An etching method capable of controlling the side wall tilt angle of lithium niobate waveguide

Through inductively coupled plasma reactive ion etching technology combined with double-layer electron beam adhesive and metal hard mask, the sidewall inclination angle of lithium niobate waveguide is adjusted using chlorine-based gas and argon gas, solving the sidewall inclination control in the prior art Difficulties and problems of by-product LiF have achieved high steep straightness and smoothness etching effects, suitable for the manufacturing of high-length and width BAS micron structures.

CN115356806BActive Publication Date: 2024-12-06SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210926873.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-03
Publication Date
2024-12-06
Estimated Expiration
2042-08-03

AI Technical Summary

Technical Problem

In the existing lithium niobate waveguide processing methods, wet etching has anisotropy problem. Using fluorine-based gas to dry etching will generate an hindering by-product LiF, and the sidewall inclination angle cannot be effectively controlled, affecting device performance.

Method used

The inductively coupled plasma reactive ion etching technology combined with a double-layer electron beam adhesive and metal hard mask is used to adjust the sidewall inclination angle of the lithium niobate waveguide using a mixed gas of chlorine-based gas and argon, and realize it through ICP-RIE technology. Etching of high steep straightness side walls.

Benefits of technology

The fine control of the inclination angle of the sidewall of the lithium niobate waveguide is achieved, avoiding the influence of the by-product LiF, and obtaining a high straightness and smooth sidewall, suitable for the manufacturing of high-level and width sub-micron structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115356806B_ABST
    Figure CN115356806B_ABST
Patent Text Reader

Abstract

The present invention relates to an etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide, comprising: providing a pre-prepared LNOI sheet as a substrate; depositing SiO on the surface of the LNOI sheet; 2 layer, SiO as the etched waveguide layer 2 Hard mask; in SiO 2 A double layer of electron beam glue is spin-coated on the surface of the layer, and a waveguide pattern is defined on the LNOI sheet; a metal layer is deposited on the surface of the double layer of electron beam glue and in the area where the waveguide pattern is exposed, and the waveguide pattern is transferred to the metal layer as a substrate for etching SiO 2 metal hard mask of the layer; using SF 6 and O 2 Mixed gas on SiO 2 The layer is etched and the remaining metal hard mask is removed; the waveguide layer is etched using a mixture of chlorine-based gas and argon gas, and the ratio of chlorine-based gas and argon gas is adjusted to control the side wall inclination angle of the lithium niobate waveguide; the remaining SiO 2 The hard mask is then removed and cleaned using the RCA standard cleaning method to obtain the final LNOI-based lithium niobate waveguide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium niobate waveguide preparation, and more specifically to an etching method capable of controlling the inclination angle of the side wall of the lithium niobate waveguide. Background Art

[0002] Lithium niobate crystal is a multifunctional material with piezoelectric, ferroelectric, acoustic, pyroelectric, nonlinear optical, photoelectric and other properties. Silicon-based lithium niobate film heterostructure can provide material support for devices such as radio frequency filters, pyroelectric detectors, surface acoustic wave filters, and high-speed electro-optic modulators. The heterogeneous integration of silicon substrates and piezoelectric substrates such as lithium niobate can be achieved by ion beam stripping technology. It is possible to prepare lithium niobate single crystal films with submicron thickness, and then bond them to SiO2 / Si substrates to form lithium niobium on insulator films (LNOI), making it possible to mass-produce high-speed electro-optic modulators compatible with CMOS processes. In order to realize the propagation and modulation of light on LNOI chips, it is very important to etch the surface of lithium niobate films into waveguides, microring resonators, grating couplers and other devices. In addition, increasing the sidewall tilt angle of lithium niobate during the etching process can effectively improve the localization of the waveguide mode of the propagated light, and provide a method for preparing lithium niobate gratings with high aspect ratios.

[0003] However, the processing of lithium niobate waveguides with high tilt angles on the sidewalls remains an international problem. In the existing preparation methods, wet etching or dry etching is usually used for the processing of lithium niobate waveguides. In wet etching, due to the influence of the crystal orientation of lithium niobate, the etching result will show strong anisotropy, affecting the transfer of the optical structure from the mask to the lithium niobate film, and the etching rate is slow. Traditional dry etching uses fluorine-based gases (such as carbon tetrafluoride CF4, sulfur hexafluoride SF6, trifluoromethane CHF3, etc.) to etch lithium niobate, which will inevitably cause the formation of lithium fluoride (LiF), thereby hindering further etching of the lithium niobate unit. In addition, the use of fluorine-based gases cannot control the tilt angle of the sidewalls of the etched waveguide. The existing technology can use proton exchange to change the chemical ratio of lithium niobate to form new compounds to increase the etching angle of the sidewalls, but this method will cause irreversible damage to the optical properties of the material and cannot achieve high-speed electro-optical modulation.

[0004] As an electro-optical modulation device, the etching angle of the lithium niobate waveguide has a great influence on the device performance, so it is necessary to explore a new etching scheme to etch a lithium niobate pattern with steep side walls. Summary of the invention

[0005] In order to solve the above-mentioned problems in the prior art, the present invention provides an etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide, which can realize the control of the inclination angle of the side wall of the etched lithium niobate waveguide, obtain a lithium niobate waveguide with a high steep side wall, and effectively avoid the influence of the by-product LiF on the etching.

[0006] The present invention provides an etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide, comprising:

[0007] Step S1, providing a pre-prepared LNOI sheet as a substrate, wherein the LNOI sheet includes a base layer, a buried oxide layer and a waveguide layer from bottom to top;

[0008] Step S2, depositing a SiO2 layer on the surface of the LNOI wafer as a SiO2 hard mask for etching the waveguide layer;

[0009] Step S3, spin coating a double-layer electron beam gel on the surface of the SiO2 layer, and etching the double-layer electron beam gel on the LNOI wafer into a shape complementary to the waveguide pattern using electron beam lithography technology;

[0010] Step S4, depositing a metal layer on the surface of the double-layer electron beam glue and the surface of the exposed SiO2 layer, and removing the double-layer electron beam glue and the metal layer thereon, and the remaining metal layer is used as a metal hard mask for etching the SiO2 layer;

[0011] Step S5, performing inductively coupled plasma reactive ion etching on the SiO2 layer using a mixed gas of SF6 and O2 to transfer the waveguide pattern on the metal layer to the SiO2 layer and remove the remaining metal hard mask;

[0012] Step S6, performing inductively coupled plasma reactive ion etching on the waveguide layer using a mixed gas of chlorine-based gas and argon gas, and adjusting the ratio of the chlorine-based gas to the argon gas to control the sidewall inclination angle of the lithium niobate waveguide;

[0013] Step S7, removing the remaining SiO2 hard mask and cleaning it using the RCA standard cleaning method to obtain the final LNOI-based lithium niobate waveguide.

[0014] Furthermore, the method for depositing the SiO2 layer in step S2 is plasma enhanced chemical vapor deposition.

[0015] Furthermore, the method of spin coating the double-layer electron beam glue in step S3 is: firstly spin coating a layer of methyl methacrylate on the surface of the SiO2 layer, and then spin coating a layer of polymethyl methacrylate on the surface of the methyl methacrylate.

[0016] Furthermore, the method of depositing the metal layer in step S4 is physical vapor deposition.

[0017] Furthermore, in the step S6, the ratio of the chlorine-based gas to the argon gas is controlled by an etcher.

[0018] Preferably, the ratio of the chlorine-based gas to the argon gas is 50:0 sccm.

[0019] Preferably, the etching rate of the waveguide layer in step S6 is 33 nm / min.

[0020] The present invention adjusts the parameters of dry etching to achieve the control of the side wall inclination angle of the etched lithium niobate waveguide, and can obtain a lithium niobate waveguide with a high steep side wall. At the same time, the chlorine-based gas used in the present invention can effectively avoid the influence of the byproduct LiF on etching. In addition, the present invention can make the side wall smoother by adjusting the etching rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of an etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide.

[0022] Figure 2(a) to Figure 2(f) is in accordance with Figure 1 Graph showing the changing process of etching lithium niobate material using the etching method.

[0023] Figure 3 Is adopted Figure 1 A scanning electron microscope image of the etching results obtained after etching the lithium niobate material using the etching method, wherein chlorine gas:argon gas = 0:50 sccm.

[0024] Figure 4 Is adopted Figure 1 A scanning electron microscope image of the etching results obtained after etching lithium niobate material using the etching method, wherein chlorine gas:argon gas = 50:0 sccm.

[0025] Figure 5 Is adopted Figure 1 A scanning electron microscope image of the etching results obtained after etching lithium niobate material using the etching method, wherein chlorine gas:argon gas = 30:20 sccm. DETAILED DESCRIPTION

[0026] The preferred embodiments of the present invention are given below in conjunction with the accompanying drawings and described in detail.

[0027] like Figure 1 As shown, the present invention provides an etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide, comprising the following steps:

[0028] Step S1, providing a pre-prepared LNOI sheet 1, and using the LNOI sheet 1 as a substrate. As shown in FIG2(a), the LNOI sheet 1 includes a base layer 11, a buried oxide layer 12, and a waveguide layer 13 from bottom to top. The base layer 11 is made of Si, which is used as a thin film carrier; the buried oxide layer 12 is made of SiO2, which has a refractive index of 1.5, and is used to achieve a certain refractive index contrast with the waveguide layer 13 (refractive index of 2.2), so that the light is localized in the waveguide layer 13 with a larger refractive index; the waveguide layer 13 is made of lithium niobate (LN), which is used to etch photonic circuits such as waveguides to transmit and manipulate light.

[0029] Step S2, as shown in FIG2(b), a hard mask layer 2 having a certain thickness is deposited on the surface of the LNOI sheet 1. The hard mask layer 2 is preferably a SiO2 layer, which serves as a SiO2 hard mask when etching the waveguide layer 13. The thickness of the SiO2 layer depends on its anti-etching ratio with the waveguide layer 13 (i.e., the speed difference between etching SiO2 and LN during dry etching), and the depth to which the waveguide layer 13 needs to be etched. In this embodiment, the thickness of the SiO2 layer is between 400nm and 1μm, preferably 800nm. In addition, in this embodiment, the method for depositing the SiO2 layer is plasma enhanced chemical vapor deposition (PECVD).

[0030] Step S3, as shown in FIG2(c), a double-layer electron beam glue 3 is spin-coated on the surface of the deposited SiO2 layer 2, and the shape of the double-layer electron beam glue is etched on the LNOI sheet 1 to be complementary to the waveguide pattern using electron beam lithography (EBL). The double-layer electron beam glue includes methyl methacrylate (MMA) and polymethyl methacrylate (PMMA). Specifically, a layer of MMA 31 is spin-coated on the surface of the SiO2 layer, and then a layer of PMMA 32 is spin-coated on the surface of the MMA.

[0031] Step S4, as shown in Figure 2(d), a metal layer 4 with a certain thickness is deposited on the surface of the PMMA of the double-layer electron beam glue and the surface of the SiO2 layer exposed relative to the double-layer electron beam glue (i.e., the area of ​​the waveguide pattern), and the double-layer electron beam glue and the metal layer thereon are removed to transfer the waveguide pattern to the metal layer through a Lift-Off process, and the remaining metal layer is used as a metal hard mask for etching the SiO2 layer.

[0032] In this embodiment, the metal layer uses metal Cr, and its thickness depends on the etching resistance ratio of Cr and SiO2, and is between 50nm and 300nm, preferably 100nm. In addition, the method of depositing metal Cr is physical vapor deposition, including thermal evaporation, electron beam evaporation, magnetron sputtering, etc. The above-mentioned Lift-Off process is specifically: using a degumming liquid (such as acetone) to remove the remaining PMMA and MMA, thereby stripping off the metal Cr outside the waveguide pattern.

[0033] Afterwards, the SiO2 layer and lithium niobate are etched using inductively coupled plasma reactive ion etching (ICP-RIE) technology, including:

[0034] In step S5, as shown in FIG2(e), the SiO2 layer 2 is subjected to inductively coupled plasma reactive ion etching using a mixed gas of SF6 and O2 to transfer the waveguide pattern on the metal Cr layer 4 to the SiO2 layer 2 and remove the remaining metal hard mask. The ratio of SF6 and O2 can be selected as required, and the metal hard mask is removed by a chromium etching solution whose main components are ammonium cerium nitrate and glacial acetic acid.

[0035] Step S6, as shown in FIG. 2(f), uses a mixture of chlorine-based gas and argon gas to perform inductively coupled plasma reactive ion etching on the waveguide layer 13, and adjusts the ratio of the chlorine-based gas to the argon gas to control the sidewall inclination angle of the lithium niobate waveguide.

[0036] The chlorine-based gas can be Cl2, BCl3 or a mixture of the two. In the present invention, the side wall inclination angle of the waveguide can be adjusted by changing the ratio of the chlorine-based gas to the argon gas. Specifically, the side wall inclination angle of the waveguide is controlled by controlling the flow ratio of the chlorine-based gas and the argon gas using an etcher. The flow range of the argon gas is 0 to 50 sccm, and the flow range of the chlorine-based gas is 0 to 50 sccm. The ion source power and bias power of the etcher are controlled to remain unchanged. When the flow rate of the argon gas is 50 sccm and the flow rate of the chlorine-based gas is 0 sccm, as shown in FIG. Figure 3 As shown in FIG. 1 , the side wall inclination angle of the waveguide obtained by etching is approximately 60°; when the flow rate of the chlorine-based gas is 50 sccm and the flow rate of the argon gas is 0 sccm, as shown in FIG. Figure 4 As shown, the side wall inclination angle of the waveguide obtained by etching is approximately 85°; when the flow rate of the chlorine-based gas is 30 sccm and the flow rate of the argon gas is 20 sccm, the side wall inclination angle of the waveguide obtained by etching is approximately 74°. In the present invention, as the ratio of argon gas to chlorine-based gas increases, the side wall inclination angle obtained by etching becomes smaller and more inclined; as the ratio of argon gas to chlorine-based gas decreases, the side wall inclination angle obtained by etching becomes larger and steeper. Therefore, when the ratio of argon gas to chlorine-based gas is controlled to be 0:50 sccm, a lithium niobate waveguide with a highly steep side wall can be obtained.

[0037] Since a fast etching rate will cause the waveguide sidewall to be rough, it is necessary to control the etching rate by controlling the ion source power and bias power in the etcher. In this embodiment, the etching rate of the waveguide layer 13 is 33 nm / min.

[0038] It can also be seen from the above three SEM images that the morphology obtained by etching with chlorine-based gas is significantly better than that obtained by etching with fluorine-based gas, and the generation of LiF that easily hinders etching is avoided. The sidewall inclination angle of the lithium niobate waveguide etched by the present invention can be greater than 80°, providing the possibility of manufacturing a high aspect ratio sub-micron structure. Moreover, the surface roughness measured by AFM is 2.87nm (Rg), which has a very high smoothness.

[0039] In step S7, as shown in FIG. 2(f), the remaining SiO2 hard mask is removed and cleaned using the RCA standard cleaning method to obtain the final LNOI-based lithium niobate waveguide.

[0040] The SiO2 hard mask is removed by using a 10% hydrofluoric acid solution or BOE.

[0041] In order to remove the inorganic particles remaining on the surface after etching, an alkaline solution of 1:1:5 of NH4OH:H2O2:H2O is used for cleaning after etching, and the solution is heated in a water bath at 85°C for 15 minutes.

[0042] In summary, the present invention provides an etching method for controlling the side wall inclination angle of a lithium niobate waveguide, which uses ICP-RIE technology and a double-layer mask etching scheme. SiO2 is etched using metal Cr as a mask, and then the etched SiO2 is used as a mask to etch LN using a mixture of chlorine-based gas and argon gas. The side wall inclination angle of the waveguide is adjusted by changing the ratio of the working gas components, so that a side wall inclination angle greater than 80° and a surface morphology with low roughness can be obtained, which provides the possibility of manufacturing high aspect ratio sub-micron structures, and also provides an etching scheme for obtaining structures that meet specific optical design requirements.

[0043] The present invention can achieve the control of the side wall inclination angle of the etched lithium niobate waveguide by simply adjusting the parameters of dry etching, and obtain a lithium niobate waveguide with a high steep side wall. At the same time, the chlorine-based gas can effectively avoid the influence of the byproduct LiF on etching, and make the side wall smoother, thereby realizing the preparation of a device structure that is more in line with the design of photonic devices.

[0044] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. An etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide, It is characterized in that include: Step S1, providing a pre-prepared LNOI sheet as a substrate, wherein the LNOI sheet includes a base layer, a buried oxide layer and a waveguide layer from bottom to top; Step S2, depositing SiO on the surface of the LNOI sheet 2 layer, as the SiO 2 Hard mask; Step S3, in the SiO 2 Spin-coating a double-layer electron beam glue on the surface of the layer, and etching the double-layer electron beam glue on the LNOI sheet into a shape complementary to the waveguide pattern by using electron beam lithography technology; Step S4, on the surface of the double-layer electron beam glue and the exposed SiO 2 A metal layer is deposited on the surface of the layer, and the double-layer electron beam glue and the metal layer thereon are removed, and the remaining metal layer is used as the etching agent for etching the SiO 2 a metal hard mask for a layer; Step S5, using SF 6 and O 2 The mixed gas has a great influence on the SiO 2 The layer is subjected to inductively coupled plasma reactive ion etching to transfer the waveguide pattern on the metal layer to the SiO 2 layer, and remove the remaining metal hard mask; Step S6, using a mixed gas of chlorine-based gas and argon gas to perform inductively coupled plasma reactive ion etching on the waveguide layer, the flow rate range of argon gas is 0-50 sccm, the flow rate range of chlorine-based gas is 0-50 sccm, and the ratio of the chlorine-based gas to the argon gas is adjusted to control the side wall inclination angle of the lithium niobate waveguide; Step S7, removing the remaining SiO 2 The hard mask is then cleaned using the RCA standard cleaning method to obtain the final LNOI-based lithium niobate waveguide.

2. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that In step S2, SiO is deposited 2 The layer is deposited by plasma enhanced chemical vapor deposition.

3. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that The method of spin coating the double-layer electron beam glue in step S3 is: firstly 2 A layer of methyl methacrylate is spin-coated on the surface of the layer, and then a layer of polymethyl methacrylate is spin-coated on the surface of the methyl methacrylate.

4. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that The method of depositing the metal layer in step S4 is physical vapor deposition.

5. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that In the step S6, the ratio of the chlorine-based gas to the argon gas is controlled by an etcher.

6. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that The ratio of the chlorine-based gas to the argon gas is 50:0 sccm.

7. The etching method capable of controlling the inclination angle of the side wall of a lithium niobate waveguide according to claim 1, It is characterized in that The etching rate of the waveguide layer in step S6 is 33 nm / min.