Method for producing silver powder
By adjusting the micelle particle size of the surface treatment agent emulsion and selecting long-chain fatty acids in the manufacture of silver powder, the problem of poor particle size distribution of silver powder in the existing technology is solved, and the manufacture of silver powder with refined particle size and low resistance is achieved, which is suitable for Conductive paste.
Patent Information
- Application Number
- CN202180019215.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-24
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-03-22
AI Technical Summary
In existing silver powder manufacturing methods, it is difficult to completely prevent the generation of coarse silver powder particles, and it is a challenge to improve the dispersibility and sintering properties of silver powder without changing the type of surface treatment agent.
By reducing the micelle particle size in the surface treatment agent emulsion during the silver powder manufacturing process, using O/W type emulsion for surface treatment ensures that the cumulative 50% particle size D50 of the surface treatment agent's micelles is 1.5 μm or less, and is preferably used Long-chain fatty acids such as palmitic acid and stearic acid serve as surface treatment agents.
It achieves refinement of particle size distribution, suppresses the generation of coarse particles, improves the dispersibility and sintering properties of silver powder, and forms low-resistance silver powder suitable for conductive pastes.
Smart Images

Figure CN115315326B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing silver powder, and more particularly, to a method for producing silver powder suitable for use in a conductive paste for forming conductive paths in elements such as electrodes and circuits of various electronic components. Background Art
[0002] In the formation of electrodes and circuits of electronic components, resin-type and sintered silver pastes were mostly used in the past. In recent years, for conductive pastes using silver powder, there is a demand for high-density conductor patterns due to miniaturization of electronic components and thinning of wiring thickness. In addition, in order to increase the focusing area of solar cells and improve power generation efficiency, thinning of finger electrodes is also required. If coarse particles are present in the silver powder contained in the silver paste, it will cause clogging of the printing plate when forming a pattern by printing, which will cause circuit disconnection. Therefore, silver powder used for conductive paste needs to be silver powder without coarse particles.
[0003] As a method for manufacturing silver powder for conductive paste, for example, Patent Document 1 discloses a method for manufacturing silver powder having excellent low-temperature sintering properties by adding formalin as a reducing agent to an aqueous solution containing a silver ammine complex and then adding an emulsion of stearic acid that acts as a dispersant for the reduced and precipitated silver powder.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2006-002228 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In the method for producing silver powder disclosed in Patent Document 1, in order to improve the dispersibility of the silver powder precipitated by reduction, the silver powder is surface treated with stearic acid as a dispersant, and the stearic acid is added in the form of an emulsion. In the method for producing silver powder disclosed in Patent Document 1, the reason why fatty acids such as stearic acid as a surface treatment agent are added in the form of an emulsion is that the fatty acids have a high melting point and are poorly soluble in water, and are difficult to be directly and uniformly dispersed in an aqueous solution in which silver powder is dispersed. Therefore, the fatty acids are emulsified in advance, that is, an emulsion in which fine micelles of the fatty acids are dispersed in water is generated, and the emulsion is added to the slurry containing the silver powder.
[0009] However, in the production method disclosed in Patent Document 1, it was found that the generation of coarse silver secondary particles could not be completely prevented.
[0010] The sinterability of the silver paste is greatly affected by the surface state of the silver powder, especially the surface treatment agent attached to the surface of the silver powder. In addition, when the surface treatment agent attached to the surface of the silver powder is changed, the combination of the organic solvent, organic resin binder, and various additives constituting the silver paste also needs to be changed. Therefore, it is desired to improve the dispersibility of the silver powder without changing the type of the surface treatment agent, and as a result, suppress the generation of coarse silver powder particles.
[0011] That is, the technical problem to be solved by the present invention is to provide a method for producing silver powder having a smaller particle size distribution than before without changing the type of surface treatment agent of the silver powder, and a method for producing silver powder having a low resistance when the silver powder is paste-formed and an electrode is formed.
[0012] Means for solving problems
[0013] The present inventors have conducted intensive studies to achieve the above-mentioned problems and have found that the dispersibility of silver powder in a slurry containing reduced and precipitated silver powder can be improved by reducing the particle size of micelles of a surface treatment agent contained in an emulsion of the surface treatment agent added in the production process of the silver powder.
[0014] Based on the above findings, the present inventors have completed the present invention described below.
[0015] That is, in order to achieve the above-mentioned problem, the present invention provides
[0016] (1) A method for producing silver powder, comprising: using a complexing agent to convert silver ions into silver complexes, and reducing the silver complexes to obtain silver powder, comprising: a silver complexing step, wherein ammonium ions are used as a complexing agent to complex the silver ions to form a silver-ammine complex aqueous solution; a reducing step, wherein a reducing agent is added to an aqueous solution containing the silver complex, and the silver complex is reduced by the reducing agent to obtain a slurry of silver powder; and an emulsion adding step, wherein an O / W type emulsion is added to the slurry of the silver powder to perform surface treatment on the silver powder, wherein the O / W type emulsion contains a volume-based cumulative 50% particle size D obtained by a laser diffraction particle size distribution measurement method. 50 The micelles of the surface treatment agent are 1.5 μm or less.
[0017] (2) In the production method of (1) above, it is preferred that the volume-based cumulative 50% particle size D of the micelles of the surface treatment agent contained in the emulsion measured by laser diffraction particle size distribution measurement is 0.1-0.2mm / s. 50 It is less than 0.4μm.
[0018] (3) In the production method of (1) or (2) above, the surface treatment agent contained in the emulsion is preferably a linear fatty acid having 8 or more carbon atoms.
[0019] (4) In the production methods of (1) to (3) above, the surface treatment agent contained in the emulsion is preferably a long-chain fatty acid having 12 or more carbon atoms.
[0020] (5) In the production methods of (1) to (4) above, the surface treatment agent contained in the emulsion is preferably one or both of palmitic acid and stearic acid.
[0021] (6) In the production methods of (1) to (4) above, the surface treatment agent contained in the emulsion is preferably linoleic acid or linolenic acid.
[0022] Effects of the Invention
[0023] By using the production method of the present invention, it is possible to obtain silver powder having a smaller particle size distribution than conventional silver powders without changing the type of the surface treatment agent of the silver powder and having a low resistance when the silver powder is paste-formed to form an electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 1 and Comparative Example 1.
[0025] Figure 2 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 2 and Comparative Example 1.
[0026] Figure 3 This is a diagram comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Comparative Examples 1 and 2.
[0027] Figure 4 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 4 and Comparative Example 1.
[0028] Figure 5 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 6 and Comparative Example 5.
[0029] Figure 6 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 7 and Comparative Example 6.
[0030] Figure 7 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 8 and Comparative Example 7.
[0031] Figure 8 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 9 and Comparative Example 8.
[0032] Fig. 9 This is a graph comparing the measurement results of the particle size distribution of micelles contained in the emulsions obtained in Example 10 and Comparative Example 9. DETAILED DESCRIPTION
[0033] [Starting material]
[0034] In the method for producing silver powder of the present invention, a complexing agent is added to an aqueous solution containing silver (1) ions as a starting material, and an aqueous solution in which a silver complex is formed is used as a starting material. As a supply source of silver ions, an inorganic silver salt such as silver nitrate (1), silver sulfate (1), silver carbonate (1), silver chloride (1), silver oxide (1) and the like, which is known for industrial use, can be used.
[0035] Regarding the silver ion concentration in the aqueous solution, there is no particular provision in the present invention, and it is preferably 0.1% by mass or more and 10% by mass or less at the stage before the reducing agent is added as described later. If the silver ion concentration is less than 0.1% by mass, the amount of silver powder that can be manufactured by one reaction decreases, so it is not preferred. In addition, when the silver ion concentration exceeds 10% by mass, the viscosity of the reaction solution after the silver particles are precipitated increases, and it is possible that the reaction solution cannot be stirred evenly, so it is not preferred.
[0036] [Complexing agent]
[0037] As the complexing agent of silver ion, chelates such as ammonium ions such as ammonia, ammonium salts, and salts of ethylenediaminetetraacetic acid (EDTA) can be used, preferably using ammonium ions that are easy to form complexes with silver ions, easy to clean and that impurities are difficult to remain. If ammonium ion is used as complexing agent, silver-ammine complex is formed in aqueous solution. At this time, because the coordination number of ammine complex is 2, more than 2 moles of ammonium ions are added per 1 mole of silver ion.
[0038] [reducing agent]
[0039] In the method for producing silver powder of the present invention, a known reducing agent can be used to reduce the silver complex to precipitate silver in a metallic state. Examples of the reducing agent include formalin, ascorbic acid, hydrazine, alkanolamine, hydroquinone, oxalic acid, formic acid, aldehydes, alcohols, organic substances such as sugars, lower oxides of metals, sodium borohydride, etc. It is preferred to use one or more of ascorbic acid, glucose, formaldehyde, hydrazine, and hydrazine carbonate, which have stable reactivity to a certain extent and can quickly reduce silver, and among them, formaldehyde, hydrazine, or hydrazine carbonate is preferably used.
[0040] The amount of the reducing agent added is preferably 1 equivalent or more relative to silver in order to increase the yield of silver. When a reducing agent with a weak reducing power is used, it may be 2 equivalents or more relative to silver, for example, 10 to 20 equivalents.
[0041] As a method for adding the reducing agent, in order to prevent aggregation of the silver powder precipitated by reduction, it is preferred to add the reducing agent at a rate of 1 equivalent of the reducing agent / minute or more relative to the amount of silver ions. In addition, during the reduction, from before the addition of the reducing agent to the end of the reduction precipitation step, it is preferred to stir the silver-ammine complex aqueous solution and the reaction solution after the precipitation of the silver particles. In addition, the temperature when the reducing agent is added to reduce and precipitate the silver particles is preferably 5°C or more and 80°C or less, and more preferably 5°C or more and 40°C or less.
[0042] [Silver powder]
[0043] In the method for producing silver powder of the present invention, when the reducing agent is used, a volume-based cumulative 50% particle size D of 50 The silver powder has a volume-based cumulative 10% particle size D as compared to the case where the emulsion of the present invention is not used. 10 , let the cumulative 90% particle size based on volume be D 90 When (D 90 -D 10 ) / D 50 The ratio, that is, the width of the particle size distribution becomes narrower and the particle size distribution becomes smaller.
[0044] [Surface treatment agent]
[0045] In the method for manufacturing silver powder of the present invention, in order to improve the dispersibility of the silver powder precipitated by reduction, the silver powder is treated with a surface treatment agent. As the surface treatment agent, a hydrophobic dispersant is preferably used, and a fatty acid or a salt thereof can be used. By using a fatty acid or a salt thereof, the adsorption of the surface treatment agent to silver and the dispersibility between the silver particles can be taken into account. Examples of fatty acids (the number of carbon atoms in brackets) include propionic acid (3), caprylic acid (8), lauric acid (12), myristic acid (14), palmitic acid (16), stearic acid (18), behenic acid (22), acrylic acid (3), oleic acid (18), linoleic acid (18), linolenic acid (18), arachidonic acid (20), etc. In the present invention, it is preferred to use a straight-chain fatty acid with a carbon number of 8 or more, and it is further preferred to use a long-chain fatty acid with a carbon number of 12 or more, and it is further preferred to use a long-chain fatty acid with a carbon number of 16 or more, and it is more preferred to use a carbon number of 20 or less. As the surface treatment agent, it is particularly preferred to use one or both of palmitic acid (melting point: 62.9° C.) and stearic acid (melting point: 69.6° C.) Moreover, linoleic acid and linolenic acid are particularly preferred in terms of reducing the viscosity during paste formation.
[0046] This is because, when the number of carbon atoms is less than 8, it is water-soluble, so the necessity of emulsification is small, and the adsorption of the surface treatment agent to silver is weak. This is because, by making the number of carbon atoms 12 or more, it is easy to obtain the dispersibility required for silver powder. Palmitic acid and stearic acid are easily available. This is because if the number of carbon atoms exceeds 20, it becomes difficult to adjust the viscosity during paste formation. It should be noted that the commercially available fatty acids exemplified above may contain other fatty acids. For example, the reagent of stearic acid is usually not 100wt% stearic acid, but also contains other fatty acids that are difficult to separate during the manufacturing process. Therefore, the above-mentioned fatty acid used for emulsification only needs to contain the fatty acid as the main component of more than 50wt% in GC-MS analysis (also called purity of more than 50%), and may contain other fatty acids in addition to the main component.
[0047] [Lotion]
[0048] Most of the above-mentioned fatty acids used as surface treatment agents are solid at room temperature and are also poorly soluble in water. Therefore, they are added to the slurry of the reduced and precipitated silver powder in a state of pre-emulsification and liquid state, so that the surface treatment agent is attached to the surface of the silver particles. It should be noted that during emulsification, a surfactant is preferably used. As surfactants, Oledor TW-P120, Emalgen 350, Emalgen 120, etc. of Kao Corporation can be cited. In emulsification, fatty acids form micelles and are dispersed in an aqueous solution as fine droplets.
[0049] The concentration of the fatty acid in the emulsion is preferably 0.1% by mass or more and less than 50% by mass. Moreover, the concentration of the fatty acid in the emulsion in a diluted state similar to when adding to an aqueous solution in the manufacture of silver powder is preferably 0.1% by mass or more and 5% by mass or less, and more preferably 1% by mass or more and 5% by mass or less.
[0050] The method for producing silver powder of the present invention is characterized in that the volume-based cumulative 50% particle size D of micelles containing fatty acid and surfactant contained in the pre-prepared emulsion is reduced to 50 The cumulative 50% particle size D 50 Preferably, the cumulative 50% particle size D is 1.0 μm or less. 50 It is more preferably 0.7 μm or less, and in order to increase the effect of reducing coarse particles, it is further preferably 0.4 μm or less. In the present invention, the cumulative 50% particle size D of the micelle is 50 The lower limit of is not particularly specified, but is, for example, 1 nm or more. 50 The determination method is described later.
[0051] The volume-based cumulative 50% particle size D of micelles contained in the commercially available stearic acid emulsion described in Patent Document 1 was measured.50 , the result is 4.0 μm. In the method for producing silver powder of the present invention, by making the particle size of micelles smaller than before, when the emulsion containing the surface treatment agent is added to the slurry containing silver powder, the dispersion speed of the emulsion in the slurry becomes faster, and the surface treatment agent can be uniformly attached to the surface of the silver particles in the slurry, thereby improving the ability to inhibit the aggregation of the silver particles. Therefore, it is believed that by reducing the cumulative 50% particle size D of the micelles 50 The volume-based cumulative 10% particle size according to the laser diffraction method is set to 1.5 μm or less, and D 10 , the cumulative 90% particle size based on volume is set as D 90 When (D 90 -D 10 ) / D 50 The width of the numerically quantified particle size distribution is narrowed, and the particle size distribution can be reduced to make the particle size more uniform (convergent) than before. In addition, even when the silver powder is made into a conductive paste, compared with the case where a large-sized surface treatment agent is attached to the surface of the silver particles in the past, the affinity of the side with a small-sized surface treatment agent attached to the solvent, resin, additive, etc. used in the conductive paste becomes better, and as a result, it is believed that the resistance of the electrode using the conductive paste is reduced.
[0052] [Preparation method of emulsion]
[0053] Specific examples of the method for preparing the emulsion include the following three methods.
[0054] (1) The volume-based cumulative 50% particle size D of the micelles of the surface treatment agent is 50 A commercially available emulsion with a particle size of 2 μm or more (original emulsion: Celosol 920 manufactured by Chukyo Oil & Fats Co., Ltd. satisfies this condition) is used as a starting material, heated to a temperature above the melting point of the surface treatment agent contained in the emulsion and above the temperature at which the surfactant and the surface treatment agent separate, and stirred by a known stirring means until the volume-based cumulative 50% particle size D of the micelles of the surface treatment agent is 1.5 μm or more. 50 After the particle size becomes 1 μm or less, the mixture is cooled. In this case, a homogenizer is preferably used as a stirring means.
[0055] (2) The volume-based cumulative 50% particle size D of the micelles of the surface treatment agent 50 A commercially available emulsion (original emulsion) with a particle size of 2 μm or more is used as a starting material, and is kept at a temperature lower than the melting point of the surface treatment agent contained in the emulsion and at which the surfactant and the surface treatment agent are separated for more than 1 minute. After confirming that a solid of the surface treatment agent is generated in the liquid, the liquid is heated to a temperature higher than the melting point of the surface treatment agent, and stirred by a known stirring means. The volume-based cumulative 50% particle size D of the micelles of the surface treatment agent is 1.5 μm. 50After the particle size becomes 1 μm or less, the mixture is cooled. In this case, a homogenizer is preferably used as a stirring means.
[0056] It should be noted that the production method described in (2) can obtain an emulsion having a smaller micelle particle size.
[0057] (3) A surfactant is added to the above-mentioned fatty acid as a surface treatment agent, and the mixture is melted at a temperature above the melting point of each fatty acid, and then boiling water is added without solidifying the mixture, and the mixture is stirred by a known stirring means until the volume-based cumulative 50% particle size D of the micelles of the surface treatment agent is 1.25 mm / s. 50 After the particle size becomes 1 μm or less, the mixture is cooled. In this case, a homogenizer is preferably used as a stirring means.
[0058] When a surface treatment agent such as a fatty acid is emulsified, the fatty acid is combined with the surfactant to form micelles. The temperature at which the nonionic surfactant that combines with the surface treatment agent to form micelles separates from the surface treatment agent is called the cloud point. Here, the temperature at which the nonionic surfactant separates from the surface treatment agent refers to the temperature of the surface treatment agent at which the bond with the nonionic surfactant begins to be disconnected when the temperature of the emulsion is increased (in Example 2 below, it is the temperature at which the solid of the fatty acid begins to be observed). In the case of the above-mentioned surfactants, the cloud point is approximately 30 to 80°C, and the cloud point of セロゾール in the following example is 60°C.
[0059] A commercially available homogenizer can be used as the homogenizer. Preferably, the front end of the shaft has a structure including a fixed outer blade and a rotating inner blade, and the homogenizer can be finely pulverized and homogenized by the effects of ultrasonic waves, high frequencies, etc. caused between the windows of the inner blade and the outer blade, for example, the Biomixer (Model: BM-4) manufactured by Nippon Seiki Co., Ltd. can be used.
[0060] The stirring conditions of the homogenizer also depend on the amount of the emulsion to be processed. For example, for an emulsion volume of 50 mL, the rotation speed of the inner blade of the homogenizer is preferably 7000 rpm or more, more preferably 10000 rpm or more. In addition, the stirring time of the homogenizer is preferably 10 seconds or more, more preferably 1 minute or more. This is because if the stirring amount (rotation speed × time) relative to the amount of liquid is small, the micelle particle size is difficult to reduce accordingly.
[0061] In addition, the cooling method may be a conventional cooling method, such as air cooling at room temperature, slow cooling using the temperature control function of a warm bath, or water cooling, and the cooling may be to room temperature or the liquid temperature of the slurry containing silver particles in the silver powder manufacturing method described later.
[0062] [Measurement method of particle size distribution of micelles contained in emulsion]
[0063] The particle size distribution of micelles of the surface treatment agent contained in the emulsion is measured using a laser diffraction particle size distribution measuring device (e.g., Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.). The dispersion medium is pure water, and the volume-based particle size distribution measurement is performed. The cumulative 10% particle size (D 10 ), cumulative 50% particle size (D 50 ), cumulative 90% particle size (D 90 ) and cumulative 95% particle size (D 95 ), maximum particle size (D max The steepness of the particle size distribution is measured by (D 90 -D 10 ) / D 50 Than for evaluation.
[0064] In the measurement of the particle size distribution, it is preferred to measure an emulsion diluted with pure water to the same dilution ratio (eg, 10 times) as when added to an aqueous solution in the production of silver powder described later.
[0065] [Method for producing silver powder]
[0066] In an embodiment of the method for producing silver powder of the present invention, ammonium ions are added to an aqueous solution containing silver ions to form a silver-ammine complex (silver complexing step), and a reducing agent is added to the obtained silver-ammine complex aqueous solution to reduce and precipitate silver particles (reduction step). After the silver particles are reduced and precipitated by the reducing agent, a volume-based cumulative 50% particle size D of micelles of which a surface treatment agent is added to a slurry containing silver particles is 50 The surface treatment agent is attached to the surface of the silver particles by making an emulsion with a particle size of 1.5 μm or less (emulsion adding step).
[0067] The amount of fatty acid contained in the added emulsion is preferably 0.1% by mass or more and 1.2% by mass or less relative to the amount of silver in the silver-ammine complex aqueous solution. When the amount of fatty acid is less than 0.1% by mass relative to the amount of silver, the frequency of generation of coarse silver particles sometimes increases. In addition, when the amount of fatty acid exceeds 1.2% by mass relative to the amount of silver, the frequency of generation of coarse silver particles sometimes increases. It is more preferred that the amount of fatty acid contained in the added emulsion is 0.1% by mass or more and 1.0% by mass or less relative to the amount of silver in the silver-ammine complex aqueous solution, and further preferably 0.8% by mass or less.
[0068] The reducing agent may be any reducing agent that can reduce and precipitate the silver particles. As described above, one or more of ascorbic acid, glucose, formaldehyde, hydrazine, and hydrazine carbonate can be used, and formaldehyde, hydrazine, or hydrazine carbonate is preferably used.
[0069] The silver-containing slurry containing silver particles surface-treated by adding an emulsion containing micelles of a surface treatment agent after reducing and precipitating the silver particles is subjected to solid-liquid separation, and the obtained solid is washed with pure water to remove impurities in the solid component. The timing of the end of the washing can be determined based on the conductivity of the water after washing. It is preferred to wash until the conductivity of the water after washing becomes 0.5 mS / m or less.
[0070] The blocky filter cake obtained after washing contains a large amount of water, so it is preferred to use a dryer such as a vacuum dryer to obtain dry silver powder. At this time, in order to prevent the silver particles from sintering each other during the drying process, the drying temperature is preferably below 100°C. In addition, the obtained silver powder can also be subjected to dry crushing treatment and classification treatment.
[0071] [Particle size distribution measurement]
[0072] Regarding the particle size distribution of silver powder, after crushing using a sample mill SK-M10 manufactured by Kyoritsu Riko Co., Ltd., 0.1 g of silver powder was dispersed in isopropyl alcohol (IPA), stirred for 2 minutes using an ultrasonic homogenizer (model: US-150T) manufactured by Nippon Seiki Seisaku-sho, Ltd., and then measured using a laser diffraction particle size distribution measuring device (microtrack MT3300EXII manufactured by Nikkiso Co., Ltd.).
[0073] [Method for producing silver paste]
[0074] Regarding the silver paste, 86.2% by mass of the silver powder obtained in the examples and comparative examples described later, 8.0% by mass of the epoxy resin (EP4901E manufactured by ADEKA), 1.6% by mass of the curing agent (Amicura MY-24 manufactured by Ajinomoto Ficinno Co., Ltd.), and 4.2% by mass of the solvent (BCA: butyl carbitol acetate) were stirred and mixed at 1400 rpm for 30 seconds using a propeller-free autorotation-revolution stirring degassing device (AR250 manufactured by Shinky Co., Ltd.) and then kneaded using a triple roll (80S manufactured by EXAKT) with a roll gap of 100 μm to 20 μm to obtain a conductive paste.
[0075] [Screen printing]
[0076] For the conductive paste obtained by the above steps, a screen printer (MT-320T manufactured by Microtech Co., Ltd.) was used to print a line pattern of 500 μm in width and 37.5 mm in length under a squeegee pressure of 0.18 MPa to form a film of the conductive paste. For the obtained film, an atmospheric circulation dryer was used to heat and cure at 200°C for 40 minutes to form a conductive film. For each conductive film obtained, a surface roughness meter (Supcom 480B-12 manufactured by Tokyo Seimitsu Co., Ltd.) was used to measure the step height difference between the unprinted film portion and the conductive film portion on the alumina substrate, thereby measuring the average thickness of the conductive film. On the other hand, a digital multimeter (R6551 manufactured by ADVANTEST Co., Ltd.) was used to measure the resistance value of each conductive film. The volume of the conductive film was obtained from the size (film thickness, width, length) of the conductive film, and the volume resistivity was obtained from the volume and the measured resistance value.
[0077] The screen-printed substrate was embedded in a resin and polished using an ion milling device ArBlade5000 manufactured by Hitachi High-Technologies Corporation to expose a cross section, and the cross section of the conductive film was observed using a scanning electron microscope (SEM).
[0078] Example
[0079] [Comparative Example 1]
[0080] Pure water was added to 5 g of a stearic acid emulsion (Cerosol 920 manufactured by Chukyo Oil Co., Ltd., containing 82% water) as an example of a commercially available emulsion, and the total liquid volume was set to 50 mL (diluted 10 times) according to the dilution ratio during the silver powder production described later. The particle size distribution of micelles contained in the emulsion was measured using Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd. The measurement results of the particle size distribution are shown in Figure 1 .
[0081] The cumulative 10% particle size D of the micelles contained in the emulsion diluted 10 times based on volume 10 0.8μm, cumulative 50% particle size D 50 4.0μm, cumulative 90% particle size D 90 The measurement results are shown in Table 1.
[0082] 162 g of industrial ammonia water with a concentration of 28% by mass (equivalent to 5.3 molar equivalents of ammonia relative to 1 mole of silver) was added to 3327 g of silver nitrate aqueous solution containing 54 g of silver to obtain a silver-ammine complex aqueous solution. 6.0 g of sodium hydroxide aqueous solution with a concentration of 20% by mass was added to the silver-ammine complex aqueous solution, and after the liquid temperature was adjusted to 28° C., while stirring the silver-ammine complex aqueous solution, an aqueous solution obtained by adding 108 g of pure water to 250 g of formalin aqueous solution (containing 37% by mass of formaldehyde and 8% by mass of methanol) was added to reduce the silver-ammine complex, thereby obtaining a slurry containing silver particles. Furthermore, after adding 6.14 g of the product obtained by diluting the above-mentioned stearic acid emulsion 10 times to the slurry containing silver particles, stirring was stopped to allow the surface-treated silver particles to settle. The liquid in which the silver particles were precipitated was filtered, washed with water until the conductivity of the liquid after passing water became 0.2 mS / m or less, and vacuum dried at 73° C. to obtain the silver powder involved in Comparative Example 1. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 2.
[0083] [Example 1]
[0084] 5g of the commercially available stearic acid emulsion was divided into a 100mL beaker, heated to 90°C on a hot plate, and then boiling water was added to make the total liquid volume 50mL. Then, a homogenizer (Biomixer BM-4, diameter of the front end of the shaft is 32mm) manufactured by Nippon Seiki Co., Ltd. was used to stir at 10000rpm for 1.5 minutes, air-cooled for 6 hours, and cooled to room temperature to obtain the emulsion of Example 1. It should be noted that the heating temperature is above the melting point of stearic acid (melting point: 69.6°C) and palmitic acid (melting point: 62.9°C), and is above the cloud point, i.e., 60°C. For the obtained emulsion, boiling water was added in a manner such that the total liquid volume becomes 50mL relative to 5g of stearic acid emulsion, and it was diluted 10 times.
[0085] The obtained emulsion was subjected to particle size distribution measurement of micelles contained in the emulsion using Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd. The results of the particle size distribution measurement are shown in FIG. Figure 1 .
[0086] Cumulative 10% particle size D based on volume of micelles contained in the emulsion 10 0.35μm, cumulative 50% particle size D 50 The cumulative 90% particle size is 0.62 μm. 90 The peak diameter was 2.3 μm. The peak top was 0.5 μm. The measurement results are shown in Table 1. By using the above-mentioned method for preparing an emulsion, the micelles contained in the commercially available stearic acid emulsion can be refined (micronized).
[0087] The silver powder of Example 1 subjected to surface treatment was obtained by the same procedure as in Comparative Example 1 except that 6.14 g of the refined emulsion was separated and added to the slurry in which the silver powder was dispersed. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 2.
[0088] As can be seen from the results in Table 2, the silver powders of Example 1 and Example 2 described later, which were obtained by adding an emulsion with a smaller particle size, have a lower (D 90 -D 10 ) / D 50 The value is small and the peak is steep.
[0089] [Example 2]
[0090] 5g of the above-mentioned commercially available stearic acid emulsion was divided into a 100mL beaker, placed in a hot water bath (constant temperature water tank) and heated to 62.8°C, and it was confirmed that a white solid was gradually generated. This is because the cloud point of the emulsifier contained in the セロゾール is 60°C. The surface treatment agent contained in the above-mentioned commercially available stearic acid emulsion is stearic acid (melting point: 69.6°C) and palmitic acid (melting point: 62.9°C) in the fatty acid. It is heated at a temperature lower than the melting point of these fatty acids, so the combination of these fatty acids and the surfactant is cut off, and the white solid solidifies. It is believed that the white suspension is a suspension of the surfactant, the solid of the fatty acid, and the water of the solvent that covers the surface of the fatty acid when the micelle is formed. 2 minutes from the start of heating, the generation of the white solid in the white suspension will not occur further, so it is kept in this state for 5 minutes.
[0091] Then, heat to 95°C on a heater to dissolve the stearic acid and palmitic acid that have become white solids into oil droplets. While the oil droplets of the above fatty acids are floating in the white suspension, add 10 mL of boiling water using a pipette, and then add boiling water until the total liquid volume reaches 50 mL. Then, move the beaker to a hot water bath (constant temperature water tank) at 80°C, stir at 10,000 rpm for 1.5 minutes using the above homogenizer, take it out of the hot water bath and air cool it for 6 hours, and cool it to room temperature to obtain the emulsion of Example 2. The results of the particle size distribution measurement of the micelles contained in the obtained emulsion are shown in Figure 2 . Again, for comparison, Figure 2 The measurement results of Comparative Example 1 are also shown.
[0092] The volume-based cumulative 10% particle size D of the micelles according to Example 2 10 0.1 μm, cumulative 50% particle size D based on volume 50 0.2μm, cumulative 90% particle size D 90The particle size distribution of the emulsion was 0.5 μm, and a finer emulsion than that of Example 1 was obtained. The measurement results are shown in Table 1. The particle size distribution of the emulsion was measured 2 weeks after the preparation, but the particle size distribution showed almost no change.
[0093] The silver powder according to Example 2 was obtained by the same procedure as in Example 1 except that 6.14 g of the emulsion obtained by the above-mentioned procedure was separated and used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 2.
[0094] [Comparative Example 2]
[0095] 5 g of the commercially available stearic acid emulsion was taken into a 100 mL beaker, pure water was added until the total liquid volume became 50 mL, and the mixture was stirred at 10000 rpm for 1.5 minutes at room temperature using the homogenizer to obtain an emulsion of Comparative Example 2. The results of the particle size distribution measurement of the micelles contained in the obtained emulsion are shown in Figure 3 In addition, for comparison, Figure 3 The measurement results of Comparative Example 1 are also shown.
[0096] The particle size distribution of micelles contained in the obtained emulsion was measured. As a result, the volume-based cumulative 10% particle size D of the micelles was 10 The cumulative 50% particle size D on a volume basis is 0.4 μm. 50 The cumulative 90% particle size is 1.8 μm. 90 It is 10.5μm.
[0097] Compared with the particle size distribution of Comparative Example 1, although the D 50 Halved, but D 90 The results of these measurements are shown in Table 1.
[0098] [Example 3]
[0099] 125 g of industrial ammonia water with a concentration of 28% by mass (equivalent to 5.4 molar equivalents of ammonia per 1 mole of silver) was added to 3100 g of silver nitrate aqueous solution containing 41 g of silver to obtain a silver-ammine complex aqueous solution. 2.28 g of sodium hydroxide aqueous solution with a concentration of 20% by mass was added to the silver-ammine complex aqueous solution, and after the liquid temperature was adjusted to 25°C, an aqueous solution obtained by diluting 10% aqueous hydrazine with a concentration of 80% by mass with 101 g of pure water was added while stirring to obtain a slurry containing silver particles. Furthermore, 12.7 g of the emulsion obtained in Example 2 was taken from the obtained slurry containing silver particles and added and stirred. Thereafter, stirring was stopped to allow the silver particles to settle, and the liquid in which the silver particles were precipitated was filtered, washed with water until the conductivity of the liquid after water flow became less than 0.2 mS / m, and vacuum dried at 73°C to obtain the silver powder of Example 3.
[0100] [Comparative Example 3]
[0101] The silver powder according to Comparative Example 3 was obtained by the same procedure as in Example 3 except that 12.7 g of the commercially available stearic acid emulsion was diluted 10 times and used.
[0102] [Example 4]
[0103] 0.775 g of stearic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 95%) as a surface treatment agent and 0.075 g of a surfactant (Emergen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80°C to dissolve the surfactant and stearic acid. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 1.5 minutes using the above-mentioned homogenizer to obtain the emulsion of Example 4. The results of the particle size distribution measurement of the micelles contained in the obtained emulsion are shown in Figure 4 . Again, for comparison, Figure 4 The measurement results of Comparative Example 1 are also shown.
[0104] The volume-based cumulative 10% particle size D of the micelle of the emulsion 10 The cumulative 50% particle size D on a volume basis is 0.2 μm. 50 0.5μm, cumulative 90% particle size D 90 The cumulative 50% particle size D of the micelles can be obtained compared with the commercially available stearic acid emulsion. 50 The results of these measurements are shown in Table 1.
[0105] The silver powder of Example 4 was obtained in the same manner as in Example 3 except that 12.7 g of the emulsion of Example 4 was separated and used.
[0106] The particle size distribution of the silver powder obtained in Examples 3 and 4 and Comparative Example 3 was measured. In addition, a silver paste was prepared according to the manufacturing method of the above-mentioned [Method for preparing silver paste], and a conductive film was formed using the obtained silver paste according to the procedure described in the above-mentioned [Screen printing], and the volume resistivity of the conductive film was determined. These results are shown in Table 2.
[0107] From the results in Table 2, it can be seen that the silver powders of Examples 3 and 4 obtained by using an emulsion having a small micelle particle size distribution have a (D 90 -D 10 ) / D 50 The value is small and the peak is steep.
[0108] The volume resistivity of the conductive film using the silver powder obtained in Examples 3 and 4 was 56.2 μΩ·cm and 66.0 μΩ·cm, respectively, which were smaller than the volume resistivity of the conductive film using the silver powder obtained in Comparative Example 3, which was 74.0 μΩ·cm.
[0109] The cross section of the conductive film was observed by SEM, and it was found that the silver particles contained in the conductive film using the silver powder obtained in Example 3 were more densely packed than the silver particles contained in the conductive film using the silver powder obtained in Comparative Example 3. The reason for this is estimated to be that by reducing the particle size of the emulsion, not only the particle size distribution is made steeper, but also the unevenness (bias) of the surface treatment agent attached to the surface of the silver particles can be suppressed.
[0110] [Example 5]
[0111] 1.75 g of linolenic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 60%) as a surface treatment agent and 0.025 g of a surfactant (Emergen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80° C. to melt the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 1.5 minutes using the above-mentioned homogenizer to obtain an emulsion of Example 5.
[0112] The volume-based cumulative 10% particle size D of the micelle of the emulsion 10 The cumulative 50% particle size D on a volume basis is 0.57 μm. 50 The cumulative 90% particle size is 1.34 μm. 90 The particle size of the micelle was 2.93 μm, and an emulsion having a small micelle particle size could be obtained.
[0113] To 3454g of silver nitrate aqueous solution containing 52g of silver, 157g of industrial ammonia water with a concentration of 28% by mass (equivalent to 5.4 molar equivalents of ammonia relative to 1 mole of silver) was added to obtain a silver-ammine complex aqueous solution. 9.6g of sodium hydroxide aqueous solution with a concentration of 20% by mass was added to the silver-ammine complex aqueous solution, and after the liquid temperature was adjusted to 25°C, an aqueous solution obtained by diluting 13g of aqueous hydrazine with a concentration of 80% by mass with 128g of pure water was added while stirring to obtain a slurry containing silver particles. For the obtained slurry containing silver particles, 5.9g of the above-mentioned linolenic acid emulsion was taken and added and stirred. After that, the stirring was stopped to allow the silver particles to settle, and the liquid in which the silver particles were precipitated was filtered, washed with water until the conductivity of the liquid after water flow became less than 0.2mS / m, and vacuum dried at 73°C to obtain the silver powder of Example 5. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 2.
[0114] [Comparative Example 4]
[0115] The silver powder of Comparative Example 4 was obtained in the same manner as in Example 5 except that 5.9 g of a product obtained by dissolving 0.21 g of linolenic acid in 5.72 g of ethanol as a surface treatment agent was added instead of the linolenic acid emulsion of Example 5. The linolenic acid was dissolved and micelles could not be measured. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 2.
[0116] [Example 6]
[0117] 0.75 g of myristic acid (Wako Special Grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a surface treatment agent and 0.075 g of a surfactant (Emarugen 350, manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80° C. to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 3 minutes using a biomixer (model: BM-4) manufactured by Nippon Seiki Co., Ltd. to obtain micelle D 50 The particle size distribution of micelles contained in the obtained emulsion is measured and the results are shown in Figure 5 . Again, for comparison, Figure 5 The measurement results of Comparative Example 5 are also shown.
[0118] The silver powder according to Example 6 was obtained by the same procedure as in Example 3 except that 14.9 g of the emulsion was used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 3.
[0119] [Comparative Example 5]
[0120] The stirring conditions of the biomixer were set to 3000 rpm for 1.5 minutes to obtain micelles. 50The silver powder of Comparative Example 5 was obtained in the same manner as in Example 6 except that the myristic acid emulsion was changed to 8.30 μm.
[0121] [Example 7]
[0122] 1 g of lauric acid (Wako Grade 1 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a surface treatment agent and 0.5 g of a surfactant (Emarugen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80°C to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 1.5 minutes using a biomixer (model: BM-4) manufactured by Nippon Seiki Co., Ltd. to obtain micelle D 50 The particle size distribution of micelles contained in the obtained emulsion is measured and the results are shown in Figure 6 In addition, for comparison, Figure 6 The measurement results of Comparative Example 6 are also shown.
[0123] The silver powder of Example 7 was obtained by the same procedure as in Example 3 except that 9.8 g of the emulsion was used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 3.
[0124] [Comparative Example 6]
[0125] The stirring conditions of the biomixer were set to 3000 rpm for 1.5 minutes to obtain micelles. 50 The silver powder of Comparative Example 6 was obtained in the same manner as in Example 7 except that the lauric acid emulsion was changed to 3.96 μm.
[0126] [Example 8]
[0127] 1.75 g of oleic acid (NAA-34 manufactured by NOF Corporation) as a surface treatment agent and 0.525 g of a surfactant (Emarugen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80° C. to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 1.5 minutes using a biomixer (model: BM-4) manufactured by Nippon Seiki Co., Ltd. to obtain micelle D 50 The results of the particle size distribution measurement of the micelles contained in the obtained emulsion are shown in Figure 7 . Again, for comparison, Figure 7 The measurement results of Comparative Example 7 are also shown.
[0128] The silver powder of Example 8 was obtained by the same procedure as in Example 3 except that 5.6 g of the emulsion was used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 3.
[0129] [Comparative Example 7]
[0130] The stirring conditions of the biomixer were set to 3000 rpm for 1.5 minutes to obtain micelles. 50 The silver powder of Comparative Example 7 was obtained in the same manner as in Example 8 except that the oleic acid emulsion was 4.05 μm.
[0131] [Example 9]
[0132] 1.75 g of linoleic acid (manufactured by Aldrich, purity 58-74%) as a surface treatment agent and 0.525 g of a surfactant (manufactured by Kao, Emergen 350) were taken into a 100 mL beaker and heated to about 80°C to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and a biomixer (model: BM-4) manufactured by Nippon Seiki Co., Ltd. was used for stirring at 10,000 rpm for 1.5 minutes to obtain micelle D 50 The results of the particle size distribution measurement of the micelles contained in the obtained emulsion are shown in Figure 8 In addition, for comparison, Figure 8 The measurement results of Comparative Example 8 are also shown.
[0133] The silver powder of Example 9 was obtained by the same procedure as in Example 3 except that 5.6 g of the emulsion was used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 3.
[0134] [Comparative Example 8]
[0135] The stirring conditions of the biomixer were set to 3000 rpm for 1.5 minutes to obtain micelles. 50 The silver powder of Comparative Example 8 was obtained in the same manner as in Example 9 except that the linoleic acid emulsion was 3.13 μm.
[0136] [Example 10]
[0137] 1.75 g of linolenic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 60%) as a surface treatment agent and 0.025 g of a surfactant (Emargen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80°C to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and a high pressure homogenizer (LV1 type, 10 mL syringe, intermittent type) manufactured by MICROFLUIDICS Corporation was used to pass the mixture once at 138 MPa to obtain a micelle D50 The particle size distribution of micelles contained in the obtained emulsion is measured and the results are shown in Fig. 9 In addition, for comparison, Fig. 9 The measurement results of Comparative Example 9 are also shown.
[0138] The silver powder of Example 10 was obtained by the same procedure as in Example 3 except that 5.6 g of the emulsion was used. The particle size distribution of the obtained silver powder was measured. The measurement results are shown in Table 3.
[0139] [Comparative Example 9]
[0140] 1.75 g of linolenic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 60%) as a surface treatment agent and 0.025 g of a surfactant (Emargen 350 manufactured by Kao Corporation) were taken into a 100 mL beaker and heated to about 80°C to dissolve the surfactant. Boiling water was added thereto until the total liquid volume became 50 mL, and the mixture was stirred at 10,000 rpm for 1.5 minutes using a biomixer (model: BM-4) manufactured by Nippon Seiki Co., Ltd. to obtain micelle D 50 It is a linoleic acid emulsion of 4.27μm.
[0141] The silver powder of Comparative Example 9 was obtained in the same manner as in Example 10 except that the above-mentioned emulsion was used.
[0142] [Table 1]
[0143] Table 1
[0144]
[0145] [Table 2]
[0146] Table 2
[0147]
[0148] [Table 3]
[0149] Table 3
[0150]
[0151] From the above results, we can see that using D 50 When the emulsion is small, the silver powder (D 90 -D 10 ) / D 50 The ratio becomes smaller and the dispersibility of silver powder improves.
Claims
1. A method for producing silver powder, which comprises using a complexing agent to convert silver ions into silver complexes, and reducing the silver complexes to obtain silver powder, comprising: a silver complexing step, wherein ammonium ions are used as a complexing agent for complexing silver ions to form a silver-ammine complex aqueous solution; a reduction step, wherein a reducing agent is added to an aqueous solution containing a silver complex, and the silver complex is reduced by the reducing agent to obtain a slurry of silver powder; and An emulsion adding step, wherein an O / W type emulsion is added to the silver powder slurry to perform surface treatment on the silver powder, wherein the O / W type emulsion contains a cumulative 50% particle size D based on volume obtained by laser diffraction particle size distribution measurement method. 50 The micelles of the surface treatment agent are 1.5 μm or less. The surface treatment agent contained in the emulsion is a straight-chain fatty acid having 8 or more carbon atoms.
2. The method for producing silver powder according to claim 1, wherein: The volume-based cumulative 50% particle size D of the micelles of the surface treatment agent contained in the emulsion obtained by laser diffraction particle size distribution measurement method is: 50 It is less than 0.4μm.
3. The method for producing silver powder according to claim 1, wherein: The surface treatment agent contained in the emulsion is a long-chain fatty acid having 12 or more carbon atoms.
4. The method for producing silver powder according to claim 3, wherein: The surface treatment agent contained in the emulsion is one or two of palmitic acid and stearic acid.
5. The method for producing silver powder according to claim 3, wherein: The surface treatment agent contained in the emulsion is either linoleic acid or linolenic acid.