A method for manufacturing a light emitting diode
By growing Mg-doped InAlGaN layer and Si-doped InAlN layer during the LED production process, the reaction conditions are controlled, and the problems of LED wavelength blue shift and brightness are solved, and the internal quantum efficiency and light output uniformity are achieved, which is small Application requirements for spacing displays.
Patent Information
- Application Number
- CN202210566526.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-05-23
AI Technical Summary
In the existing LED epitaxial material growth method, the band gap width of the material is limited, resulting in the LED light emission wavelength easily moving towards the short wave direction, which cannot meet the application needs of small-pitch display screens, and the light emission wavelength varies greatly under different current conditions. The brightness and color requirements of the display cannot be met.
Using a new light emitting diode manufacturing method, including growing Mg-doped InAlGaN layer and Si-doped InAlN layer, the "Al-In" bond and double-barrier layer structure are formed by controlling the reaction chamber pressure and temperature, reducing the formation of N voids and electrons. Overflow phenomenon improves the composite luminescence efficiency and light output uniformity of the quantum well layer.
It effectively reduces the wavelength blue shift of LEDs, improves internal quantum efficiency and brightness, meets the application needs of small-pitch displays, and reduces the working voltage.
Smart Images

Figure CN114937723B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a method for manufacturing a light emitting diode. Background Art
[0002] Light-Emitting Diode (LED) is a semiconductor electronic device that converts electrical energy into light energy. When current flows through the LED, the electrons and holes in the LED recombine in its multi-quantum wells to emit monochromatic light. As a new type of efficient, environmentally friendly, green solid-state lighting source, LED is currently widely used for indoor and outdoor lighting, as well as traffic lights, car lights, indoor and outdoor lighting and display screens.
[0003] In the current LED epitaxial material growth method, the bandgap width of the material is limited, the ground state in the quantum well increases, and the LED's emission wavelength tends to move toward the short-wave direction, that is, blue shift occurs. When different currents are injected into the fine-pitch display to change the luminous intensity, the amount of blue shift of the LED's emission wavelength will vary greatly, which cannot meet the application needs of fine-pitch display screens.
[0004] In summary, it is urgent to develop new LED chip manufacturing methods to reduce wavelength blue shift and improve the internal quantum efficiency and brightness of LEDs to meet the application needs of small-pitch display screens. Summary of the invention
[0005] The invention adopts a new light emitting diode manufacturing method to reduce the wavelength blue shift and improve the internal quantum efficiency and brightness of the LED.
[0006] The light emitting diode manufacturing method of the present invention comprises the following steps: processing a substrate, growing a low-temperature GaN buffer layer, growing a non-doped GaN layer, growing an n-type GaN layer, growing a Mg-doped InAlGaN layer, growing a quantum well layer, growing a Si-doped InAlN layer, growing an AlGaN electron blocking layer, growing a P-type GaN layer, and cooling down, wherein:
[0007] The growing of the Mg-doped InAlGaN layer is specifically:
[0008] The pressure of the reaction chamber is controlled at 100-300 mbar, NH3, TMGa, Cp2Mg, TMAl and TMIn are introduced, and a Mg-doped InAlGaN layer with a thickness of 20-70 nm is grown on the n-type GaN layer. During the growth process, the temperature of the reaction chamber is controlled to gradually decrease from 1200°C to 600°C;
[0009] The growing of the Si-doped InAlN layer is specifically:
[0010] The pressure of the reaction chamber is controlled at 100-320mba, the temperature of the reaction chamber is increased to 900-950°C, NH3, SiH4, TMAl and TMIn are introduced, and a Si-doped InAlN layer with a thickness of 10-50nm is grown on the quantum well layer. During the growth process, the TMIn source is periodically interrupted so that the band gap energy level of the Si-doped InAlN layer is greater than the band gap energy level of the quantum well layer, and the Al component is controlled to gradually decrease from 35% to 8%, wherein the time for TMIn interruption and introduction into the reaction chamber is 8s and 4s, respectively.
[0011] Preferably, the specific process of processing the substrate is:
[0012] At a temperature of 1000°C to 1100°C, H2 is introduced, the pressure in the reaction chamber is maintained at 100 to 300 mbar, and the sapphire substrate is treated for 5 to 10 minutes.
[0013] Preferably, the specific process of growing the low-temperature GaN buffer layer is:
[0014] The temperature is lowered to 500-600°C, the pressure of the reaction chamber is maintained at 300-600 mbar, NH3, TMGa and H2 are introduced, and a low-temperature GaN buffer layer with a thickness of 20-40 nm is grown on the sapphire substrate;
[0015] The temperature is raised to 1000-1100°C, the pressure in the reaction chamber is maintained at 300-600 mbar, NH3 and H2 are introduced, and the temperature is kept at 300-500 seconds to etch the low-temperature GaN buffer layer into irregular island shapes.
[0016] Preferably, the specific process of growing the undoped GaN layer is:
[0017] The temperature is raised to 1000-1200°C, the pressure in the reaction chamber is maintained at 300-600 mbar, NH3, TMGa and H2 are introduced, and a 2-4 μm non-doped GaN layer is continuously grown.
[0018] Preferably, the specific process of growing the n-type GaN layer is:
[0019] The reaction chamber pressure is maintained at 300-600 mbar, the temperature is maintained at 1000-1200°C, NH3, TMGa, H2 and SiH4 are introduced, and a 3-4 μm Si-doped n-type GaN layer is continuously grown.
[0020] Preferably, the specific process of growing the quantum well layer is:
[0021] The reaction chamber pressure was controlled at 300-320 mbar, the reaction chamber temperature was controlled at 620-640°C, N2, NH3, TMGa and TMIn were introduced, and In with a thickness of 3-4 nm was grown. xGa (1-x) N well layer, wherein x=0.15 to 0.25;
[0022] The pressure in the reaction chamber is controlled to be constant, the temperature in the reaction chamber is increased to 800-820°C, N2, NH3 and TMGa are introduced, and a GaN barrier layer with a thickness of 8-10 nm is grown;
[0023] Grow periodically x Ga (1-x) The steps of the N well layer and the GaN barrier layer have 3 to 13 cycles.
[0024] Preferably, the specific process of growing the AlGaN electron blocking layer is:
[0025] Under the conditions of temperature of 900-950° C., reaction chamber pressure of 200-400 mbar, and introduction of NH 3 , TMGa, H 2 , TMAl and Cp 2 Mg, an AlGaN electron blocking layer with a thickness of 40-60 nm is grown.
[0026] Preferably, the specific process of growing the P-type GaN layer is:
[0027] The reaction chamber pressure is maintained at 100-300mba and the temperature is maintained at 950-1000°C, and NH3, TMGa, H2 and Cp2Mg are introduced to continuously grow a 50-200nm Mg-doped P-type GaN layer.
[0028] Preferably, the specific process of cooling down is:
[0029] Cool down to 650-680℃, keep warm for 20-30min, turn off the heating system and gas supply system, and cool with the furnace.
[0030] Compared with the traditional growth method, the production method of the present invention achieves the following effects:
[0031] 1. The present invention inserts a Mg-doped InAlGaN layer before growing the quantum well. On the one hand, since Al atoms have a lower principal quantum number and a wider orbital energy gap than In atoms, due to the linear merging effect of atomic orbitals, Al atoms form "Al-In" bonds (or "In-Mg-Al" bonds) in the InAlGaN layer, which increases the In x Ga (1-x)The bandgap width of the N well layer causes the ground state in the quantum well to decrease, reducing the wavelength of the LED to move toward the short-wave direction, thereby reducing the wavelength blue shift; on the other hand, since the growth temperature gradually decreases from a high temperature of 1200°C to a low temperature of 600°C, it is more difficult for N voids to form, which can reduce the N voids inside the InAlGaN layer, and the In atoms carried in the InAlGaN layer react with the N voids extending to the InAlGaN layer in advance, reducing the probability of N voids extending to the quantum well layer to form photon annihilation points, which can improve the composite luminescence efficiency of the carriers in the quantum well layer, thereby improving the brightness of the LED. The InAlGaN layer is doped with Mg, which can promote the increase and migration of holes, and with the potential barrier of the InAlGaN layer, the holes can enter the InAlGaN layer more evenly. x Ga (1-x) The N / GaN quantum well layer improves the internal quantum efficiency while also improving the uniformity of light output.
[0032] 2. The present invention inserts a Si-doped InAlN layer after the quantum well and periodically interrupts the TMIn source to make the band gap energy level of the Si-doped InAlN layer greater than the band gap energy level of the quantum well layer. At this time, the InAlN layer and the AlGaN electron barrier layer form a double barrier layer structure, which can effectively prevent electron overflow and improve the internal quantum efficiency. In the process of growing the InAlN layer, by adjusting the Al component from 35% to 8%, the lattice constant of the InAlN layer can be matched with that of the quantum well, thereby releasing stress, making the Si-doped InAlN layer free of polarization effect, increasing the equivalent band gap energy level of the quantum well, and reducing the wavelength blue shift. In addition, the InAlN layer is doped with Si, which can promote the increase and migration of electrons, allowing more electrons to enter the quantum well, thereby improving the internal quantum efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0034] Figure 1 A schematic diagram of an LED epitaxial structure prepared by the method of the present invention;
[0035] Figure 2 A schematic diagram of an LED epitaxial structure prepared by an existing traditional method;
[0036] Among them, 1. sapphire substrate, 2. low-temperature GaN buffer layer, 3. undoped GaN layer, 4. n-type GaN layer, 5. Mg-doped InAlGaN layer, 6. multi-quantum well layer, 7. Si-doped InAlN layer, 8. AlGaN electron blocking layer, 9. P-type GaN layer, 61. In x Ga (1-x)N well layer, 62, GaN barrier layer. DETAILED DESCRIPTION
[0037] The present application is further described in detail below in conjunction with the accompanying drawings, but is not intended to limit the present application.
[0038] Example 1
[0039] This embodiment adopts the light emitting diode manufacturing method provided by the present invention, and uses MOCVD to grow GaN-based LED epitaxial wafers. The specific growth method is as follows (for epitaxial structure, please refer to Figure 1 ):
[0040] A method for manufacturing a light-emitting diode comprises, in sequence: processing a sapphire substrate 1, growing a low-temperature GaN buffer layer 2, growing a non-doped GaN layer 3, growing an n-type GaN layer 4, growing a Mg-doped InAlGaN layer 5, growing a quantum well layer 6, growing a Si-doped InAlN layer 7, growing an AlGaN electron blocking layer 8, growing a P-type GaN layer 9, and cooling; wherein,
[0041] Step 1: Processing a sapphire substrate 1.
[0042] Specifically, the step 1 is further as follows:
[0043] At a temperature of 1000-1100° C. and a reaction chamber pressure of 100-300 mbar, H 2 is introduced and the sapphire substrate is treated for 5-10 minutes.
[0044] Step 2: growing a low-temperature GaN buffer layer 2 and forming irregular islands in the low-temperature GaN buffer layer 2 .
[0045] Specifically, the step 2 is further as follows:
[0046] Under the conditions of a temperature of 500-600° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 , TMGa, and H 2 , growing the low-temperature GaN buffer layer 2 on the sapphire substrate 1 , wherein the thickness of the low-temperature GaN buffer layer 2 is 20-40 nm;
[0047] Under the conditions of a temperature of 1000-1100° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 and H 2 , the temperature is maintained for 300-500 seconds to form the irregular small islands on the low-temperature GaN buffer layer 2 .
[0048] Step 3: growing a non-doped GaN layer 3.
[0049] Specifically, the step 3 is further as follows:
[0050] The undoped GaN layer 3 is grown under the conditions of a temperature of 1000-1200° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 , TMGa and H 2 . The thickness of the undoped GaN layer 3 is 2-4 μm.
[0051] Step 4: growing an n-type GaN layer 4.
[0052] Specifically, the step 4 is further as follows:
[0053] The reaction chamber pressure is maintained at 300-600 mbar, the temperature is maintained at 1000-1200° C., NH 3 , TMGa, H 2 and SiH 4 are introduced, and a 3-4 μm Si-doped n-type GaN layer 4 is continuously grown.
[0054] Step 5: Grow a Mg-doped InAlGaN layer.
[0055] Specifically, the step 5 is further as follows:
[0056] The reaction chamber pressure is controlled at 100-300 mbar, NH3, TMGa, Cp2Mg, TMAl and TMIn are introduced, and a Mg-doped InAlGaN layer with a thickness of 20-70 nm is grown on the n-type GaN layer. During the growth process, the reaction chamber temperature is controlled to gradually decrease from 1200°C to 600°C.
[0057] Step 6: Grow the quantum well layer.
[0058] Specifically, the step 6 is further as follows:
[0059] The pressure of the reaction chamber is controlled at 300-320 mbar, the temperature of the reaction chamber is controlled at 620-640°C, N2, NH3, TMGa and TMIn are introduced, and In with a thickness of 3-4 nm is grown. x Ga (1-x) N well layer 61, wherein x=0.15-0.25;
[0060] The pressure of the reaction chamber is controlled to be constant, the temperature of the reaction chamber is increased to 800-820° C., N2, NH3, and TMGa are introduced, and a GaN barrier layer 62 with a thickness of 8-10 nm is grown;
[0061] Grow periodically x Ga (1-x) The steps of forming the N well layer 61 and the GaN barrier layer 62 have 3 to 13 cycles.
[0062] Step 7: growing a Si-doped InAlN layer 7 .
[0063] Specifically, the step 7 is further as follows:
[0064] The reaction chamber pressure is controlled at 100-320mba, the reaction chamber temperature is increased to 900-950°C, NH3, SiH4, TMAl and TMIn are introduced, and a Si-doped InAlN layer 7 with a thickness of 10-50nm is grown on the quantum well layer. During the growth process, the TMIn source is periodically interrupted so that the band gap energy level of the Si-doped InAlN layer 7 is greater than the band gap energy level of the quantum well layer 6, and the Al component is controlled to gradually decrease from 35% to 8%, wherein the time for TMIn interruption and introduction into the reaction chamber is 8s and 4s, respectively.
[0065] Step 8: growing an AlGaN electron blocking layer 8.
[0066] Specifically, the step 8 is further as follows:
[0067] The AlGaN electron blocking layer 8 is grown at a temperature of 900-950° C., a reaction chamber pressure of 200-400 mbar, and NH 3 , TMGa, H 2 and TMAl are introduced. The thickness of the AlGaN layer 8 is 40-60 nm.
[0068] Step 9: growing a P-type GaN layer 9.
[0069] Specifically, the step 9 is further as follows:
[0070] Under the conditions of a temperature of 950-1000° C., a reaction chamber pressure of 100-300 mbar, and introduction of NH 3 , 20-100 sccm of TMGa, H 2 and Cp 2 Mg, a Mg-doped P-type GaN layer 9 with a thickness of 50-200 nm is grown.
[0071] Step 8: Keep the temperature at 650-680°C for 20-30 minutes, then turn off the heating system and the gas supply system, and cool with the furnace.
[0072] Example 2
[0073] The following is a comparative example, that is, a conventional method for manufacturing a light emitting diode (see the epitaxial structure for details). Figure 2 ).
[0074] Step 1: At a temperature of 1000-1100° C. and a reaction chamber pressure of 100-300 mbar, introduce H 2 and treat the sapphire substrate for 5-10 minutes.
[0075] Step 2: growing a low-temperature GaN buffer layer 2 and forming irregular islands in the low-temperature GaN buffer layer 2 .
[0076] Specifically, the step 2 is further as follows:
[0077] Under the conditions of a temperature of 500-600° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 , TMGa, and H 2 , growing the low-temperature GaN buffer layer 2 on the sapphire substrate 1 , wherein the thickness of the low-temperature GaN buffer layer 2 is 20-40 nm;
[0078] Under the conditions of a temperature of 1000-1100° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 and H 2 , the temperature is maintained for 300-500 seconds to form the irregular islands on the low-temperature GaN buffer layer 2 .
[0079] Step 3: growing a non-doped GaN layer 3.
[0080] Specifically, the step 3 is further as follows:
[0081] The undoped GaN layer is grown under the conditions of a temperature of 1000-1200° C., a reaction chamber pressure of 300-600 mbar, and introduction of NH 3 , TMGa, and H 2 . The thickness of the undoped GaN layer 3 is 2-4 μm.
[0082] Step 4: growing an n-type GaN layer 4.
[0083] Specifically, the step 4 is further as follows:
[0084] Under the conditions of temperature of 1000-1200° C., reaction chamber pressure of 300-600 mbar, and introduction of NH 3 , TMGa, H 2 and SiH 4 , a Si-doped n-type GaN layer 4 is grown, wherein the thickness of the n-type GaN layer 4 is 3-4 μm.
[0085] Step 5: growing an InGaN / GaN multi-quantum well layer 6 .
[0086] Specifically, the growing of the multi-quantum well layer 6 is further:
[0087] The reaction chamber pressure was controlled at 300-320 mbar, the reaction chamber temperature was lowered to 620-640°C, N2, NH3, TMGa and TMIn were introduced, and In with a thickness of 3-4 nm was grown. x Ga (1-x) N well layer 61, wherein x=0.15-0.25;
[0088] The pressure of the reaction chamber is controlled to be constant, the temperature of the reaction chamber is increased to 800-820° C., N2, NH3, and TMGa are introduced, and a GaN barrier layer 62 with a thickness of 8-10 nm is grown;
[0089] Grow periodically x Ga (1-x)The steps of forming the N well layer 61 and the GaN barrier layer 62 have 3 to 13 cycles.
[0090] Step 6: growing an AlGaN electron blocking layer 8.
[0091] Specifically, the step 8 is further as follows:
[0092] The AlGaN electron blocking layer 8 is grown at a temperature of 900-950° C., a reaction chamber pressure of 200-400 mbar, and the introduction of NH 3 , TMGa, H 2 and TMAl. The thickness of the AlGaN layer 8 is 40-60 nm.
[0093] Step 7: Grow a P-type GaN layer 9.
[0094] Specifically, the step 9 is further as follows:
[0095] Under the conditions of a temperature of 950-1000° C., a reaction chamber pressure of 100-300 mbar, and introduction of NH 3 , TMGa, H 2 and Cp 2 Mg, a Mg-doped P-type GaN layer 9 with a thickness of 50-200 nm is grown.
[0096] Step 8: Keep the temperature at 650-680°C for 20-30 minutes, then turn off the heating system and the gas supply system, and cool with the furnace.
[0097] According to the above-mentioned Example 1 and Example 2, Sample 1 and Sample 2 were prepared respectively. Sample 1 and Sample 2 were plated with an ITO layer of about 150nm under the same pre-process conditions, Cr / Pt / Au electrodes of about 1500nm under the same conditions, and protective layer SiO2 of about 100nm under the same conditions. Then, the samples were ground and cut into 635μm*635μm (25mil*25mil) chip particles under the same conditions. Then, 1000 grains were selected at the same position of Sample 1 and Sample 2, and packaged into white light LEDs under the same packaging process. The photoelectric performance of Sample 1 and Sample 2 was tested using an integrating sphere under the condition of a driving current of 150mA.
[0098] Table 1 Comparison of electrical parameters of sample 1 and sample 2
[0099]
[0100] The data obtained by the integrating sphere are analyzed and compared. It can be seen from Table 1 that the luminous efficiency of the LED (sample 1) prepared by the manufacturing method provided by the present invention is significantly improved, the wavelength blue shift is smaller, and the operating voltage is also reduced. This is because the patent adopts a new technical solution to improve the luminous efficiency of the LED and reduce the wavelength blue shift.
[0101] The light emitting diode manufacturing method of the present invention achieves the following effects:
[0102] 1. The present invention inserts a Mg-doped InAlGaN layer before growing the quantum well. On the one hand, since Al atoms have a lower principal quantum number and a wider orbital energy gap than In atoms, due to the linear merging effect of atomic orbitals, Al atoms form "Al-In" bonds (or "In-Mg-Al" bonds) in the InAlGaN layer, which increases the In x Ga (1-x) The bandgap width of the N well layer causes the ground state in the quantum well to decrease, reducing the wavelength of the LED to move toward the short-wave direction, thereby reducing the wavelength blue shift; on the other hand, since the growth temperature gradually decreases from a high temperature of 1200°C to a low temperature of 600°C, it is more difficult for N voids to form, which can reduce the N voids inside the InAlGaN layer, and the In atoms carried in the InAlGaN layer react with the N voids extending to the InAlGaN layer in advance, reducing the probability of N voids extending to the quantum well layer to form photon annihilation points, which can improve the composite luminescence efficiency of the carriers in the quantum well layer, thereby improving the brightness of the LED. The InAlGaN layer is doped with Mg, which can promote the increase and migration of holes, and with the potential barrier of the InAlGaN layer, the holes can enter the InAlGaN layer more evenly. x Ga (1-x) The N / GaN quantum well layer improves the internal quantum efficiency while also improving the uniformity of light output.
[0103] 2. The present invention inserts a Si-doped InAlN layer after the quantum well and periodically interrupts the TMIn source to make the band gap energy level of the Si-doped InAlN layer greater than the band gap energy level of the quantum well layer. At this time, the InAlN layer and the AlGaN electron barrier layer form a double barrier layer structure, which can effectively prevent electron overflow and improve the internal quantum efficiency. In the process of growing the InAlN layer, by adjusting the Al component from 35% to 8%, the lattice constant of the InAlN layer can be matched with that of the quantum well, thereby releasing stress, making the Si-doped InAlN layer free of polarization effect, increasing the equivalent band gap energy level of the quantum well, and reducing the wavelength blue shift. In addition, the InAlN layer is doped with Si, which can promote the increase and migration of electrons, allowing more electrons to enter the quantum well, thereby improving the internal quantum efficiency.
[0104] Since the method part has described the embodiment of the present application in detail, the expanded description of the structure and method corresponding parts involved in the embodiment is omitted here and will not be repeated. For the description of the specific content in the structure, please refer to the content of the method embodiment, which is not specifically limited here.
[0105] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A method for manufacturing a light emitting diode, characterized in that: Including in order: The steps include processing the substrate, growing a low-temperature GaN buffer layer, growing an undoped GaN layer, growing an n-type GaN layer, growing a Mg-doped InAlGaN layer, growing a quantum well layer, growing a Si-doped InAlN layer, growing an AlGaN electron barrier layer, growing a P-type GaN layer, and cooling the layer, wherein: The growing of the Mg-doped InAlGaN layer is specifically: The pressure of the reaction chamber is controlled at 100-300 mbar, NH3, TMGa, Cp2Mg, TMAl and TMIn are introduced, and a Mg-doped InAlGaN layer with a thickness of 20-70 nm is grown on the n-type GaN layer. During the growth process, the temperature of the reaction chamber is controlled to gradually decrease from 1200°C to 600°C; The growing of the Si-doped InAlN layer is specifically: The pressure of the reaction chamber is controlled at 100-320mba, the temperature of the reaction chamber is increased to 900-950°C, NH3, SiH4, TMAl and TMIn are introduced, and a Si-doped InAlN layer with a thickness of 10-50nm is grown on the quantum well layer. During the growth process, the TMIn source is periodically interrupted so that the band gap energy level of the Si-doped InAlN layer is greater than the band gap energy level of the quantum well layer, and the Al component is controlled to gradually decrease from 35% to 8%, wherein the time for TMIn interruption and introduction into the reaction chamber is 8s and 4s, respectively.
2. A method for manufacturing a light emitting diode according to claim 1, characterized in that: At a temperature of 1000-1100° C., H 2 is introduced, the pressure in the reaction chamber is maintained at 100-300 mbar, and the sapphire substrate is treated for 5-10 minutes.
3. A method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the low-temperature GaN buffer layer is as follows: The temperature is lowered to 500-600°C, the pressure of the reaction chamber is maintained at 300-600 mbar, NH3, TMGa and H2 are introduced at a flow rate, and a low-temperature GaN buffer layer with a thickness of 20-40 nm is grown on a sapphire substrate; The temperature is raised to 1000-1100°C, the pressure in the reaction chamber is maintained at 300-600 mbar, NH3 and H2 are introduced, and the temperature is kept at 300-500 seconds to etch the low-temperature GaN buffer layer into irregular island shapes.
4. A method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the non-doped GaN layer is: The temperature is raised to 1000-1200°C, the pressure in the reaction chamber is maintained at 300-600 mbar, NH3, TMGa and H2 are introduced, and a 2-4 μm non-doped GaN layer is continuously grown.
5. The method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the n-type GaN layer is: The reaction chamber pressure is maintained at 300-600 mbar, the temperature is maintained at 1000-1200°C, NH3, TMGa, H2 and SiH4 are introduced, and a 3-4 μm Si-doped n-type GaN layer is continuously grown.
6. The method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the quantum well layer is as follows: The reaction chamber pressure was controlled at 300-320 mbar, the reaction chamber temperature was controlled at 620°C-640°C, N2, NH3, TMGa and TMIn were introduced, and In with a thickness of 3-4 nm was grown. x Ga (1-x) N well layer, wherein x=0.15 to 0.25; The pressure in the reaction chamber is controlled to be constant, the temperature in the reaction chamber is increased to 800°C to 820°C, N2, NH3, and TMGa are introduced, and a GaN barrier layer with a thickness of 8 to 10 nm is grown; Grow periodically x Ga (1-x) The steps of the N well layer and the GaN barrier layer have 3-13 cycles.
7. The method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the AlGaN electron blocking layer is as follows: Under the conditions of temperature of 900-950° C., reaction chamber pressure of 200-400 mbar, and introduction of NH 3 , TMGa, H 2 and TMAl, an AlGaN electron blocking layer with a thickness of 40-60 nm is grown.
8. The method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of growing the P-type GaN layer is as follows: The reaction chamber pressure is maintained at 100-300mba and the temperature is maintained at 950-1000°C. NH3, TMGa, H2 and Cp2Mg are introduced at a flow rate to continuously grow a 50-200nm Mg-doped P-type GaN layer.
9. The method for manufacturing a light emitting diode according to claim 1, characterized in that: The specific process of the cooling is as follows: Cool down to 650-680℃, keep warm for 20-30min, turn off the heating system and gas supply system, and cool with the furnace.