A low melting point chloride composite electrolyte, preparation method and application thereof

A low-melting-point chloride composite electrolyte addresses the volatilization and blockage issues in the NaCl-KCl system by using a mixed molten salt electrolyte with refractory metal chlorides, enabling efficient electrolysis and refining of zirconium and hafnium.

CN114703511BActive Publication Date: 2024-12-06GRINM RESOURCES & ENVIRONMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210504213.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-10
Publication Date
2024-12-06
Estimated Expiration
2042-05-10

AI Technical Summary

Technical Problem

The high sublimation points of zirconium and hafnium chlorides in the NaCl-KCl system cause volatilization and difficulty in continuous electrolysis, leading to equipment blockages and low reaction rates in the preparation of high-purity metal zirconium and hafnium.

Method used

A low-melting-point chloride composite electrolyte is prepared by mixing a low-melting-point molten salt electrolyte with refractory metal chlorides, such as zirconium tetrachloride, hafnium tetrachloride, or tungsten hexachloride, ensuring the molten salt electrolyte's melting point is below the sublimation point of these chlorides, facilitating a solid-phase reaction.

Benefits of technology

The solution prevents volatilization of refractory metal chlorides, allowing continuous electrolysis and refining, thereby improving reaction efficiency and preventing equipment blockages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114703511B_ABST
    Figure CN114703511B_ABST
Patent Text Reader

Abstract

The present application provides a low-melting-point chloride composite electrolyte, a preparation method and its application, wherein the low-melting-point chloride composite electrolyte is obtained by melting and mixing a low-melting-point molten salt electrolyte and a refractory metal chloride according to a preset mass ratio; in the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride or tungsten hexachloride. The present application changes the melting point of the molten salt electrolyte to be lower than the sublimation point of the refractory metal chloride, thereby avoiding the sublimation of the refractory metal chloride into a gaseous state and reducing the reaction rate during preparation; and solves the volatilization and continuous addition problems of refractory metal chlorides when electrolyzing, refining or electroplating refractory metals (zirconium, hafnium, tungsten) using a chloride composite electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrochemical metallurgy, and in particular to a low melting point chloride composite electrolyte, a preparation method and an application thereof. Background Art

[0002] The demand for nuclear power in clean substitution and electric energy substitution is increasing. Among them, metal zirconium and hafnium have excellent nuclear properties and can be used in nuclear reactor structural materials and control materials to meet the demand for nuclear power in clean substitution and electric energy substitution. Therefore, how to prepare and purify metal zirconium and hafnium is particularly important.

[0003] At present, the main methods for preparing and purifying metal zirconium and hafnium include magnesium thermal reduction, iodination and molten salt electrolysis. Among them, magnesium thermal reduction is the main method for producing metal zirconium and hafnium, but the purity of the obtained metal zirconium and hafnium is low. The iodination method can effectively remove most impurities and purify and refine metal zirconium and hafnium, but the cost of this method is slightly high. Compared with magnesium thermal reduction and iodination, molten salt electrolysis is not only low-cost but also can obtain high-purity metal zirconium and hafnium.

[0004] The molten salt electrolyte systems for preparing metal zirconium and hafnium by molten salt electrolysis mainly include fluoride system, fluoride-chloride system and chloride system. The use of fluoride and fluoride-chloride systems is easy to obtain powdered zirconium and hafnium products, and the cathode product has a high salt inclusion rate, resulting in a high oxygen content after subsequent water washing treatment; while the use of the chloride system is easy to obtain dendritic metal deposition, and the cathode product has a low salt inclusion rate. Therefore, the chloride system has certain advantages.

[0005] In the chloride system, a NaCl-KCl system is usually used with zirconium or hafnium chloride to prepare a chloride composite electrolyte, and then metal zirconium and hafnium are prepared by electrolysis or refining. However, the sublimation points of zirconium and hafnium chlorides are approximately 331°C and 317°C, respectively, and the NaCl-KCl eutectic melting point is approximately 675°C, which is higher than the sublimation point of zirconium and hafnium chlorides. Therefore, during the preparation process, zirconium and hafnium chlorides will sublimate into a gaseous state. Since it is a gas-solid phase reaction, the reaction rate is reduced, resulting in a too low concentration of valuable metal ions in the electrolyte, making it difficult to obtain a chloride composite electrolyte that meets the requirements of electrolysis. In addition, during the subsequent electrolysis, since zirconium and hafnium chlorides are sublimated into a gaseous state, it is difficult to add zirconium and hafnium chlorides to the electrolytic cell, and they are easy to volatilize, causing the equipment evacuation tube and argon inlet to be blocked, resulting in the inability to carry out electrolysis continuously.

[0006] Therefore, the research and development of a low-melting-point chloride composite electrolyte is of great practical significance for molten salt electrolysis, electrolytic refining or electroplating of metal zirconium and hafnium. Summary of the invention

[0007] The present application provides a low-melting-point chloride composite electrolyte and a preparation method thereof, aiming to improve the preparation efficiency of the chloride composite electrolyte and solve the problem of volatilization and continuous addition of refractory metal chloride when using the chloride composite electrolyte to electrolyze or refine refractory metals (especially refractory metals such as zirconium and hafnium).

[0008] To achieve the above purpose, the technical solution of this application is implemented as follows:

[0009] In a first aspect, the present application provides a low-melting-point chloride composite electrolyte, wherein the low-melting-point chloride composite electrolyte is obtained by melting and mixing a low-melting-point molten salt electrolyte and a refractory metal chloride according to a preset mass ratio;

[0010] In the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride or tungsten hexachloride.

[0011] Preferably, the low melting point molten salt electrolyte is a binary molten salt electrolyte or a ternary molten salt electrolyte, and the binary molten salt electrolyte comprises: LiCl 45-55 -RbCl 45-55 or LiCl 45-55 -CsCl 45-55 , the ternary molten salt electrolyte is LiCl 40-70 -KCl l0-30 -CsCl 20-30 , where the subscript in the lower right corner of the chemical formula represents the mole percentage of each component.

[0012] Preferably, the preset mass ratio is 100:0~50.

[0013] In a second aspect, the present application provides a method for preparing a low-melting-point chloride composite electrolyte, which is used to prepare the low-melting-point chloride composite electrolyte of the first aspect, and the preparation method comprises:

[0014] Step 1: Weigh an alkali metal chloride salt, grind it for 10-60 min, add it into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with inert gas. Heat it to 600-900°C under a positive pressure of 1500-2000 Pa, keep it warm for 1-3 h, and cool it to room temperature to obtain a low-melting-point molten salt electrolyte.

[0015] Step 2: After crushing the low-melting-point molten salt electrolyte into a particle size less than 100 mesh, mix it with the refractory metal chloride according to a preset mass ratio, mix it evenly and place it in a closed reactor, fill it with argon gas to maintain a slight positive pressure, heat it to 280-330° C., keep it warm for 2-6 hours, and cool it to room temperature to obtain the low-melting-point chloride composite electrolyte;

[0016] Among them, in the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride, and tungsten hexachloride.

[0017] Preferably, the alkali metal chloride salt comprises: two or three of LiCl, KCl, CsCl and RbCl; and the low melting point molten salt electrolyte is prepared from the alkali metal chloride salt.

[0018] Preferably, the alkali metal chloride salt is one of LiCl-RbCl, LiCl-CsCl and LiCl-KCl-CsCl; and the low melting point electrolyte is prepared from the alkali metal chloride salt.

[0019] Preferably, the low melting point molten salt electrolyte is a binary molten salt electrolyte or a ternary molten salt electrolyte, and the binary molten salt electrolyte comprises: LiCl 45-55 -RbCl 45-55 or LiCl 45-55 -CsCl 45-55 , the ternary molten salt electrolyte is LiCl 40-70 -KCl l0-30 -CsCl 20-30 , where the subscript in the lower right corner of the chemical formula represents the mole percentage of each component.

[0020] Preferably, in step 2, the preset mass ratio is 100:0-50.

[0021] Preferably, before step 1, the method further includes:

[0022] Under a vacuum state with an absolute pressure of ≤100 Pa, the alkali metal chloride salt and the refractory metal chloride are heated to 200-250° C. at a heating rate of 3-5° C. / min, and then vacuumized and kept warm for 6-24 h to obtain the alkali metal chloride salt and refractory metal chloride after vacuum dehydration.

[0023] In a third aspect, the present application provides an application of the low melting point chloride composite electrolyte of the first aspect, the application comprising:

[0024] The low melting point chloride composite electrolyte is used for electrolysis, refining or electroplating of any metal among zirconium, hafnium and tungsten.

[0025] Compared with the prior art, this application has the following advantages:

[0026] The present application provides a low-melting-point chloride composite electrolyte, a preparation method and an application thereof, wherein the low-melting-point chloride composite electrolyte is obtained by melting and mixing a low-melting-point molten salt electrolyte and a refractory metal chloride according to a preset mass ratio; in the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride, and tungsten hexachloride. The present application obtains an electrolyte having a melting point lower than the sublimation point of the refractory metal chloride by preparing molten salt electrolytes in different proportions, that is, by reducing the temperature when the molten salt electrolyte reacts with the refractory metal chloride, so as to avoid the problem of the refractory metal chloride sublimating into a gaseous state before the molten salt electrolyte during preparation, thereby reducing the reaction rate; the problem of the volatilization of refractory metal chloride causing the blockage of the equipment evacuation pipe and the argon inlet when the chloride composite electrolyte is used for electrolysis, refining or electroplating of refractory metals (zirconium, hafnium, tungsten) is solved; in addition, the problem of the difficulty of adding refractory metal chloride to the electrolytic cell during continuous electrolysis, refining or electroplating is solved at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A flow chart of the steps of a low melting point chloride composite electrolyte provided in an embodiment of the present application;

[0028] Figure 2 This is a diagram of an electrolytically refined zirconium product according to an embodiment of the present application. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, the above-mentioned objects, features and advantages of the present application are made more obvious and easy to understand by those of ordinary skill in the art without making creative work. The preferred implementation modes of the present application will be described in detail in conjunction with the embodiments below. It should be understood that the following embodiments are given only for the purpose of illustration and are not intended to limit the scope of the present application. Those skilled in the art may make various modifications and replacements to the present application without departing from the purpose and spirit of the present invention. The materials, reagents, etc. used in the following embodiments, if not otherwise specified, can all be obtained from commercial sources.

[0030] In a first aspect, the present application provides a low-melting-point chloride composite electrolyte, wherein the low-melting-point chloride composite electrolyte is obtained by melting and mixing a low-melting-point molten salt electrolyte and a refractory metal chloride according to a preset mass ratio;

[0031] In the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride, and tungsten hexachloride.

[0032] In this embodiment, in the low melting point chloride composite electrolyte, the melting point of the low melting point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride. Therefore, when preparing the chloride composite electrolyte, the refractory metal chloride will not sublimate into a gaseous state. Compared with the gas phase-solid phase reaction, the solid phase-solid phase reaction rate is faster.

[0033] Preferably, the low melting point molten salt electrolyte is a binary molten salt electrolyte or a ternary molten salt electrolyte, and the binary molten salt electrolyte comprises: LiCl 45-55 -RbCl 45-55 or LiCl 45-55 -CsCl 45-55 , the ternary molten salt electrolyte is LiCl 40-70 -KCl l0-30 -CsCl 20-30 , where the lower right subscript of the chemical formula represents the molar percentage of each component. The melting point of the low melting point molten salt electrolyte under this composition is lower than the sublimation point of zirconium tetrachloride, hafnium tetrachloride and tungsten hexachloride.

[0034] In a specific implementation, the low-melting-point molten salt electrolyte can also be prepared from two or three of LiCl, KCl, CsCl and RbCl. The melting point of the prepared low-melting-point molten salt electrolyte can be controlled within the range of 263-675°C. Further, the melting point of the low-melting-point molten salt electrolyte can be controlled within the range of 263-330°C, so that the melting point temperature is lower than the sublimation temperature of the metal chloride of zirconium (331°C), the metal chloride of hafnium (317°C) and the metal chloride of tungsten (347°C).

[0035] Preferably, the preset mass ratio is 100:0~50.

[0036] In this embodiment, the low melting point molten salt electrolyte and the refractory metal chloride are melted and mixed in a mass ratio of 100:0 to 50. The preset mass ratio is a minimum range, and when the preset mass ratio is greater than this range, the refractory metal chloride may not react completely.

[0037] In a second aspect, the present application provides a method for preparing a low melting point chloride composite electrolyte, which is used to prepare the low melting point chloride composite electrolyte of the first aspect, referring to Figure 1 , shows a step flow chart of a low melting point chloride composite electrolyte provided in an embodiment of the present application, such as Figure 1 As shown, the preparation method comprises the following steps:

[0038] Step 1: Weigh the alkali metal chloride salt, grind it for 10 to 60 minutes, add it into the crucible and place it in a heating furnace. After evacuating the furnace, fill it with inert gas. Under a positive pressure of 1500 to 2000 Pa, heat it to 600 to 900 ° C, keep it warm for 1 to 3 hours, and cool it to room temperature to obtain a low melting point molten salt electrolyte.

[0039] In specific implementation, the inert gas may be argon, nitrogen or other inert gases.

[0040] Step 2: After the low-melting-point molten salt electrolyte is crushed into a particle size less than 100 mesh, it is mixed with a refractory metal chloride according to a preset mass ratio. After mixing evenly, it is placed in a closed reactor, and under the condition of filling with argon to maintain a slight positive pressure, the temperature is raised to 280-330°C, kept warm for 2-6 hours, and cooled to room temperature to obtain the low-melting-point chloride composite electrolyte.

[0041] In the specific implementation, the selected alkali metal chloride salt can be two or three of LiCl, KCl, CsCl and RbCl, and the refractory metal chloride is any one of zirconium tetrachloride, hafnium tetrachloride and tungsten hexachloride. The melting point of the low-melting-point molten salt electrolyte prepared by using the above-mentioned alkali metal chloride salt can be controlled within the range of 263-675°C. Further, the melting point of the low-melting-point molten salt electrolyte can be controlled within the range of 263-330°C, so that the melting point temperature is lower than the sublimation temperature of zirconium tetrachloride (331°C), hafnium tetrachloride (317°C) and tungsten hexachloride (347°C). In this case, in step 2, setting the reaction temperature to 280-330°C can ensure that zirconium tetrachloride, hafnium tetrachloride and tungsten hexachloride will not sublimate into a gaseous state, while ensuring that the prepared low-melting-point molten salt electrolyte has melted.

[0042] In this embodiment, the slight positive pressure is characterized by the situation that the pressure of the environment is 200-400 Pa higher than the atmospheric pressure; the argon gas filled is high-purity argon gas with a purity of ≥99.999%.

[0043] Preferably, the alkali metal chloride salt is one of LiCl-RbCl, LiCl-CsCl and LiCl-KCl-CsCl; and the low melting point electrolyte is prepared from the alkali metal chloride salt.

[0044] Preferably, the low melting point molten salt electrolyte is a binary molten salt electrolyte and a ternary molten salt electrolyte, and the binary molten salt electrolyte includes: LiCl 45-55 -RbCl 45-55 or LiCl 45-55 -CsCl 45-55 ; The ternary molten salt electrolyte is: LiCl 40-70 -KCl l0-30 -CsCl20-30 , where the lower right subscript of the chemical formula represents the molar percentage of each component. The melting point of the low melting point molten salt electrolyte under this composition is lower than the sublimation point of zirconium tetrachloride, hafnium tetrachloride and tungsten hexachloride.

[0045] Preferably, in step 2, the preset mass ratio is 100:0-50.

[0046] In this embodiment, the low melting point molten salt electrolyte and the refractory metal chloride are melted and mixed in a mass ratio of 100:0 to 50. The preset mass ratio is a minimum range, and when the preset mass ratio is greater than this range, the refractory metal chloride may not react completely.

[0047] Preferably, before step 1, the method further includes:

[0048] Under a vacuum state with an absolute pressure of ≤100 Pa, the alkali metal chloride salt and the refractory metal chloride are heated to 200-250° C. at a heating rate of 3-5° C. / min, and then vacuumized and kept warm for 6-24 h to obtain the alkali metal chloride salt and refractory metal chloride after vacuum dehydration.

[0049] In this embodiment, in order to effectively remove the adsorbed water in the alkali metal chloride salt and the refractory metal chloride and reduce the water and oxygen content in the electrolyte, before step 1, the alkali metal chloride salt and the refractory metal chloride need to be vacuum dehydrated.

[0050] In a third aspect, the present application provides an application of the low melting point chloride composite electrolyte of the first aspect, the application comprising:

[0051] The low melting point chloride composite electrolyte is used for electrolysis, refining or electroplating of any metal among zirconium, hafnium and tungsten.

[0052] In a specific implementation, the low-melting-point chloride composite electrolyte is used for electrolysis, refining or electroplating of any one of zirconium, hafnium and tungsten, including: placing the metal to be refined (zirconium, hafnium, tungsten) as an anode raw material in an electrolytic cell as an anode, then adding a corresponding appropriate amount of low-melting-point chloride composite electrolyte, heating the electrolyte under argon protection according to a set program until the electrolyte melts, and after the chloride composite electrolyte in the electrolytic cell is completely melted, inserting a cathode at 0.1-2A / cm 2 Electrolytic refining is carried out at a current density of . After 2 to 4 hours of electrolytic refining, the cathode is slowly lifted out of the molten salt liquid surface and raised to the cooling chamber for cooling. After it is completely cooled, the cathode product is taken out. After cooling, the cathode product is washed with deionized water to remove the mixed electrolyte to obtain a refined metal product. When electrolyzing or electroplating refractory metals alone, the graphite electrode is used as an inert anode, and there is no need to add the corresponding metal as the anode raw material. The specific process is consistent with refining.

[0053] Reference Figure 2 , shows an electrolytically refined zirconium product diagram of an embodiment of the present application, such as Figure 2 As shown, the zirconium obtained by electrolytic refining is in a dendritic shape.

[0054] Based on the common knowledge in this field, the above-mentioned preferred conditions can be combined with each other to obtain a specific implementation method.

[0055] Example 1

[0056] This embodiment takes LiCl and RbCl raw materials to prepare a low melting point molten salt electrolyte, and then adds ZrCl4 to react to generate a (Li, Rb)2ZrCl6 low melting point chloride composite electrolyte as an example.

[0057] Before the preparation, LiCl, RbCl and ZrCl4 were heated to 200°C at a heating rate of 3°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then vacuumed and kept warm for 6 h to obtain LiCl, RbCl and ZrCl4 after vacuum dehydration.

[0058] Next, we will start preparing the (Li, Rb)2ZrCl6 low melting point chloride composite electrolyte.

[0059] Step 1: Weigh LiCl and RbCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 600 °C under a positive pressure of 1500 Pa, keep it warm for 1 h, and cool it to room temperature to obtain LiCl 45 -RbCl 55 ;

[0060] Step 2: LiCl 45 -RbCl 55 After being crushed into a particle size less than 100 mesh, it is mixed with refractory metal chloride in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and heated to 280°C while maintaining a slightly positive pressure with argon gas with a purity of ≥99.999%. It is kept warm for 2 hours and cooled to room temperature to obtain (Li, Rb)2ZrCl6.

[0061] Example 2

[0062] This embodiment takes LiCl and RbCl raw materials to prepare a low melting point molten salt electrolyte, and then adds HfCl4 to react to generate (Li, Rb)2HfCl6 low melting point chloride composite electrolyte as an example.

[0063] Before the preparation, LiCl, RbCl and HfCl4 were heated to 250°C at a heating rate of 5°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then vacuumed and kept warm for 12 h to obtain LiCl, RbCl and HfCl4 after vacuum dehydration.

[0064] Next, we will start preparing the (Li, Rb)2HfCl6 low melting point chloride composite electrolyte.

[0065] Step 1: Weigh LiCl and RbCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating, fill it with argon. Heat to 900 °C under a positive pressure of 2000 Pa, keep it warm for 3 h, and cool it to room temperature to obtain LiCl 55 -RbCl 45 ;

[0066] Step 2: LiCl 55 -RbCl 45 After being crushed into a particle size less than 100 mesh, it is mixed with refractory metal chloride in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and heated to 330°C while maintaining a slightly positive pressure with argon gas with a purity of ≥99.999%. It is kept warm for 6 hours and cooled to room temperature to obtain (Li, Rb)2HfCl6.

[0067] Example 3

[0068] This embodiment takes LiCl and CsCl raw materials to prepare a low melting point molten salt electrolyte, and then adds ZrCl4 to react to generate a (Li, Cs)2ZrCl6 low melting point chloride composite electrolyte as an example.

[0069] Before the preparation, LiCl, CsCl and ZrCl4 were heated to 230°C at a heating rate of 4°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then vacuumed and kept warm for 24 h to obtain LiCl, CsCl and ZrCl4 after vacuum dehydration.

[0070] Next, we will start preparing the (Li, Cs)2ZrCl6 low melting point chloride composite electrolyte.

[0071] Step 1: Weigh LiCl and CsCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 800 °C under a positive pressure of 1700 Pa, keep it warm for 2 h, and cool it to room temperature to obtain LiCl. 45 -CsCl 55 ;

[0072] Step 2: LiCl 45 -CsCl 55After being crushed into a particle size less than 100 mesh, it is mixed with refractory metal chloride in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and heated to 300°C while maintaining a slightly positive pressure with argon gas with a purity of ≥99.999%. It is kept warm for 4 hours and cooled to room temperature to obtain (Li, Cs)2ZrCl6.

[0073] Example 4

[0074] This embodiment takes LiCl and CsCl raw materials to prepare a low melting point molten salt electrolyte, and then adds HfCl4 to react to generate (Li, Cs)2HfCl6 low melting point chloride composite electrolyte as an example.

[0075] Before the preparation, LiCl, CsCl and HfCl4 were heated to 200°C at a heating rate of 5°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then vacuumed and kept warm for 12 h to obtain LiCl, CsCl and HfCl4 after vacuum dehydration.

[0076] Next, we will start preparing the (Li, Cs)2HfCl6 low melting point chloride composite electrolyte.

[0077] Step 1: Weigh LiCl and CsCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 600 °C under a positive pressure of 1500 Pa, keep it warm for 1 h, and cool it to room temperature to obtain LiCl 55 -CsCl 45 ;

[0078] Step 2: LiCl 55 -CsCl 45 After being crushed into a particle size less than 100 mesh, it is mixed with refractory metal chloride in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and heated to 280°C while maintaining a slightly positive pressure with argon gas of purity ≥99.999%. It is kept warm for 2 hours and cooled to room temperature to obtain (Li, Cs)2HfCl6.

[0079] Example 5

[0080] This embodiment takes LiCl, KCl and CsCl raw materials to prepare a low melting point molten salt electrolyte, and then adds ZrCl4 to react to generate a (Li, K, Cs)2ZrCl6 low melting point chloride composite electrolyte as an example.

[0081] Before the preparation, LiCl, KCl, CsCl and ZrCl4 were heated to 200°C at a heating rate of 5°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then evacuated and kept warm for 12 h to obtain LiCl, KCl, CsCl and ZrCl4 after vacuum dehydration.

[0082] Next, we will start preparing the (Li, K, Cs)2ZrCl6 low melting point chloride composite electrolyte.

[0083] Step 1: Weigh LiCl, KCl, and CsCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 600 °C under a positive pressure of 1500 Pa, keep it warm for 1 h, and cool it to room temperature to obtain LiCl 40 -KCl 30 -CsCl 30 ;

[0084] Step 2: LiCl 40 -KCl 30 -CsCl 30 After being crushed into a particle size less than 100 mesh, it is mixed with refractory metal chloride in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and heated to 280°C while maintaining a slightly positive pressure with argon gas with a purity of ≥99.999%. It is kept warm for 2 hours and cooled to room temperature to obtain (Li, K, Cs)2ZrCl6.

[0085] Example 6

[0086] This embodiment takes the preparation of a low melting point molten salt electrolyte using LiCl, KCl and CsCl raw materials, and then adding HfCl4 to react to generate a (Li, K, Cs)2HfCl6 low melting point chloride composite electrolyte as an example.

[0087] Before the preparation, LiCl, KCl, CsCl and HfCl4 were heated to 200°C at a heating rate of 5°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then evacuated and kept warm for 12 h to obtain LiCl, KCl, CsCl and HfCl4 after vacuum dehydration.

[0088] Next, we will start preparing the (Li, K, Cs)2HfCl6 low melting point chloride composite electrolyte.

[0089] Step 1: Weigh LiCl, KCl, and CsCl, grind them for 10 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 900 °C under a positive pressure of 2000 Pa, keep it warm for 3 h, and cool it to room temperature to obtain LiCl 70 -KCl l0-CsCl 20 ;

[0090] Step 2: LiCl 70 -KCl l0 -CsCl 20 After being crushed into a particle size less than 100 mesh, it is mixed with HfCl4 in a mass ratio of 100:30. After being evenly mixed, it is placed in a closed reactor and filled with argon gas with a purity of ≥99.999% to maintain a slightly positive pressure. The temperature is raised to 300°C and kept for 6 hours. After being cooled to room temperature, (Li, K, Cs)2HfCl6 is obtained.

[0091] Example 7

[0092] This embodiment takes LiCl, KCl and CsCl raw materials to prepare a low melting point molten salt electrolyte, and then adds WCl6 to react to generate (Li, K, Cs)2WCl8 low melting point chloride composite electrolyte as an example.

[0093] Before the preparation, LiCl, KCl, CsCl and WCl6 were heated to 200°C at a heating rate of 5°C / min under a vacuum state with an absolute pressure of ≤100 Pa, and then evacuated and kept warm for 12 h to obtain LiCl, KCl, CsCl and WCl6 after vacuum dehydration.

[0094] Next, we will start preparing the (Li, K, Cs)2WCl8 low melting point chloride composite electrolyte.

[0095] Step 1: Weigh LiCl, KCl and CsCl, grind them for 30 min, add them into a crucible and place it in a heating furnace. After evacuating the furnace, fill it with argon gas. Heat it to 600 °C under a positive pressure of 1500 Pa, keep it warm for 1 h, and cool it to room temperature to obtain LiCl 50 -KCl 25 -CsCl 25 ;

[0096] Step 2: LiCl 50 -KCl 25 -CsCl 25 After being crushed into a particle size less than 100 mesh, it is mixed with WCl6 in a mass ratio of 100:20. After being evenly mixed, it is placed in a closed reactor and heated to 330°C while maintaining a slightly positive pressure with argon gas of purity ≥99.999%. It is kept warm for 2 h and cooled to room temperature to obtain (Li, K, Cs)2WCl8.

[0097] The above is a detailed introduction to a low-melting-point chloride composite electrolyte, a preparation method and an application thereof provided by the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for a person skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a low melting point chloride composite electrolyte, characterized in that: The method comprises: In a vacuum state with an absolute pressure of ≤100 Pa, LiCl, KCl, CsCl and a refractory metal chloride are heated to 200°C at a heating rate of 5°C / min, and then vacuumized and kept warm for 12 hours to obtain LiCl, KCl, CsCl and a refractory metal chloride after vacuum dehydration, wherein the refractory metal chloride is ZrCl4 or HfCl4; Weigh low-melting-point molten salt electrolytes LiCl, KCl, and CsCl respectively, grind them for 10 to 30 min, add them into a crucible and place it in a heating furnace. After evacuating, fill it with argon gas. Heat it to 600 to 900 ° C under a positive pressure of 1500 to 2000 Pa, keep it warm for 1 to 3 h, and cool it to room temperature to obtain a low-melting-point molten salt electrolyte. The low-melting-point molten salt electrolyte is LiCl 40 -KCl 30 -CsCl 30 or LiCl 70 -KCl l0 -CsCl 20 , where the lower right subscript of the chemical formula represents the mole percentage of each component; The low-melting-point molten salt electrolyte is crushed into a particle size less than 100 mesh, and then mixed with the refractory metal chloride in a mass ratio of 100:

30. After being evenly mixed, the mixture is placed in a closed reactor, and the mixture is heated to 280-300° C. while being filled with argon gas with a purity of ≥99.999% to maintain a slight positive pressure. The mixture is kept warm for 2-6 hours, and then cooled to room temperature to obtain the low-melting-point chloride composite electrolyte, wherein the low-melting-point chloride composite electrolyte is (Li, K, Cs)2ZrCl6 or (Li, K, Cs)2HfCl6; Among them, in the low-melting-point chloride composite electrolyte, the melting point of the low-melting-point molten salt electrolyte is lower than the sublimation point of the refractory metal chloride.