as above)
[0111] Among monomers M1A, a monomer represented by the following formula (M1B) is more preferred.
[0112] [Chemical formula 12]
[0113]
[0114] (where L and X are the same as above)
[0115] In the formulae (M1), (M1A) and (M1B), PL is a polymerizable group represented by any one of the following formulae (PL-1) to (PL-5).
[0116] [Chemical formula 13]
[0117]
[0118] In formulas (PL-1) to (PL-5), Q 1 , Q 2 and Q 3 is a hydrogen atom, a linear or branched alkyl group having 1 to 10 carbon atoms, or a linear or branched alkyl group having 1 to 10 carbon atoms substituted with a halogen. 1 or the bonding site of L. Among the above monomers, some are commercially available, and some can be produced from known substances by known production methods.
[0119] Preferred examples of the monomer M1 include those represented by the following formulae (M1-1) to (M1-5).
[0120] [Chemical formula 14]
[0121]
[0122] (wherein, PL is the same as above; p is an integer from 2 to 9)
[0123] The monomer having a structure that exhibits only liquid crystallinity (hereinafter, also referred to as monomer M2) is a monomer in which a polymer derived from the monomer exhibits liquid crystallinity and the polymer can form a mesogen group at a side chain site.
[0124] The mesogen group on the side chain may be a group that forms a mesogen structure independently, such as biphenyl and phenyl benzoate, or a group that forms a mesogen structure by hydrogen bonding the side chains, such as benzoic acid. The mesogen group on the side chain preferably has the following structure.
[0125] [Chemical formula 15]
[0126]
[0127] As a more specific example of the monomer M2, it is preferred to have a structure having: a polymerizable group derived from at least one of free radical polymerizable groups selected from hydrocarbons, (meth)acrylates, itaconates, fumarates, maleates, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene, and siloxane, and a structure consisting of at least one of formulas (1) to (13). The monomer M2 is particularly preferably a monomer having a (meth)acrylate as a polymerizable group, and preferably a monomer having -COOH at the end of the side chain.
[0128] Preferred examples of the monomer M2 include monomers represented by the following formulae (M2-1) to (M2-11).
[0129] [Chemical formula 16]
[0130]
[0131] [Chemical formula 17]
[0132]
[0133] (where PL and p are the same as above)
[0134] In addition, other monomers may be copolymerized within a range that does not impair the performance of photoreactivity and / or liquid crystal properties. Examples of other monomers include monomers that are industrially available and can undergo free radical polymerization. Specific examples of other monomers include unsaturated carboxylic acids, acrylate compounds, methacrylate compounds, maleimide compounds, acrylonitrile, maleic anhydride, styrene compounds, vinyl compounds, and the like.
[0135] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid.
[0136] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthracene acrylate, anthracene methyl acrylate, phenyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-propyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecanyl acrylate, and 8-ethyl-8-tricyclodecanyl acrylate.
[0137] Examples of the methacrylate compound include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthracene methacrylate, anthracene methyl methacrylate, phenyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecanyl methacrylate, and 8-ethyl-8-tricyclodecanyl methacrylate.
[0138] Examples of the vinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, propyl vinyl ether, etc. Examples of the styrene compound include styrene, 4-methylstyrene, 4-chlorostyrene, 4-bromostyrene, etc. Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, N-cyclohexylmaleimide, etc.
[0139] From the viewpoint of photoreactivity, the content of the side chain a in the side chain type polymer of the present invention is preferably 20 to 99.9 mol %, more preferably 30 to 95 mol %, and even more preferably 40 to 90 mol %.
[0140] From the viewpoint of the phase difference value, the content of the side chain b in the side chain type polymer of the present invention is preferably 0.1 to 80 mol %, more preferably 5 to 70 mol %, and further preferably 10 to 60 mol %.
[0141] As described above, the side chain type polymer of the present invention may contain other side chains. When the total content of the side chain a and the side chain b does not satisfy 100 mol %, the content of the other side chains is the remainder.
[0142] The manufacturing method of the side chain polymer of component (A) is not particularly limited, and a general method adopted in industry can be utilized. Specifically, it can be manufactured by free radical polymerization, cationic polymerization or anionic polymerization of the vinyl group of the above-mentioned monomer M1, monomer M2 and other desired monomers. Among them, free radical polymerization is particularly preferred from the viewpoints of the ease of reaction control, etc.
[0143] As the polymerization initiator for radical polymerization, known compounds such as radical polymerization initiators (radical thermal polymerization initiators, radical photopolymerization initiators) and reversible addition-fragmentation chain transfer (RAFT) polymerization agents can be used.
[0144] The free radical thermal polymerization initiator is a compound that generates free radicals by heating to a temperature higher than the decomposition temperature. Examples of the free radical thermal polymerization initiator include ketone peroxides (methyl ethyl ketone peroxide, cyclohexanone peroxide, etc.), diacyl peroxides (acetyl peroxide, benzoyl peroxide, etc.), hydroperoxides (hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, etc.), dialkyl peroxides (di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, etc.), peroxyacetals (dibutyl peroxycyclohexane, etc.), peroxyalkyl esters (tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, tert-amyl peroxy-2-ethylcyclohexane, etc.), persulfates (potassium persulfate, sodium persulfate, ammonium persulfate, etc.), and azo compounds (azobisisobutyronitrile and 2,2'-bis(2-hydroxyethyl)azobisisobutyronitrile, etc.). The radical thermal polymerization initiator may be used alone or in combination of two or more.
[0145] The free radical photopolymerization initiator is not particularly limited as long as it is a compound that initiates free radical polymerization by light irradiation. Examples of the free radical photopolymerization initiator include benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexylphenyl ketone, isopropylbenzoin ether, isobutylbenzoin ether, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, camphorquinone, benzanthrone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 4-Dimethylaminobenzoic acid ethyl ester, 4-dimethylaminobenzoic acid isopentyl ester, 4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-pentyloxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine (Trichloromethyl)-s-triazine, 4-[pN,N-bis(ethoxycarbonylmethyl)]-2,6-bis(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4'-methoxyphenyl)-s-triazine, 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-mercaptobenzothiazole, 3,3'-carbonylbis(7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(4-ethoxycarbonylphenyl)-1, 2'-Bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinopropionyl)-9-n-dodecylcarbazole, 1-hydroxycyclohexylphenyl ketone, bis(5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4'-di(methoxycarbonyl)-4,3'-di(tert-butylperoxycarbonyl)benzophenone, 4,4'-di(methoxycarbonyl)-3,3'-di(tert-butylperoxycarbonyl)benzophenone, 2-(3-methyl-3H-benzothiazol-2-ylidene)-1-naphth-2-yl-ethanone, 2-(3-methyl-1,3-benzothiazol-2(3H)-ylidene)-1-(2-benzoyl)ethanone, etc. The free radical photopolymerization initiator may be used alone or in combination of two or more.
[0146] The radical polymerization method is not particularly limited, and emulsion polymerization, suspension polymerization, dispersion polymerization, precipitation polymerization, bulk polymerization, solution polymerization, and the like can be used.
[0147] The organic solvent used in the polymerization reaction is not particularly limited as long as it is a solvent in which the generated polymer is dissolved. Specific examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methyl-ε-caprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethylphosphoric acid triamide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, dipentene, ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, methyl Cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol-tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene Glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, 1,4-dioxane, n-hexane, n-pentane, n-octane, diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-acetate Butyl ester, propylene glycol monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, etc.
[0148] Above-mentioned organic solvent can use 1 kind alone, also can mix and use 2 or more kinds.In addition, even if it is the solvent of the polymkeric substance that does not dissolve generation, in the scope that the polymkeric substance that generates does not separate out, also can mix and use with above-mentioned organic solvent.In addition, in free radical polymerization, the oxygen in the organic solvent becomes the reason that hinders polyreaction, so organic solvent preferably uses the organic solvent of degassing as far as possible.
[0149] The polymerization temperature during free radical polymerization can be selected from any temperature of 30 to 150° C., preferably in the range of 50 to 100° C. In addition, the reaction can be carried out at any concentration. If the concentration is too low, it is difficult to obtain a high molecular weight polymer. If the concentration is too high, the viscosity of the reaction solution becomes too high, and uniform stirring becomes difficult. Therefore, the monomer concentration is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. The reaction can be carried out at a high concentration at the beginning, and then an organic solvent is added.
[0150] In the above-mentioned free radical polymerization reaction, if the ratio of the free radical polymerization initiator is large relative to the monomer, the molecular weight of the obtained polymer becomes small, and if the ratio of the free radical polymerization initiator is small relative to the monomer, the molecular weight of the obtained polymer becomes large, so the ratio of the free radical initiator is preferably 0.1 to 10 mol% relative to the monomer to be polymerized. In addition, various monomer components, solvents, initiators, etc. may also be added during polymerization.
[0151] When the polymer produced is recovered from the reaction solution obtained by the above reaction, the reaction solution is put into a poor solvent to precipitate the polymer. Examples of the poor solvent used in the precipitation include methanol, acetone, hexane, heptane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, diethyl ether, methyl ethyl ether, water, and the like. After the polymer precipitated by being put into the poor solvent is filtered and recovered, it can be dried at room temperature or by heating under normal pressure or reduced pressure. In addition, if the operation of dissolving the recovered polymer in an organic solvent again and reprecipitating and recovering it is repeated 2 to 10 times, the impurities in the polymer can be reduced. Examples of the poor solvent at this time include alcohols, ketones, hydrocarbons, and the like. If three or more poor solvents selected from them are used, the efficiency of purification is further improved, so it is preferred.
[0152] Taking into account the strength of the obtained coating film, workability during coating film formation, and uniformity of the coating film, the weight average molecular weight of the side chain polymer (A) of the present invention as measured by GPC (Gel Permeation Chromatography) is preferably 2,000 to 2,000,000, more preferably 2,000 to 1,000,000, and even more preferably 5,000 to 200,000.
[0153] [(B) Silane coupling agent]
[0154] The polymer composition of the present invention contains (B) a silane coupling agent. The silane coupling agent is preferably a silane compound represented by the following formula (B).
[0155] [Chemical formula 18]
[0156]
[0157] In formula (B), R21 R is a reactive functional group. 22 R is a hydrolyzable group. 23 is a methyl group or an ethyl group. x is an integer of 0 to 3. y is an integer of 1 to 3.
[0158] As R 21 The reactive functional group represented by , includes amino, urea, (meth)acryloyloxy, vinyl, epoxy, mercapto and groups having an oxetane structure, etc., preferably amino, urea, (meth)acryloyloxy and groups having an oxetane structure, etc. Groups having an oxetane structure are particularly preferred.
[0159] As R 22 The hydrolyzable group represented by may be a halogen atom, an alkoxy group having 1 to 3 carbon atoms, an alkoxyalkoxy group having 2 to 4 carbon atoms, etc. Examples of the halogen atom include a chlorine atom, a bromine atom, etc. The alkoxy group having 1 to 3 carbon atoms is preferably a linear or branched group, specifically a methoxy group, an ethoxy group, a n-propoxy group, and an isopropoxy group. In addition, specific examples of the alkoxyalkoxy group having 2 to 4 carbon atoms include a methoxymethoxy group, a 2-methoxyethoxy group, an ethoxymethoxy group, and a 2-ethoxyethoxy group.
[0160] Specific examples of the silane coupling agent (B) include 3-aminopropyltrichlorosilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrichlorosilane, allyltrimethoxysilane, allyltriethoxysilane, Silane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propyltrimethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propyltriethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propylmethyldimethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propylmethyldiethoxysilane, and the like.
[0161] Among them, 3-(3-ethyloxetane-3-ylmethoxy)propyltrimethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propyltriethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propylmethyldimethoxysilane, 3-(3-ethyloxetane-3-ylmethoxy)propylmethyldiethoxysilane, etc. are particularly preferred. As the above-mentioned silane coupling agent, commercially available products can be used.
[0162] In the polymer composition of the present invention, the content of the (B) silane coupling agent is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the polymer.
[0163] [(C) Organic solvent]
[0164] The organic solvent of the component (C) is not particularly limited as long as it is an organic solvent that dissolves the polymer component. Specific examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methyl-ε-caprolactam, 2-pyrrolidone, N-ethyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethylphosphoric acid triamide, γ-butyrolactone, 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, 1,3-dimethyl-2-imidazolidinone, ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, cyclohexanone, ethylene carbonate, propylene carbonate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, and the like. These may be used alone or in combination of two or more.
[0165] [Other ingredients]
[0166] The polymer composition of the present invention may contain components other than components (A) to (C). Examples thereof include, but are not limited to, solvents and compounds that improve film thickness uniformity and surface smoothness when the polymer composition is applied, and compounds that improve adhesion between the phase difference material and the substrate.
[0167] Specific examples of solvents (poor solvents) for improving uniformity of film thickness and surface smoothness include isopropyl alcohol, methoxymethylpentyl alcohol, methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethyl carbitol acetate, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether. , propylene glycol tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutyl Olefins, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methyl cyclohexene, propyl ether, dihexyl ether, 1-hexanol, n-hexane, n-pentane, n-octane, ethyl ether, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate , 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-butoxy-2-propanol, 1-phenoxy-2-propanol, propylene glycol diacetate, propylene glycol-1-monomethyl ether-2-acetate, propylene glycol-1-monoethyl ether-2-acetate, 2-(2-ethoxypropoxy)propanol and the like solvents having low surface tension.
[0168] The above-mentioned poor solvent can be used alone or in combination of two or more. When the above-mentioned poor solvent is used, its content is preferably 5 to 80% by mass, more preferably 20 to 60% by mass in the solvent in order not to significantly reduce the solubility of the entire solvent contained in the polymer composition.
[0169] As compounds that improve the uniformity of film thickness and surface smoothness, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be cited. More specifically, for example, Eftop (registered trademark) 301, EF303, EF352 (manufactured by Tohkem Products Co., Ltd.), MEGAFAC (registered trademark) F171, F173, R-30, R-40 (manufactured by DIC Co., Ltd.), FLUORAD FC430, FC431 (manufactured by 3M Co., Ltd.), AsahiGuard (registered trademark) AG710 (manufactured by AGC Co., Ltd.), SURFLON (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by AGC SEIMICHEMICAL Co., Ltd.), etc. The content of the above-mentioned surfactant is preferably 0.01 to 2 parts by mass, and more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of component (A).
[0170] Furthermore, in order to improve the adhesion between the substrate and the phase difference material and prevent the degradation of characteristics due to light such as backlight, a phenoplast-based compound or an epoxy-containing compound may be added to the polymer composition.
[0171] Specific examples of the phenolic plastic additive are shown below, but the invention is not limited thereto.
[0172] [Chemical formula 19]
[0173]
[0174] Specific examples of the epoxy group-containing compound include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-xylene diamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane.
[0175] When using a compound that improves adhesion to a substrate, the content is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the polymer component contained in the polymer composition. If the content is less than 0.1 parts by mass, the effect of improving adhesion cannot be expected, and if it is more than 30 parts by mass, the orientation of the liquid crystal may sometimes deteriorate.
[0176] As an additive, a photosensitizer can also be used. As the photosensitizer, a colorless sensitizer and a triplet sensitizer are preferred.
[0177] Examples of the photosensitizer include aromatic nitro compounds, coumarins (7-diethylamino-4-methylcoumarin, 7-hydroxy-4-methylcoumarin), ketocoumarins, carbonyl dicoumarins, aromatic 2-hydroxyketones (2-hydroxybenzophenone, mono- or di-p-(dimethylamino)-2-hydroxybenzophenone, etc.), acetophenones, anthraquinones, xanthone, thioxanthone, anthrone, thiazolines (2-benzoylmethylene-3-methyl-β-naphthothiazoline, 2-(β-naphthoylmethylene)-3-methyl-β-naphthothiazoline, etc.), oxazoline (2-(4-biphenoyl)-3-methyl-β-naphthoylmethylene)-3-methyl-β-naphthoylthiazoline, 2-(4-biphenoyl)-3-methyl-β-naphthoylthiazoline, 2-(p-fluorobenzoylmethylene)-3-methyl-β-naphthoylthiazoline, etc.), oxazoline (2-(4-biphenoyl)-3-methyl-β-naphthoylmethylene)-3-methyl-β-naphthoylthiazoline, etc.), Acylmethylene-3-methyl-β-naphthooxazoline, 2-(β-naphthoylmethylene)-3-methylbenzoxazoline, 2-(α-naphthoylmethylene)-3-methylbenzoxazoline, 2-(4-biphenylmethylene)-3-methylbenzoxazoline, 2-(β-naphthoylmethylene)-3-methyl-β-naphthooxazoline, 2-(4-biphenylmethylene)-3-methyl-β-naphthooxazoline, 2-(p-fluorobenzoylmethylene)-3-methyl -β-naphthoxazoline, etc.), benzothiazole, nitroaniline (m- or p-nitroaniline, 2,4,6-trinitroaniline, etc.), nitroacenaphthene (5-nitroacenaphthene, etc.), 2-[(m-hydroxy-p-methoxy)phenyl]benzothiazole, benzoin alkyl ether, N-alkylated phthaloyl ketone, acetophenone ketal (2,2-dimethoxyphenylacetophenone, etc.), naphthalene (2-naphthylmethanol, 2-naphthoic acid, etc.), anthracene (9-anthracenemethanol, 9-anthracenecarboxylic acid, etc.), benzopyran, azoindolizine, merolocoumarin, etc. Among them, aromatic 2-hydroxyketone (benzophenone), coumarin, ketocoumarin, carbonylbiscoumarin, acetophenone, anthraquinone, xanthone, thioxanthone and acetophenone ketal are preferred.
[0178] In the polymer composition of the present invention, in addition to the above-mentioned substances, dielectrics and conductive substances may be added to change the electrical properties such as the dielectric constant and conductivity of the phase difference material within the range that does not impair the effects of the present invention. In addition, cross-linking compounds may be added to increase the hardness and density of the film when the phase difference material is made.
[0179] [Preparation of polymer composition]
[0180] The polymer composition of the present invention is preferably prepared as a coating liquid in a manner suitable for forming a monolayer phase difference material. That is, the polymer composition used in the present invention is preferably prepared as a solution obtained by dissolving (A) component and (B) component, and the above-mentioned solvent or compound for improving film thickness uniformity and surface smoothness, and the compound for improving the adhesion of the liquid crystal alignment film to the substrate in the organic solvent of (C) component. Here, the content of (A) component is preferably 1 to 30% by mass in the composition of the present invention.
[0181] The polymer composition of the present invention may contain other polymers in addition to the polymer of component (A) without damaging the liquid crystal performance and photosensitivity. In this case, the content of other polymers in the polymer component is preferably 0.5 to 80% by mass, more preferably 1 to 50% by mass. Examples of other polymers include side chain polymers that are not photosensitivity capable of showing liquid crystal properties, such as poly(meth)acrylates, polyamic acids, and polyimides.
[0182] [Method for producing single-layer phase difference material]
[0183] As described above, the method for producing a patterned single-layer phase difference material of the present invention includes the following steps (I) to (III).
[0184] (I) a step of coating a polymer composition containing a liquid crystalline polymer on a substrate to form a coating film, wherein the liquid crystalline polymer has a property that the orientation property increases with the exposure amount at an exposure amount lower than an optimum exposure amount, and the orientation property decreases with the exposure amount at an exposure amount higher than the optimum exposure amount;
[0185] (II) a step of irradiating the coating film obtained in step (I) with ultraviolet rays twice to generate a high anisotropy region and a low anisotropy region, wherein at least one of the irradiations is performed through a mask and at least one of the irradiations is performed with polarized ultraviolet rays, wherein the high anisotropy region has high optical anisotropy due to the irradiation with polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy due to the amount of ultraviolet rays being insufficient in a region below an optimum exposure amount and being excessive in a region above an optimum exposure amount; and
[0186] (III) A step of heating the coating film obtained in the step (II) to obtain a phase difference material.
[0187] [Step (I)]
[0188] (I) is a process of coating a polymer composition containing a liquid crystal polymer on a substrate to form a coating film, wherein the liquid crystal polymer has the property that the more exposure the exposure is, the more the orientation increases at an exposure amount lower than the optimum exposure amount, and the more exposure the exposure is, the less the orientation decreases at an exposure amount higher than the optimum exposure amount. More specifically, the composition is coated on a substrate (e.g., a silicon / silicon dioxide covered substrate, a silicon nitride substrate, a substrate covered with a metal such as aluminum, molybdenum, chromium, etc., a glass substrate, a quartz substrate, an ITO substrate, etc.), a film (e.g., a triacetyl cellulose (TAC) film, a cycloolefin polymer film, a polyethylene terephthalate film, a resin film such as an acrylic film), etc. by rod coating, spin coating, flow coating, roller coating, slit coating, spin coating followed by slit coating, an inkjet method, a printing method, etc. After coating, the solvent may be evaporated by heating means such as a hot plate, a heat circulation oven or an IR (infrared) oven, preferably at 50 to 200° C., more preferably at 50 to 150° C., to obtain a coating film.
[0189] [Step (II)]
[0190] In step (II), the coating film obtained in step (I) is irradiated with ultraviolet rays twice to generate a high anisotropy region and a low anisotropy region, wherein at least one irradiation is performed through a mask and at least one irradiation is performed using polarized ultraviolet rays, the high anisotropy region has high optical anisotropy by irradiating with polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy by making the amount of ultraviolet rays insufficient in a region below the optimal exposure amount and excessive in a region above the optimal exposure amount. More specific embodiments of the above steps include the following steps (II-1) to (II-3).
[0191] [Step (II-1)]
[0192] Step (II-1) is to irradiate the first ultraviolet light through a mask in such a way that only the region to which anisotropy is desired is covered. The ultraviolet light at this time may be full-light ultraviolet light or polarized ultraviolet light. Then, the mask is removed and polarized ultraviolet light is irradiated. Thus, while the portion covered by the mask during the first irradiation is given anisotropy by irradiating only polarized ultraviolet light once, the region irradiated by the first ultraviolet light is irradiated with ultraviolet light for the second time, thereby reducing the anisotropy.
[0193] [Step (II-2)]
[0194] After the first ultraviolet irradiation using polarized ultraviolet rays in step (II-2), the second ultraviolet irradiation is performed through a mask in a manner that only covers the area to be given anisotropy. The ultraviolet rays during the second irradiation can be full-light ultraviolet rays or polarized ultraviolet rays. Thus, when the portion covered by the mask during the second irradiation is given anisotropy by irradiating only the polarized ultraviolet rays once, the anisotropy is reduced in the area irradiated by the second ultraviolet rays.
[0195] [Step (II-3)]
[0196] After the first ultraviolet irradiation using full-light ultraviolet light in step (II-3), polarized ultraviolet light irradiation is performed for the second time through a mask in a manner that only covers the area where anisotropy is not desired. The full-light ultraviolet light during the first irradiation is preferably less than the irradiation amount of the second polarized ultraviolet light. Thus, while the portion not covered by the mask during the second irradiation is given anisotropy by irradiating the polarized ultraviolet light, anisotropy is suppressed only in the area irradiated by the first ultraviolet light.
[0197] It should be noted that when irradiating polarized ultraviolet rays, polarized ultraviolet rays are irradiated to the substrate from a certain direction via a polarizing plate. As the ultraviolet rays used, ultraviolet rays with a wavelength range of 100 to 400 nm can be used. It is preferred to select the best wavelength via a filter or the like according to the type of coating used. In addition, for example, ultraviolet rays with a wavelength range of 290 to 400 nm can be selected to selectively cause a photocrosslinking reaction. As the ultraviolet rays, for example, light radiated by a high-pressure mercury lamp can be used.
[0198] The irradiation amount of polarized ultraviolet rays depends on the coating used. The irradiation amount is preferably set to be within the range of 1 to 70% of the amount of polarized ultraviolet rays that achieves the maximum value of ΔA (hereinafter also referred to as ΔAmax), which is the difference between the ultraviolet absorbance in the direction parallel to the polarization direction of the polarized ultraviolet rays in the coating, and the ultraviolet absorbance in the direction perpendicular to the polarization direction of the polarized ultraviolet rays, more preferably within the range of 1 to 50%.
[0199] The pattern shape and pattern size of the exposure mask used are not particularly limited. Examples of the pattern shape include a line pattern shape, a line / space (L / S) pattern shape, and a dot shape. As the pattern size, a pattern of micrometer size can be formed. For example, by using an exposure mask having a fine pattern of an L / S pattern shape, a fine L / S pattern of about 0.5 to 500 μm can be formed.
[0200] [Step (III)]
[0201] In step (III), the coating film obtained by irradiating the polarized ultraviolet rays in step (II) is heated. By heating, the coating film can be provided with an orientation controllable capability.
[0202] The heating may be performed by using a heating means such as a hot plate, a heat circulation oven, an IR (infrared) oven, etc. The heating temperature may be determined in consideration of the temperature at which the liquid crystallinity of the coating film to be used is expressed.
[0203] The heating temperature is preferably within the range of the temperature at which the polymer contained in the above-mentioned polymer composition exhibits liquid crystallinity (hereinafter referred to as the liquid crystal manifestation temperature). In the case of a thin film surface such as a coating, it is expected that the liquid crystal manifestation temperature of the coating surface is lower than the liquid crystal manifestation temperature when the above-mentioned polymer is observed as a body. Therefore, the heating temperature is more preferably within the temperature range of the liquid crystal manifestation temperature of the coating surface. That is, the range of the heating temperature after polarized ultraviolet irradiation is preferably a temperature with a lower limit of 10°C lower than the lower limit of the range of the liquid crystal manifestation temperature of the polymer used, and a temperature with a lower limit of 10°C lower than the upper limit of its liquid crystal temperature range. If the heating temperature is lower than the above-mentioned temperature range, there is a tendency that the amplification effect of the anisotropy of the coating obtained by heat becomes insufficient. In addition, if the heating temperature is too high compared to the above-mentioned temperature range, there is a tendency that the state of the coating is close to the isotropic liquid state (isotropic phase), in which case it is sometimes difficult to reorient in one direction by self-organization.
[0204] It should be noted that the liquid crystal display temperature refers to a temperature above the liquid crystal transition temperature at which a phase transition occurs from a solid phase to a liquid crystal phase on the surface of a polymer or coating film, and below the isotropic phase transition temperature (Tiso) at which a phase transition occurs from a liquid crystal phase to an isotropic phase. For example, the liquid crystal property is displayed below 130°C, which means that the liquid crystal transition temperature at which a phase transition occurs from a solid phase to a liquid crystal phase is below 130°C.
[0205] The thickness of the coating film formed after heating can be appropriately selected in consideration of the height difference, optical properties, and electrical properties of the substrate used, and is preferably 0.5 to 10 μm, for example.
[0206] The single-layer retardation material of the present invention thus obtained has optical properties suitable for use in display devices, recording materials, and the like, and is particularly suitable as an optical compensation film such as a polarizing plate and a retardation plate for a liquid crystal display.
[0207] Example
[0208] Hereinafter, the present invention will be described in more detail with reference to Synthesis Examples, Preparation Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0209] The monomer M1 having a photoreactive group and the monomer M2 having a liquid crystal group used in the embodiment are shown below. M1 and M2 are synthesized as shown below. M1 is synthesized according to the synthesis method described in International Publication No. 2011 / 084546. M2 is synthesized according to the synthesis method described in Japanese Patent Publication No. 9-118717. It should be noted that the side chain derived from M1 exhibits photoreactivity and liquid crystal properties, and the side chain derived from M2 only has liquid crystal properties.
[0210] [Chemical formula 20]
[0211]
[0212] In addition, the abbreviations of the reagents used in this example are shown below.
[0213] (Organic Solvent)
[0214] THF: Tetrahydrofuran
[0215] NMP: N-ethyl-2-pyrrolidone
[0216] BCS: Butyl Cellosolve
[0217] PGME: Propylene glycol monomethyl ether
[0218] (Polymerization initiator)
[0219] AIBN: 2,2'-azobisisobutyronitrile
[0220] (Polymerization initiator)
[0221] (additive)
[0222] TESOX-D: 3-ethyl-3-[3-(triethoxysilyl)propoxymethyl]oxetane
[0223] [Chemical formula 21]
[0224]
[0225] [Synthesis Example] Synthesis of Methacrylate Polymer Powder P1
[0226] M1 (49.9 g: 150 mmol) and M2 (68.9 g: 225 mmol) were dissolved in THF (482.2 g), degassed with a diaphragm pump, and then AIBN (1.23 g: 7.5 mmol) was added and degassed again. Thereafter, the mixture was reacted at 60° C. for 8 hours to obtain a methacrylate polymer solution. The polymer solution was added dropwise to a mixed solution of methanol (3020 g) and pure water (1200 g), and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure to obtain 101.1 g of methacrylate polymer powder P1.
[0227] [Preparation Example] Preparation of polymer solution
[0228] Methacrylate polymer powder P1 (20.0 g) obtained in Polymer Synthesis Example P1 was added to NMP (50.0 g) and stirred at room temperature for 3 hours to dissolve. PGME (10.0 g), BCS (20.0 g), TESOX-D (1.00 g) and MEGAFACE R-40 (0.01 g) were added to the solution and stirred to obtain polymer solution Q1.
[0229] [Preparation of a substrate for evaluating phase difference]
[0230] [Example 1]
[0231] The polymer solution Q1 was filtered through a filter with a pore size of 5.0 μm, and then spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Then, the coating surface was irradiated with polarized ultraviolet rays at 20 mJ / cm 2 After that, the film was irradiated with full-light ultraviolet light of 100 mJ / cm through an exposure mask with L / S=30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate R1 with a retardation film.
[0232] [Example 2]
[0233] After filtering the polymer solution Q1 with a filter having an aperture of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with full-light ultraviolet light at 100 mJ / cm2 through an exposure mask having L / S=30 μm. 2 After that, remove the exposure mask and irradiate with polarized ultraviolet light at 20mJ / cm 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated for 20 minutes using a hot plate at 140° C. to obtain a substrate R2 with a retardation film.
[0234] [Example 3]
[0235] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with full-light ultraviolet light at 10 mJ / cm 2 After that, the film was irradiated with polarized ultraviolet light at 20 mJ / cm through an exposure mask with L / S = 30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated for 20 minutes using a hot plate at 140° C. to obtain a substrate R3 with a retardation film.
[0236] [Example 4]
[0237] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Next, the film was irradiated with polarized ultraviolet light at 20 mJ / cm2 in a manner perpendicular to the polarization axis of the first polarized ultraviolet light through an exposure mask having L / S=30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated for 20 minutes using a hot plate at 140° C. to obtain a substrate R4 with a retardation film.
[0238] [Example 5]
[0239] After filtering the polymer solution Q1 with a filter having an aperture of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm2 through an exposure mask having L / S=30 μm. 2 Next, the exposure mask was removed and polarized ultraviolet light was irradiated at 20 mJ / cm2 perpendicular to the polarization axis of the first polarized ultraviolet light. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate R5 with a retardation film.
[0240] [Example 6]
[0241] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2Next, the film was irradiated with polarized ultraviolet light at a speed of 100 mJ / cm2 in parallel with the polarization axis of the first polarized ultraviolet light through an exposure mask having L / S=30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate R6 with a retardation film.
[0242] [Example 7]
[0243] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Next, the film was irradiated with polarized ultraviolet light at a speed of 200 mJ / cm2 in parallel with the polarization axis of the first polarized ultraviolet light through an exposure mask having L / S=30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate R7 with a retardation film.
[0244] [Example 8]
[0245] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Next, the film was irradiated with polarized ultraviolet light at a speed of 400 mJ / cm2 in parallel with the polarization axis of the first polarized ultraviolet light through an exposure mask having L / S=30 μm. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate R8 with a retardation film.
[0246] [Comparative Example 1]
[0247] After filtering the polymer solution Q1 through a filter with an aperture of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm2 through an exposure mask with L / S=20 μm. 2 (313 nm conversion) After the polarized ultraviolet exposure, the substrate was heated for 20 minutes using a hot plate at 140° C., thereby obtaining a substrate S1 with a retardation film.
[0248] The exposure steps of Examples 1 to 8 and Comparative Example 1 are summarized as shown in Table 1. It should be noted that in Examples 1, 2, 4 to 8, the portion covered by the exposure mask forms a high anisotropic region (hereinafter, also referred to as anisotropic phase region), and the portion not covered by the exposure mask forms a low anisotropic region (hereinafter, also referred to as isotropic phase region). In Example 3, the region covered by the exposure mask forms an isotropic phase.
[0249] [Table 1]
[0250]
[0251] [Fabrication of HAZE evaluation substrate]
[0252] [Preparation of substrate T1]
[0253] The polymer solution Q1 was filtered through a filter with a pore size of 5.0 μm, and then spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Then, the coating surface was irradiated with polarized ultraviolet rays at 20 mJ / cm 2 (313 nm conversion) After ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T1 with a retardation film. The substrate T1 is a substrate simulating the HAZE of the anisotropic region of Examples 1 and 2, Examples 4 to 8, and Comparative Example 1.
[0254] [Preparation of substrate T2]
[0255] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with full-light ultraviolet light at 10 mJ / cm 2 (313nm conversion), then irradiated with polarized ultraviolet light 20mJ / cm 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T2 with a retardation film. The substrate T2 was a substrate simulating the HAZE of the anisotropic region of Example 3.
[0256] [Preparation of substrate T3]
[0257] The polymer solution Q1 was filtered through a filter with a pore size of 5.0 μm, and then spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Then, the coating surface was irradiated with polarized ultraviolet rays at 20 mJ / cm 2 (313nm conversion) and then irradiated with full-light ultraviolet light 100mJ / cm 2(313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate S3 with a retardation film. The substrate T3 is a substrate simulating the HAZE of the isotropic phase region of Example 1.
[0258] [Preparation of substrate T4]
[0259] The polymer solution Q1 was filtered through a filter with an aperture of 5.0 μm, and then spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with full-light ultraviolet light at 100 mJ / cm 2 (313nm conversion), then irradiated with polarized ultraviolet light 20mJ / cm 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T4 with a retardation film. The substrate T4 was a substrate simulating the HAZE of the isotropic phase region of Example 2.
[0260] [Production of substrate T5]
[0261] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Next, the coating surface was irradiated with full-light ultraviolet light at 10 mJ / cm 2 (313 nm conversion) After ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T5 with a retardation film. The substrate T5 is a substrate simulating the HAZE of the isotropic phase region of Example 3.
[0262] [Production of substrate T6]
[0263] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Then, the polarized ultraviolet light was irradiated at 20 mJ / cm2 in a manner perpendicular to the polarization axis of the first polarized ultraviolet light. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T6 with a retardation film. The substrate T6 was a substrate simulating the HAZE of the isotropic phase region of Examples 4 and 5.
[0264] [Production of substrate T7]
[0265] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Then, the polarized ultraviolet light was irradiated in parallel with the polarization axis of the first polarized ultraviolet light at 100 mJ / cm 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T7 with a retardation film. The substrate T7 is a substrate simulating the HAZE of the isotropic phase region of Example 6.
[0266] [Production of substrate T8]
[0267] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Then, the polarized ultraviolet light was irradiated at 200 mJ / cm2 in a manner parallel to the polarization axis of the first polarized ultraviolet light. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T8 with a retardation film. The substrate T8 is a substrate simulating the HAZE of the isotropic phase region of Example 7.
[0268] [Production of substrate T9]
[0269] After filtering the polymer solution Q1 through a filter with a pore size of 5.0 μm, spin coating was applied to a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. The coating surface was irradiated with polarized ultraviolet light at 20 mJ / cm 2 Then, the polarized ultraviolet light was irradiated at 400 mJ / cm2 in a manner parallel to the polarization axis of the first polarized ultraviolet light. 2 (313 nm conversion) After the second ultraviolet exposure, the substrate was heated on a hot plate at 140° C. for 20 minutes to obtain a substrate T9 with a retardation film. The substrate T9 is a substrate simulating the HAZE of the isotropic phase region of Example 8.
[0270] [Manufacturing of substrate T10]
[0271] After filtering the polymer solution Q1 with a filter having an aperture of 5.0 μm, the solution was spin-coated on a glass substrate with a transparent electrode and dried on a hot plate at 70°C for 240 seconds to form a retardation film with a film thickness of 3.0 μm. Subsequently, the solution was heated on a hot plate at 140°C for 20 minutes to obtain a substrate T10 with a retardation film. The substrate T10 simulates the HAZE substrate in the isotropic phase region of Comparative Example 1.
[0272] [Phase difference evaluation]
[0273] The retardation values at 550 nm of the retardation film-bearing substrates R1 to R8 and the retardation film-bearing substrate S1 were evaluated using Axo Step manufactured by Axo Metrix.
[0274] [HAZE review]
[0275] The HAZE of the retardation film-attached substrates T1 to T10 was evaluated using HAZE Meter HZ-V3 manufactured by Suga Test Instruments Co., Ltd. Table 2 shows the results.
[0276] [Table 2]
[0277]
[0278] According to the results in Table 2, the comparison between Examples 1 to 8 and Comparative Example 1 shows that the HAZE value of the isotropic phase region is suppressed by irradiating the isotropic phase region with ultraviolet rays. However, due to the difference in irradiation process, the phase difference values of the anisotropic phase and the isotropic phase of Examples 1 to 8 are different. Among them, in Examples 4 and 5, in addition to the suppressed HAZE value, the difference between the phase difference values of the anisotropic phase and the isotropic phase is large, and the anisotropic phase exhibits a high phase difference value, resulting in a very good result that the phase difference value of the isotropic phase is suppressed. In addition, according to Examples 6 to 8, it can be seen that as the second polarized exposure amount increases, the phase difference value of the isotropic phase is suppressed. The reason is that the methacrylate polymer powder P1 has the property of reduced orientation at an exposure amount higher than the optimal exposure amount.
[0279] Industrial Applicability
[0280] The method of the present invention is useful as a method for producing a patterned single-layer phase difference material in which the HAZE value of the isotropic phase region is suppressed.
Claims
1. A method for manufacturing a patterned single-layer phase difference material, wherein include: (I) a step of coating a polymer composition containing a liquid crystal polymer on a substrate to form a coating film, wherein the liquid crystal polymer has a property that the orientation property increases with the exposure amount at an exposure amount lower than an optimal exposure amount, and the orientation property decreases with the exposure amount at an exposure amount higher than the optimal exposure amount; (II) a step of irradiating the coating film obtained in step (I) with ultraviolet rays twice to generate a high anisotropy region and a low anisotropy region, wherein at least one of the irradiations is performed through a mask and at least one of the irradiations is performed using polarized ultraviolet rays, wherein the high anisotropy region has high optical anisotropy due to the irradiation with polarized ultraviolet rays, and the low anisotropy region has relatively low optical anisotropy due to the amount of ultraviolet rays being insufficient in a region below an optimum exposure amount and being excessive in a region above an optimum exposure amount; and (III) A step of heating the coating film obtained in the step (II) to obtain a phase difference material.
2. The method for manufacturing a patterned single-layer phase difference material according to claim 1, in, The polymer composition comprises: (A) a side chain polymer having a side chain having a photoreactive site represented by the following formula (a); (B) a silane coupling agent; and (C) an organic solvent; In formula (a), R 1 is an alkylene group having 1 to 30 carbon atoms, wherein one or more hydrogen atoms in the alkylene group may be substituted by a fluorine atom or an organic group; in addition, R 1 -CH 2 CH 2 - may or may not be substituted by -CH=CH-, R 1 -CH 2 - is or is not substituted by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-; wherein the adjacent -CH 2 - will not be substituted by these groups at the same time; in addition, -CH 2 -For or not for R 1 The terminal -CH 2 -; R 2 is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed cyclic group; R 3 is a single bond, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)-O-; R is an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group or a nitro group, and when c ≥ 2, each R is the same or different; a is 0, 1, or 2; b is 0 or 1; c is an integer satisfying 0≤c≤2b+4; The dotted lines are the bonding sites.
3. The method for manufacturing a patterned single-layer phase difference material according to claim 2, in, The side chain having a photoreactive site is represented by the following formula (a1), In formula (a1), R 1 , R 2 and a are the same as above; R 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-; The benzene ring in formula (a1) may be substituted with a substituent selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group, and a nitro group; The dotted lines are the bonding sites.
4. The method for manufacturing a patterned single-layer phase difference material according to claim 2 or 3, in, (A) The side chain type polymer also has a side chain that exhibits only liquid crystallinity.
5. The method for manufacturing a patterned single-layer phase difference material according to claim 4, in, The side chain that only exhibits liquid crystallinity is a liquid crystal side chain represented by any one of the following formulae (1) to (13); In formula (1) to formula (13), A 1 , A 2 are each independently a single bond, -O-, -CH 2 -, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-C(=O)-, -CH=CH-C(=O)-O- or -OC(=O)-CH=CH-; R 11 For-No 2 , -CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms; R 12 is a group selected from the group consisting of phenyl, naphthyl, biphenyl, furyl, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, and a group obtained by combining them, and the hydrogen atom bonded to them is or is not replaced by -NO 2 , -CN, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms; R 13 For hydrogen atoms, -NO 2 、-CN、-CH=C(CN) 2 , -CH=CH-CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms; E is -C(=O)-O- or -OC(=O)-; d is an integer from 1 to 12; k1 to k5 are each independently an integer of 0 to 2, wherein the total of k1 to k5 is 2 or more; k6 and k7 are each independently an integer of 0 to 2, wherein the sum of k6 and k7 is 1 or more; m1, m2 and m3 are each independently an integer from 1 to 3; n is 0 or 1; Z 1 and Z 2 are each independently a single bond, -C(=O)-, -CH 2 O-, -CH=N- or -CF 2 -; The dotted lines are the bonding sites.
6. The method for manufacturing a patterned single-layer phase difference material according to claim 5, in, The side chain that only exhibits liquid crystallinity is a liquid crystal side chain represented by any one of formulae (1) to (11). 7 . A single-layer phase difference material, which is produced by the method according to claim 1 .