Rubber mixture with improved properties

By using a large amount of 1,2-vinyl non-functionalized liquid polybutadiene in the rubber mixture, the changes in the characteristics of rubber products caused by plasticizer migration are solved, and the tensile strength of rubber products and the rolling resistance of tires are improved. Performance, achieving low fuel consumption and good winter driving performance.

CN115485329BActive Publication Date: 2024-11-26EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180033090.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-04
Filing Date
2021-04-12
Publication Date
2024-11-26
Estimated Expiration
2041-04-12

AI Technical Summary

Technical Problem

Plasticizers used in existing rubber mixtures migrate over time, resulting in changes in the characteristics of rubber products such as increased hardness and deterioration of elasticity, and their use leads to deterioration of tire rolling resistance and increased fuel consumption.

Method used

Using a large amount of 1,2-vinyl non-functionalized liquid polybutadiene with an average molecular weight of 1500 to 5000 g/mol, as part of the rubber mixture, rubber products are prepared by vulcanization, improving the processing characteristics of the rubber and tires Dynamic mechanical properties.

Benefits of technology

Improves the processing characteristics of the rubber mixture and the tensile strength and elongation of the vulcanized rubber products, reduces the rolling resistance and wear of the tires, improves the performance of driving in winter and snow, and reduces fuel consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003926051950000041
    Figure BDA0003926051950000041
  • Figure BDA0003926051950000051
    Figure BDA0003926051950000051
  • Figure BDA0003926051950000111
    Figure BDA0003926051950000111
Patent Text Reader

Abstract

The present invention relates to a rubber mixture comprising rubber and liquid polybutadiene, which is liquid at a temperature of 20° C. and a pressure of 98.0665 kPa, wherein the liquid polybutadiene consists only of C- and H-atoms and has an average molecular weight (Mw) of 1500 to 5000 g / mol as determined by gel permeation chromatography as described in the present specification; to a method for preparing a rubber product by vulcanization using the rubber mixture of the present invention as a raw material; and to a rubber product obtained by the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber mixture comprising rubber and liquid polybutadiene which is liquid at a temperature of 20° C. and a pressure of 98.0665 kPa, wherein the liquid polybutadiene consists only of C- and H-atoms and has an average molecular weight (Mw) of 1500 to 5000 g / mol as determined by gel permeation chromatography as described in the present specification; to a method for preparing a rubber product by vulcanization using the rubber mixture of the present invention as a raw material; and to a rubber product obtained by the method. Background Art

[0002] So-called "green tires" are a trend in the automotive industry. The main goals are to reduce rolling resistance and therefore fuel consumption, improve wet grip, while keeping wear resistance constant. Adding precipitated silica to the formulation can achieve this goal, but the silica employed shows poor compatibility with the rubber matrix. This problem is currently being improved by adding silanes as compatibilizers. The covalent bonding between the filler and the polymer makes the wear level of silica-filled tires consistent with that of carbon black-filled tires.

[0003] Thus, JP 2008-031244 discloses a tire tread rubber composition consisting of at least either natural rubber or synthetic rubber and a filler component consisting of silica alone or of silica and carbon black, wherein the silica consists of at least amorphous spherical silica particles having an average particle size of 0.05 to 1.00 μm.

[0004] JP 2015-083649, US 20140121316 or EP 2266819 describe the functionalization of anionically polymerized polybutadiene. EP 1479698 describes the functionalization of polybutadiene having a vinyl content of less than 2%.

[0005] EP 2818505 proposes rubber mixtures in which diene rubbers are reacted with acrylamide and / or with silane- or tin-modified acrylamides. The preparation of the systems described in the prior art is highly complex.

[0006] WO 2019 / 044888 A1 (EP 3677637 A1) describes a rubber composition comprising a modified liquid polybutadiene comprising functional groups such as hydroxyl groups, having a vinyl content of less than 70% and an Mw of 1000 to 15000 g / mol.

[0007] WO2019 / 044889 A1 (EP 3677635 A1) describes a rubber composition comprising a diene-based modified liquid rubber comprising functional groups derived from silane compounds, having a vinyl content of less than 70% and an Mw of 15,000 to 120,000 g / mol.

[0008] WO2019 / 044893 A1 (EP 3677638 A1) describes a rubber composition for heavy-load tires comprising a diene-based modified liquid rubber, the diene-based modified liquid rubber comprising functional groups derived from silane compounds, having a vinyl content of 30% to less than 70% and an Mw of 1000 to 120000 g / mol.

[0009] JP 2019094463 A describes a rubber composition for tires and pneumatic tires comprising a liquid polybutadiene having a vinyl content of greater than 80% and an Mw of 1000 to 18000 g / mol, most preferably 1000 to 5000 g / mol.

[0010] DE 10 2015 210424 A1 describes a rubber composition comprising a modified liquid polybutadiene rubber containing silicone end groups, having a vinyl content of less than 70% and an Mw of 500 to 12 000 g / mol and a plasticizer.

[0011] EP 1 035 164 A1 describes a rubber composition for tire treads comprising a liquid polybutadiene having a vinyl content of about 85% and an Mw of 4700 g / mol.

[0012] JP 2009 203288 A describes a rubber composition comprising a liquid polybutadiene having a vinyl content of less than 50% and an Mw of 2000 to 10000 g / mol. The composition further comprises an ester plasticizer.

[0013] WO 2019 / 044891 A1 (US 2020 / 207957 A1) describes a rubber composition comprising a diene-based modified liquid rubber comprising functional groups derived from silane compounds, having a vinyl content of less than 70% and an Mw of 15,000 to 120,000 g / mol.

[0014] US 2018 / 072874 A1 describes a rubber composition comprising a diene-based modified liquid rubber comprising a functional group derived from a carboxyl-containing nitrone compound.

[0015] Many rubber mixtures used in the rubber and tire industry contain plasticizers in order to make processing easier and to adjust the mechanical and dynamic mechanical properties according to the requirements of the end-use application.

[0016] A significant disadvantage of using plasticizers is that they tend to migrate out of articles made from (vulcanized) rubber over time. As a result, the properties of the rubber article also change over time.

[0017] Externally perceptible indicators of this effect are, for example, an increase in hardness and / or embrittlement of the vulcanized rubber, which is accompanied by a deterioration in elasticity.

[0018] Many plasticizer oils contain high amounts of aromatic compounds. Currently, there is a high demand to reduce or even eliminate such materials in rubber applications for environmental and health reasons.

[0019] In order to solve this type of problem and challenge, reactive plasticizers are often used. A kind of reactive plasticizer is for example liquid polybutadiene (see for example US 7,411,018 B2). Reactive plasticizers improve the processing of rubber mixtures, and additional advantage is that they react with other parts of this rubber mixture, and therefore can not migrate from vulcanized rubber products basically.

[0020] However, if a tire is equipped with a tread based on a rubber mixture containing such a reactive plasticizer, the use of the reactive plasticizer results in a tire having deteriorated rolling resistance and higher fuel consumption.

[0021] There is therefore a need for improved rubber mixtures which are obtainable in a simple manner and which exhibit improved properties. Summary of the invention

[0022] When comparing the use of different liquid polybutadienes, the inventors surprisingly found that liquid polybutadienes comprising a large amount of 1,2-vinyl groups not only improve the processing of such rubber mixtures, but also improve the rolling resistance of tires (treads) made from the rubber mixtures.

[0023] The present invention therefore relates to a rubber mixture comprising rubber and a liquid polybutadiene which is liquid at a temperature of 20° C. and a pressure of 98.0665 kPa, wherein the liquid polybutadiene consists exclusively of C- and H-atoms and has an average molecular weight (Mw) of 1500 to 5000 g / mol as determined by gel permeation chromatography as described in the present description and contains a large amount of 1,2-vinyl groups (as claimed in the claims).

[0024] The invention also relates to a method for producing a rubber product by vulcanization using the rubber mixture of the invention as a raw material.

[0025] The invention further relates to a rubber article obtainable by the process according to the invention.

[0026] The rubber mixtures according to the invention have very good processing properties, which are manifested by very good dynamic mechanical properties.

[0027] The rubber articles obtained by vulcanization using the rubber mixture of the invention as raw material have the advantage that they exhibit high tensile strength values ​​as well as high elongation at break values.

[0028] The advantage of the tires or tire treads obtained by processing and vulcanizing the rubber mixture according to the invention is that they show good rolling resistance, low wear and good winter / snow driving characteristics. The advantage of low rolling resistance is that the use of such tires helps to reduce the fuel consumption of vehicles. DETAILED DESCRIPTION

[0029] Mixtures, methods and products / uses according to the present invention are described hereinafter by way of example, without any intention to limit the present invention to these exemplary embodiments. When the scope, general formula or category of the compound are described below, these are intended to not only cover the corresponding scope or group of the compound explicitly mentioned, but also cover all sub-scopes and sub-groups of the compound that can be obtained by omitting a single value (scope) or compound. In the case of citing documents in the context of this specification, their contents, especially with regard to the relevant circumstances mentioned herein, should fully constitute a part of the disclosure of the present invention. Unless otherwise noted, the percentages described hereinafter are by weight. In the case of reporting average values ​​hereinafter, unless otherwise noted, these are numerical average values. In the case of mentioning the properties of materials such as viscosity, etc. hereinafter, unless otherwise noted, these are the properties of materials at 25 ° C. In the case of using chemical (empirical) formulas in the present invention, the specified index can be not only an absolute value, but also an average value.

[0030] The present invention relates to a rubber mixture comprising rubber and liquid polybutadiene, the polybutadiene being liquid at a temperature of 20° C. and a pressure of 98.0665 kPa, wherein the liquid polybutadiene comprises monomer units derived from 1,3-butadiene

[0031]

[0032] and

[0033]

[0034] And wherein the proportion of A in all the monomer units derived from 1,3-butadiene present in the liquid polybutadiene is 55 to 70 mol%, and wherein the sum of the proportions of B and C in all the monomer units derived from 1,3-butadiene present in the liquid polybutadiene is 30 to 45 mol%, and the liquid polybutadiene consists only of C- and H-atoms and has an average molecular weight (Mw) of 1500 to 5000 g / mol as determined by gel permeation chromatography as described in the present specification.

[0035] Liquid polybutadiene consists only of C- and H-atoms. Therefore, preferred liquid polybutadiene is non-functionalized polybutadiene. Liquid polybutadiene preferably has an average molecular weight (Mw) of 1750 to 3500 g / mol as determined by gel permeation chromatography (as described in the Examples section below).

[0036] The liquid polybutadiene preferably has a viscosity at 23° C. of 1000 to 12000 mPas, more preferably 3000 to 9000 mPas, most preferably 5000 to 7000 mPas, measured as described in the Examples section.

[0037] Suitable liquid polybutadiene can be obtained by catalytic polymerization as described in WO 2018130703 A1 (EP 3348589 B1), in particular in Examples 1 to 3.

[0038] The rubber mixture according to the invention may additionally comprise one or more rubbers, one or more fillers, preferably precipitated silica and / or silanes, preferably carbon black, and optionally further rubber additives.

[0039] Fillers that can be used in the rubber mixture of the present invention include, for example:

[0040] - Carbon black: The preferred carbon black used in the present invention is prepared by lamp black, furnace black or gas black process and preferably has a carbon black content of 20 to 200 m 2 / g BET surface area, such as SAF, ISAF, HSAF, HAF, FEF or GPF black. The carbon black may also contain heteroatoms, such as Si.

[0041] - silicon dioxide, preferably precipitated silicon dioxide, prepared, for example, by precipitation of solutions of silicates, preferably water glass, or by flame hydrolysis of silicon halides, preferably having a carbon content of 5 to 1000 m 2 The precipitated silica may preferably have a specific surface area of ​​20 to 400 m 2 / g, particularly preferably 80 to 280 m 2 / g, very particularly preferably from 150 to 210 m 2 / g, particularly preferably 80 to 185m 2 The precipitated silica may have an average primary particle size of 5 to 400 nm, preferably 7 to 100 nm, particularly preferably 7 to 40 nm. The silica may also optionally be in the form of a mixed oxide with other metal oxides such as oxides of Al, Mg, Ca, Ba, Zn and titanium.

[0042] - Synthetic silicates, for example aluminum silicates, alkaline earth metal silicates such as magnesium silicate or calcium silicate, or zeolites. Synthetic silicates preferably have a molecular weight of 20 to 400 m 2 / g and a primary particle size of 10 to 400 nm.

[0043] - Natural silicates, for example kaolin, mica, kieselguhr, diatomaceous earth, talc, wollastonite or clay, or other naturally occurring silicas.

[0044] - Glass fibres and glass fibre products (felts, wires, fabrics) or glass beads.

[0045] - Biopolymeric or biooligomeric fillers, for example natural or modified starch, cellulose, amylose, amylopectin, cellulose acetate, maltose, cellobiose, lactose, sucrose, raffinose, glycogen, pectin, chitin or natural or modified proteins.

[0046] - Other oxide fillers, such as aluminum oxide, aluminum hydroxide or aluminum trihydrate, zinc oxide, boron oxide, magnesium oxide or oxides of other transition metals, such as titanium dioxide, or fumed silica.

[0047] The rubber mixtures of the invention preferably comprise, based on 100 parts by weight of rubber, in each case 0 to 150 parts by weight, more preferably 10 to 150 parts by weight, of precipitated silica, 0 to 100 parts by weight, more preferably 1 to 10 parts by weight, of carbon black, and 1 to 50 parts by weight, more preferably 10 to 40 parts by weight, even more preferably 20 to 30 parts by weight, of liquid polybutadiene.

[0048] Preferred rubber mixtures according to the invention comprise in each case 10 to 150 parts by weight of precipitated silica, 0 to 100 parts by weight, more preferably 1 to 10 parts by weight, of carbon black, and 1 to 50 parts by weight, more preferably 10 to 40 parts by weight, even more preferably 20 to 30 parts by weight, of liquid polybutadiene, based on 100 parts by weight of rubber.

[0049] A further preferred rubber mixture of the invention comprises, based on 100 parts by weight of rubber, in each case 0 to 150 parts by weight, more preferably 0 to 10 parts by weight, of precipitated silica, 1 to 100 parts by weight, more preferably 5 to 50 parts by weight, of carbon black, and 1 to 50 parts by weight, more preferably 10 to 40 parts by weight, even more preferably 20 to 30 parts by weight, of liquid polybutadiene.

[0050] It may be advantageous if the rubber mixture according to the invention contains one or more organosilanes. Preferably, the rubber mixture according to the invention contains 0.5 to 20 parts by weight, preferably 1 to 16 parts by weight, particularly preferably 2 to 12 parts by weight, very particularly preferably 3 to 7 parts by weight of one or more organosilanes, based on 100 parts by weight of rubber.

[0051] The one or more organosilanes may be silicone oil, alkylsilane, vinylsilane, ethoxysilyl-containing mercaptoorganosilane, ethoxysilyl-containing thiocyanatoorganosilane, ethoxysilyl-containing blocked mercaptoorganosilane and / or ethoxysilyl-containing di / polysulfide alkoxysilane.

[0052] The one or more organosilanes may preferably be triethoxyalkylsilane, triethoxyvinylsilane, triethoxytriethoxysilyl-containing mercaptoorganosilane, triethoxysilyl-containing thiocyanatoorganosilane, triethoxysilyl-containing blocked mercaptoorganosilane or triethoxysilyl-containing di / polysulfided alkoxysilane.

[0053] Additional organosilanes that may be employed include those having a C8H 17 -O-, C 10 H 21 -O-, C 12 H 25 -O-, C 14 H 29 -O-, C 16 H 33 -O- or C 18 H 37 -O-group mercaptoorganyl (alkoxysilane).

[0054] Additional organosilanes that may be employed include those having a C8H 17 -O-, C 10 H 21 -O-, C 12 H 25 -O-, C 14 H 29 -O-, C 16 H33 -O- or C 18 H 37 -O-group blocked mercaptoorganyl (alkoxysilane), or a blocked mercaptoorganyl (alkoxysilane) with a difunctional alcohol (diol) bonded to silicon (such as the silanes of the NXT LowV, NXT Ultra-LowV or NXT Z-series products from Momentive).

[0055] Additional organosilanes that may be employed include polysulfided alkoxysilanes of the formula:

[0056] EtO-Si(Me)2-CH2-CH2-CH2-S2-CH2-CH2-CH2-Si(Me)2(OEt),

[0057] EtO-Si(Me)2-CH2-CH2-CH2-S3-CH2-CH2-CH2-Si(Me)2(OEt) or

[0058] EtO-Si(Me)2-CH2-CH2-CH2-S4-CH2-CH2-CH2-Si(Me)2(OEt).

[0059] Further organosilanes which may be added to the rubber mixture of the invention include 3-mercaptopropyl(triethoxysilane) (e.g. Si 263 from Evonik Industries AG), 3-thiocyanatopropyl(triethoxysilane) (e.g. Si 264 from Evonik Industries AG), bis(triethoxysilylpropyl)polysulfide (e.g. Si 69 from Evonik Industries AG), bis(triethoxysilylpropyl)disulfide (e.g. Si 266 from Evonik Industries AG).

[0060] Further organosilanes which may be employed include mercaptoorganosilanes containing alkyl polyether alcohols (eg Si 363 from Evonik Industries AG), thiocyanatoorganosilanes containing alkyl polyether alcohols or / and blocked mercaptoorganosilanes containing alkyl polyether alcohols or polysulfided silanes containing alkyl polyether alcohols.

[0061] The mercapto organosilane containing alkyl polyether alcohol may be a compound of formula (I):

[0062] (X)3Si-R 3 -SH (I)

[0063] wherein X is an alkyl, alkoxy or alkyl polyether group, and at least one X is an alkyl polyether group, R 3It is a branched or unbranched, saturated or unsaturated, substituted or unsubstituted aliphatic, aromatic or mixed aliphatic / aromatic divalent hydrocarbon group.

[0064] The blocked mercapto organosilane containing alkyl polyether alcohol may be a compound of formula (II):

[0065] (X)3Si-R 4 -SC(O)-R 5 (II)

[0066] wherein X is an alkyl, alkoxy or alkyl polyether group, and at least one X is an alkyl polyether group, R 4 is a branched or unbranched, saturated or unsaturated, substituted or unsubstituted aliphatic, aromatic or mixed aliphatic / aromatic divalent hydrocarbon group, and R 5 is a branched or unbranched, saturated or unsaturated, substituted or unsubstituted aliphatic, aromatic or mixed aliphatic / aromatic monovalent hydrocarbon group, preferably C1-C 25 -, particularly preferably C2-C 22 -, very particularly preferably C7-C 17 -, most preferably C 11 -C 16 - Hydrocarbyl.

[0067] The rubber in the rubber mixture according to the present invention can be a rubber or a mixture of different rubbers. Preferably, the rubber in the rubber mixture according to the present invention is a mixture of different rubbers. The rubber in the rubber mixture of the present invention can be selected from natural rubber and / or synthetic rubber. Preferred synthetic rubbers are described in, for example, W.Hofmann, Kautschuktechnologie [Rubber Technology], Genter Verlag, Stuttgart 1980. These particularly include polybutadiene (BR), polyisoprene (IR), styrene / butadiene copolymers (SBR) with a styrene content of 1 to 60% by weight, preferably 2 to 50% by weight, isobutylene / isoprene copolymers (IIR), butadiene / acrylonitrile copolymers (NBR) with a styrene content of 5 to 60% by weight, preferably 10 to 50% by weight, partially hydrogenated or fully hydrogenated NBR rubber (HNBR), ethylene / propylene / diene copolymers (EPDM) and mixtures of such rubbers. In particular, anionically polymerized S-SBR rubbers, preferably those having a glass transition temperature above -50°C, and mixtures thereof with diene rubbers are of interest for the production of motor vehicle tires. Preferably employable rubbers include natural rubber or mixtures of natural rubber with diene rubbers, preferably polybutadiene, polyisobutylene or styrene butadiene copolymers.

[0068] Most preferably, the rubber in the rubber mixture according to the invention is a mixture of neodymium butadiene rubber (Nd-BR) and styrene-butadiene random copolymer (S-SBR).

[0069] The rubber mixtures according to the invention may additionally contain rubber auxiliary products, such as reaction accelerators, aging stabilizers, heat stabilizers, light stabilizers, antiozonants, processing aids, plasticizers, resins, tackifiers, blowing agents, dyes, pigments, waxes, extenders, organic acids, inhibitors, metal oxides and / or activators such as triethanolamine, polyethylene glycol, hexanetriol, which are known from the rubber industry.

[0070] Rubber additives are preferably used in typical amounts determined particularly by end-uses. Based on rubber, typical amounts are, for example, amounts of 0.1 to 50 parts by weight. It is generally advisable to add additional crosslinking agents. Other known crosslinking agents that can be used include sulfur or peroxide. Rubber mixtures of the present invention may additionally include vulcanization accelerators. Examples of suitable vulcanization accelerators include mercaptobenzothiazoles, sulfonamides, guanidines, thiurams, dithiocarbamates, thioureas and thiocarbonates. Based on 100 parts by weight of rubber, vulcanization accelerators and sulfur or peroxides may be used in amounts of 0.1 to 10 parts by weight, preferably 0.1 to 5 parts by weight.

[0071] By using mixing procedures and mixing equipment known in the art, rubber mixture according to the present invention can be obtained. The blending of rubber and liquid polybutadiene of the present invention and optionally present filler and any rubber auxiliary agent can preferably be carried out in conventional mixing devices such as rollers, internal mixers and mixing extruders. It is also possible to obtain rubber mixture according to the present invention by mixing so-called liquid phases as described in the prior art, continuous liquid phase mixing or combining masterbatches.

[0072] The addition of liquid polybutadiene and / or the addition of filler, preferably the addition of liquid polybutadiene and the addition of filler, is preferably carried out at a material temperature of 50°C to 200°C, more preferably at 80°C to 185°C, even more preferably at 100°C to 185°C, particularly preferably at a material temperature of 130°C to 170°C, but can also be carried out at a material temperature of 40°C to 100°C at a later or very early stage, for example together with further rubber additives.

[0073] Liquid polybutadiene can be added to the mixing operation either in pure form or applied to an organic or inorganic support. Preferred support materials are silicon dioxide, natural or synthetic silicates, aluminum oxide, waxes, polymers, in particular polyethylene or polyethylene wax, or carbon black.

[0074] The rubber mixtures according to the invention can be used for every purpose for which the rubber mixtures of the prior art are likewise suitable. The rubber mixtures according to the invention can preferably be used for the production of mouldings, in particular pneumatic tyres, lightweight tyres or tyre treads.

[0075] Preferably, in the method for preparing rubber products by the vulcanization of the rubber mixture according to the present invention, the rubber mixture of the present invention is used as raw material. Therefore, the present invention also relates to the method of the present invention for preparing rubber products by the vulcanization of the rubber mixture, wherein the rubber mixture of the present invention is used as raw material. The vulcanization of the rubber mixture of the present invention is preferably carried out at a temperature of 100 ℃ to 200 ℃, preferably 130 ℃ to 180 ℃, optionally under a pressure of 10 to 200 bars. The vulcanized rubber thus obtained is suitable for producing molded products. The rubber mixture of the present invention can be used for producing tires, profiles, cable sheaths, hoses, transmission belts, conveyor belts, tire treads, soles, sealing rings and damping elements. If necessary, for one of the above listed products, the rubber mixture of the present invention can also be vulcanized with an alternative vulcanization method with a continuous or discontinuous process, in which, for example, radiation such as microwaves or hot salt baths are used in the continuous or discontinuous process.

[0076] The present invention further relates to a rubber article (product) obtained by the method according to the present invention. The rubber article according to the present invention is preferably a tire or one or more parts of a tire. More preferably, the rubber article according to the present invention is a tire tread. Most preferably, the rubber article according to the present invention is an all-season tire or a snow (winter) tire or their tire tread.

[0077] Even without further elaboration, it is believed that one skilled in the art will be able to utilize the above detailed description to the broadest extent.Therefore, the preferred embodiments and examples should be construed as merely disclosed as descriptive and not intended to be limiting in any way.

[0078] The present invention will now be described in more detail with reference to Examples.Alternative embodiments of the present invention can be obtained similarly.

[0079] Example

[0080] Raw materials used:

[0081] The raw materials used are given in Table 1 below.

[0082] Table 1: Raw materials used

[0083]

[0084] The amount of vinyl monomer units is determined by IR spectroscopy as described below.

[0085] LBR 60% is obtainable as described in Example 3 of WO 2018130703 A1.

[0086] method:

[0087] Determination of microstructure:

[0088] The IR spectrum using polybutadiene standards is used for the determination of the molar ratio of monomeric units according to formula (A), (B) and (C). 80 to 250 mg of the polybutadiene sample to be detected is dissolved in 10 mL of carbon disulfide (CS2). If a large amount of monomeric units of formula (A) are expected, a low concentration (e.g., 80 mg of sample) of the polybutadiene is used, and if a large amount of monomeric units of formula (C) are expected, a higher concentration (e.g., 250 mg of sample) of the polybutadiene is used. The determination is completed using an IR cuvette (KBr) with a thickness of 0.5 mm. The solvent is subtracted and the concentration is measured at 1100 to 600 cm -1 The spectrum is displayed within the evaluation range of the extinction. If the obtained extinction exceeds 1, the measurement is repeated using a lower concentration of polybutadiene. The extinction above the baseline is determined for the following signals:

[0089] Trans-1,4-polybutadiene: 968 cm -1

[0090] 1,2-Polybutadiene: 911cm -1

[0091] Cis-1,4-polybutadiene: 730cm -1

[0092] The molar ratio of the monomer units was calculated according to the following formula:

[0093] %Comp(i)=Ext(i)*100% / (E(i)*c*d*)

[0094] in,

[0095] Ext(i) = Extinction above baseline

[0096] E(i) = extinction coefficient (substance specific, determined by calibration measurements) [E] = L / (g*cm)

[0097] d = cuvette thickness in cm

[0098] c = sample concentration in g / L.

[0099] Mooney viscosity:

[0100] The Mooney viscosity of the raw rubber mixture was determined at 100°C. The value M was determined according to DIN 53523 / 3, ISO 289-1S (1+4) / MU, and the value M was determined according to DIN 53523 / 3, ISO 289-2 L (1+4) / MU.

[0101] Tensile Strength:

[0102] The maximum tensile strength in MPa and the elongation at break in % of the vulcanized rubber were determined in accordance with DIN 53504 / ISO 37. The measurements were done using standard dumbbell S1 type test specimens at a temperature of 23° C. The pull-out speed was set to 500 mm / min.

[0103] Shore A hardness:

[0104] The Shore A hardness in SH of the vulcanized rubber was determined according to ISO 7619-1 using a test temperature of 23°C.

[0105] Ball rebound rate:

[0106] The rebound resilience in % of the vulcanized rubber was determined according to ASTM D 2632 using a steel ball with a weight of 28 g and a diameter of 19 mm and a drop height of 500 mm.

[0107] Viscoelasticity:

[0108] The viscoelastic properties of the vulcanized rubber were determined according to ASTM D 6601-02, DIN 53513 / ISO 4664-1, and ISO 1827.

[0109] The maximum loss factor (tan delta max) was determined according to ASTM D 6601-02 at 60°C and 1.6 Hz over the elongation range of 0.28% to 42.0% using an RPA2000 from Alpha Technologies as described in the February 1997 Operator's Manual.

[0110] The complex modulus E* of the vulcanized rubber in MPa was determined according to DIN 53513 / ISO 4664-1 using a Zwick Rel 2100 servohydraulic testing machine from ZwickRoell GmbH & Co. KG at 16 Hz with an initial force of 50 N, an amplitude force of 25 N, a temperature conditioning time of 5 minutes, and the values ​​were recorded after a test time of 30 seconds.

[0111] use The complex shear modulus G* and the dissipation factor tan δ in MPa were determined according to ISO 1827 using a 4000N (serial number 1101, NETZSCH GABO Instruments GmbH) in temperature sweep mode with 1.6 Hz, 0.2% dynamic deformation, 0.0% static deformation and a temperature range of -80°C to 80°C.

[0112] The molecular weight of polybutadiene was determined using gel permeation chromatography. The measurement was carried out at 40°C in tetrahydrofuran (THF) at a concentration of 1 g / L and a flow rate of 0.3 ml / min. Chromatographic separation was achieved using a PSS SDV Micro 5μ / 4.6×30mm pre-column and a PSS SDV Micro linear S 5μ / 4.6×250mm (2×) separation column. Detection was by means of an RI detector. Calibration was carried out by means of a polybutadiene standard (PSS-Kit polybutadiene-1,4, Mp 831-106000, part number: PSS-bdfkit, Mn: 1830 / 4330 / 9300 / 18000 / 33500).

[0113] Viscosity:

[0114] The viscosity of the polybutadiene was determined in accordance with DIN 53018 using a rheometer Physica MCR 301 from ANTON PAAR Germany GmbH (cone and plate).

[0115] Embodiment 1:

[0116] For stage 1, 2 and 3, the formulations for the rubber mixtures are described in the following Table 2. In this table, the unit phr means parts by weight based on 100 parts of the rubber (S-SBR and Nd-BR) employed. In the rubber mixtures of the invention, liquid polybutadiene (LBR) was employed in different amounts as a substitute for the plasticizer oil "TDAE".

[0117] Table 2 Composition of the rubber mixture used

[0118]

[0119] The amount of plasticizer oil, for example LBR XX% and TDAE, was given to the mixture using processable LDPE bags with a low melting point (Polybeutel 150×200 mm, IGEFA Handelsgesellschaft) each filled with 5.0 phr.

[0120] General processes for preparing rubber mixtures and their vulcanizates are described in “Rubber Technology Handbook”, W. Hofmann, Hanser Verlag 1994.

[0121] The equipment and parameters for processing each rubber mixture are given below in Table 3a for stage 1, in Table 3b for stage 2 and in Table 3c for stage 3.

[0122] Table 3a Equipment and parameters used for processing each rubber mixture in stage 1

[0123]

[0124] Table 3b Equipment and parameters used for processing each rubber mixture in stage 2

[0125]

[0126] Table 3c Equipment and parameters used for processing each rubber compound in stage 3

[0127]

[0128] The Mooney viscosity of the rubber mixtures (sheets) obtained after stages 1 and 3 was determined as described above. The results are given in Table 4.

[0129] The rubber mixture obtained after stage 3 is vulcanized to obtain test plates and test specimens. 95 The optimum curing time is 17 minutes at 165°C in a typical vulcanizing press with a compression pressure of 130 bar. 95 The times were determined according to the DIN 53529 / 3 procedure at 165° C. by means of a moving die rheometer (rotorless rheometer).

[0130] The rubber test was performed according to the test method described above. The results of the rubber test are also given in Table 4.

[0131] Table 4 Results of rubber testing

[0132]

[0133] Compared to rubber mixtures I to III, the rubber mixture IV according to the invention has improved processability, which is indicated by the lower Mooney viscosity values ​​of the rubber mixture IV according to the invention after the 1st and 3rd stages.

[0134] Surprisingly, compared to all other mixtures, the rubber mixture IV used in the present invention achieves an enhanced strengthening effect because it not only has the highest tensile strength, but also has the highest elongation at break. At nearly the same hardness, dynamic data can be well compared. Compared to reference rubber mixtures I, II and III, the rubber mixture IV according to the present invention has a lower hysteresis in the dynamic test at 60°C, which is important for predicting rolling resistance. This can be seen in the increased ball rebound value, i.e., the improved value compared to other compounds containing liquid polybutadiene, and is confirmed in the maximum minimum value of tan δ measured at 60°C. Therefore, if a tire is equipped with a tread based on a rubber mixture according to the present invention, the rubber mixture according to the present invention should achieve improved rolling resistance and lower fuel consumption.

[0135] At the same time, the rubber mixture IV according to the invention can achieve high dynamic complex moduli (E* and G* at 60°C) measured at an elevated temperature of 60°C, which is an indicator for predicting dry road traction of passenger car tires according to the literature. In particular, compared to reference rubber mixtures II and III, improved dry handling of passenger car tires equipped with tread rubbers of the rubber mixture IV according to the invention can be expected. In addition, compared to reference rubber mixtures II and III, the rubber mixture IV according to the invention shows a higher loss factor value at -10°C. According to the relevant literature, this should achieve improved winter properties and / or have a positive effect on wet road grip if the mixture is used as the basis for a winter tire tread mixture.

Claims

1. A rubber mixture comprising rubber and liquid polybutadiene, wherein the polybutadiene is liquid at a temperature of 20° C. and a pressure of 98.0665 kPa, characterized in that The liquid polybutadiene comprises monomer units derived from 1,3-butadiene and wherein the proportion of A in all the monomer units derived from 1,3-butadiene present in the liquid polybutadiene is 55 to 70 mol %, and wherein the sum of the proportions of B and C in all the monomer units derived from 1,3-butadiene present in the liquid polybutadiene is 30 to 45 mol %, and the liquid polybutadiene consists only of C- and H-atoms and has an average molecular weight Mw of 1500 to 5000 g / mol as determined by gel permeation chromatography; the measurement by gel permeation chromatography is carried out at 40° C. in tetrahydrofuran (THF) at a concentration of 1 g / L and a flow rate of 0.3 ml / min; wherein a PSSSDV Micro 5μ / 4.6×30 mm pre-set column and a PSSSDV Micro linear S Chromatographic separation is achieved by a 5μ / 4.6×250mm (2×) separation column; detection is performed by means of an RI detector; calibration is performed by means of a polybutadiene standard; wherein the polybutadiene standard is PSS-Kit polybutadiene-1,4, Mp 831-106000, part number: PSS-bdfkit, Mn: 1830 / 4330 / 9300 / 18000 / 33500.

2. The rubber mixture according to claim 1, characterized in that Based on 100 parts by weight of rubber, the mixture comprises in each case 0 to 150 parts by weight of precipitated silica, 0 to 100 parts by weight of carbon black and 1 to 50 parts by weight of the liquid polybutadiene.

3. The rubber mixture according to any one of claims 1 or 2, characterized in that The mixture comprises an organosilane.

4. The rubber mixture according to claim 3, characterized in that The mixture includes 0.5 to 20 parts by weight of the organosilane based on 100 parts by weight of the rubber.

5. The rubber mixture according to any one of claims 1 or 2, characterized in that The rubber is one type of rubber or a mixture of different types of rubbers.

6. The rubber mixture according to any one of claims 1 or 2, characterized in that The rubber is selected from natural rubber and / or synthetic rubber.

7. The rubber mixture according to claim 5, characterized in that The rubber is a mixture of Nd-BR and S-SBR.

8. The rubber mixture according to claim 6, characterized in that The rubber is a mixture of Nd-BR and S-SBR.

9. The rubber mixture according to any one of claims 1 or 2, characterized in that The liquid polybutadiene has an average molecular weight Mw of 1750 to 3500 g / mol, as determined by gel permeation chromatography.

10. A method for preparing a rubber product by vulcanizing a rubber mixture, characterized in that As starting material a rubber mixture according to any one of claims 1 to 9 is used.

11. Rubber product obtained by the method according to claim 10.

12. The rubber product according to claim 11, characterized in that It is a tire or part of a tire.

13. The rubber product according to claim 12, characterized in that It is the tire tread.

14. The rubber product according to claim 12 or 13, characterized in that The tires are all-season tires or snow winter tires.