Electrochemical devices and electronic devices

By using a stacked current collector of a first substrate and a second substrate with moderate differences in tensile strength in an electrochemical device, the problem of dislocation peeling caused by the expansion of the pole piece is solved, and the safety and cycle performance of the device are improved.

CN114784222BActive Publication Date: 2024-10-29NINGDE AMPEREX TECHNOLOGY LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210416933.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-29
Estimated Expiration
2041-03-29

Smart Images

  • Figure CN114784222B_ABST
    Figure CN114784222B_ABST
Patent Text Reader

Abstract

Embodiments of the present application provide an electrochemical device and an electronic device. The electrochemical device includes a first pole piece, and the first pole piece includes a current collector and an active material layer. The current collector includes a first substrate and a second substrate that are stacked. The second substrate is arranged between the first substrate and the active material layer, and the tensile strength Rm1 of the first substrate and the tensile strength Rm2 of the second substrate satisfy: 100MPa≤Rm1‑Rm2≤400MPa. The embodiments of the present application can simultaneously suppress the ductile deformation of the pole piece and improve the demolding problem of the active material layer by adopting a current collector including a first substrate and a second substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent with application number 202110334935.3 filed on March 29, 2021 and invention name “Electrochemical device and electronic device”. Technical Field

[0002] The present application relates to the field of electrochemical energy storage, and in particular to electrochemical devices and electronic devices. Background Art

[0003] Electrochemical devices (such as lithium-ion batteries) expand during the cycle process, especially the active material layer in the pole piece. This causes the current collector in the pole piece to expand and deform in the X and Y directions in its plane coordinate system, and may also cause the active material layer and the current collector to peel off, greatly affecting the safety and cycle performance of the electrochemical device. Summary of the invention

[0004] An embodiment of the present application provides an electrochemical device, the electrochemical device comprising a first pole piece, the first pole piece comprising a current collector and an active material layer. The current collector comprises a first substrate and a second substrate stacked together. The second substrate is disposed between the first substrate and the active material layer, and the tensile strength Rm1 of the first substrate and the tensile strength Rm2 of the second substrate satisfy: 100MPa≤Rm1-Rm2≤400MPa.

[0005] In some embodiments, the thickness d1 of the first substrate and the thickness d2 of the second substrate satisfy: 0.5≤d1 / d2≤2.5. In some embodiments, 400MPa≤Rm1≤1000MPa, 1MPa≤Rm2≤600MPa.

[0006] In some embodiments, the first substrate comprises at least one of an alloy material, an inorganic ceramic material, a rolled copper foil, an electrodeposited nickel foil, or a rolled nickel foil. In some embodiments, the second substrate comprises at least one of a porous copper foil, an electrodeposited copper foil, a foamed copper foil, or a conductive polymer material. In some embodiments, the conductive polymer material comprises a conductive agent and a polymer material. In some embodiments, the conductive agent comprises a carbon material. In some embodiments, the polymer material comprises at least one of polyethylene, polypropylene, polystyrene, epoxy resin, or phenolic resin.

[0007] In some embodiments, the current collector further includes a first bonding layer disposed between the first substrate and the second substrate and bonding the first substrate and the second substrate.

[0008] In some embodiments, the elongation of the first substrate is less than or equal to 25%, and the elongation of the second substrate is less than or equal to 25%. In some embodiments, in the thickness direction of the first pole piece, the projection of the active material layer is located within the projection area of ​​the second substrate. In some embodiments, the total thickness of the first substrate and the second substrate is 4μm to 20μm. In some embodiments, the active material layer is in contact with the second substrate. In some embodiments, the first pole piece also includes a conductive layer disposed between the active material layer and the second substrate, and the conductive layer is in contact with the active material layer and the second substrate, respectively.

[0009] In some embodiments, the active material layer includes a negative electrode active material, the negative electrode active material includes a silicon-based material, and the silicon-based material includes at least one of silicon, a silicon alloy, a silicon oxide, or a silicon-carbon composite.

[0010] In some embodiments, the current collector also includes a third substrate, the third substrate is stacked with the first substrate, the first substrate is arranged between the third substrate and the second substrate, the active material layer is also arranged on the third substrate, and the tensile strength Rm1 of the first substrate and the tensile strength Rm3 of the third substrate satisfy: 100MPa≤Rm1-Rm3≤400MPa.

[0011] In some embodiments, the electrochemical device further includes a tab connected to the first substrate or the second substrate of the first electrode sheet, and a thickness of the first substrate or the second substrate connected to the tab is greater than or equal to 3 μm.

[0012] Another embodiment of the present application provides an electronic device, comprising the above-mentioned electrochemical device.

[0013] In the embodiment of the present application, a current collector including a first substrate and a second substrate is used, and the tensile strength Rm1 of the first substrate and the tensile strength Rm2 of the second substrate satisfy: 100MPa≤Rm1-Rm2≤400MPa. The second substrate with a smaller tensile strength can improve the peeling phenomenon of the active material layer, and the first substrate with a larger tensile strength can improve the ductility and deformation of the first pole piece. Therefore, the current collector of the present application can simultaneously suppress the ductility and deformation of the pole piece and improve the demolding of the active material layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A schematic diagram of a first pole piece in some embodiments of the present application is shown, which is cut along a plane defined by a thickness (Z) direction and a width (Y) direction of a current collector.

[0015] Figure 2 A schematic diagram of a first pole piece in some embodiments of the present application, cut along a plane defined along the thickness direction and the width direction of the current collector, is shown.

[0016] Figure 3A schematic diagram of a first pole piece in some embodiments of the present application, cut along a plane defined along the thickness direction and the width direction of the current collector, is shown.

[0017] Figure 4 A schematic diagram of a first pole piece in some embodiments of the present application, cut along a plane defined along the thickness direction and the width direction of the current collector, is shown.

[0018] Figure 5 A top view of a current collector in some embodiments of the present application is shown. DETAILED DESCRIPTION

[0019] The following embodiments may enable those skilled in the art to more fully understand the present application, but do not limit the present application in any way.

[0020] The active material layer of the electrode of the electrochemical device expands during the cycle process, causing the current collector in the electrode to expand and deform in the X and Y directions in its plane coordinate system. It may also cause the misalignment and peeling (i.e., delamination) between the active material layer and the current collector, greatly affecting the safety and cycle performance of the electrochemical device.

[0021] To this end, an embodiment of the present application provides an electrochemical device, which includes a first electrode. In some embodiments, the first electrode can be a positive electrode or a negative electrode. In some embodiments, Figure 1 As shown, the first electrode sheet 10 includes a current collector 101 and an active material layer 102. In some embodiments, the current collector 101 includes a first substrate 111 and a second substrate 112 that are stacked. In some embodiments, the second substrate 112 is at least partially disposed between the first substrate 111 and the active material layer 102. It should be understood that although Figure 1 In the figure, the active material layer 102 is shown to completely cover the second substrate 112, but this is only exemplary and not intended to be limiting, and the active material layer 102 may only partially cover the second substrate 112. In addition, the second substrate 112 may partially cover the first substrate 111.

[0022] In some embodiments, the tensile strength Rm1 of the first substrate and the tensile strength Rm2 of the second substrate satisfy: 100MPa≤Rm1-Rm2≤400MPa. In some embodiments, during the stretching process of the current collector sample, the material enters the strengthening stage after the yielding stage. As the transverse cross-sectional size is significantly reduced, the maximum force Fb borne when it is broken is divided by the original cross-sectional area So of the sample. The stress is called tensile strength or strength limit Rm, in MPa. Tensile strength represents the maximum ability of a material to resist damage under tension. The calculation formula is:

[0023] Rm=Fb / So

[0024] Where: Fb is the maximum force that the sample bears when it is broken, in N (Newton); So is the original cross-sectional area of ​​the sample, in mm 2 The tensile strength is usually measured using a universal material testing machine.

[0025] In some embodiments, the active material layer 102 expands during the cycle process, thereby generating stress. When the second substrate 112 with a relatively small tensile strength is subjected to the stress, it can move in the mutually perpendicular X and Y directions (such as Figure 5 The second substrate 112 can expand with the active material layer 102, so that the peeling or demolding of the active material layer 102 can be improved. When the first substrate 111 is subjected to the stress generated by the expansion of the active material layer 102, the tensile strength of the first substrate 111 is relatively large, so the elongation and deformation of the first pole piece 10 can be alleviated. Therefore, the current collector 101 of the present application can simultaneously suppress the elongation and deformation of the first pole piece 10 and improve the demolding of the active material layer 102.

[0026] In some embodiments, if the difference between the tensile strength Rm1 of the first substrate 111 and the tensile strength Rm2 of the second substrate 112 is too small, the tensile strength Rm1 of the first substrate 111 is too small or the tensile strength Rm2 of the second substrate 112 is too large. If the tensile strength Rm1 of the first substrate 111 is too small, it will be difficult for the first substrate 111 to suppress the ductile deformation of the first electrode 10, and if the tensile strength Rm2 of the second substrate 112 is too large, the second substrate 112 cannot improve the demolding of the active material layer 102. On the other hand, if the difference between the tensile strength Rm1 of the first substrate 111 and the tensile strength Rm2 of the second substrate 112 is too large, the tensile strength Rm1 of the first substrate 111 is too large or the tensile strength Rm2 of the second substrate 112 is too small. If the tensile strength Rm1 of the first substrate 111 is too large, the effect of the second substrate 112 in improving the demolding of the active material layer 102 will be weakened, and if the tensile strength Rm2 of the second substrate 112 is too small, the second substrate 112 will be demolded from the first substrate 111 together with the active material layer 102.

[0027] In some embodiments, the thickness d1 of the first substrate 111 and the thickness d2 of the second substrate 112 satisfy: 0.5≤d1 / d2≤2.5. In some embodiments, the thickness of a material is more related to the tensile strength of the material. In order to obtain a suitable difference between the tensile strength Rm1 of the first substrate 111 and the tensile strength Rm2 of the second substrate 112, the thickness d1 of the first substrate 111 and the thickness d2 of the second substrate 112 are controlled to satisfy: 0.5≤d1 / d2≤2.5.

[0028] In some embodiments, 400MPa≤Rm1≤1000MPa, 1MPa≤Rm2≤600MPa. In some embodiments, if the tensile strength Rm1 of the first substrate 111 is too small, the effect of the first substrate 111 in suppressing the ductility and deformation of the first pole piece 10 will be relatively limited; if the tensile strength Rm1 of the first substrate 111 is too large, the effect of the second substrate 112 in improving the demolding of the active material layer 102 will be weakened. In some embodiments, if the tensile strength Rm2 of the second substrate 112 is too small, in order to adapt to the first substrate 111, the tensile strength Rm1 of the first substrate 111 is usually required to be small, which will weaken the effect of the first substrate 111 in suppressing the ductility and deformation of the first pole piece 10; if the tensile strength Rm2 of the second substrate 112 is too large, it will be difficult to achieve the effect of the second substrate 112 in improving the demolding of the active material layer 102.

[0029] In some embodiments, the first substrate 111 includes at least one of an alloy material, an inorganic ceramic material, a rolled copper foil, an electrodeposited nickel foil, or a rolled nickel foil. In some embodiments, the alloy material includes stainless steel. These materials can provide the first substrate 111 with a suitable tensile strength Rm1. Rolled copper foil is usually a product (usually with a thickness of 4 to 100 microns and a width of <800 mm) formed by repeated rolling and annealing of a high-precision copper strip (usually less than 150 microns) using the principle of plastic processing. Its ductility, bending resistance, and conductivity are better than those of electrodeposited copper foil, and its copper purity is also higher than that of electrodeposited copper foil.

[0030] In some embodiments, the second substrate 112 includes at least one of a porous copper foil, an electrodeposited copper foil, a foam copper foil, or a conductive polymer material. In some embodiments, the conductive polymer material includes a conductive agent and a polymer material. In some embodiments, the conductive agent includes a carbon material. In some embodiments, the polymer material includes at least one of polyethylene, polypropylene, polystyrene, epoxy resin, or phenolic resin. These materials of the second substrate 112 can provide the second substrate 112 with a suitable tensile strength Rm2. In some embodiments, the electrodeposited copper foil is usually formed by the deposition of copper ions in the electrolyte on a smooth rotating stainless steel plate (or titanium plate) circular cathode roller; the porous copper foil is usually a copper foil material with three-dimensional porous features, which has a huge surface area. On the one hand, it can carry more active materials, thereby increasing the capacity of the electrochemical device, and on the other hand, it can provide a larger reaction interface for the electrode reaction to increase the power of the electrochemical device; the foam copper foil is usually a multifunctional material with a large number of connected or unconnected holes evenly distributed in the copper matrix. The foam copper has good conductivity and ductility, and the preparation cost is lower than that of the foam nickel, and the conductivity is better.

[0031] In some embodiments, the first substrate 111 and the second substrate 112 can be combined together by any suitable method, including but not limited to calendaring, electrodeposition, evaporation, and bonding. Figure 2 As shown, the current collector 101 further includes a first bonding layer 113 , and the first bonding layer 113 bonds the first substrate 111 and the second substrate 112 .

[0032] In some embodiments, the elongation of the first substrate 111 is less than or equal to 25%, and the elongation of the second substrate 112 is less than or equal to 25%. If the elongation of the first substrate 111 or the second substrate 112 is too large, the first pole piece 10 will be easily stretched and deformed.

[0033] In this application, the elongation refers to the percentage of the maximum extension of the length of the substrate sample after the substrate sample is stretched and broken in a tensile test to the original gauge length of the substrate sample. That is, the original gauge length of the substrate sample is L1, the maximum extension of the length of the substrate sample when it is stretched and broken is L2, and the elongation ε = L2 × 100% / L1.

[0034] In some embodiments, in the thickness direction of the first electrode sheet 10 (Z direction, perpendicular to the X direction and Y direction of the first electrode sheet 10 or the current collector 101), the projection of the active material layer 102 is located within the projection area of ​​the second substrate 112. That is, the active material layer 102 is not in direct contact with the first substrate 111. In this way, the second substrate 112 can better alleviate the demolding of the active material layer 102, avoiding the demolding of the active material layer 102 caused when the active material layer 102 is in direct contact with the first substrate 111. This is because the tensile strength of the first substrate 111 is relatively large, and when the active material layer 102 expands during the cycle, it is easy to be dislocated and peeled from the first substrate 111 in direct contact.

[0035] In some embodiments, the total thickness of the first substrate 111 and the second substrate 112 is 4 μm to 20 μm. If the total thickness of the first substrate 111 and the second substrate 112 is too small, it may be difficult to suppress the ductility and deformation of the first electrode 10 and improve the demolding of the active material layer 102. If the total thickness of the first substrate 111 and the second substrate 112 is too large, it is not conducive to improving the energy density of the electrochemical device.

[0036] In some embodiments, the active material layer 102 includes a negative electrode active material, the negative electrode active material includes a silicon-based material, and the silicon-based material includes at least one of silicon, silicon alloy, silicon oxide, or silicon-carbon composite. These silicon-based materials have a large expansion rate (up to 300%) during the cycle process, and the current collector of the present application can improve the expansion problem when the active material layer includes a silicon-based material.

[0037] In some embodiments, Figure 1 As shown, the active material layer 102 is in contact with the second substrate 112. In some embodiments, as Figure 3 As shown, the first pole piece may further include a conductive layer 103 disposed between the active material layer 102 and the second substrate 112, and the conductive layer 103 is connected to the active material layer 102 and the second substrate 112, respectively. In some embodiments, the conductive layer 103 includes a carbon material and a binder, and the binder may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. In some embodiments, the mass ratio of the carbon material and the binder in the conductive layer 103 may be 70 to 90: 10 to 30. In some embodiments, the carbon material may include at least one of carbon fiber, carbon nanotubes, graphene or conductive carbon black. It should be understood that this is only exemplary, and the conductive layer 103 may also include other suitable materials and mass ratios.

[0038] In some embodiments, Figure 4 As shown, the current collector 101 also includes a third substrate 114, the third substrate 114 and the first substrate 111 are stacked, the first substrate 111 is disposed between the third substrate 114 and the second substrate 112, the active material layer 102 is also disposed on the third substrate 114, and the tensile strength Rm1 of the first substrate 111 and the tensile strength Rm3 of the third substrate 114 satisfy: 100MPa≤Rm1-Rm3≤400MPa. In some embodiments, the third substrate 114 may include the same material as the second substrate 112, so that the current collector 101 forms a sandwich structure. Of course, the third substrate 114 may also include a material different from the second substrate 112. By making the tensile strength Rm1 of the first substrate 111 and the tensile strength Rm3 of the third substrate 114 satisfy: 100MPa≤Rm1-Rm3≤400MPa, it is possible to suppress the ductile deformation of the first electrode 10 and improve the demolding problem of the active material layer 102 provided on the third substrate 114. This can be seen in the description of the combination of the first substrate 111 and the second substrate 112, which will not be repeated here.

[0039] In some embodiments, the electrochemical device further comprises a pole ear connected to the first substrate 111 or the second substrate 112 of the first pole piece 10, and the thickness of the first substrate 111 or the second substrate 112 connected to the pole ear is greater than or equal to 3 μm. When the thickness of the first substrate 111 or the second substrate 112 is greater than or equal to 3 μm, it is convenient to weld the pole ear and ensure the stability of the welded structure, thereby ensuring the stability of the performance of the electrochemical device. In some embodiments, the thickness of the first substrate 111 or the second substrate 112 connected to the pole ear is less than or equal to 10 μm. If the thickness is too large, it is not conducive to the improvement of the energy density of the electrochemical device.

[0040] In some embodiments, the first substrate 111 may be conductive or non-conductive. In some embodiments, the first substrate 111 is conductive when the tab is connected to the first substrate 111. In some embodiments, each of the first substrate 111, the second substrate 112, and the third substrate 114 may be independently a single-layer substrate or a multi-layer composite.

[0041] In some embodiments, when the first pole piece 10 is a positive electrode, the current collector 101 is a positive electrode current collector, and the active material layer 102 is a positive electrode active material layer. In some embodiments, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, lithium nickel cobalt manganese oxide, or lithium nickel manganese oxide. In some embodiments, the positive electrode active material layer may further include a conductive agent. In some embodiments, the conductive agent in the positive electrode active material layer may include at least one of conductive carbon black, Ketjen black, lamellar graphite, graphene, carbon nanotubes, or carbon fibers. In some embodiments, the positive electrode active material layer may further include a binder, and the binder in the positive electrode active material layer may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin, or polyfluorene. In some embodiments, the mass ratio of the positive electrode active material, the conductive agent and the binder in the positive electrode active material layer may be (78-99): (0.1-10): (0.1-10). In some embodiments, the thickness of the positive electrode active material layer may be 10 μm to 200 μm. It should be understood that the above description is only an example, and the positive electrode active material layer of the positive electrode may adopt any other suitable material, thickness and mass ratio.

[0042] In some embodiments, the positive electrode current collector of the positive electrode may be Al foil, and of course, other current collectors commonly used in the art may also be used. In some embodiments, the thickness of the positive electrode current collector of the positive electrode may be 1 μm to 200 μm. In some embodiments, the positive electrode active material layer may be coated only on a partial area of ​​the positive electrode current collector of the positive electrode.

[0043] In some embodiments, when the first pole piece 10 is a negative electrode, the current collector 101 is a negative electrode current collector, and the active material layer 102 is a negative electrode active material layer. In some embodiments, the negative electrode active material may include at least one of graphite, hard carbon, silicon, silicon oxide or organosilicon. In some embodiments, the negative electrode active material layer may further include a conductive agent and a binder. In some embodiments, the conductive agent in the negative electrode active material layer may include at least one of conductive carbon black, Ketjen black, flake graphite, graphene, carbon nanotubes or carbon fibers. In some embodiments, the binder in the negative electrode active material layer may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin or polyfluorene. In some embodiments, the mass ratio of the negative electrode active material, the conductive agent and the binder in the negative electrode active material layer may be (78 to 98.5): (0.1 to 10): (0.1 to 10). It should be understood that the above description is only an example, and any other suitable materials and mass ratios may be used. In some embodiments, the negative electrode current collector of the negative electrode may be at least one of copper foil, nickel foil or carbon-based current collector.

[0044] In some embodiments, the electrochemical device may further include a separator disposed between the positive electrode and the negative electrode. In some embodiments, the separator includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. Especially polyethylene and polypropylene, they have a good effect on preventing short circuits and can improve the stability of the battery through the shutdown effect. In some embodiments, the thickness of the separator is in the range of about 5 μm to 500 μm.

[0045] In some embodiments, the surface of the isolation membrane may further include a porous layer, the porous layer being disposed on at least one surface of the substrate of the isolation membrane, the porous layer comprising inorganic particles and a binder, the inorganic particles being selected from at least one of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter in the range of about 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The porous layer on the surface of the separator can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the separator, and enhance the adhesion between the separator and the pole piece.

[0046] In some embodiments of the present application, the electrode assembly of the electrochemical device is a wound electrode assembly, a stacked electrode assembly, or a folded electrode assembly. In some embodiments, the positive electrode and / or the negative electrode of the electrochemical device can be a multi-layer structure formed by winding or stacking, or a single-layer structure in which a single-layer positive electrode, a separator, and a single-layer negative electrode are stacked.

[0047] In some embodiments, the electrochemical device includes a lithium ion battery, but the present application is not limited thereto. In some embodiments, the electrochemical device may further include an electrolyte. The electrolyte may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte, the electrolyte including a lithium salt and a non-aqueous solvent. The lithium salt is selected from one or more of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB or lithium difluoroborate. For example, the lithium salt is selected from LiPF6 because it has high ionic conductivity and can improve cycle characteristics.

[0048] The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents or a combination thereof.

[0049] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.

[0050] Examples of chain carbonate compounds are diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) or combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.

[0051] Examples of the carboxylic acid ester compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.

[0052] Examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0053] Examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphoric acid esters or combinations thereof.

[0054] In some embodiments of the present application, taking a lithium-ion battery as an example, a positive electrode, a separator, and a negative electrode are wound or stacked in sequence to form an electrode component, and then encapsulated in, for example, an aluminum-plastic film, injected with an electrolyte, formed, and encapsulated to form a lithium-ion battery. Then, the prepared lithium-ion battery is subjected to a performance test.

[0055] Those skilled in the art will appreciate that the above-described method for preparing an electrochemical device (eg, a lithium-ion battery) is only an example, and other methods commonly used in the art may be used without departing from the disclosure of the present application.

[0056] Embodiments of the present application also provide electronic devices including the above-mentioned electrochemical devices. The electronic devices of the embodiments of the present application are not particularly limited, and they can be any electronic devices known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0057] Some specific embodiments and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example, and for the sake of simplicity, the negative electrode is used as an example of the first pole piece for illustration, and the positive electrode may also adopt the structure of the first pole piece.

[0058] Comparative Example 1

[0059] Preparation of positive electrode: Aluminum foil is used as the positive electrode current collector of the positive electrode, and the positive electrode active material lithium cobalt oxide, conductive agent conductive carbon black, and polyvinylidene fluoride are dissolved in N-methylpyrrolidone (NMP) solution at a weight ratio of 97.8:1.4:0.8 to form a slurry of the positive electrode active material layer, and the slurry is coated on the positive electrode current collector with a coating thickness of 80μm to obtain a positive electrode active material layer. Then, the positive electrode is obtained after drying, cold pressing, and cutting.

[0060] Preparation of negative electrode: artificial graphite, silicon oxide (SiO), sodium carboxymethyl cellulose (CMC) and binder styrene butadiene rubber are dissolved in deionized water at a weight ratio of 82.7:15:1.3:1 to form a negative electrode slurry. A single layer of 4μm thick electrodeposited copper foil (tensile strength of 380MPa) is used as the negative electrode current collector, and the negative electrode slurry is coated on both sides of the negative electrode current collector to obtain two negative electrode active material layers, and the mass content of silicon in each negative electrode active material layer is dried, and the negative electrode is obtained after cutting.

[0061] Preparation of isolation membrane: The isolation membrane substrate is 8 μm thick polyethylene (PE), and a 2 μm alumina ceramic layer is coated on both sides of the isolation membrane substrate. Finally, 2.5 mg of binder polyvinylidene fluoride (PVDF) is coated on both sides of the ceramic layer and dried.

[0062] Preparation of electrolyte: In an environment with a water content of less than 10 ppm, add LiPF6 to a non-aqueous organic solvent (ethylene carbonate (EC): propylene carbonate (PC) = 50:50, weight ratio), the concentration of LiPF6 is 1.15 mol / L, mix well, and obtain an electrolyte.

[0063] Preparation of lithium-ion battery: stack the positive electrode, separator and negative electrode in order, so that the separator is between the positive electrode and the negative electrode to play a role of isolation, and wind them to obtain the electrode assembly. Place the electrode assembly in the outer packaging aluminum plastic film, remove moisture at 80°C, inject the above electrolyte and package, and obtain the lithium-ion battery through the process of formation, degassing, trimming and other processes.

[0064] In Comparative Example 2, the negative electrode current collector uses a 4 μm thick electrodeposited nickel foil, and other parameters are the same as those of Comparative Example 1.

[0065] In comparative example 3, the second substrate of the negative electrode current collector is 8 μm thick conductive styrene with a tensile strength of 146 MPa, and the first substrate is 8 μm thick rolled copper foil with a tensile strength of 620 MPa. The second substrate is composited on both sides of the first substrate by hot pressing process, the hot pressing temperature is 80°C, and the hot pressing pressure is 1.5 MPa. Then, the negative electrode material with a silicon content of 15% is coated on both sides of the negative electrode current collector.

[0066] In Comparative Examples 4 to 7 and Examples 1 to 7, only the composition of the negative electrode current collector is different from that of Comparative Example 3, and the rest is referred to Comparative Example 3. In Examples 8 to 10, only the composition of the negative electrode current collector and the silicon content of the negative electrode active material layer are different from that of Comparative Example 3, and the rest is referred to Comparative Example 3.

[0067] The test methods for various parameters of this application are described below.

[0068] Elongation test of pole piece:

[0069] When a lithium-ion battery is fully charged, it will expand in the XY and Z directions. The current collector is affected by the expansion force of the pole piece, resulting in extension in the XY direction. In the length direction of the pole piece (X direction), take 2 samples from the head, middle, tail, and empty foil area of ​​the pole piece (the area where the current collector is provided with an active material layer), paste them on a glass plate, isolate the air with transparent tape, and then use a charge coupled device (CCD) to measure the width of the pole piece. In theory, the empty foil area will not expand and can be used as a benchmark. The full charge XY extension = full charge area pole piece width / empty foil area width - 1, and the average value of the six samples is taken to obtain the XY extension rate. The XY extension rate can reflect the deformation of the material to a certain extent.

[0070] Tensile strength and elongation test:

[0071] The most common method for measuring tensile strength in China is to use a universal material testing machine to measure the tensile / compressive strength of materials. The specific test steps are:

[0072] (1) Use a sampler to cut five long current collector samples with a width of 15 mm and a length of 200 mm from the sample in the horizontal and vertical directions.

[0073] (2) Clamp the two ends of the specimen on the upper and lower clamps of the equipment respectively. The long axis direction of the specimen should coincide with the center line of the upper and lower clamps.

[0074] (3) Set test speed, sample width and other parameter information.

[0075] (4) Click the Start Test option to start the test.

[0076] (5) The instrument automatically calculates and displays the final test results.

[0077] Among them, tensile strength (Rm) is the stress obtained by dividing the maximum force Fb that the current collector sample withstands during the stretching process by the original cross-sectional area So of the sample, in MPa.

[0078] Whether to test the film:

[0079] Visual observation is usually used. Obvious stratification can be seen after the electrode is demoulded. The electrode is very easy to fall off after being touched, and the current collector will have some wrinkles.

[0080] Table 1 shows various parameters and evaluation results of Examples 1 to 10 and Comparative Examples 1 to 7.

[0081] Table 1

[0082]

[0083]

[0084] Here, “ / ” means non-existence, the same below.

[0085] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that, compared with using a single-layer current collector, using a current collector including a first substrate and a second substrate can significantly reduce the elongation of the pole piece and improve the demolding of the pole piece.

[0086] By comparing Example 2 and Comparative Examples 3 to 4, it can be seen that when the difference in tensile strength between the first substrate and the second substrate is less than 100 MPa or greater than 400 MPa, although the elongation of the pole piece is reduced due to the use of the first substrate with high tensile strength, demolding of the pole piece occurs.

[0087] By comparing Example 7 with Comparative Examples 5 to 7, it can be seen that when the thickness ratio of the first substrate to the second substrate is less than 0.5 or greater than 2.5, the pole piece is peeled off.

[0088] By comparing Examples 1 to 10, it can be seen that the composite current collectors with various structures can achieve the effect of reducing the elongation and improving the demolding of the pole piece when the difference in tensile strength between the first substrate and the second substrate is 100 MPa to 400 MPa.

[0089] By comparing Examples 8 and 9, it can be seen that a thicker current collector can reduce the elongation of the electrode.

[0090] By comparing Examples 9 and 10, it can be seen that as the silicon content of the negative electrode active material layer increases, the elongation of the electrode sheet also increases accordingly.

[0091] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of disclosure involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features. For example, the above features are replaced with the technical features with similar functions disclosed in the present application.

Claims

1. An electrochemical device comprising a first electrode, wherein: The first pole piece includes: A current collector comprising a first substrate and a second substrate stacked in layers; an active material layer, wherein the second substrate is disposed between the first substrate and the active material layer, the tensile strength Rm1 of the first substrate and the tensile strength Rm2 of the second substrate satisfy the following conditions: 520 MPa ≤ Rm1 ≤ 800 MPa, 100 MPa ≤ Rm1 - Rm2 ≤ 400 MPa, the elongation of the first substrate is less than or equal to 25%, and the elongation of the second substrate is less than or equal to 25%; The total thickness of the first substrate and the second substrate is 4 μm to 20 μm, the thickness d1 of the first substrate and the thickness d2 of the second substrate satisfy: 0.5≤d1 / d2≤2.5, the first substrate includes at least one of an alloy material, an inorganic ceramic material, a rolled copper foil, an electrodeposited nickel foil or a rolled nickel foil, and the second substrate includes at least one of a porous copper foil, an electrodeposited copper foil, a foam copper foil or a conductive polymer material.

2. The electrochemical device according to claim 1, wherein The conductive polymer material includes a conductive agent and a polymer material, the conductive agent includes a carbon material, and the polymer material includes at least one of polyethylene, polypropylene, polystyrene, epoxy resin or phenolic resin.

3. The electrochemical device according to claim 1, wherein The current collector further includes a first bonding layer disposed between the first substrate and the second substrate and bonding the first substrate and the second substrate.

4. The electrochemical device according to claim 1, wherein In the thickness direction of the first pole piece, the projection of the active material layer is located within the region of the projection of the second substrate.

5. The electrochemical device according to claim 1, wherein The active material layer includes a negative electrode active material. The negative electrode active material includes a silicon-based material. The silicon-based material includes at least one of silicon, a silicon alloy, a silicon oxide, and a silicon-carbon composite.

6. The electrochemical device according to claim 1, wherein The active material layer is in contact with the second substrate; or The first pole piece further includes a conductive layer disposed between the active material layer and the second substrate, wherein the conductive layer is in contact with the active material layer and the second substrate respectively.

7. The electrochemical device according to claim 1, wherein The current collector also includes a third substrate, which is stacked with the first substrate, the first substrate is arranged between the third substrate and the second substrate, and the active material layer is also arranged on the third substrate. The tensile strength Rm1 of the first substrate and the tensile strength Rm3 of the third substrate satisfy: 100MPa≤Rm1-Rm3≤400MPa.

8. The electrochemical device according to claim 1, wherein The electrochemical device further includes a tab connected to the first substrate or the second substrate of the first electrode sheet, and a thickness of the first substrate or the second substrate connected to the tab is greater than or equal to 3 μm.

9. An electronic device comprising the electrochemical device according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite current collector, electrode plate and electrochemical device