A kind of preparation method of polypyrrole modified graphite felt

The polypyrrole coating structure is controlled on the surface of the graphite felt through the galvanostatic pulse polymerization method, which solves the problem of insufficient two-electron oxygen reduction activity of the graphite felt material, significantly increases the accumulation rate and electrochemical activity of H2O2, and improves the redox performance.

CN115207355BActive Publication Date: 2024-10-29SICHUAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210816005.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-12
Publication Date
2024-10-29
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

The existing graphite felt material has a small specific surface area, poor hydrophilicity, and low two-electron oxygen reduction activity. It is difficult to effectively catalyze the two-electron reduction reaction of oxygen, which limits the electrochemical production efficiency of hydrogen peroxide.

Method used

The polypyrrole coating structure is controlled on the surface of graphite felt through galvanostatic pulse polymerization, and the polymerization time, pulse number and interval time are optimized to form a polypyrrole-modified graphite felt electrode with high electrochemical activity.

Benefits of technology

It significantly improves the two-electron oxygen reduction activity and electrochemical activity specific surface area of ​​the graphite felt electrode, increases the accumulation rate of H2O2, and enhances the redox performance, which has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115207355B_ABST
    Figure CN115207355B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing polypyrrole modified graphite felt, comprising the steps of dissolving pyrrole and sulfate in water to prepare a solution, then using the solution as an electrolyte, graphite felt as an anode, and platinum as a cathode, and performing electrochemical polymerization under constant current conditions; polymerization pulse time: 50 to 200 seconds, pulse interval time: 120 to 240 seconds, pulse number: 10 to 20 times; total polymerization time 1000 to 1500 seconds. The polypyrrole modified graphite felt electrode prepared by the present invention has excellent two-electron oxygen reduction activity and electrochemical active specific surface area within a specific range of polymerization pulse time, interval time and pulse number, and significantly improves the H2O2 accumulation rate as a redox electrode, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of carbon material modification, and in particular relates to a method for preparing polypyrrole modified graphite felt. Background Art

[0002] Hydrogen peroxide is widely used in the chemical, papermaking, environmental protection and other industries as an oxidant, bleaching agent, and disinfectant. The global annual consumption of hydrogen peroxide reaches about 6.5 million tons / year, of which China accounts for 3.2 million tons. At present, more than 98% of the world's hydrogen peroxide is produced by the anthraquinone method. As of 2018, my country's domestic production accounts for more than 50% of the world's total production capacity, with a production capacity of about 3.7 million tons / year, and the plant capacity is generally 5×10 4 t / a. However, the unstable nature of hydrogen peroxide seriously affects the safety of transportation and restricts the transportation radius, which is very unfavorable for small-scale applications such as wastewater treatment. Distributed on-site production can avoid the cost and danger of transportation and storage, which is of great significance for small-scale applications of hydrogen peroxide.

[0003] In an acidic electrolyte solution, oxygen undergoes two-electron reduction at the cathode to generate H 2 O 2 (Formula 1), a 4-electron reduction occurs to generate H 2 O (Formula 2). H can be produced by electrochemical oxygen reduction reaction 2 O 2 However, the 4-electron reduction of oxygen and the hydrogen evolution reaction (Equation 3) must be suppressed. In addition, H 2 O 2 Self-decomposition or catalytic decomposition under the action of electrodes (Formula 4).

[0004] O 2 +2e - +H + →H 2 O 2 E 0 =0.695V(vs.SHE) (1)

[0005] O 2 +4e - +H + →H 2 OE 0 =1.229V(vs.SHE) (2)

[0006] 2e - +H + →H 2 ↑E 0 =0V(vs.SHE) (3)

[0007] H 2 O2 +2H + +2e - →2H 2 OE 0 =1.763V(vs.SHE) (4)

[0008] Graphite felt materials are non-toxic, chemically stable, have good corrosion resistance, high hydrogen evolution potential and low cost, which provide a good basis for them to be used as redox electrode materials. However, graphite felt-like carbon materials have a small specific surface area, poor hydrophilicity, and low two-electron oxygen reduction activity, so they must be modified to improve the production of H 2 O 2 The introduction of heteroatoms such as N, O, and S and metal atoms into carbon materials can reduce the stability of adjacent carbon atoms, increase the defects on the surface of carbon materials, and improve the electrochemical activity of oxygen reduction in carbon materials. Heteroatom modification can improve the electron supply capacity of carbon materials as cathodes, enhance the adsorption of oxygen on electrodes, and promote H 2 O 2 The pyrrole-type carbon-nitrogen structure is particularly effective in catalyzing the two-electron reduction reaction of oxygen. Polypyrrole contains abundant pyrrole-type carbon-nitrogen structures, which adsorb oxygen molecules and increase their bond length and reduce their bond order, thus catalyzing the two-electron reduction reaction of oxygen.

[0009] The main polymerization methods of pyrrole are chemical oxidation and electrochemical polymerization. Among them, the electrochemical polymerization method is simpler and easier to control, which is conducive to the polymerization of pyrrole on the surface of graphite felt to form a film. Although there have been reports on the modification of graphite felt with polypyrrole, such as Ruan Chi et al. used pyrrole monomer as raw material to modify the surface of graphite felt by electrochemical oxidation polymerization, and studied the effects of the type of polymerization supporting electrolyte and polymerization time on the two-electron oxygen reduction performance of the modified graphite felt (Ruan Chi, Liu Changjun, Yue Hairong, et al. Oxygen reduction performance and application of polypyrrole modified graphite felt electrode [J]. Fine Chemicals, 2020, 37(9): 1896-1903, 1917. DOI: 10.13550 / j.jxhg.20200325.). However, there is still a lack of systematic understanding of the electrochemical polymerization method to regulate the structure of the polypyrrole film layer on the surface of graphite felt. Summary of the invention

[0010] The present invention studies the process of regulating the structure and morphology of the polypyrrole coating on the surface of graphite felt by constant current pulse polymerization, investigates the influence of polymerization time, pulse number and interval time on the morphology and electrochemical properties of the polypyrrole modified graphite felt electrode, optimizes the polymerization modification process parameters, and finally obtains a polypyrrole modified graphite felt electrode with excellent redox performance.

[0011] The present invention provides a method for preparing polypyrrole modified graphite felt, comprising the following steps:

[0012] (1) dissolving pyrrole and sulfate in water to prepare a solution;

[0013] (2) With graphite felt as anode, platinum as cathode, and the solution of step (1) as electrolyte, electrochemical polymerization is carried out under constant current conditions; polymerization pulse time: 50 to 200 s, pulse interval time: 120 to 240 s, pulse number: 10 to 20 times; total polymerization time: 1000 to 1500 s.

[0014] Furthermore, the total polymerization time is 1000 s; preferably, the polymerization pulse time is 100 s, the pulse interval time is 120 s, and the number of pulses is 10 times.

[0015] Furthermore, in the solution of step (1), the concentration of pyrrole is 0.1-0.3 mol / L, and the concentration of sulfate is 0.03-0.07 mol / L.

[0016] Furthermore, the concentration of pyrrole in the above solution is 0.2 mol / L, and the concentration of sulfate is 0.05 mol / L.

[0017] Furthermore, the constant current in step (2) is a constant current of 0.01A.

[0018] Furthermore, the graphite felt in step (2) is pretreated as follows: the graphite felt is first ultrasonically cleaned with anhydrous ethanol, then ultrasonically cleaned with ultrapure water, and finally vacuum dried.

[0019] Furthermore, the anhydrous ethanol ultrasonic cleaning time is 1 hour, the ultrapure water ultrasonic cleaning time is 1 hour, and the vacuum drying is vacuum drying at 60° C. for 8 hours.

[0020] Furthermore, the graphite felt described in step (2) has a thickness of 5 mm.

[0021] The present invention also provides polypyrrole modified graphite felt prepared by the above method.

[0022] The present invention also provides the use of the polypyrrole modified graphite felt as a redox electrode.

[0023] Beneficial effects of the present invention: The present invention effectively regulates the polypyrrole structure and electrochemical properties of the graphite felt fiber surface by adjusting the polymerization pulse time, interval time and pulse number; the prepared polypyrrole modified graphite felt electrode has excellent two-electron oxygen reduction activity and electrochemically active specific surface area, and as a redox electrode, significantly improves H 2 O 2 Accumulation rate, has good application prospects.

[0024] The "total polymerization time" of the present invention is the total time of applying pulses, that is, the product of the polymerization pulse time and the number of pulses.

[0025] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0026] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 SEM images of graphite felt samples, (a) GF; (b) 1(1000s-0s)-GF; (c, d) 10(50s-120s)-GF; (e) 10(100s-120s)-GF; (f) 10(100s-60s)-GF.

[0028] Figure 2 These are the infrared spectra of GF, 1(1000s-0s)-GF, and 10(100s-120s)-GF.

[0029] Figure 3 is the electrochemically active specific surface area of ​​graphite felt with different polymerization times.

[0030] Figure 4 is the electrochemical active specific surface area of ​​graphite felt at different pulse intervals.

[0031] Figure 5 Cyclic voltammetry curves of graphite felt and modified graphite felt electrodes (scan rate 50 mV / s; potential range 0 V to -1.4 V; electrolyte 0.05 mol / L Na 2 SO 4 solution, pH=3, oxygen flow rate of 100 mL / min).

[0032] Figure 6 The cyclic voltammetry curves of graphite felt samples with different pyrrole doping amounts (scan rate 50 mV / s; potential range 0 V to -1.4 V; electrolyte 0.05 mol / L Na 2 SO 4 solution, pH=3, oxygen flow rate of 100 mL / min).

[0033] Figure 7 is the effect of the polymerization pulse time on the H 2 O 2 Effect of accumulation rate (electrolyte: 0.05 mol / L Na 2 SO4 solution, pH=3; oxygen flow rate is 100 mL / min; potential is -0.45 V).

[0034] Figure 8 Cyclic voltammetry curves of graphite felt samples with different pulse times (scan rate 50 mV / s; potential range 0 V to -1.4 V; electrolyte 0.05 mol / L Na 2 SO 4 solution, pH=3, oxygen flow rate of 100 mL / min).

[0035] Fig. 9 (a)H of graphite felt electrode samples with different pulse times 2 O 2 Cumulative concentration curve; (b) current efficiency (electrolyte: 0.05 mol / L Na 2 SO 4 solution, pH=3; oxygen flow rate is 100 mL / min; potential is -0.45 V).

[0036] Fig.10 Cyclic voltammetry curves of samples at different time intervals (scan rate 50 mV / s; potential range 0 V to -1.4 V; electrolyte 0.05 mol / L Na 2 SO 4 solution, pH=3, oxygen flow rate of 100 mL / min).

[0037] Fig.11 is the (a)H of the graphite felt electrode sample 2 O 2 Cumulative concentration curve; (b) current efficiency (electrolyte: 0.05 mol / L Na 2 SO 4 solution, pH=3; oxygen flow rate 100 mL / min; potential -0.45 V). DETAILED DESCRIPTION

[0038] The anhydrous ethanol, hydrogen peroxide, sodium sulfate, potassium ferrocyanide and potassium titanium oxalate of the present invention were purchased from Chengdu Cologne Chemical Co., Ltd.; pyrrole was purchased from Adamas Reagent Co., Ltd. All reagents were analytically pure, and the laboratory water was ultrapure water. Graphite felt, 5 mm thick, was purchased from Tieling Shenhe Carbon Fiber Materials Co., Ltd.; calomel electrode R0232 and platinum mesh electrode Pt310 (10 mm×10 mm) were purchased from Tianjin Aida Hengsheng Technology Development Co., Ltd.

[0039] Unless otherwise specified, the raw materials and equipment used in the present invention are all known products obtained by purchasing commercially available products.

[0040] Example 1: Preparation of polypyrrole-modified graphite felt electrode of the present invention

[0041] After the graphite felt was cut into a size of 20mm×20mm×5mm, it was ultrasonically cleaned with anhydrous ethanol and ultrapure water for 1 hour respectively, and then vacuum dried at 60°C for 8 hours for use. The electrochemical polymerization of pyrrole-modified graphite felt was carried out in a three-electrode diaphragmless electrolytic cell. The working solution for the electrochemical polymerization was 50mL of an aqueous solution containing 0.05mol / L sodium sulfate and 0.2mol / L pyrrole. Under mechanical agitation, the pretreated 20mm×20mm×5mm graphite felt was used as the anode and the 10mm×10mm platinum mesh electrode was used as the cathode. Electrochemical polymerization was carried out under a constant current of 0.01A. The polymerization pulse time was 100s (t 1 ), pulse interval 120s(t 2 ), the number of pulses is 10 times (n). After the polymerization reaction is completed, the graphite felt electrode is rinsed with deionized water and dried to obtain the corresponding polypyrrole modified graphite felt sample, which is marked as n (t 1 -t 2 )-GF means 10(100-120)-GF.

[0042] Example 2: Preparation of polypyrrole-modified graphite felt electrode of the present invention

[0043] According to the preparation method of Example 1, the pulse interval time was adjusted to 240s (t 2 ), and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 10(100-240)-GF.

[0044] Example 3: Preparation of polypyrrole-modified graphite felt electrode of the present invention

[0045] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 50 s (t 1 ), the pulse number was adjusted to 20 times (n), and the other conditions remained unchanged, to obtain the corresponding polypyrrole-modified graphite felt sample, which was marked as 20(50-120)-GF.

[0046] Example 4: Preparation of polypyrrole-modified graphite felt electrode of the present invention

[0047] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 50 s (t 1 ), the pulse interval is adjusted to 240s (t 2 ), the pulse number was adjusted to 20 times (n), and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 20(50-240)-GF.

[0048] Comparative Example 1: Preparation of polypyrrole-modified graphite felt electrode

[0049] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 1000 s (t 1 ), the pulse interval is adjusted to 0s(t 2 ), the pulse number was adjusted to 1 (n), (i.e., the pulse was applied continuously for 1000 s) and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 1(1000-0)-GF.

[0050] Comparative Example 2: Preparation of polypyrrole-modified graphite felt electrode

[0051] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 50 s (t 1 ), the pulse interval is adjusted to 120s (t 2 ), and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 10(50-120)-GF.

[0052] Comparative Example 3: Preparation of polypyrrole-modified graphite felt electrode

[0053] According to the preparation method of Example 1, the pulse interval time was adjusted to 60s (t 2 ), and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 10(100-60)-GF.

[0054] Comparative Example 4: Preparation of polypyrrole-modified graphite felt electrode

[0055] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 50 s (t 1 ), the pulse interval is adjusted to 60s (t 2 ), the pulse number was adjusted to 20 times (n), and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 20(50-60)-GF.

[0056] Example 5: Preparation of polypyrrole-modified graphite felt electrode of the present invention

[0057] According to the preparation method of Example 1, the polymerization pulse time was adjusted to 200 s (t 1 ), and the other conditions remained unchanged, and the corresponding polypyrrole-modified graphite felt sample was obtained, which was marked as 10(200-120)-GF.

[0058] Comparative Example 6: Unmodified graphite felt electrode

[0059] The graphite felt was cut into a size of 20 mm × 20 mm × 5 mm, and then ultrasonically cleaned with anhydrous ethanol and ultrapure water for 1 hour, respectively, and then vacuum dried at 60 °C for 8 hours, which was recorded as GF.

[0060] The beneficial effects of the present invention are demonstrated by experimental examples below.

[0061] Experimental Example 1: Structural Characterization

[0062] 1. Experimental methods

[0063] The morphology of the graphite felt fiber before and after surface modification was obtained by scanning electron microscopy (JEOL JSM7610F, JEOL Ltd.), and the functional group composition of the fiber surface was analyzed by transmission spectrum obtained by Fourier transform infrared spectrometer (Nicolet iS50FT-IR, Thermal Fisher Scientific). The infrared transmission sample was prepared by grinding and mixing 0.12g of dry KBr and 0.01g of sample and then pressing them into sheets. The hydrophilic and hydrophobic properties of the graphite felt electrode material were measured by contact angle meter (JC2000C1, Shanghai Zhongchen Digital Technology Equipment Co., Ltd.).

[0064] 2. Experimental results

[0065] The surface of graphite felt fibers before and after polypyrrole modification was analyzed by field emission scanning electron microscopy ( Figure 1 The surface of unmodified graphite felt fibers is smooth and the fiber diameter is about 20 μm ( Figure 1 a). The polypyrrole-modified graphite felts of Comparative Example 1 and Comparative Example 2 ( Figure 1 The outer wall of the graphite felt fiber in b and c) is uniformly covered with a certain thickness of polypyrrole layer. The polypyrrole shell layer is tightly attached to the graphite felt fiber, but a strong external force can break the graphite fiber, and the polypyrrole shell layer can break and peel off from the graphite felt fiber. Figure 1 The results of Comparative Example 2 and Example 1 in d and e show that the thickness of the polypyrrole shell increases with the extension of the polymerization time. When the total polymerization time is extended from 500 s to 1000 s, the thickness increases from 240 nm to 640 nm accordingly. Figure 1 The results of Example 1 and Comparative Example 3 in e and f show that the extension of the pulse interval time increases the thickness of the polypyrrole shell layer. When the pulse interval time is extended from 60s to 120s, the thickness of the polypyrrole shell layer increases from 400nm to 640nm.

[0066] Further infrared spectroscopy analysis was performed on unmodified GF (Comparative Example 6), 1 (1000s-0s)-GF (Comparative Example 1) and 10 (100s-60s)-GF (Comparative Example 3). Figure 2 ). 1550 cm-1 was detected in both samples 1(1000s-0s)-GF and 10(100s-60s)-GF. -1 、1148cm -1 、1043cm -1 and 976cm -1The four absorption peaks correspond to the symmetrical stretching vibration peak of C=C on the pyrrole ring, the stretching vibration peak of CN, the bending vibration peak of NH, and the bending vibration peak of CH.

[17] The infrared characteristics of pyrrole structure were not detected on the unmodified GF. However, all samples showed -1 and 1386cm -1 There are infrared absorption peaks, corresponding to the stretching vibration peak of C=C in the graphite structure and the stretching vibration peak of CO on the carbon fiber surface. The analysis of infrared spectrum and scanning electron microscope shows that the graphite felt fiber has been successfully coated with polypyrrole by electrochemical polymerization. At the same time, under the same test conditions, Figure 2 The infrared absorption spectrum intensity of the 10(100s-60s)-GF sample is significantly stronger than that of the 1(1000s-0s)-GF, indicating that the polypyrrole content in 10(100s-60s)-GF is higher than that in 1(1000s-0s)-GF.

[0067] The above results show that multiple interval pulse polymerization is more conducive to the deposition and coating modification of polypyrrole on the surface of graphite felt. In addition, the extension of polymerization time and pulse interval time will affect the thickness of the polypyrrole coating shell.

[0068] Experimental Example 2: Performance Characterization

[0069] 1. Experimental methods

[0070] 1.1 Electrochemical performance and electrochemically active specific surface area determination

[0071] Using a CHI660D electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd.), the graphite felt sample was used as the working electrode, the platinum mesh was used as the counter electrode, the standard calomel electrode (SCE) was used as the reference electrode, and 0.05 mol / L Na 2 SO 4 The solution was used as the electrolyte to construct a three-electrode test system to test the oxygen reduction activity of the electrode. Before the cyclic voltammetry (CV) scan test, oxygen was passed through the electrolyte for 10 minutes to saturate the dissolved oxygen. During the test, oxygen was continuously bubbled into the electrolyte at a flow rate of 100 mL / min. The scan range was -1.4 V to 0 V (vs. SCE, all potentials are relative to the SCE electrode unless otherwise specified in this article), and the scan rate was 50 mV / s.

[0072] The electrochemical active surface area of ​​the sample is expressed as K 3 [Fe(CN) 6 ] is the probe molecule, and the peak current I obtained by cyclic voltammetry scanning in a three-electrode system p (A) is calculated by the Randles-Sevcik equation. Set A Vis the electrochemically active specific surface area per unit volume of graphite felt, cm 2 / cm 3 ; V G The volume of the graphite felt electrode used in the test, 2.0 cm 3 ; Then the electrochemical active area A = A V V G , cm 2 The electrochemical active surface area is calculated according to formula (5). The electrolyte tested is 0.01 mol / LK 3 [Fe(CN) 6 ] and 1.0 mol / L KCl mixed electrolyte solution, the scanning speed was 10 mV / s, and the scanning range was -0.3 V to 0.8 V.

[0073] I p =2.69×10 2 ×A V V G D 1 / 2 n 3 / 2 γ 1 / 2 C (5)

[0074] Where: D represents the diffusion coefficient of the probe molecule, which is 7.6×10 -6 cm 2 / s; n = 1, the number of electron transfers in the electrode reaction; γ is the potential scanning rate, 10 mV / s; C is the concentration of the probe molecule, 10 -5 mol / cm 3 .

[0075] 1.2 Oxygen reduction activity test

[0076] The oxygen reduction reaction experiment was carried out in an electrolytic cell without a diaphragm, with a Luggin capillary as a salt bridge connected to a standard calomel electrode (SCE) as a reference electrode, polypyrrole-modified graphite felt as a working electrode, a platinum mesh electrode as a counter electrode, and an electrolyte of 0.05 mol / L Na at pH 3. 2 SO 4 Solution. Before the test, oxygen was passed for 10 minutes to saturate the dissolved oxygen. During the test, oxygen was continuously bubbled to the vicinity of the working electrode at a flow rate of 100 mL / min through a 3 mm outer diameter polytetrafluoroethylene tube. The cathode potential was controlled by an electrochemical workstation and was constant at -0.45 V (vs. SCE). 1.4 mL of sample was taken from the electrolytic cell every 30 minutes, and the H 2 O 2 The concentration was determined and the current efficiency (CE) was calculated according to formula (6).

[0077]

[0078] Where: n = 2, which is the number of electron transfers required to generate hydrogen peroxide; F is the Faraday constant, which is 96486C / mol; C H2O2 is the H in the electrolyte 2 O 2 is the concentration, mol / L; V is the volume of the electrolyte, L; i is the current, A; t is the reaction time, s.

[0079] 2. Experimental results

[0080] 2.1 Effect of polypyrrole modification on the electrochemically active specific surface area of ​​graphite felt

[0081] The electrochemically active specific surface area is an important indicator of the electrochemical performance of the electrode. 3 [Fe(CN) 6 ] was used as the probe molecule to measure the electrochemically active specific surface area of ​​each graphite felt sample by cyclic voltammetry ( Figure 3 The results show that polypyrrole modification can significantly increase the electrochemically active specific surface area of ​​graphite felt electrode. The electrochemically active specific surface area of ​​polypyrrole-modified graphite felt material first increases with the polymerization pulse time (t 1 ) increases first and then decreases with the extension of the polymerization pulse time. When the polymerization pulse time is 100-200s (Example 1, Comparative Example 5), the electrochemically active specific surface area is greater than that of the unmodified graphite felt (Comparative Example 5), and the electrochemically active specific surface area of ​​Example 1 is significantly higher than that of Comparative Example 5. From the perspective of the total polymerization time, it also shows a trend of first increasing and then decreasing: when the total polymerization time is 1000s (Example 1, Comparative Example 1), the electrochemically active specific surface area is higher than that of the total polymerization time of 500s and 2000s. Therefore, it is appropriate to take the polymerization pulse time as 100s and the total polymerization time as 1000s. The electrochemically active specific surface area of ​​the obtained sample 10 (100s-120s)-GF (Example 1) is the largest, reaching 1.5028cm 2 / cm 3 .

[0082] The effect of different pulse intervals on the electrochemically active specific surface area of ​​polypyrrole-modified graphite felt was further investigated. Figure 4 It shows that under the conditions of the same polymerization pulse time and total polymerization time, the electrochemically active specific surface area will first increase and then decrease with the extension of the pulse interval time. When the pulse interval time is 120-240s (Examples 1-4), the electrochemically active specific surface area is greater than that of the material with a pulse interval time of 60s (Comparative Examples 3-4). When the pulse interval time is 120s, the corresponding specific surface area is the largest.

[0083] 2.2 Effect of polypyrrole modification on the oxygen reduction activity of graphite felt electrode

[0084] In the dissolved oxygen saturated Na2 SO 4 The cyclic voltammetry curve of graphite felt sample was measured in solution ( Figure 5 ). The results show that the modification of polypyrrole causes the starting potential of the oxygen reduction reaction to shift toward the positive potential direction. The starting potentials of the oxygen reduction reaction on GF (Comparative Example 6), 1 (1000s-0s)-GF (Comparative Example 1) and 10 (100s-120s)-GF (Example 1) are -0.5V, -0.45V and -0.2V, respectively. 1 (1000s-0s)-GF and 10 (100s-120s)-GF show a wide current peak response in the range of -0.3V to -0.9V, which mainly corresponds to the two-electron oxygen reduction reaction, i.e., H 2 O 2 The electrochemical generation process of polypyrrole-modified graphite felt electrode showed stronger two-electron oxygen reduction reaction activity. Among them, 10(100s-120s)-GF had the largest current response and the highest two-electron oxygen reduction activity.

[0085] 2.3 Effect of electrochemical polymerization modification process conditions on the electrochemical properties of graphite felt electrodes

[0086] 2.3.1 Effect of pyrrole deposition amount (pyrrole coating thickness)

[0087] In the range of -0.2V to -0.5V, it corresponds to the two-electron oxygen reduction reaction, namely H 2 O 2 The electrochemical generation process, in the range of -0.9V to -1.1V, corresponds to the 4-electron oxygen reduction reaction, that is, H 2 The generation process of O. Figure 6 It can be found that in the range corresponding to the two-electron oxygen reduction reaction, the current response of sample 10(50s-120s)-GF (Comparative Example 2) is higher than that of 10(100s-120s)-GF (Example 1), 10(200-120s)-GF (Comparative Example 5), and GF (Comparative Example 6), and the current response decreases with the increase of polymerization time. Figure 1 It can be seen that with the increase of polymerization time, the amount of pyrrole deposition increases, the polypyrrole film layer on the graphite felt surface becomes thicker, the resistance of the sample becomes larger, and the current response gradually decreases. For sample 10(50s-120s)-GF, the current response is also strong in the range of -0.9V to -1.1V, indicating that sample 10(50s-120s)-GF promotes the two-electron oxygen reduction reaction and its competitive reaction, namely the four-electron oxygen reduction reaction. Therefore, H 2 O 2 The growth trends of output and current response are different.

[0088] Specifically, H 2 O2 The growth of production can be seen from Figure 7 It can be seen that the H of the unmodified graphite felt (GF, Comparative Example 6) 2 O 2 The accumulation rate is 8.130 mol / m 3 Graphite felt / h, while sample 1 (1000s-0s)-GF (Comparative Example 1) H 2 O 2 The accumulation rate is 13.335 mol / m 3 This indicates that polypyrrole modification significantly improves the two-electron oxygen reduction performance of graphite felt electrode. 2 O 2 The cumulative concentration of increases first and then decreases with the extension of the pyrrole polymerization pulse time. This indicates that the coating thickness of polypyrrole can also be adjusted by the polymerization pulse time to adjust the electrochemical properties of the modified graphite felt electrode, and there is an optimal pyrrole coating thickness. In contrast, the pyrrole coating thickness is optimal when the polymerization pulse time is 100s, and H 2 O 2 The accumulation rate was the largest, reaching 25.775 mol / (h·m 3 ).

[0089] 2.3.2 Effect of polymerization pulse time on oxygen reduction activity of polypyrrole-modified graphite felt

[0090] The cyclic voltammetry curves of the modified graphite felt electrode prepared by changing the polymerization pulse time and pulse number under the condition of a certain total polymerization time were analyzed. Under the condition of a certain total polymerization time, the increase in the number of pulses represents the decrease in the polymerization pulse time. The results show that ( Figure 8 ) electrode in the potential range of -0.3V to -0.9V, the oxygen reduction response current increases with the increase of pulse number, that is, the decrease of polymerization pulse time. The shorter the polymerization pulse time, the greater the amount of pyrrole that can enter the graphite felt fiber, the thicker the polypyrrole film wrapped by the graphite felt fiber film, the higher the two-electron oxygen reduction reaction activity of the sample, and the stronger the current response.

[0091] Oxygen reduction to generate H 2 O 2 Experimental results ( Fig. 9 a) Indicates H 2 O 2 The accumulation rate of decreases with the decrease of pulse number, that is, the extension of polymerization pulse time. The more pulses there are, the shorter the polymerization pulse time is, the thicker the polypyrrole film layer on the surface of the graphite felt fiber is, the higher the two-electron oxygen reduction reaction activity of the sample is, and the H 2 O 2When the polymerization pulse time is 1000s, 100s, and 50s, the H per cubic meter of graphite felt per hour is 2 O 2 The accumulation rate is 14.645 mol / m 3 Graphite felt / h, 18.290mol / m 3 Graphite felt / h, 19.880mol / m 3 Graphite felt / h, much larger than the initial graphite felt material 8.130mol / m 3 Graphite felt / h. When the number of cycles increases from 10 to 20 and the polymerization pulse time decreases from 100s to 50s, H 2 O 2 The increase in production is not obvious. Fig. 9 b shows the current efficiency of the samples corresponding to different polymerization pulse times. It can be seen from the figure that after 2 hours, the current efficiencies of 1(1000s-0s)-GF, 10(100s-60s)-GF, and 20(50s-60s)-GF under the same conditions reached 47.57%, 56.68%, and 56.16%, respectively. The current efficiency decreases with the extension of the polymerization pulse time. The shorter the polymerization pulse time, the thicker the polypyrrole film layer on the surface of the graphite felt fiber, the greater the resistance, the greater the loss, and the lower the current efficiency. Comprehensive H 2 O 2 The cumulative concentration curve and current efficiency show that the H 2 O 2 The yield of H of the sample after 20 cycles 2 O 2 The difference in yield is small, but the former corresponds to a slightly higher current efficiency. Therefore, 10 cycles is the optimal number of cycles.

[0092] 2.3.3 Effect of interval time on electrode oxygen reduction activity

[0093] The generation of H on the polypyrrole modified graphite felt was investigated under the same polymerization pulse time and pulse number but different interval times. 2 O 2 The activity ( Fig.10 ), the results show that the electrode response current of the sample increases with the increase of the pulse interval time in the range of -0.3V to -0.9V. When the interval time increases from 60s to 120s, the pyrrole monomer is better dispersed into the graphite felt fiber under mechanical stirring, and can more evenly coat the graphite felt fiber during polymerization. The thickness of the polypyrrole film increases, and the electrochemically active specific surface area also increases. As the interval time increases, the two-electron oxygen reduction reaction activity of the sample becomes stronger, and the current response becomes stronger.

[0094] In 0.05 mol / L Na2 SO 4 The oxygen reduction reaction of the modified electrodes obtained at different time intervals to generate H 2 O 2 Performance ( Fig.11 ). The results show that ( Fig.11 a) H on the electrode 2 O 2 The accumulation rate of H increases with the increase of the interval time. When the interval time is extended from 60s to 120s, the H 2 O 2 The accumulation rate is from 18.290 mol / m 3 Graphite felt / h increased to 25.775mol / m 3 Graphite felt / h. Prolonging the pulse interval makes the two-electron oxygen reduction activity of the sample higher, H 2 O 2 The accumulated concentration increases.

[0095] According to the above analysis, the polypyrrole film thickness, resistance and current efficiency of sample 10 (100s-120s)-GF are the largest, the resistance is the largest and the current efficiency is the smallest, as shown in Figure (11b). At the same time, the pyrrole deposition is the largest and the two-electron oxygen reduction activity is the largest. The large amount of polypyrrole doping can enhance the electrochemical activity of the graphite felt sample, but also increase the resistance of the sample, increase the energy consumption and reduce the current efficiency.

[0096] In summary, the present invention effectively regulates the polypyrrole structure and electrochemical properties of the graphite felt fiber surface by adjusting the polymerization pulse time, interval time and pulse number; within the specific range of polymerization pulse time, interval time and pulse number, the prepared polypyrrole modified graphite felt electrode has excellent two-electron oxygen reduction activity and electrochemically active specific surface area, and as a redox electrode, it significantly improves H 2 O 2 The accumulation rate, especially under the conditions of polymerization time of 100 s, interval time of 120 s, and pulse number of 10 times, the polypyrrole modified graphite felt electrode has the best two-electron oxygen reduction activity and the largest electrochemical active specific surface area of ​​1.5028 cm 2 / cm 3 , and its H 2 O 2 The accumulation rate is the largest, which is 25.775 mol / m 3 Graphite felt / h, is the H on the unmodified graphite felt electrode 2 O 2 The accumulation rate is 3.17 times that of the original material, which has good application prospects.

Claims

1. A method for preparing polypyrrole modified graphite felt, characterized in that: The steps include: (1) dissolving pyrrole and sulfate in water to prepare a solution; (2) With graphite felt as anode, platinum as cathode, and the solution of step (1) as electrolyte, electrochemical polymerization is carried out under constant current conditions; polymerization pulse time: 50 to 200 s, pulse interval time: 120 to 240 s, pulse number: 10 to 20 times; total polymerization time: 1000 to 1500 s.

2. The preparation method according to claim 1, characterized in that The total polymerization time is 1000s.

3. The preparation method according to claim 2, characterized in that: Polymerization pulse time: 100 s, pulse interval: 120 s, pulse number: 10 times.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The concentration of pyrrole in the solution of step (1) is 0.1-0.3 mol / L, and the concentration of sulfate is 0.03-0.07 mol / L.

5. The preparation method according to claim 4, characterized in that: The concentration of pyrrole in the solution is 0.2 mol / L, and the concentration of sulfate is 0.05 mol / L.

6. The preparation method according to any one of claims 1 to 3, characterized in that: The constant current in step (2) is a constant current of 0.01A.

7. The preparation method according to any one of claims 1 to 3, characterized in that: The graphite felt in step (2) is pretreated as follows: the graphite felt is first ultrasonically cleaned with anhydrous ethanol, then ultrasonically cleaned with ultrapure water, and finally vacuum dried.

8. The preparation method according to claim 7, characterized in that: The anhydrous ethanol ultrasonic cleaning time is 1 hour, the ultrapure water ultrasonic cleaning time is 1 hour, and the vacuum drying is vacuum drying at 60° C. for 8 hours.

9. The preparation method according to any one of claims 1 to 3, characterized in that: The graphite felt described in step (2) has a thickness of 5 mm.

10. Polypyrrole modified graphite felt prepared by the method according to any one of claims 1 to 9.

11. Use of the polypyrrole-modified graphite felt according to claim 10 as a redox electrode.

Citation Information

Patent Citations

  • Method for preparing polypyrrole / graphene composite film material

    CN102329424A

  • Polypyrrole / graphite felt composite electrode and preparation method thereof

    CN103560017A

  • Aminated Fe3O4@SiO2 nanoparticles and application thereof in polypyrrole modified microbial fuel cell anode

    CN111463441A