A high-precision four-ridge horn antenna unit die-casting method
Through flow rate segmentation control and internal flow channel design, combined with standard sliders and multi-step process, the technical problem of four-ridge horn antenna unit molding is solved, high-precision and low-cost die-casting is achieved, shortening the manufacturing cycle and meeting the complexity Telecommunication performance requirements for structure.
Patent Information
- Application Number
- CN202211300216.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-24
AI Technical Summary
Traditional machining methods are difficult to achieve high precision, low cost and rapid molding of four-ridge horn antenna units. The existing die-casting process has problems such as uneven wall thickness, narrow and deep gaps between ridges, small transition corners and poor overall accuracy. Direct forming.
Adopt flow rate segment control and internal runner design, combined with the concept of standard sliders, through die casting process simulation and mold design, smelting and refining of aluminum alloys, die casting molding, sawing runners and slag packs, sandblasting and annealing treatment, Finishing and post-processing steps ensure high-precision molding of the speaker.
High-precision die-casting molding of four-ridge horn antenna units is achieved, shortening the manufacturing cycle by about 400%, ensuring the moldability and dimensional accuracy of narrow gaps, and meeting the telecommunication performance requirements of complex structures.
Smart Images

Figure CN115709269B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronic manufacturing, and in particular relates to a high-precision four-ridge horn antenna unit die-casting method. Background Art
[0002] Horn antenna units are widely used in measurement and control electronic equipment. Adding a four-ridge structure inside the horn can meet the demand for increased working bandwidth. A large-scale equipment requires tens of thousands of horn antenna units. Its four-ridge horn has the characteristics of narrow gaps between ridges (0.7mm) and deep (25mm), large difference in thickness between the solid inner ridge and the outer wall (ratio>2.5), small transition radius of the inner cavity (<0.5mm), and high overall accuracy requirements (±0.05mm). The traditional method of brazing after machining has problems such as poor accuracy consistency, high production cost and long cycle. A low-cost, high-precision rapid prototyping method is urgently needed.
[0003] The patent with announcement number CN110544830A proposes a manufacturing process for a double-ridged sealed horn antenna. The horn body adopts a metal casting method to manufacture a double-ridged horn with uniform wall thickness suitable for an inward-concave type. The above method is suitable for a horn structure with uniform wall thickness and relatively simple structural features, but is not suitable for the structural feature manufacturing of a four-ridged horn. The four-ridged horn is intended to adopt a die-casting rapid prototyping process, but there are problems such as uneven wall thickness, narrow and deep gaps between ridges, small transition radius, and high overall precision, resulting in extremely poor die-casting processability and difficulty in direct molding. Therefore, it is urgent to overcome the molding technology difficulties in the die-casting molding of the four-ridged horn, ensure the structural characteristics and dimensional accuracy of the four-ridged horn, and form the mass production capacity of the four-ridged die-cast horn. Summary of the invention
[0004] The present invention proposes a high-precision four-ridged horn antenna unit die-casting molding method, which overcomes the technical difficulties in the ridged horn molding technology in the prior art. By adopting segmented flow rate control and setting internal flow channels in the thicker parts of the horn, the temperature change consistency and molding quality of various parts of the horn are improved; the concept of a standard slider is proposed, and its surface is strengthened to improve the formability of narrow gap parts and the life of mold molding, thereby realizing the mass production of high-precision four-ridged horn antenna unit die-casting molding structure, and ensuring the high-precision technical requirements of the horn. This method includes die-casting process simulation and mold design, smelting and refining of aluminum alloy, die-casting molding, sawing flow channels and slag bags, sandblasting and annealing, finishing and post-processing steps. The specific steps are as follows:
[0005] Step 1: Die casting process simulation and mold design
[0006] The antenna unit is simulated and analyzed for structural features, mold temperature, pouring temperature and pouring speed, and a standard slider is designed to ensure the die-casting formability of the speaker gap, increase internal runner cooling, and improve the consistency of temperature changes and molding quality of various parts of the speaker.
[0007] Step 2: Melting and refining of aluminum alloy
[0008] Die-cast aluminum alloy is used for smelting, and the alloy melt is purified by inert gas refining and vacuum degassing.
[0009] Step 3: Die Casting
[0010] Die casting is carried out on the die casting machine. Before die casting, the water valve is opened to ensure smooth circulation and cooling in the inner flow channel. After die casting is completed, the die casting blank is inspected.
[0011] Step 4: Sawing the flow channel and slag bag
[0012] Sawing the runners and slag bags from the die-cast blank.
[0013] Step 5: Sandblasting
[0014] Use 80-120 mesh sandblasting to treat the speaker surface.
[0015] Step 6: Annealing
[0016] Stress relief annealing of die-cast parts.
[0017] Step 7: Finishing
[0018] According to the design requirements, the installation mating surfaces of the upper and lower end faces of the horn antenna unit are finely processed.
[0019] Step 8: Post-processing
[0020] Mechanical grinding is used to remove the oxide scale on the surface of the casting, and then the corresponding pickling is carried out, followed by conductive oxidation. After conductive oxidation, the speaker is ultrasonically cleaned; then the primer and topcoat are sprayed to jointly improve the corrosion resistance and bonding strength of the film layer; the mounting holes are processed to complete the final part inspection.
[0021] The beneficial effects of the present invention are
[0022] 1) The standard slider design enables the speaker with narrow gap (0.7mm) to be die-cast and quickly replaceable in production, effectively meeting the high efficiency and economic requirements of complex and special structure die-casting parts.
[0023] 2) The four-ridge curve equation accuracy and other dimensional accuracy of the four-ridge horn die-casting blank are both ±0.05mm, and the dimensional accuracy meets the complex structural requirements of the horn antenna unit.
[0024] 3) The standing wave test, gain coefficient and other telecommunication indicators of the four-ridged horn array are consistent with the simulation results, meeting the telecommunication test requirements of the horn antenna unit.
[0025] 4) The die-casting manufacturing time of the four-ridged horn is shortened by about 400% compared to the brazing molding time, and the production cycle is shortened from the expected 10 months to 2 months, greatly shortening the manufacturing cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a cross-sectional view of the four-ridged horn model.
[0027] Figure 2 The flowchart of the method is shown in FIG.
[0028] Figure 3 This is a die casting mold diagram.
[0029] Figure 4 This is a schematic diagram of a standard slider.
[0030] Figure 5 This is an analysis diagram of the average wall thickness of the casting. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Take the aluminum alloy (YL113) four-ridge horn antenna unit as an example, see the attached Figure 1 The die-casting method of the present invention is used to manufacture the same. The process flow is shown in the attached Figure 2 , specifically including the following steps:
[0033] (1) Die-casting process simulation and mold design: Magma software was used to perform mold flow simulation analysis (DFM) on structural features, mold temperature, pouring temperature and pouring speed for the four-ridge horn antenna unit structure. The structural optimization and die-casting process optimization were carried out based on the simulation results. In particular, a standard slider was designed for the narrow gap (0.7mm) horn structure that is difficult to die-cast. Figure 4 As shown in the figure, the slider is made of special steel and the surface is strengthened to ensure the die-casting formability of the speaker gap; through the wall thickness analysis of the speaker structure, as shown in the attached Figure 5 As shown in the figure, the difference in thickness ratio between the side wall of the speaker and the ridge and base is greater than 2.5, so an internal flow channel cooling design is added at this position to improve the temperature change consistency and molding quality of various parts of the speaker; a die-casting mold is designed, as shown in the attached figure. Figure 3 shown.
[0034] (2) Melting and refining of aluminum alloy: Die-cast aluminum alloy YL113 ingots are used for melting. The composition of die-cast aluminum alloy is shown in the following table. In order to improve the corrosion resistance of the product, the Cu content is required to be strictly controlled at 1.5%-2%. Inert gas refining and vacuum degassing are used to purify the alloy melt to reduce alloy pollution and effectively remove gas and solid inclusions in the melt.
[0035] Table Die Casting Aluminum Alloy Chemical Composition
[0036] Si Cu Mn Mg Fe Ni Ti Zn Pb Sn Al 9.5-12 1.5-2 ≤0.5 ≤0.3 ≤1.2 ≤0.5 / ≤1.0 ≤0.1 ≤0.1 the remaining
[0037] (3) Die casting: Die casting is carried out on a 280T die casting machine. The mold drawing is as attached. Figure 3 As shown; at the first and last stages of every 2,000 die-cast parts, the accuracy of the speaker parts and standard sliders is measured. If they do not meet the requirements, the sliders are replaced to ensure the formability of the speaker gap (0.7mm); the water valve is opened before die-casting to ensure smooth circulation and cooling of the inner flow channel; the following main optimized process parameters are used for die-casting:
[0038] Table Die Casting Main Process Parameters
[0039]
[0040] After die casting is completed, the die casting blank is inspected, and the requirements are: a) Use visual and fluorescent detection methods to confirm that there are no obvious cracks, cold shuts, deformations and other defects on the casting surface. b) The ejector pin mark is convex <0.5mm, the assembly surface is not allowed to have a convex ejector pin mark, and the processing surface concave ejector pin mark is concave <0.3mm.
[0041] (4) Sawing the runner and slag bag: Use the vertical band saw S-360H to saw the runner and slag bag of the die-casting blank. The residual of the runner and overflow groove is required to be ≤2.5mm, and the casting must not be damaged; use a file or 80# sandpaper to grind off the burrs, especially the burrs at the parting line of the product must be cleaned up, and do not use a coarse file.
[0042] (5) Sand blasting: Use 80-120 mesh sand blasting to treat the speaker surface.
[0043] (6) Annealing treatment: Stress relief annealing is performed on the die-cast parts: the heat treatment temperature is 290℃-310℃, the holding time is 2-4h, and the parts are cooled in air or in the furnace.
[0044] (7) Finishing: According to the technical requirements of the drawings, the installation surfaces of the upper and lower ends of the ridge speaker are finished to ensure the product's precision dimensions.
[0045] (8) Post-processing: Use mechanical grinding to remove the oxide scale on the surface of the casting, then carry out the corresponding pickling and polishing, followed by conductive oxidation. After conductive oxidation, the speaker must be ultrasonically cleaned; spray the primer and topcoat to jointly improve the corrosion resistance and bonding strength of the film layer; process the mounting holes and grooves, and complete the final part inspection.
[0046] Through the above steps, a four-ridged horn antenna unit can be prepared by aluminum alloy die-casting. In this implementation, the die-casting mold adopts a one-out-two form, and each device can complete the manufacture of about 1,800 to 2,500 antenna units per day, with a total production time of about 2 hours for the entire process; the design of the standard slider avoids the overall scrapping of the mold, making the difficult-to-form structure in the horn have efficient and economical productivity; the performance test of the aluminum alloy four-ridged horn antenna unit sample was carried out, and after measurement, the tensile strength was 230MPa, and the elongation after fracture was 2%, which met the performance indicators; the dimensional inspection of the finished four-ridged horn antenna unit was carried out, and the actual measured accuracy of the four-ridged curve equation was ±0.03mm, and the accuracy of other dimensions and positions such as wall thickness and hole depth were within ±0.05mm, and the dimensional inspection was qualified; the telecommunications performance test was carried out on the aluminum alloy four-ridged horn unit composed of 4×6 small arrays and the large array composed of multiple small arrays, and the telecommunications indicators such as standing wave and gain coefficient were tested. The indicators all met the performance requirements of electronic equipment, and the data stability was good. The relevant appraisal of the unit was completed, and it was first applied to a key national electronic equipment product.
[0047] The present invention is not limited to the above specific implementations, and the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made to the above implementations based on the technical essence of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-precision four-ridge horn antenna unit die-casting method, characterized in that: It includes die-casting process simulation and mold design, aluminum alloy smelting and refining, die-casting, sawing flow channel and slag bag, sandblasting and annealing, finishing and post-processing steps. The specific steps are as follows: Step 1: Die casting process simulation and mold design The mold flow simulation analysis was conducted on the structural characteristics, mold temperature, pouring temperature and pouring speed of the four-ridged horn antenna unit, and a standard slider was designed to ensure the die-casting formability of the gap of the four-ridged horn antenna unit, increase internal flow channel cooling, and improve the temperature change consistency and molding quality of each part of the four-ridged horn antenna unit; Step 2: Melting and refining of aluminum alloy Die-cast aluminum alloy is used for smelting, and the alloy melt is purified by inert gas refining and vacuum degassing; Step 3: Die Casting Die casting is performed on a die casting machine. Before die casting, the water valve is opened to ensure smooth circulation and cooling of the internal flow channel. After die casting is completed, the die casting blank is inspected. The inspection standards for the die casting blank are as follows: a) visual and fluorescent inspection methods are used to confirm that there are no obvious cracks, cold shuts, and deformation defects on the surface of the die casting blank; b) The ejector pin mark is convex less than 0.5mm, the assembly surface is not allowed to have a convex ejector pin mark, and the concave ejector pin mark on the machined surface is less than 0.3mm; Step 4: Sawing the flow channel and slag bag Sawing the runners and slag bags from the die-cast blanks; Step 5: Sandblasting Use 80-120 mesh spray material to sandblast the surface of the quad-ridge horn antenna unit; Step 6: Annealing Stress relief annealing of die-cast parts; Step 7: Finishing According to the design requirements, the installation and matching surfaces of the upper and lower end surfaces of the four-ridged horn antenna unit are finely processed; Step 8: Post-processing Mechanical grinding is used to remove the oxide scale on the surface of the four-ridged horn antenna unit, and then acid pickling is performed, followed by conductive oxidation. After conductive oxidation, the four-ridged horn antenna unit is ultrasonically cleaned; then primer and topcoat are sprayed to jointly improve the corrosion resistance and bonding strength of the film layer; mounting holes are processed to complete the final inspection of the four-ridged horn antenna unit.
2. A high-precision four-ridged horn antenna unit die-casting method as claimed in claim 1, characterized in that: The internal flow channel is located at the position where the side wall of the quad-ridged horn antenna unit contacts the ridge and the base.
3. A high-precision four-ridged horn antenna unit die-casting method as claimed in claim 1, characterized in that: Aluminum alloy YL113 ingot is used for smelting, and the Cu content is controlled at 1.5%-2%.
4. A high-precision four-ridged horn antenna unit die-casting method as claimed in claim 1, characterized in that: In the third step, the pouring temperature of the die casting is 670-690° C., the mold temperature is 250-280° C., and the pressure holding cooling time is 6-7 seconds.
5. A high-precision four-ridged horn antenna unit die-casting method as claimed in claim 1, characterized in that: During the die-casting process, the accuracy of the four-ridged horn antenna unit parts and the standard slider needs to be measured. If it does not meet the requirements, the standard slider must be replaced.
6. A high-precision four-ridged horn antenna unit die-casting method as claimed in claim 1, characterized in that: In the sixth step, the heat treatment temperature of the die-cast parts is 290° C.-310° C., the holding time is 2-4 hours, and the parts are cooled in air or in the furnace.
Citation Information
Patent Citations
Manufacturing process method of double-ridge sealed horn antenna
CN110544830A
Production process of aluminum alloy frame suitable for being subjected to anodic oxidation and integrally formed by die casting
CN107263017A
High-performance automobile part production technological process
CN108251676A
An aluminum alloy hub side die with a heat dissipation structure
CN202726014U
Die-casting die with high thermal conductivity
CN212525999U