Electrospinning nanofiber and its preparation method and application
By using laser and photothermal agent to control the jet temperature during electrospinning, the fiber convergence and redissolution problems caused by untimely solvent volatility are solved, and the nanofiber diameter uniformity and filter material quality factors are improved, which meets the The demand for industrial production.
Patent Information
- Application Number
- CN202211066542.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-08-31
AI Technical Summary
During electrospinning, the solvent volatilization is not timely caused by fiber confluence or redissolution, and the jet excitation is uncontrollable, resulting in the nanofiber diameter distribution being too wide and the uniformity is insufficient. Needle-free electrospinning cannot achieve uniform doping of coarse and fine fibers, affecting filtration Material quality factor.
By using laser during electrospinning, the jet is heated in segments in combination with photothermal agent in the spinning liquid, the jet temperature is controlled to achieve uniformity and stability of the spinning product, and selectively controlled heating is used for partial solution Method, precisely control the jet temperature to improve the stability of the spinning process and the quality of the product.
It has achieved good uniformity in nanofiber diameter and stable spinning process, improved the filter material quality factor, reduced equipment energy consumption, avoided solvent residue and fiber silk convergence problems, and met the needs of industrial production.
Smart Images

Figure CN115404558B_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to an electrostatic spinning nanofiber and a preparation method and application thereof. Background Art
[0002] With the development of modern science and technology, higher and higher requirements are placed on material properties. Among the materials that are rapidly developed and widely used, nanofibers have extremely broad application prospects in high-performance drives, energy engineering, filtration materials, medical hygiene and catalysis due to their unique size effect. It has become one of the important pillars driving the progress of contemporary science and technology. Therefore, higher requirements are placed on the efficient and stable preparation technology of nanofibers.
[0003] Electrospinning technology is considered to be one of the most effective means for preparing nanofibers in recent years due to its advantages such as simple manufacturing equipment and controllable process. Electrospinning is a process that uses high-voltage static electricity to charge a polymer solution. When the electric field force overcomes the surface tension and viscosity of the solution, a tiny jet will be ejected from the surface of the solution. The jet will be stretched and thinned under the action of the electric field force. As the solution evaporates, it will eventually solidify into nanofibers with diameters ranging from tens to hundreds of nanometers.
[0004] On the one hand, in electrospinning production, the random splitting of the jet during flight causes the product fiber diameter distribution to be too wide, and the microscopic morphology is poorly controllable, which limits the application of electrospinning nanofibers. There is currently no clear solution; in addition, the problem of fiber spooling or even re-dissolution caused by untimely solvent evaporation has an adverse effect on continuous production. Currently, the basic methods used to improve solvent evaporation are to replace or blend volatile solvents, increase the receiving distance, and increase the spinning environment temperature. In view of the adverse effects of untimely solvent evaporation, the scheme of replacing or blending volatile solvents will lead to a large adjustment of the spinning process parameters, and there is a question of whether the new solvent can pass the environmental assessment requirements; increasing the receiving distance requires simultaneously increasing the power supply voltage to ensure the excitation effect, and the spinning parameters will also change accordingly; increasing the spinning environment temperature will make it easier for the solute to precipitate on the online electrode or needle, resulting in the inhibition of jet excitation, which seriously reduces the stability and efficiency of spinning production.
[0005] On the other hand, in the preparation process of high-efficiency and low-resistance air filtration nanofiber filter materials, in order to solve the problem of low quality factor of nanofiber filter materials, needle electrospinning can be used to use different nozzles to spray out nanofibers mixed with coarse and fine fibers to improve the quality factor of the filter materials. However, the yield of needle electrospinning technology is too low to meet actual production needs, while the more efficient needle-free electrospinning cannot achieve uniform mixing of coarse and fine fibers.
[0006] Therefore, it is urgent to develop an electrospinning technology that can achieve uniform distribution of nanofibers, controllable solvent volatilization, high filter material quality factor and can be industrially produced. Summary of the invention
[0007] In order to overcome the problems of fiber tangling and even re-dissolution caused by untimely volatilization of the spinning product fiber solvent and uncontrollable jet excitation during the electrospinning process of the prior art, thereby causing the defects of too wide distribution of nanofiber diameters, insufficient uniformity, and low quality factor of the obtained filter material, the present invention provides an electrospun nanofiber and its preparation method and application. The preparation method provided by the present invention can realize the control of the microstructure of electrospun nanofibers, and can solve the problem of tangling and even re-dissolution of nanofiber products on the collection substrate when using conventional solvents. The obtained nanofibers have good diameter uniformity and a stable spinning process, and the quality factor of the obtained filter material is also greatly improved.
[0008] In view of the problems existing in the background technology, the inventors have continuously explored and experimentally found that compared with the spinning solution temperature and the ambient temperature, the jet temperature is the more critical factor affecting the final morphology and structure of the electrospinning product. On this basis, the present invention proposes for the first time a method for selective controllable heating of a partial solution, that is, by controlling the jet temperature during the spinning process, the temperature control during the electrospinning process is achieved, thereby controlling the morphology and structure of the electrospinning product and the stability of the spinning process. However, the jet is a dynamic process after the spinning solution is excited and before it reaches the collection substrate. It is extremely difficult to perform segmented temperature control on it, and it is difficult to achieve with the prior art.
[0009] After a lot of creative work, the inventors finally chose laser as the energy source to irradiate and heat the solidification area of the jet excited by the electric field during the electrospinning process. At the same time, a photothermal agent was added to the spinning solution to cooperate with the laser to achieve precise control of the jet temperature, thereby improving the uniformity and safety of the electrospinning products and the stability of the spinning process, solving the problems of insufficient uniformity of electrospinning products, fiber stranding and even re-dissolution in the prior art, and at the same time, obtaining nanofiber filter materials with good quality factors.
[0010] The present invention solves the above technical problems through the following technical solutions:
[0011] The present invention provides a method for preparing electrospun nanofibers, which comprises the following steps: electrospinning a spinning solution;
[0012] The spinning solution comprises a polymer, a solvent and a photothermal agent;
[0013] During the electrospinning process, laser is used to heat the jet; the heating starts in the area 20% before the end of the jet stabilization period, and in the area 20% before the end of the jet stabilization period, the jet also starts to split and stretch.
[0014] Figure 1 The figure shows a schematic diagram of the electrospinning process. In the present invention, the electrospinning process is roughly divided into three sections. The first stage is zone 1, where the spinning solution is coated on the wire electrode and the charge accumulates. The spinning solution overcomes the surface tension and viscosity under the action of the high-voltage electric field to form a jet; the second stage is zone 2, where the jet is stretched under the continuous action of the electric field force, and then split and thinned; the third stage is zone 3, which is the solidification zone, from here upward until it is blocked and collected by the substrate. In this interval, the solution evaporates quickly, forming a shell-like structure on the surface of the jet, which makes it difficult to split the jet, and then significantly reduces it. The jet stretching and thinning effect mainly occurs, and the solvent evaporation rate is significantly improved compared with the previous stage, so as to reduce the residual amount of solvent in the collected product.
[0015] In the present invention, the laser opening position may be 1 to 10 cm above the jet excitation end, for example, 2 cm, 4 cm or 8 cm.
[0016] In the present invention, the termination point of the laser may be 2 cm below the collecting substrate.
[0017] In the present invention, the polymer may be a polymer commonly used in the art, preferably one or more of a flexible polymer, an elastic polymer and a rigid polymer; the flexible polymer is preferably one or more of polyaniline, polyvinyl pyrrolidone, polyvinyl alcohol and polyvinylidene fluoride.
[0018] In the present invention, the mass content of the polymer may be 10-25%, such as 10%, 18% or 20%, wherein the percentage is the mass of the polymer to the mass of the spinning solution.
[0019] In the present invention, the photothermal agent can be a conventional substance in the art that can absorb light energy and convert it into thermal energy, preferably one or more of graphene, carbon nanotubes and indocyanine green.
[0020] In the present invention, the mass content of the photothermal agent may be 0.1% to 5%, preferably 0.5% to 4%, such as 1% or 3%, wherein the percentage is the mass of the photothermal agent to the mass of the spinning solution.
[0021] The use of photothermal agent can achieve uniform distribution of heat energy inside the jet, avoiding heat accumulation leading to partial solidification of the jet, affecting the uniformity of the spinning process and the performance of the product fiber. At the same time, it can also improve the utilization rate of the laser and avoid excessive waste of energy.
[0022] In the present invention, the solvent can be a conventional solvent in the art that can dissolve the polymer, preferably dimethylacetamide (DMAC), dimethylformamide (DMF), nitrogen methyl pyrrolidone (NMP), acetone, ethanol or water, and more preferably nitrogen methyl pyrrolidone.
[0023] In the present invention, the amount of the solvent can be 70% to 89.9%, such as 77% or 89%, wherein the percentage refers to the percentage of the mass of the solvent to the mass of the spinning solution.
[0024] In the present invention, the source of the laser can be a laser transmitter, and preferably a Kepler laser beam collector is used to constrain the laser spot diameter of the laser transmitter to be smaller than the diameter of the wire electrode and the focus is located at the lower half of the wire electrode; more preferably, the laser dot matrix of the laser transmitter is located outside the two ends of the wire electrode fixing device, the laser is output in a slit-like manner, the output power and the opening height are adjustable, and there is no height difference in the vertical direction between the lasers emitted from the left and right sides, so that the sum of the energy received by the excited jet is the same.
[0025] Turning on laser heating at the above-mentioned locations is beneficial to appropriately increase the temperature of the spinning solution and facilitate the splitting process. Since the jet has not yet started to split and stretch at this time, the specific surface area is small. Properly increasing the temperature will not cause the solvent to evaporate too quickly to form a shell layer and inhibit jet splitting. It can reduce the diameter of the initial splitting jet, and thus prevent the diameter of the collected product fiber from increasing too much. If laser irradiation is started above this point, a higher laser intensity is required, and the specific surface area of the jet increases sharply after the splitting begins. Combined with high-intensity laser irradiation, the solvent will evaporate too quickly, which will seriously inhibit the jet splitting. Finally, the fiber diameter of the nanofiber product is significantly increased and cannot meet the size requirements.
[0026] In the present invention, the intensity of the laser can be 0.4 to 7.0 w / cm 2 ; For example, 5w / cm 2 .
[0027] In the present invention, the duration of turning on and off the laser is between 0.5 and 5 seconds.
[0028] In the present invention, the voltage of the electrospinning may be 10 to 45 kV, such as 15 kV, 25 kV or 40 kV.
[0029] In the present invention, the electrospinning time may be 15 to 60 minutes, for example 30 minutes.
[0030] In the present invention, the receiving distance of the electrospinning may be 20 to 40 cm, such as 30 cm, 35 cm or 32 cm.
[0031] In the present invention, the spinning solution flow rate of the electrospinning may be 15 to 100 mL / h, such as 20 mL / h or 40 mL / h.
[0032] In one embodiment of the present invention, the spinning solution includes 0.1% to 1.5% of a photothermal agent, the laser is turned on 2 cm to 10 cm above the jet excitation end, and the termination point is 2 cm below the collecting substrate. When the laser intensity is 0.4 to 2.0 w / cm 2 between.
[0033] In one embodiment of the present invention, the spinning solution includes 0.1% to 5% of a photothermal agent, the laser is turned on 2 cm to 10 cm above the jet excitation end, and the termination point is 2 cm below the collecting substrate. When the laser intensity is 0.4 to 5.0 w / cm 2 between.
[0034] In one embodiment of the present invention, the spinning solution includes 2.5% to 5% of a photothermal agent, the laser is turned on 1 cm to 10 cm above the jet excitation end, and the termination point is 2 cm below the collecting substrate. When the laser intensity is 0.4 to 7.0 w / cm 2 The duration of laser on and off is between 0.5 and 5 seconds. If the photothermal agent content is too low, the opening position is too high, or the laser intensity is too low, the jet will not heat up enough when receiving laser irradiation, and its splitting process cannot be suppressed, and the effect of introducing coarse fibers is not good. If the laser on and off duration is too short, too few coarse fibers will be introduced, and the quality factor will not be significantly improved. If the laser on and off duration is too long, a clear coarse and fine fiber interface will be formed, and the effect of improving the quality factor is not good.
[0035] The invention also provides a nanofiber prepared by the above preparation method.
[0036] The present invention also provides a nanofiber comprising 0.1 to 5 wt% of a photothermal agent;
[0037] During the electrospinning process, under the conditions of the same heating time and the same spinning voltage, the difference between the maximum diameter and the minimum diameter of the nanofiber is 0 to 260 nm.
[0038] In the present invention, the difference between the maximum diameter and the minimum diameter of the nanofiber may be 20-210 nm, preferably 50-130 nm, such as 70 nm.
[0039] In the present invention, the nanofibers do not have an ultrafine fiber vine-like structure in their morphology.
[0040] In the present invention, the filter material quality factor of the nanofiber may be 0.1000-0.1500, for example, 0.1019.
[0041] The present invention also provides application of the nanofiber in the field of filter materials.
[0042] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0043] The reagents and raw materials used in the present invention are commercially available.
[0044] The positive and progressive effects of the present invention are:
[0045] (1) The present invention is as follows Figure 1 The area No. 3 shown provides suitable output power and conversion efficiency, improves the volatilization rate of the organic solvent in the nanofiber in this section, reduces the amount of solvent residue in the nanofiber accumulation product, and improves the mechanical properties of the nanofiber collection product. It also reduces the difficulty of the solution excitation process above the wire electrode, reduces the lower limit of the jet excitation of needle-free electrospinning, and reduces the overall energy consumption of the equipment. Compared with the overall spinning environment temperature rise, this method will not affect the jet stable excitation in area No. 1 and the jet splitting process in area No. 2, has no negative effect on the spinning process, and has low energy consumption.
[0046] (2) The jet splitting inhibition effect of different diameters under the same environment is greatly different, and finally the uniformity of fiber diameter is improved. Under the same conditions, it is impossible to achieve a good jet excitation control effect by controlling the ambient temperature, wire electrode temperature or spinning solution temperature, and it is easy to have a negative impact on other processes.
[0047] (3) In a preferred embodiment, by controlling the position and time of starting and stopping the laser, coarse and fine fibers with good doping and overlapping are obtained, with the coarse fiber diameter distributed between 520 and 730 nm and the fine fiber diameter distributed between 80 and 210 nm; and the fibers also have a relatively high quality factor. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 Schematic diagram of the electrospinning process.
[0049] Figure 2 Schematic diagram of the location structure of the laser transmitter.
[0050] Figure 3 This is an electron microscope image of the nanofibers prepared in Example 1.
[0051] Figure 4 This is an electron microscope image of the nanofibers prepared in Example 2.
[0052] Figure 5 This is an electron microscope image of the nanofiber filter material prepared in Example 3.
[0053] Figure 6 This is the electron microscope image of the nanofiber prepared in Comparative Example 1.
[0054] Figure 7This is the electron microscope image of the nanofiber prepared in Comparative Example 2.
[0055] Figure 8 This is the electron microscope image of the nanofiber filter material prepared in Comparative Example 3. DETAILED DESCRIPTION
[0056] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0057] Example 1
[0058] (1) preparing a spinning solution: dissolving 10 g of polyaniline in 89 g of nitrogen-methylpyrrolidone, adding 1 g of carbon nanotubes, and stirring to obtain a spinning solution with a uniformly dispersed polyaniline mass fraction of 10%;
[0059] (2) Preparation of nanofibers: The spinning solution is placed in a Figure 2 Electrospinning was performed in the electrospinning device equipped with a laser transmitter. The starting height of the laser source was adjusted to 8 cm above the jet excitation end and the ending point was 2 cm below the collecting substrate. The laser intensity was 2 w / cm 2 In the electrospinning process, the applied electrostatic voltage is 15 kV, the spinning solution flow rate is 20 mL / h, the receiving distance is 30 cm, and the spinning time is 30 min.
[0060] Example 2
[0061] (1) Preparation of spinning solution: 15 g of polyvinyl pyrrolidone (PVP) and 5 g of polyvinyl alcohol (PVA) were physically blended and dissolved in 77 g of distilled water, and then 3 g of indocyanine green was added and stirred to obtain a spinning solution with a uniformly dispersed PVP-PVA mass fraction of 20%;
[0062] (2) Preparation of nanofibers: The spinning solution is placed in a Figure 2 The electrospinning is performed in the electrospinning device equipped with a laser transmitter. The starting height of the laser source is adjusted to 4 cm above the jet excitation end. The laser intensity here is 0 w / cm 2 The laser intensity increases proportionally in the vertical direction and reaches a maximum value of 4.5w / cm at 10cm above the wire. 2 , and then the intensity stabilized to the end point, that is, collecting 2 cm below the substrate to obtain nanofibers. During the electrospinning process, the applied electrostatic voltage was 25 kV, the spinning solution flow rate was 40 mL / h, the receiving distance was 35 cm, and the spinning time was 30 min.
[0063] Example 3
[0064] (1) Preparation of spinning solution: 18 g of polyvinylidene fluoride (PVDF) was dissolved in 77 g of dimethylacetamide, and 5 g of nanographene was added and stirred to obtain a spinning solution with a mass fraction of 18% of uniformly dispersed PVDF;
[0065] (2) Preparation of nanofiber filter material: The above spinning solution is placed in a Figure 2 Electrospinning is performed in an electrospinning device equipped with a laser transmitter. The laser dot matrix start position is 2 cm above the jet excitation end, and the end point is 2 cm below the collection substrate. The laser intensity is 6.0 w / cm 2 , the laser is turned on and off for 2s, and the nanofiber filter material is obtained. In the electrostatic spinning process, the applied electrostatic voltage is 40kV, the spinning solution flow rate is 50mL / h, the receiving distance is 32cm, and the spinning time is 30min. Comparative Example 1
[0066] (1) preparing a spinning solution: dissolving 10 g of polyaniline in 90 g of nitrogen methyl pyrrolidone to obtain a spinning solution having a polyaniline mass fraction of 10%;
[0067] (2) Preparation of nanofibers: The spinning solution is subjected to electrospinning in a conventional electrospinning device to obtain nanofibers; during the electrospinning process, the applied electrostatic voltage is 15 kV, the spinning solution flow rate is 20 mL / h, the receiving distance is 30 cm, and the spinning time is 30 min.
[0068] Comparative Example 2
[0069] (1) Preparation of spinning solution: 15 g of polyvinyl pyrrolidone (PVP) and 5 g of polyvinyl alcohol (PVA) were physically blended and dissolved in 80 g of distilled water to obtain a spinning solution with a PVP-PVA mass fraction of 20%;
[0070] (2) Preparation of nanofibers: The spinning solution was electrospun in a conventional electrospinning device to obtain nanofibers; during the electrospinning process, the applied electrostatic voltage was 25 kV, the spinning solution flow rate was 40 mL / h, the receiving distance was 35 cm, and the spinning time was 30 min.
[0071] Comparative Example 3
[0072] (1) Preparation of spinning solution: 18 g of polyvinylidene fluoride (PVDF) was dissolved in 82 g of dimethylacetamide to obtain a spinning solution with a PVDF mass fraction of 18%;
[0073] (2) Preparation of nanofiber filter material: The above spinning solution was electrospun in a conventional electrospinning device to obtain the nanofiber filter material. During the electrospinning process, the applied electrostatic voltage was 40 kV, the spinning solution flow rate was 50 mL / h, the receiving distance was 32 cm, and the spinning time was 30 min.
[0074] Effect Example 1
[0075] To use Figure 1 The nanofibers produced by the electrospinning device with the structure shown were characterized.
[0076] Figure 3 This is an electron microscope image of the nanofiber prepared in Example 1; it can be observed that the fibers are no longer bonded but only overlapped, and there is no fiber-coupling phenomenon, which is an ideal microstructure. The measured solvent residue is less than 1ppm, which meets the safety detection standards.
[0077] Figure 6 This is an electron microscope image of the nanofiber prepared in Comparative Example 1; since the high boiling point solvent will cause a large amount of unvolatile solvent to exist during the spinning process, this will cause the product fiber to have problems such as doubling and partial bonding. Figure 6 As shown, the quality and microstructure of the spinning product are seriously affected, and the product has a high level of residual solvent and cannot pass the safety test.
[0078] Figure 4 This is an electron microscope image of the nanofibers prepared in Example 2; it can be observed that the fibers are uniform and have no bifurcations, are distributed between 210 and 280 nm, have no ultrafine fiber vine-like structure, and the uniformity of the fiber diameter is significantly improved.
[0079] Figure 7 This is an electron microscope image of the nanofibers prepared in Comparative Example 2; the diameters of the nanofibers are distributed between 50 and 450 nm, and there are a large number of ultrafine fiber vine-like structures. This structure easily leads to unstable mechanical properties and poor uniformity of the formed fiber membrane, which is not the expected product morphology.
[0080] Figure 5 This is an electron microscope image of the nanofiber filter material prepared in Example 3; it can be observed that the coarse fiber diameter is distributed between 520 and 730 nm, the fine fiber diameter is distributed between 80 and 210 nm, the coarse fibers and the fine fibers are well mixed and overlapped, and no obvious coarse and fine fiber hierarchical structure is observed.
[0081] Figure 8 This is an electron microscope image of the nanofiber filter material prepared in Comparative Example 3; it can be observed that the fiber distribution range is between 70 and 180 nm, and the fibers are relatively thin.
[0082] Research has found that if the photothermal agent content is too high, the opening point is too low, or the laser intensity is too high, although relatively uniform nanofibers can be obtained, the fiber diameter is too large and cannot meet the initial product requirements; if the photothermal agent content is too low, the opening point is too high, or the laser intensity is too low, the temperature will not rise enough and the fiber diameter uniformity cannot achieve the ideal effect.
[0083] Effect Example 2
[0084] Filtration performance test: carried out according to EN1822 European standard test method.
[0085] The quality factor is calculated as:
[0086]
[0087] Where:
[0088] Q—quality factor; α—filtration removal efficiency for PM0.3; △P—filtration pressure drop of filter material.
[0089] The nanofiber filter material prepared in Comparative Example 3 has a particle removal rate of 99.84%, a pressure drop of 75 Pa, and a quality factor of 0.0825.
[0090] The particle removal rate of the nanofiber filter material prepared in Example 3 is 99.82%, the pressure drop is 62Pa, and the quality factor is 0.1019. The quality factor of the nanofiber filter material obtained in Example 3 is significantly improved compared with that of the nanofiber filter material obtained in Comparative Example 3. This can be attributed to the fact that the nanofiber membrane overlapped by coarse and fine fibers has a lower stacking density, which reduces collisions when air passes through the filter material, thereby reducing the pressure drop.
[0091] In summary, the present invention solves the defects of the prior art in that excessive solvent residue leads to fiber tangling and even redissolution and the fiber diameter distribution of needle-free electrospinning products is too wide through the interaction of laser and photothermal agent. The nanofibers prepared from the same solid content solution (such as Example 2 and Comparative Example 2) have a diameter distribution of 50 to 450 nm before using the preparation method, and the diameter distribution of the nanofibers obtained after applying the method is 210 to 280 nm, and the quality factor of the nanofiber filter material is greatly improved.
Claims
1. A method for preparing electrospun nanofibers, characterized in that: It includes the following steps: The spinning solution is subjected to electrostatic spinning; The spinning solution comprises a polymer, a solvent and a photothermal agent; During the electrospinning process, laser is used to heat the jet; the heating starts in the area 20% before the end of the jet stabilization period, and in the area 20% before the end of the jet stabilization period, the jet does not start to split and stretch; The laser opening position is located 1 to 10 cm above the jet excitation end; The mass content of the photothermal agent is 0.1%~5%; The laser is turned on and off for a duration of 0.5 to 5 seconds; The intensity of the laser is 0.4~7.0 w / cm 2 .
2. The method for preparing electrospun nanofibers according to claim 1, characterized in that: The polymer is one or more of a flexible polymer, an elastic polymer and a rigid polymer; And / or, the photothermal agent is one or more of graphene, carbon nanotubes and indocyanine green; And / or, the solvent is dimethylacetamide, dimethylformamide, nitrogen methyl pyrrolidone, acetone, ethanol or water.
3. The method for preparing electrospun nanofibers according to claim 2, characterized in that: The flexible high molecular polymer is polyaniline, polyvinyl pyrrolidone, polyvinyl alcohol and polyvinylidene fluoride; And / or, the solvent is nitrogen methyl pyrrolidone or water.
4. The method for preparing electrospun nanofibers according to claim 1, characterized in that: The mass content of the polymer is 10-25%, wherein the percentage is the mass fraction of the polymer relative to the mass fraction of the spinning solution; And / or, the mass content of the photothermal agent is 0.5% to 4%, wherein the percentage is the mass fraction of the photothermal agent relative to the mass fraction of the spinning solution; And / or, the amount of the solvent used is 70% to 89.9%, wherein the percentage is the percentage of the mass of the solvent to the mass of the spinning solution.
5. The method for preparing electrospun nanofibers according to claim 4, characterized in that: The mass content of the polymer is 10%, 18% or 20%; And / or, the mass content of the photothermal agent is 1% or 3%; And / or, the amount of the solvent used is 77% or 89%.
6. The method for preparing electrospun nanofibers according to claim 1, characterized in that: The source of the laser is a laser transmitter.
7. The method for preparing electrospun nanofibers according to claim 6, characterized in that: The source of the laser is a Kepler-type laser beam collector that constrains the laser spot diameter of the laser transmitter to be smaller than the diameter of the wire electrode and the focus is located at the lower half of the wire electrode.
8. The method for preparing electrospun nanofibers according to claim 7, characterized in that: The laser dot matrix of the laser transmitter is located outside the two ends of the wire electrode fixing device, the laser is output in a slit-like manner, the output power and the opening height are adjustable, and there is no height difference in the vertical direction between the lasers emitted from the left and right sides.
9. The method for preparing electrospun nanofibers according to any one of claims 6 to 8, characterized in that: The laser start position is 2 cm, 4 cm or 8 cm above the jet excitation end; and / or the laser end position is 2 cm below the collection substrate; And / or, the intensity of the laser is 5 w / cm 2 .
10. The method for preparing electrospun nanofibers according to claim 1, characterized in that: The voltage of the electrospinning is 10-45 kV; And / or, the electrospinning time is 15 to 60 min; And / or, the receiving distance of the electrospinning is 20 to 40 cm; And / or, the spinning solution flow rate of the electrospinning is 15-100 mL / h.
11. The method for preparing electrospun nanofibers according to claim 10, characterized in that: The voltage of the electrospinning is 15 kV, 25 kV or 40 kV; And / or, the electrospinning time is 30 min; and / or, the receiving distance of the electrospinning is 30 cm, 35 cm or 32 cm; And / or, the spinning solution flow rate of the electrospinning is 20 mL / h or 40 mL / h.
12. The method for preparing electrospun nanofibers according to claim 1, wherein: The spinning solution includes 0.1% to 5% of a photothermal agent. The laser is turned on 2 cm to 10 cm above the jet excitation end, and the end point is 2 cm below the collecting substrate. The laser intensity is 0.4 to 5.0 w / cm 2 between; Alternatively, the spinning solution includes 0.1% to 1.5% of a photothermal agent, the laser is turned on 2 cm to 10 cm above the jet excitation end, the end point is 2 cm below the collecting substrate, and the laser intensity is 0.4 to 2.0 w / cm 2 between; Alternatively, the spinning solution includes 2.5% to 5% of a photothermal agent, the laser is turned on 1 cm to 10 cm above the jet excitation end, the end point is 2 cm below the collecting substrate, and the laser intensity is 0.4 to 7.0 w / cm 2 The laser is turned on and off for a period of 0.5 to 5 seconds.
13. A nanofiber obtained by the preparation method according to any one of claims 1 to 12.
14. A nanofiber according to claim 13, characterized in that The components include 0.1-5wt% of a photothermal agent; during the electrospinning process, under the conditions of the same heating time and the same spinning voltage, the difference between the maximum diameter and the minimum diameter of the nanofiber is 0-260nm.
15. Use of the nanofiber according to claim 13 or 14 in the field of filter materials.