A lithium battery electrode sheet and preparation method thereof

By blending cyclic phosphorus-based monomers into the lithium-ion battery electrode slurry and polymerizing in situ, an electrode sheet of phosphorus-based polymer material is generated, which solves the thermal runaway and safety problems of lithium-ion battery and achieves higher cycles Stability and safety while maintaining electrochemical properties.

CN115881959BActive Publication Date: 2024-11-19BEIJING WELION NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111163141.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-30
Publication Date
2024-11-19
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

Due to the insufficient thermal stability and chemical stability of the organic liquid electrolyte used in lithium-ion batteries, it is easy to cause thermal runaway under conditions such as overcharge, short circuit, needle puncture, and high temperature. The existing phosphorus-based flame retardants take effect at high temperatures. It cannot fundamentally suppress the battery temperature and affect the battery performance.

Method used

Blend phosphorus-based monomers containing a ring-like structure in the electrode slurry and polymerize in situ to form electrode sheets containing phosphorus-based polymer materials to form thin polymer layers to protect active material particles and lower the surface of electrode particles Activity, inhibits the side reaction between active materials and electrolytes, and improves battery safety performance.

Benefits of technology

It significantly reduces the battery cell surface temperature, avoids fire and explosion, improves the cycle stability and safety of the battery, and maintains good electrochemical performance and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115881959B_ABST
    Figure CN115881959B_ABST
Patent Text Reader

Abstract

The present application provides an electrode sheet for lithium battery and a preparation method thereof, comprising a current collector and an electrode material covered on the current collector, the electrode material comprising an electrode active material, a conductive agent and a binder, the electrode sheet for lithium battery is a positive electrode sheet and / or a negative electrode sheet, the electrode material further comprises a phosphorus-based polymer material formed by monomer polymerization; the mass proportion of the phosphorus-based polymer material in the electrode material is 0.06-15%. The polymer material containing phosphorus groups and cyclic structures provided in the present application can be applied to batteries, and plays a role in improving battery safety, improving battery ion transmission, improving battery cycle stability, and extending battery service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to an electrode sheet for a lithium battery and a preparation method thereof. Background Art

[0002] Lithium-ion batteries (LIBs) have the advantages of high energy density, long cycle life, low self-discharge rate and no memory effect, and have broad application prospects in the field of new energy electric vehicles. With the continuous development of science and technology, the requirements for the performance of lithium-ion batteries are getting higher and higher. With the continuous improvement of battery energy density, safety issues are becoming increasingly prominent.

[0003] Lithium-ion batteries face serious safety hazards mainly because the electrolyte they use is an organic liquid electrolyte, which has insufficient thermal and chemical stability, making the battery prone to thermal runaway under conditions such as overcharging, short circuit, puncture, and high temperature. At present, the electrolytes widely used in lithium-ion batteries are carbonate or ether electrolytes. In order to improve their safety, phosphorus-based compounds can be added to the electrolyte as flame retardants. Phosphorus-based flame retardants can produce phosphorus-based free radicals at high temperatures, cut off the chain reaction during the combustion of the electrolyte, and thus have a flame retardant effect to a certain extent. However, these phosphorus-based flame retardants usually can only exert their flame retardant effect at temperatures above 200°C; in addition, due to their properties such as high viscosity, high freezing point, chemical or electrochemical instability, they can only be used as additives and cannot fundamentally inhibit the temperature rise of the battery; and generally speaking, a large amount of phosphorus-based compounds need to be added to achieve good results. The addition of excessive phosphorus-based compounds often has a negative impact on other aspects of the battery performance, such as reducing energy density, charge and discharge rate, cycle stability, etc., thereby greatly reducing the overall performance of the battery.

[0004] Therefore, it is urgent to develop a comprehensive solution that can suppress thermal runaway of battery cells, improve the safety of electrodes and battery cells, and ensure that the battery cells have good electrochemical performance. Summary of the invention

[0005] In order to solve the above problems, the present application provides an electrode sheet for lithium batteries, which is prepared by mixing a phosphorus-based monomer containing a ring structure with an electrode slurry, coating it on a current collector, and polymerizing it in situ to generate an electrode sheet for lithium batteries containing a phosphorus-based polymer material. The in-situ mixing method in the electrode slurry is adopted to coat the surface of the electrode active material particles with a thin layer of polymer material containing phosphorus groups. Compared with general polymer electrolytes, the polymer layer has higher thermal stability and electrochemical stability, which can effectively reduce the surface activity of the electrode particles, reduce the direct contact between the active material particles and the electrolyte, inhibit the side reaction between the active material and the electrolyte, and improve the battery safety performance; in addition, the polymer layer can maintain a low interface impedance during the battery cycle, and at the same time, homogenize the ion flow, so that the electrode has good capacity performance and cycle stability, and ensures the electrochemical performance of the battery.

[0006] According to one aspect of the present application, there is provided an electrode sheet for a lithium battery, comprising a current collector and an electrode material covered on the current collector, the electrode material comprising an electrode active material, a conductive agent and a binder, the electrode sheet for a lithium battery is a positive electrode sheet and / or a negative electrode sheet; the electrode material further comprises a phosphorus-based polymer material formed by polymerization of monomers; the mass proportion of the phosphorus-based polymer material in the electrode material is 0.06 to 15%; the monomer comprises a monomer A; the monomer A is at least one of the compounds shown in formula I,

[0007]

[0008] Wherein, M1 is selected from any one of C, N, P, S, and Si; R1 to R4 are independently selected from any one of a chain or a ring having no, containing or not containing a substituent, and when R1 is selected from a chain containing or not containing a substituent, the chain is a pure carbon chain or a carbon chain containing only one heteroatom; represents a cyclic structure; A1 represents that any position of the cyclic structure can be substituted by a substituent.

[0009] Optionally, R1 contains at least one unsaturated bond and / or at least one heteroatom; the heteroatom includes N, O, P, S, Si, and F; R3 to R4 are independently selected from any one of none, a saturated carbon chain consisting of 1 to 10 carbon atoms, or an unsaturated carbon chain.

[0010] Preferably, R3 is selected from or -OR, R is selected from any one of H, Li, a halogen atom, a chain or a ring with or without a substituent;

[0011] Preferably, the OR is OLi;

[0012] Preferably, the chain or ring containing or not containing a substituent is a chain or ring consisting of 1 to 8 atoms.

[0013] Optionally, the monomer further comprises a monomer B; the monomer B is selected from at least one of the compounds shown in formula II,

[0014]

[0015] Wherein, M3 is selected from C, N, P, S, Si; R 12 -R 14 Independently selected from any one of a chain or a ring with no substituent, with substituent or without substituent.

[0016] Optionally, R 14 It is selected from a ring or a chain containing at least one heteroatom, and any position of the ring or the chain can be substituted by a substituent.

[0017] Optionally, the molar ratio of the monomer B to the monomer A is α, wherein 0<α≤1.

[0018] Optionally, the monomer and the initiator are added during the slurry mixing process of the electrode material, and polymerized in situ to form the phosphorus-based polymer material.

[0019] Optionally, the weight fractions of the components in the electrode material are: 80-99 parts of electrode active material, 0.5-10 parts of conductive agent, 0.5-10 parts of binder, and 0.1-15 parts of monomer.

[0020] According to another aspect of the present application, there is provided a method for preparing an electrode sheet for a lithium battery as described above, wherein the preparation method is in-situ polymerization.

[0021] Optionally, the preparation method comprises:

[0022] (1) taking the above-mentioned portions of electrode active material, conductive agent, binder, monomer, and initiator, and mixing them uniformly to prepare a mixed slurry;

[0023] (2) coating the mixed slurry on a current collector and polymerizing the mixed slurry in situ to obtain the electrode sheet for a lithium battery;

[0024] The conditions of in-situ polymerization are as follows: the in-situ polymerization temperature is 55 to 125° C., and the in-situ polymerization time is 0.1 to 30 min.

[0025] The mass of the initiator is 0.1% to 2% of the mass of the monomer; the coating condition is: the coating speed is 0.5 m / min to 70 m / min.

[0026] According to another aspect of the present application, a battery is provided, comprising at least one of the electrode sheet for a lithium battery as described above and the electrode sheet for a lithium battery obtained by any of the preparation methods as described above.

[0027] Technical effect:

[0028] (1) The present application provides a novel lithium battery electrode sheet system, that is, a monomer containing a phosphorus group and a ring structure is mixed into an electrode slurry, and an electrode sheet containing a phosphorus-based polymer material is obtained through in-situ polymerization. The phosphorus-based polymer material has a protective effect on the active material on the surface of the electrode sheet, can reduce the surface activity of the active particles of the electrode sheet, and inhibit the temperature rise of the battery, thereby significantly reducing the surface temperature of the battery cell, avoiding the danger of fire and explosion of the battery; and achieving the condition of taking into account high energy density, greatly improving the safety of the battery. It also has a strong anti-extrusion ability and can maintain the structure and performance of the battery itself, thereby improving the safety of the battery, improving the cycle stability of the battery, and extending the service life of the battery.

[0029] (2) The present application uses an in-situ blending method in the electrode slurry to coat the surface of the electrode particles with a thin layer of polymer material containing phosphorus groups and cyclic structures. Compared with general polymer electrolytes, this polymer layer has higher thermal stability and electrochemical stability, which can effectively reduce the surface activity of the electrode particles, reduce the direct contact between the active material particles and the electrolyte, inhibit the side reactions between the active material and the electrolyte, and improve the battery safety performance; in addition, the polymer layer can maintain a low interfacial impedance during the battery cycle, while homogenizing the ion flow, so that the electrode has good capacity and cycle stability, and ensures the electrochemical performance of the battery. In addition, the in-situ curing preparation process is simple, safe and environmentally friendly, greatly reducing the use and emission of organic solvents, compatible with existing liquid battery processes, and easy to quickly promote industrialization. Compared with the non-in-situ curing process, the in-situ curing process can better improve the battery safety and electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a comparison chart of battery cycle curves of battery 1-1, battery 1-2, battery 1-5 and blank battery 1 of the present application;

[0031] Figure 2 It is a graph of battery puncture test results of battery 1-1(a), battery 1-2(b), battery 12-1(c), blank battery 1(d), battery 1-11(e) and battery 1-15(f) of the present application. DETAILED DESCRIPTION

[0032] The specific implementation of the present application is described below in conjunction with the accompanying drawings.

[0033] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. In addition, the reagents, materials and operating procedures used herein are reagents, materials and conventional procedures widely used in the corresponding fields. At the same time, in order to better understand the present invention, the definitions and explanations of the relevant terms are provided below.

[0034] In the embodiments of the present application, the polymerization degrees p and n of the polymer units in the polymer material structure can be calculated using the number average molecular weight method.

[0035] The number-average molecular weight is the most commonly used method for calculating the degree of polymerization. Polymer materials are composed of polymer units with the same chemical composition but different degrees of polymerization. The number-average molecular weight (Mn) can be obtained by averaging the number of molecules. Number-average molecular weight = sum of molecular weights of each component * number of moles of component / total number of moles. The calculation formula of number-average molecular weight is prior art and will not be described in detail here.

[0036] In this example, the H NMR spectrum 1 In H NMR, s represents a singlet, d represents a doublet, t represents a triplet, q represents a quartet, m represents a multiplet (multiplet greater than four, such as a quintet, sextet, etc.), dd represents a doublet, and dt represents a doublet; the number before the bracket represents the chemical shift, and the number before H in the bracket represents the number of H, such as 2.22 (s, 2H), which means that there are two Hs with a chemical shift of 2.22, and the peak is a singlet. Other situations can be deduced by analogy and will not be repeated.

[0037] In this example, MS (ESI) m / z …… (MH) + Represents mass spectrum.

[0038] In the embodiments of the present application, the corresponding substances of the English abbreviations are as follows: ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC); lithium nitrate (LiNO3), fluoroethylene carbonate (FEC), diethylene sulfate (DTD), lithium tetrafluorooxalate phosphate (LiPC2O2F4), 1,3-propane sultone (1,3-PS), lithium difluorophosphate (LiPO2F2), vinylene carbonate (VC); lithium difluorooxalatoborate (LiODFB), lithium hexafluorophosphate (LiPF6), lithium bis(fluoromethylsulfonyl)imide (LiFSI); azobisisobutyronitrile (AIBN), dibenzoyl peroxide (BPO).

[0039] In the embodiments of the present application, 0.5C / 0.5C means charging at a rate of 0.5C and discharging at a rate of 0.5C.

[0040] In the present application, monomers for preparing phosphorus-based polymer materials are mixed in positive and negative electrode slurries, and through an in-situ curing process, pole pieces containing polymer materials are formed to further prepare the battery.

[0041] Wherein, the battery assembly also includes electrodes, a separator and an electrolyte membrane.

[0042] It should be noted that the application methods shown in the following examples are only preferred application methods for the monomer / battery material. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention. In addition, unless otherwise specified, all reagents used in the following examples are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also easily obtained by those skilled in the art. The operation methods without specific conditions in the following examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0043] Example 1

[0044] A lithium battery electrode sheet comprises a current collector and an electrode material covering the current collector, wherein the electrode material comprises an electrode active material, a conductive agent and a binder, and the lithium battery electrode sheet is a positive electrode sheet and / or a negative electrode sheet; the electrode sheet also comprises a phosphorus-based polymer material formed by monomer polymerization; the mass proportion of the phosphorus-based polymer material in the electrode material is 0.06 to 15%.

[0045] Optionally, the mass proportion of the phosphorus-based polymer material in the electrode material is 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or any two of the values.

[0046] Preferably, the phosphorus-based polymer material accounts for 0.1-5% by mass in the electrode material.

[0047] Optionally, the mass proportion of the phosphorus-based polymer material in the electrode material is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 3%, 3.5%, 4%, 4.5%, 5% or any two of the values.

[0048] If the content of phosphorus-based polymer material is less than 0.06%, it is difficult to coat a thin layer of phosphorus-containing polymer material on the surface of the electrode active material particles, and the improvement of battery safety is not obvious; if the content of phosphorus-based polymer material is greater than 15%, although it can greatly improve the safety of the battery, it will reduce the energy density and cycle performance of the battery, so it is preferably 0.06-15%, and more preferably 0.1-5%.

[0049] Optionally, the monomer and the initiator are added during the slurry mixing process of the electrode material, and polymerized in situ to form the phosphorus-based polymer material.

[0050] Optionally, the monomer includes monomer A; the monomer A is at least one of the compounds shown in formula I,

[0051]

[0052] Wherein, M1 is selected from any one of C, N, P, S, and Si; R1 to R4 are independently selected from any one of a chain or a ring having no, containing or not containing a substituent, and when R1 is selected from a chain containing or not containing a substituent, the chain is a pure carbon chain or a carbon chain containing only one heteroatom; represents a cyclic structure; A1 represents that any position of the cyclic structure can be substituted by a substituent.

[0053] Alternatively, "containing only one heteroatom" means that the chain may contain one or more heteroatoms, but all the heteroatoms contained therein are of the same type, for example, it may contain one or more oxygen atoms but does not contain any other heteroatoms.

[0054] Optionally, R1-R4 are independently selected from a chain, wherein the chain is a chain of 1 to 15 atoms;

[0055] Preferably, the chain is a chain of 1 to 10 atoms,

[0056] Preferably, the chain is a chain of 2 to 6 atoms,

[0057] Optionally, the chain includes at least one of a saturated carbon chain, an unsaturated carbon chain, a saturated hetero chain, and an unsaturated hetero chain.

[0058] Optionally, the atoms located on the chain are selected from at least one of C, S, N, O, P, B or Si.

[0059] Optionally, R3-R4 are independently selected from any one of none, a saturated carbon chain consisting of 1 to 10 carbon atoms, or an unsaturated carbon chain.

[0060] Optionally, R1-R4 independently contain a ring, and the ring is a three- to eighteen-membered ring.

[0061] Preferably, the ring is a four- to ten-membered ring.

[0062] Preferably, the ring is a five- to eight-membered ring, such as a five-membered ring or a six-membered ring.

[0063] Optionally, the ring includes a single ring, a linked ring, a combined ring, a bridged ring or a spiro ring.

[0064] Optionally, the atoms located on the ring are selected from C, P, S, Si, N or O.

[0065] Optionally, the monocyclic ring includes at least one of a saturated carbocyclic ring, an unsaturated carbocyclic ring, a saturated heterocyclic ring, an unsaturated heterocyclic ring (—C═O), an aromatic carbocyclic ring, and an aromatic heterocyclic ring.

[0066] Optionally, the substituents include: at least one of H, a halogen atom, =O, =S, an alkyl group, a heteroalkyl group, an alkenyl group, a heteroalkenyl group, an alkynyl group, a heteroalkynyl group, a hydroxyl group, a carbonyl group, an aldehyde group, a carbonate group, a haloformyl group, a carboxyl group, an ester group, a peroxy group, an amine group (primary amine, secondary amine, tertiary amine, quaternary ammonium salt), an imino group (C=N), an imide (C(=O)NC(=O)), an azo group, a nitrate ester (RONO2), a phosphate group, a thioether group, a disulfide group, a cyano group, a sulfonic acid group, a sulfonyl group, an amide group, a nitro group, a pyridyl group, an acyloxy group, a phenyl group, a benzyl group, a benzyloxy group, a phenoxy group, an acetyl group, a benzoyl group, and a benzyloxycarbonyl group.

[0067] Optionally, any H in the above substituents may be substituted by halogen.

[0068] Optionally, the halogen includes fluorine, chlorine, bromine, iodine, and astatine.

[0069] Preferably, the halogen is fluorine.

[0070] Optionally, R1 contains at least one unsaturated bond and / or at least one heteroatom; the heteroatom includes N, O, P, S, Si, and F.

[0071] Preferably, the unsaturated bond is =0.

[0072] Preferably, R1 contains at least one Among them, -O is directly connected to P or M1 or indirectly connected through a chain and / or a ring, and -C=O is directly connected to P or M1 or indirectly connected through a chain and / or a ring.

[0073] The ester group between P and the double bond can effectively improve the electrochemical properties of the battery, such as the initial efficiency and capacity retention rate, and can improve the ability to suppress the temperature rise of the battery, further improving the safety of the battery and extending the service life of the battery.

[0074] Optionally, R1 is selected from -O or -C=O is directly connected to P.

[0075] The oxygen atom in the ester group is directly connected to phosphorus, which can make the charge flow within the molecule smoother and stabilize the entire molecular structure, thus having a better cooling effect.

[0076] Optionally, the P atom is connected to a C atom in the chain by at least one bond.

[0077] The P atom has at least one bond connected to the C atom on the chain, that is, there is a PC chain bond. Compared with all the bonds of all P atoms being directly connected to heteroatoms or rings, it can better promote the role of the phosphorus group and is more helpful to improve the safety of polymer materials.

[0078] Preferably, -C=O is indirectly linked to M1 via a chain consisting of 1 to 10 atoms.

[0079] Preferably, -C=O is indirectly connected to M1 through a chain consisting of 2-8 atoms, and the chain contains at least one heteroatom (the heteroatom only includes O). This helps to improve the mechanical properties of the material itself.

[0080] Optionally, R3 is selected from Or -OR, R is selected from any one of H, Li, halogen, a chain or a ring with or without a substituent.

[0081] The chain or ring containing or not containing a substituent is a chain or ring consisting of 1 to 8 atoms.

[0082] Preferably, the -OR is -OLi.

[0083] Optionally, R3 is selected from or -OLi.

[0084] Preferably, R3 is R4 is none.

[0085] The ring structure in the substituent directly connected to the P atom can improve the ability to suppress the temperature rise of the battery, thereby making the battery safer.

[0086] Preferably, the substituent represented by A1 is substituted by one or more halogens.

[0087] Preferably, the substituent represented by A1 is substituted by one or more F.

[0088] Preferably, the halogen atom is F and the chain contains at least one heteroatom.

[0089] Optionally, the The cyclic structure represented by is selected from a monocyclic or polycyclic ring, wherein the monocyclic ring is selected from a three- to twelve-membered saturated carbocyclic ring, a saturated heterocyclic ring, an unsaturated carbocyclic ring or an unsaturated heterocyclic ring, and the polycyclic ring is selected from a fused ring, a bridged ring, a spiro ring, and a linked ring formed by combining any two of the monocyclic rings.

[0090] Preferably, the monocyclic ring is selected from a five- to six-membered unsaturated carbocyclic ring or an unsaturated heterocyclic ring.

[0091] Preferably, the monocyclic ring is selected from a five- to six-membered unsaturated heterocyclic ring.

[0092] Optionally, the monomer further comprises a monomer B; the monomer B is selected from at least one of the compounds shown in formula II,

[0093]

[0094] Wherein, M3 is selected from C, N, P, S, Si; R 12 ~R 14 Independently selected from any one of a chain or a ring with no substituent, with substituent or without substituent.

[0095] Optionally, R 14 is selected from a ring or chain containing at least one heteroatom, any position of the ring or chain can be substituted by a substituent;

[0096] Preferably, R 14 is selected from a ring or chain containing at least two heteroatoms and containing at least one =0 in the ring or chain.

[0097] Preferably, R 14 Selected from Wherein, A1 and A2 represent that the atoms in the ring / chain can be substituted by a substituent.

[0098] Optionally, the molar ratio of the monomer B to the monomer A is α, wherein 0<α≤1.

[0099] Optionally, the molar ratio α of the monomer A to the monomer B is 0.01, 0.02, 0.025, 0.05, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1 or any ratio between any two ratios.

[0100] Optionally, the monomer and the initiator are added during the slurry mixing process of the electrode material, and polymerized in situ to form the phosphorus-based polymer material.

[0101] Optionally, the weight fractions of the components in the electrode material are: 80-99 parts of electrode active material, 0.5-10 parts of conductive agent, 0.5-10 parts of binder, and 0.1-15 parts of monomer.

[0102] Optionally, the electrode active material is 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts, 98 parts, 99 parts or any two parts.

[0103] Optionally, the conductive agent is 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts or any two parts.

[0104] Optionally, the binder is 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts or any two parts.

[0105] Optionally, the phosphorus-based polymer material is 0.1 parts, 0.5 parts, 0.8 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or any two parts.

[0106] Example 2

[0107] A method for preparing an electrode sheet for a lithium battery, the electrode sheet is consistent with the electrode sheet for a lithium battery described in Example 1, and will not be described in detail here. The preparation method is prepared by in-situ polymerization. Specifically, the preparation method comprises:

[0108] (1) taking the above-mentioned portions of electrode active material, conductive agent, binder, monomer, and initiator, and mixing them uniformly to prepare a mixed slurry;

[0109] (2) The mixed slurry is coated on a current collector, and in-situ polymerized at a temperature of 55 to 125° C. for a reaction time of 0.1 to 30 min to obtain the electrode sheet for a lithium battery.

[0110] Optionally, the in-situ polymerization temperature is 55°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 125°C or any two of the above values.

[0111] Optionally, the in situ polymerization time is 0.1 min, 0.2 min, 0.3 min, 0.4 min, 0.5 min, 0.6 min, 0.7 min, 0.8 min, 0.9 min, 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min, 30 min or any two of the numerical values.

[0112] Optionally, the mass of the initiator is 0.1% to 2% of the mass of the monomer; the coating condition is: the coating speed is 0.5 m / min to 70 m / min.

[0113] Optionally, the mass of the initiator is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% of the mass of the monomer or any two of the values.

[0114] Optionally, the coating speed is 0.5 m / min, 0.6 m / min, 0.7 m / min, 0.8 m / min, 0.9 m / min, 1 m / min, 2 m / min, 3 m / min, 4 m / min, 5 m / min, 6 m / min, 7 m / min, 8 m / min, 9 m / min, 10 m / min, 20 m / min, 30 m / min, 40 m / min, 50 m / min, 60 m / min, 70 m / min or any two of the values.

[0115] Optionally, the mass ratio of the electrode active material, the conductive agent and the binder is (80-99): (0.5-10): (0.1-10).

[0116] Optionally, the initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, dibenzoyl peroxide, tert-butyl perbenzoate, and methyl ethyl ketone peroxide.

[0117] Optionally, the method for preparing the electrode sheet for a lithium battery comprises:

[0118] (1) adding electrode active materials, conductive agents, binders, monomers and initiators into a solvent and mixing them evenly to obtain a mixed slurry with a certain fluidity; (2) coating the mixed slurry in step (1) onto a current collector, controlling the coating speed to be 0.5 m / min to 70 m / min, baking at 55 to 125° C. to initiate in-situ polymerization of the monomers for a time of 0.1 to 30 min, and then rolling to obtain an electrode plate.

[0119] Optionally, the solvent is an organic solvent.

[0120] Optionally, the organic solvent is selected from at least one of ethylene carbonate, fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl formate, ethyl formate, propyl formate, butyl formate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, δ-valerolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 2-methyl-1,3-dioxolane, ethylene glycol dimethyl ether, polyethylene glycol, cyclopentane, dimethyl sulfoxide, triethylene glycol dimethyl ether, fluorinated 1,4-dimethoxybutane, bis(2,2,2-trifluoroethyl) ether, tetramethylsilane, and tetraethylene glycol dimethyl ether.

[0121] In the slurry of the present application, there is no limitation on the manner and order of adding the electrode active material, conductive agent, binder, monomer and initiator, and they can be added together or in batches.

[0122] Preferably, the electrode active material and the conductive agent are first added to the solvent, and then the monomer, the initiator and the binder are added after being mixed evenly.

[0123] This is because during the mixing process, the material will have a temperature rise, which will trigger in-situ polymerization of some monomers. In order to reduce polymerization, the monomer and initiator can be added in the latter order. In addition, when CMC and SBR are used as negative electrode binders, SBR is prone to demulsification due to long-term high-speed stirring, which will destroy its structure and reduce adhesion. Therefore, SBR is added last and stirred at a low speed.

[0124] Optionally, the mixed slurry further includes at least one of an auxiliary agent and an additive.

[0125] Optionally, the auxiliary agent is selected from at least one of lithium salts, inorganic oxide particles and fast ion conductors.

[0126] Optionally, the lithium salt is selected from one or more of lithium trifluoromethanesulfonate (LiCF3SO2), lithium bis(trifluoromethanesulfonic acid)imide (LiN(CF3SO2)2), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium chloride (LiCl), lithium iodide (LiI), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium hexafluoroarsenate (LiAsF6).

[0127] The inorganic particles are selected from SiO2, ZrO2, Al2O3, TiO2, BaTiO3, CeO2, CuO, ZnO, MnO, MnO2, silicates, aluminosilicates, borosilicates and formula A x B y O z At least one inorganic particle selected from the group consisting of an oxygen-containing acid salt of, or any one of the functionalized above inorganic particles, wherein A is an alkali metal or an alkaline earth metal, B is selected from the group consisting of Al, Mn, Si, Ti, Zn, Zr, Fe and Cu, and x, y, z are the numbers of corresponding atoms so that the total charge of the oxygen-containing acid salt is 0.

[0128] Optionally, the fast ion conductor is an oxide solid electrolyte; the oxide solid electrolyte particles include at least one of the following compounds: Li NASICON structure 1+x1 Al x1 Ge 2-x1 (PO4)3 or its isomorphous heteroatom doped compounds, Li 1+x2 Al x2 Ti 2-x2 (PO4)3 or its isomorphous heteroatom doped compounds, perovskite structured Li 3x3 La 2 / 3-x3 TiO3 or its isomorphous heteroatom doped compounds, Li 3 / 8 Sr 7 / 16 Ta 3 / 4 Hf 1 / 4 O3 or its isomorphous heteroatom doped compound, Li 2x4-y1 Sr 1-x4 Ta y1 Zr 1-y1 O3 or its isomorphous heteroatom doped compounds, antiperovskite structured Li 3-2x5 M x5 HalO, Li3OCl or its isomorphous heteroatom doped compounds, 2Li with LISICON structure 4-x6 Si 1-x6 Px6O4 or its isomorphous heteroatom doped compounds, Li 14 ZnGe4O16 or its isomorphous heteroatom-doped compound, Li in garnet structure 7-x7 La3Zr 2-x7 O 12 or its isomorphous heteroatom-doped compound; wherein, 0 < x1 ≤ 0.75, 0 < x2 ≤ 0.5, 0.06 ≤ x3 ≤ 0.14, 0.25 ≤ y1 ≤ 1, x4 = 0.75y1, 0 ≤ x5 ≤ 0.01, 0.5 ≤ x6 ≤ 0.6; 0 ≤ x7 < 1; M includes Mg 2+ , Ca 2+ , Sr 2+ or Ba 2+ or a combination of any one or at least two of them; Hal is Cl or I.

[0129] Optionally, the additive includes one or a combination of fluoroethylene carbonate, vinylene carbonate, trimethyl phosphate, triethyl phosphate, succinic anhydride, 18-crown-6, triphenyl phosphite, ethylene ethylene carbonate, trimethyl borate, lithium difluorobis(oxalato)phosphate, lithium tetrafluorobis(oxalato)phosphate, tributyl phosphate, biphenyl, vinylene sulfite, difluorodiphenylsilane, lithium bis(fluorosulfonyl)imide, tributyl borate, ethoxypentafluorocyclotriphosphazene, ethylene sulfate, lithium nitrate, 1,3-propane sultone, lithium difluorophosphate, diethyl sulfite, succinonitrile.

[0130] Optionally, the method for preparing the positive electrode sheet includes:

[0131] S1: Under the condition that the dew point temperature ≤ -30 °C, add the positive electrode active material, conductive agent, binder, polymerizable monomer and initiator into the solvent and mix evenly in a mixer. During the mixing process, the temperature of the material will rise, which will cause in-situ polymerization of some monomers to obtain a mixed slurry with certain fluidity; S2: Coat the mixed slurry in S1 onto the current collector, control the coating speed to be 0.5 m / min to 70 m / min, bake at 55 to 125 °C for 0.1 to 20 min to initiate in-situ polymerization of the monomers, and then roll to obtain the positive electrode sheet.

[0132] Preferably, the dew point temperature ≤ -45 °C.

[0133] More preferably, the dew point temperature ≤ -60 °C.

[0134] The electrode sheet for the lithium battery includes a positive electrode sheet and / or a negative electrode sheet.

[0135] When preparing the positive electrode sheet, a positive electrode active material and a conductive agent and a binder suitable for the positive electrode need to be added.

[0136] Optionally, the positive electrode active material used in the positive electrode plate may include one or more of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium-rich manganese oxide. 0.83 Co 0.12 Mn 0.05 O2、LiNi 0.8 Co 0.15 Al 0.05 Any one of O2.

[0137] Lithium cobalt oxide LiCoO2 is abbreviated as LCO, LiNi 0.83 Co 0.12 Mn 0.05 O2 is abbreviated as Ni83, LiNi 0.8 Co 0.15 Al 0.05 O2 is abbreviated as NCA.

[0138] Optionally, the method for preparing the negative electrode sheet includes:

[0139] S3: adding negative electrode active material, conductive agent, binder, polymerizable monomer and initiator into solvent and mixing evenly in a mixer to obtain a mixed slurry with certain fluidity; S4: coating the mixed slurry in S3 onto the current collector, controlling the coating speed to be 0.5m / min~70m / min, baking at 55~125℃ for 0.1~20min to initiate in-situ polymerization of the monomer, and then rolling to obtain the negative electrode sheet.

[0140] Alternatively, the negative electrode active material may include one or more of graphite, silicon, soft carbon, hard carbon, silicon-carbon composite material, silicon-oxygen-carbon, lithium titanate, mesocarbon microbeads, molybdenum disulfide, silicon oxide, silicon, metallic lithium or metallic lithium alloy.

[0141] It should be noted that in the technical solution provided in the present application, no matter what synthesis method or process is used, a phosphorus-based polymer material as shown in Formula III, Formula IV or Formula V can be formed by the reaction of monomer A itself or the reaction between monomer A and monomer B. If in certain special cases, other products are obtained by the reaction of monomer A itself or monomer A and monomer B, these products are also within the scope of protection of the present application.

[0142] Optionally, the phosphorus-based polymer material comprises one of the compounds having the structure of Formula III, Formula IV or Formula V,

[0143]

[0144] Wherein, m is selected from 0.01 to 1, indicating that there is one in every 1 / m -[M1-M2]-polymer units. Connected to M1 or M2; p is selected from an integer between 10-10000, representing the degree of polymerization of the -[M1-CH2]- polymerization unit; n is selected from an integer between 5-1000, representing the degree of polymerization of the -[M3-CH2]- polymerization unit.

[0145] Optionally, m is selected from 0.01 to 1, such as 0.02, 0.05, 0.1, 0.2, 0.3, 0.5, 0.8, and 1, which means that there is one in every 1 / m -[M1-M2]-polymer units. Connected to M1 or M2. Can be omitted when m is 1.

[0146] Preferably, m is selected from 0.1 to 1.

[0147] Optionally, p is selected from an integer between 10 and 10000, such as 10, 20, 50, 80, 100, 500, 1000, 2000, 3000, 5000, 6000, 8000, and 10000, which represents that there are p -[M1-M2]- polymerization units in the structure of Formula 1.

[0148] Preferably, p is selected from an integer between 30 and 8000.

[0149] Optionally, n is selected from an integer between 5 and 1000, such as 10, 20, 30, 50, 80, 100, 150, 200, 250, 300, 350, 400, 450, 500, 600, 800, 900, 1000, etc., indicating that there are n -[M3-M4]- polymerization units in the structure.

[0150] Preferably, n is 10-800.

[0151] Preferably, p>n.

[0152] Example 3

[0153] A battery comprises at least one of the electrode sheet for a lithium battery as described above and the electrode sheet for a lithium battery obtained according to any of the preparation methods as described above.

[0154] The battery can be a liquid battery, a hybrid solid-liquid battery or an all-solid-state battery (hybrid solid-liquid batteries and all-solid-state batteries are collectively referred to as solid-state batteries).

[0155] The battery comprises a battery cell and a packaging shell, wherein the battery cell comprises a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode. The positive electrode and / or the negative electrode is an electrode sheet for a lithium battery provided by the present invention or an electrode sheet for a lithium battery prepared according to the method of the present invention. The separator can be one of a polyolefin separator, a cellulose separator, a polyimide separator, a polyamide separator, an aramid separator, a PET non-woven separator, a ceramic coated separator, a solid electrolyte coated separator, and a PVDF coated separator; the packaging shell can be one of a soft-package aluminum-plastic film, a steel shell, an aluminum shell, and a cylinder.

[0156] In practical applications, the electrolyte may be an existing commercial electrolyte for lithium secondary batteries, or may be independently prepared. The present invention has no particular limitation on its composition and ratio.

[0157] Example 4

[0158] 1. Preparation of positive electrode slurry

[0159] The positive electrode active material, conductive agent, binder, and fast ion conductor are mixed uniformly according to the data ratios listed in Table 1 C1-C6 to obtain positive electrode slurries with a certain fluidity, which are named C1, C2, ... C6 respectively. Among them, the conductive agent is carbon nanotubes and conductive carbon black (CNT+Super-P, the mass ratio of the two is 1:2), and the binder is polyvinylidene fluoride (PVDF). The ratio is the mass ratio of the positive electrode active material, binder, conductive agent, and fast ion conductor.

[0160] The positive electrode materials are LiCoO2 (abbreviated as LCO), LiNi 0.83 Co 0.12 Mn 0.05 O2 (abbreviated as Ni83), LiNi 0.8 Co 0.15 Al 0.05 O2 (abbreviated as NCA). The fast ion conductor is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 (abbreviated as LATP), Li 6.4 LqCy 1.6 Ta 0.6 O 12 (abbreviated as LLZO).

[0161] Table 1 Components and ratios of positive electrode slurry

[0162]

[0163] 2. Preparation of negative electrode slurry

[0164] Add the negative electrode active material, conductive agent and binder to deionized water according to the data listed in Table 2 and mix and stir evenly to obtain negative electrode slurries with certain fluidity, which are named F1, F2 and F3 respectively; or directly use metal lithium as the negative electrode F4. The ratio is the mass ratio of the negative electrode active material, the binder and the conductive agent.

[0165] Table 2 Components and ratios of negative electrode slurry

[0166] serial number Negative electrode active material Conductive agent Binder Proportion F1 Silicon Oxygen Carbon CNT+Super-P CMC+SBR 96:2:2 F2 Natural graphite CNT+Super-P CMC+SBR 96:2:2 F3 Silicon Carbon CNT+Super-P CMC+SBR 96:2:2 F4 Lithium Metal —— —— ——

[0167] The silicon-carbon material comes from Liyang Tianmu Pioneer Battery Material Technology Co., Ltd., SL450A-SOC; the silicon-oxygen-carbon material comes from BYD New Energy Materials Co., Ltd., S450-2A; the binder is sodium carboxymethyl cellulose and styrene-butadiene rubber (CMC+SBR).

[0168] 3. Diaphragm

[0169] Table 3 Diaphragm

[0170]

[0171]

[0172] 4. Electrolyte

[0173] In practical applications, the electrolyte may be an existing commercial electrolyte for lithium secondary batteries, or may be independently prepared. The present invention has no particular limitation on its composition and ratio.

[0174] Table 4 Preparation of electrolyte

[0175]

[0176] Preparation method of blank battery:

[0177] As shown in Table 5-1, the negative electrode active material, conductive agent and binder are mixed evenly to form a negative electrode slurry, which is then coated on the copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , control the coating speed, blow dry and roll press to obtain a blank negative electrode sheet.

[0178] As shown in Table 5-1, the positive electrode active material, binder, conductive agent, and fast ion conductor are mixed evenly to form a positive electrode slurry, which is then coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm 2 , blow dry and roll press to obtain a blank positive electrode sheet.

[0179] As shown in Table 5-1, the negative electrode sheets, positive electrode sheets and separators are stacked and baked to obtain dry cells, and then the electrolyte is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the cell to be fully soaked, thereby obtaining a blank battery.

[0180] Experimental Example 1-1

[0181] Monomer A1: Monomer B1:

[0182] Preparation method: Monomer A1: by (CAS:79-41-4) and (CAS: 1707-03-5) undergoes esterification reaction under acid catalysis to obtain monomer A1.

[0183] Monomer B1: Under nitrogen protection, add 0.2 mmol 2mL dry dichloromethane was cooled to 0℃, and 0.2mmol of acryloyl chloride was added dropwise. After addition, the mixture was stirred for 1h, and then returned to room temperature for 1h. 5mL of water was added, and the mixture was extracted with 3×5mL of dichloromethane. The organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, and distilled under reduced pressure. Column chromatography was used to obtain Under nitrogen protection, 0.2 mmol 2 mL of dry tetrahydrofuran was cooled to -78°C, and n-butyl lithium n-hexane solution was added dropwise. After the addition, the mixture was stirred for 30 minutes, returned to room temperature and stirred for 1 hour, and distilled under reduced pressure to obtain monomer B1.

[0184] H NMR spectrum of monomer A1 1 H NMR (300MHz, DMSO, δppm): 7.72 (s, 4H), 7.46 (s, 4H), 2.01 (s, 3H), 6.43 (s, 1H), 6.18 (s, 1H).

[0185] H NMR spectrum of monomer B1 1 H NMR (300MHz, DMSO, δppm): 4.31 (q, 2H), 4.47 (t, 2H), 2.01 (s, 3H), 6.48 (s, 1H), 6.40 (s, 1H).

[0186] Preparation method of negative electrode sheet 1-1 and battery 1-1:

[0187] As shown in Table 5, monomers A1, B1 and initiator AIBN were mixed into the prepared negative electrode slurry F1 and mixed evenly, and coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2, control the coating speed, polymerize in situ at a certain temperature for a period of time, blow dry, and roll press to obtain the negative electrode sheet 1-1.

[0188] The positive electrode slurry C1 is coated on the aluminum foil, and the surface capacity of the control electrode is 5 mAh / cm 2 , blow drying, and roller pressing to obtain a positive electrode sheet 1-1.

[0189] The negative electrode sheet 1-1, the positive electrode sheet 1-1 and the separator S1 containing the battery material are stacked and baked to obtain a dry battery cell, and then the electrolyte E1 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 1-1 containing battery materials.

[0190] Experimental Example 1-2

[0191] Preparation method of negative electrode sheet 1-2 and battery 1-2:

[0192] The preparation method of the negative electrode sheet 1-2 is substantially the same as the preparation method of the negative electrode sheet 1-1, except that the monomers A1 and B1 are replaced by the monomer A1, and the remaining steps are the same to obtain the negative electrode sheet 1-2;

[0193] The preparation method of battery 1-2 is substantially the same as that of battery 1-1, except that negative electrode plate 1-1 is replaced by negative electrode plate 1-2, and the remaining steps are the same to obtain battery 1-2.

[0194] Comparative Examples 1-3

[0195] Monomer K1:

[0196] The difference between the monomer K1 and the monomer A1 is that K1 does not contain a cyclic structure.

[0197] Preparation method of negative electrode sheet 1-3 and battery 1-3:

[0198] The preparation method of the negative electrode sheet 1-3 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 is replaced by the monomer K1, and the remaining steps are the same to obtain the negative electrode sheet 1-3;

[0199] The preparation method of battery 1-3 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-3, and the remaining steps are the same to obtain battery 1-3.

[0200] Comparative Examples 1-4

[0201] Monomer K2:

[0202] The difference between the monomer K2 and the monomer A1 is that K2 does not contain a cyclic structure.

[0203] Preparation method of negative electrode sheet 1-4 and battery 1-4:

[0204] The preparation method of the negative electrode sheet 1-4 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 is replaced by the monomer K2, and the remaining steps are the same to obtain the negative electrode sheet 1-4;

[0205] The preparation method of battery 1-4 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-4, and the remaining steps are the same to obtain battery 1-4.

[0206] Comparative Examples 1-5

[0207] Monomer D1:

[0208] The difference between the monomer D1 and the monomer A1 is that D1 does not contain a phosphorus group.

[0209] Preparation method of negative electrode sheet 1-5 and battery 1-5:

[0210] The preparation method of the negative electrode sheet 1-5 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 is replaced by the monomer D1, and the remaining steps are the same to obtain the negative electrode sheet 1-5;

[0211] The preparation method of battery 1-5 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-5, and the remaining steps are the same to obtain battery 1-5.

[0212] Comparative Examples 1-6

[0213] Monomer D2:

[0214] The difference between the monomer D2 and the monomer A1 is that D2 does not contain a phosphorus group.

[0215] Preparation method of negative electrode sheet 1-6 and battery 1-6:

[0216] The preparation method of the negative electrode sheet 1-6 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 is replaced by the monomer D2, and the remaining steps are the same to obtain the negative electrode sheet 1-6;

[0217] The preparation method of battery 1-6 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-6, and the remaining steps are the same to obtain battery 1-6.

[0218] Comparative Examples 1-7

[0219] Monomer K3:

[0220] Preparation method of negative electrode sheet 1-7 and battery 1-7:

[0221] The preparation method of the negative electrode sheet 1-7 is substantially the same as the preparation method of the negative electrode sheet 1-1, except that the monomers A1 and B1 are replaced with monomers A1 and K3, and the remaining steps are the same to obtain the negative electrode sheet 1-7;

[0222] The preparation method of battery 1-7 is substantially the same as that of battery 1-1, except that negative electrode plate 1-1 is replaced with negative electrode plate 1-7. The remaining steps are the same to obtain battery 1-7.

[0223] Comparative Examples 1-8

[0224] Preparation method of negative electrode sheet 1-8 and battery 1-8:

[0225] The preparation method of the negative electrode sheet 1-8 is substantially the same as the preparation method of the negative electrode sheet 1-1, except that the monomers A1 and B1 are replaced by the monomer B1, and the remaining steps are the same to obtain the negative electrode sheet 1-8;

[0226] The preparation method of battery 1-8 is substantially the same as that of battery 1-1, except that negative electrode plate 1-1 is replaced with negative electrode plate 1-8, and the remaining steps are the same to obtain battery 1-8.

[0227] Comparative Examples 1-9

[0228] Preparation method of negative electrode sheet 1-9 and battery 1-9:

[0229] The preparation method of the negative electrode sheet 1-9 is substantially the same as the preparation method of the negative electrode sheet 1-1, except that the initiator AIBN in Experimental Example 1-1 is not added, and the remaining steps are the same to obtain the negative electrode sheet 1-9;

[0230] The preparation method of battery 1-9 is substantially the same as that of battery 1-1, except that negative electrode plate 1-1 is replaced with negative electrode plate 1-9. The remaining steps are the same to obtain battery 1-9.

[0231] Due to the lack of initiator, monomer A1 and monomer B1 do not polymerize.

[0232] Comparative Examples 1-10

[0233] Preparation method of negative electrode sheet 1-10 and battery 1-10:

[0234] The preparation method of the negative electrode sheet 1-10 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the initiator AIBN in Experimental Example 1-2 is not added, and the remaining steps are the same to obtain the negative electrode sheet 1-10;

[0235] The preparation method of battery 1-10 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-10, and the remaining steps are the same to obtain battery 1-10.

[0236] Due to the lack of initiator, monomer A1 does not polymerize.

[0237] Comparative Examples 1-11

[0238] Preparation method of negative electrode sheet 1-11 and battery 1-11:

[0239] The preparation method of the negative electrode sheet 1-11 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 and AIBN are not added, and the remaining steps are the same to obtain the negative electrode sheet 1-11;

[0240] The preparation method of battery 1-11 is roughly the same as that of battery 1-2, except that the negative electrode plate 1-2 is replaced by the negative electrode plate 1-11, and the monomer A1 and the initiator AIBN are added to the electrolyte E1. The positive electrode plate, the negative electrode plate and the separator are stacked and baked to obtain a dry battery cell, and the above-mentioned electrolyte is injected into the battery cell to initiate in-situ polymerization of the monomer at 60°C. The remaining steps are the same to obtain battery 1-11.

[0241] Comparative Examples 1-12

[0242] Preparation method of negative electrode sheet 1-12 and battery 1-12:

[0243] The preparation method of the negative electrode sheet 1-12 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomers A1 and AIBN are not added. The remaining steps are the same. After obtaining the negative electrode sheet, a solution containing A1 and AIBN is applied to the surface of the negative electrode sheet, and in-situ polymerization is performed at a certain temperature to obtain a negative electrode sheet 1-12 having a phosphorus-based polymer material on the surface.

[0244] The preparation method of battery 1-12 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-12, and the remaining steps are the same to obtain battery 1-12.

[0245] Comparative Examples 1-13

[0246] Preparation method of negative electrode sheet 1-13 and battery 1-13:

[0247] The preparation method of the negative electrode sheet 1-13 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 is not added, and the remaining steps are the same to obtain the negative electrode sheet 1-13;

[0248] A solution containing A1 and AIBN is applied to the surface of the separator S1, and in-situ polymerization is initiated at 60° C. to obtain a separator 1-13 having a phosphorus-based polymer material on the surface;

[0249] The preparation method of battery 1-13 is substantially the same as that of battery 1-2. The negative electrode plate 1-2 is replaced by the negative electrode plate 1-13, and the diaphragm S1 is replaced by the diaphragm 1-13. The remaining steps are the same to obtain battery 1-13.

[0250] Comparative Examples 1-14

[0251] Preparation method of positive electrode sheet 1-14 and battery 1-14:

[0252] Applying a solution containing A1 and AIBN to the surface of the positive electrode sheet 1-1, initiating in-situ polymerization of the monomers at 60° C., and obtaining a positive electrode sheet 1-14 having a phosphorus-based polymer material on the surface;

[0253] The preparation method of battery 1-14 is substantially the same as that of battery 1-2, except that the negative electrode sheet 1-2 is replaced by the negative electrode sheet 1-13, and the positive electrode sheet 1-1 is replaced by the positive electrode sheet 1-14. The remaining steps are the same to obtain battery 1-14.

[0254] Comparative Examples 1-15

[0255] Preparation method of negative electrode sheet 1-15 and battery 1-15:

[0256] First, monomer A1 is in situ polymerized at 60°C under the action of initiator AIBN to obtain polymer material G1-15, and then polymer material G1-15 is mixed into negative electrode slurry F1 and mixed evenly. The remaining steps are roughly the same as the preparation method of negative electrode plate 1-2 to obtain negative electrode plate 1-15.

[0257] The preparation method of battery 1-15 is substantially the same as that of battery 1-2. The negative electrode plate 1-2 is replaced with the negative electrode plate 1-15. The remaining steps are the same to obtain battery 1-15.

[0258] Comparative Examples 1-16

[0259] Preparation method of electrolyte E1-16, negative electrode sheet 1-16 and battery 1-16:

[0260] Monomer A1 and AIBN were added to E1, stirred to form a uniform solution, and then in-situ polymerized at 60° C. to obtain polymer electrolyte E1-16.

[0261] The preparation method of the negative electrode sheet 1-16 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that the monomer A1 and AIBN are not added, and the remaining steps are the same to obtain the negative electrode sheet 1-16;

[0262] The preparation method of battery 1-16 is substantially the same as that of battery 1-2. The negative electrode plate 1-2 is replaced by the negative electrode plate 1-16, and the electrolyte E1 is replaced by the electrolyte E1-16. The remaining steps are the same to obtain battery 1-16.

[0263] Experimental Example 1-17

[0264] Preparation method of positive electrode sheet 1-17, negative electrode sheet 1-17 and battery 1-17:

[0265] The preparation method of the positive electrode sheet 1-17 is substantially the same as the preparation method of the positive electrode sheet 12-2, except that the monomer A12 is replaced by the monomer A1, and the remaining steps are the same to obtain the positive electrode sheet 1-17;

[0266] The preparation method of the negative electrode sheet 1-17 is substantially the same as the preparation method of the negative electrode sheet 12-2, except that the monomer A12 is replaced by the monomer A1, and the remaining steps are the same to obtain the negative electrode sheet 1-17;

[0267] The preparation method of battery 1-17 is roughly the same as that of battery 12-2, except that the positive electrode sheet 12-2 is replaced by the positive electrode sheet 1-17, and the negative electrode sheet 12-2 is replaced by the negative electrode sheet 1-17. The remaining steps are the same to obtain battery 1-17.

[0268] Comparative Examples 1-18

[0269] Monomer K4: triphenyl phosphate (TPP)

[0270] The preparation method of battery 1-18 is substantially the same as that of blank battery 1, except that K4 accounting for 0.8% by mass of the negative electrode active material is added to the electrolyte E1. The remaining steps are the same to obtain battery 1-18.

[0271] Comparative Examples 1-19

[0272] Preparation method of negative electrode sheet 1-19 and battery 1-19:

[0273] The preparation method of the negative electrode sheet 1-19 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that 0.8% of the monomer A1 of the electrode active material is replaced with 0.04% of the monomer A1, and the amount of the initiator is adjusted accordingly according to the amount of the monomer A1. The remaining steps are the same, and the negative electrode sheet 1-19 can be obtained.

[0274] The preparation method of battery 1-19 is substantially the same as that of battery 1-2, except that the negative electrode plate 1-2 is replaced by the negative electrode plate 1-19, and the remaining steps are the same to obtain battery 1-2.

[0275] Comparative Examples 1-20

[0276] Preparation method of negative electrode sheet 1-20 and battery 1-20:

[0277] The preparation method of the negative electrode sheet 1-20 is substantially the same as the preparation method of the negative electrode sheet 1-2, except that 0.8% of the monomer A1 of the electrode active material is replaced with 16% of the monomer A1, and the amount of the initiator is adjusted accordingly according to the amount of the monomer A1. The remaining steps are the same, and the negative electrode sheet 1-20 can be obtained.

[0278] The preparation method of battery 1-20 is substantially the same as that of battery 1-2, except that negative electrode plate 1-2 is replaced by negative electrode plate 1-20, and the remaining steps are the same to obtain battery 1-2.

[0279] Experimental Example 2-1

[0280] Monomer A2: Monomer B2:

[0281] Preparation method: Monomer A2 is an existing substance, CAS number is 60421-10-5;

[0282] The preparation method of monomer B2 is similar to that of monomer A1 in Example 1. (CAS: 79-10-7) and (CAS: 1433993-67-9) to obtain monomer B2;

[0283] Monomer A2 MS (ESI) m / z 593.15 (MH) + ; Monomer B2 MS (ESI) m / z 208.00 (MH) + .

[0284] Preparation method of negative electrode sheet 2-1 and battery 2-1:

[0285] As shown in Table 5, monomers A2, B2 (the molar ratio of B2 to A2 is 0.4) and initiator AIBN are mixed into the prepared negative electrode slurry F2 and mixed evenly, and then coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , controlling the coating speed, polymerizing in situ at a certain temperature for a period of time, air drying, and roller pressing to obtain a negative electrode sheet 2-1;

[0286] The positive electrode slurry C2 is coated on the aluminum foil, and the surface capacity of the control electrode is 5 mAh / cm2 , blow drying and roller pressing to obtain the positive electrode sheet 2-1.

[0287] The negative electrode sheet 2-1, the positive electrode sheet 2-1 and the separator S2 containing the battery material are stacked and baked to obtain a dry battery cell, and then the electrolyte E2 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 2-1 containing battery materials.

[0288] Experimental Example 2-2

[0289] Preparation method of negative electrode sheet 2-2 and battery 2-2:

[0290] The preparation method of the negative electrode sheet 2-2 is substantially the same as the preparation method of the negative electrode sheet 2-1, except that the monomers A2 and B2 are replaced by the monomer A2, and the remaining steps are the same to obtain the negative electrode sheet 2-2;

[0291] The preparation method of battery 2-2 is substantially the same as that of battery 2-1, except that negative electrode plate 2-1 is replaced by negative electrode plate 2-2, and the remaining steps are the same to obtain battery 2-2.

[0292] Comparative Examples 2-3

[0293] Preparation method of negative electrode sheet 2-3 and battery 2-3:

[0294] The preparation method of the negative electrode sheet 2-3 is substantially the same as the preparation method of the negative electrode sheet 2-1, except that the monomers A2 and B2 are not added, and the remaining steps are the same to obtain the negative electrode sheet 2-3;

[0295] The preparation method of battery 2-3 is roughly the same as that of battery 2-1. The negative electrode plate 2-1 is replaced with the negative electrode plate 2-3, and the monomers A2, B2 and the initiator AIBN are added to the electrolyte E2. The positive electrode plate, the negative electrode plate and the separator are stacked and baked to obtain a dry battery cell. The above electrolyte is injected into the battery cell, and the monomer is initiated to polymerize in situ at 60°C. The remaining steps are the same to obtain battery 2-3.

[0296] Experimental Example 3-1

[0297] Monomer A3: Monomer B3:

[0298] Preparation method: Monomer A3 is an existing substance, Reaxys ID: 32890736, MS (ESI) m / z 540.15 (MH) + .

[0299] Monomer B3: Add 0.2mmol of sulfonate substrate 1 and 2mL of dry dichloromethane to a 25mL Schlenk tube, freeze with liquid nitrogen, replace with nitrogen in vacuum, return to room temperature, add 0.2mmol of NBS under nitrogen protection, heat to 40℃ and stir for 8h, terminate the reaction, distill under reduced pressure, and obtain the intermediate with bromine substitution at the α-position of the olefin double bond of the sulfonate substrate by column chromatography. The bromine-substituted intermediate in the previous step is added to 2mL of dichloromethane, benzyltriethylammonium chloride (TEBAC) and 0.2mmol of NaF, and stir for 8h at 40℃. Cool to room temperature, add 5mL of water, extract with 3×5mL of dichloromethane, combine the organic phases, wash with saturated NaCl, dry with anhydrous sodium sulfate, filter, distill under reduced pressure, and obtain the fluorinated sulfonate intermediate by column chromatography.

[0300] Under nitrogen protection, 0.2 mmol of intermediate 2 was added to a 25 mL Schlenk tube, 200 μL (1 M) borane tetrahydrofuran complex was added dropwise, and the mixture was stirred at room temperature for 30 min. 70 μL 3 M sodium hydroxide was added first, followed by 20 μL hydrogen peroxide (30% wt), and the mixture was stirred for 30 min. 5 mL of dichloromethane and 5 mL of water were added, and 3×5 mL of dichloromethane was extracted. The organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, evaporated under reduced pressure, and column chromatography was performed to obtain the intermediate

[0301] Under nitrogen protection, 0.2 mmol of the intermediate was added to a 25 mL Schlenk tube. 0.2 mmol of acryloyl chloride was added dropwise to 2 mL of dry dichloromethane, stirred at room temperature for 30 min, the reaction was terminated, 5 mL of water was added, and the mixture was extracted with 3×5 mL of dichloromethane. The organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, distilled under reduced pressure, and column chromatography was performed to obtain monomer B3. MS (ESI) m / z 224.02 (MH) + .

[0302] Preparation method of negative electrode sheet 3-1 and battery 3-1:

[0303] As shown in Table 5, monomers A3, B3 (the molar ratio of B3 to A3 is 0.1) and initiator AIBN are mixed into the prepared negative electrode slurry F3 and mixed evenly, and then coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , control the coating speed, polymerize in situ at a certain temperature for a period of time, blow dry, and roll press to obtain the negative electrode sheet 3-1.

[0304] The positive electrode slurry C3 is coated on the aluminum foil, and the surface capacity of the control electrode is 5 mAh / cm 2 , blow drying and roller pressing to obtain the positive electrode sheet 3-1.

[0305] The negative electrode sheet 3-1, the positive electrode sheet 3-1 and the separator S2 containing the battery material are stacked and baked to obtain a dry battery cell, and then the electrolyte E3 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 3-1 containing battery materials.

[0306] Experimental Example 3-2

[0307] Preparation method of negative electrode sheet 3-2 and battery 3-2:

[0308] The preparation method of the negative electrode sheet 3-2 is substantially the same as the preparation method of the negative electrode sheet 3-1, except that the monomers A3 and B3 are replaced by the monomer A3, and the remaining steps are the same to obtain the negative electrode sheet 3-2;

[0309] The preparation method of battery 3-2 is substantially the same as that of battery 3-1, except that negative electrode plate 3-1 is replaced by negative electrode plate 3-2, and the remaining steps are the same to obtain battery 3-2.

[0310] Experimental Example 4-1

[0311] Monomer A4: Monomer B4:

[0312] Preparation method:

[0313] Monomer A4: Under nitrogen protection, add 0.2 mmol to a 25 mL Schlenk tube. 2 mL of dry tetrahydrofuran was cooled to -78°C, and 0.2 mmol of n-butyl lithium n-hexane solution was added dropwise. After the addition was completed, the mixture was stirred for half an hour, returned to room temperature, and distilled under reduced pressure to obtain monomer A4.

[0314] Monomer B4: Under nitrogen protection, add 0.2 mmol substrate into a 25 mL Schlenk tube. 2mL of 1,4-dioxane, 0.2mmol of liquid bromine and 3.6μL of water were added dropwise in sequence. After addition, the temperature was raised to 90℃ for reaction for 6h. 5mL of water was added and extracted with 3×5mL of dichloromethane. The organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, evaporated under reduced pressure, and column chromatography was performed to obtain the intermediate

[0315] Under nitrogen protection, 0.2 mmol of intermediate 4 and 2 mL of dry dichloromethane were added to a 25 mL Schlenk tube, cooled to 0 °C, and 0.2 mmol of DAST reagent (diethylaminosulfur trifluoride) was added. The reaction was continued for 1 h, and the intermediate was obtained by vacuum distillation and column chromatography. Will and NaOH were added to acetonitrile solvent containing 20% ​​water and heated at 80°C for 8h to obtain the intermediate

[0316] Under nitrogen protection, 0.2 mmol of the intermediate was added to a 25 mL Schlenk tube. Add 1 mL of dry dichloromethane, cool to 0°C, add dropwise a mixture of freshly prepared crotonoyl chloride and dichloromethane, react for 1 h after the addition is complete, return to room temperature to react for 1 h, add 5 mL of water, extract with 3×5 mL of dichloromethane, combine the organic phases, wash with saturated NaCl, dry over anhydrous sodium sulfate, filter, distill under reduced pressure, and obtain monomer B4 by column chromatography.

[0317] H NMR spectrum of monomer A4 1 H NMR (300MHz, DMSO, δppm): 7.24 (d, 2H), 7.31 (d, 2H), 7.26 (d, H), 2.95 (m, 2H), 4 .38(dd, 2H), 4.31(dd, 2H), 2.79(t, 2H), 2.01(s, 3H), 6.48(s, 1H), 6.40(s, 1H).

[0318] H NMR spectrum of monomer B4 1 H NMR (300MHz, DMSO, δppm): 6.62 (dd, 1H), 8.07 (dd, 1H), 2.92 (d, 2H), 6.07 (m, 1H), 5.25 (s, 1H), 5.32 (t, 1H).

[0319] Preparation method of negative electrode sheet 4-1 and battery 4-1:

[0320] As shown in Table 5, monomers A4, B4 (the molar ratio of B4 to A4 is 0.01) and initiator AIBN are mixed into the prepared negative electrode slurry F3 and mixed evenly, and coated on copper foil to control the electrode surface capacity of 5.3 mAh / cm 2 , control the coating speed, polymerize in situ at a certain temperature for a period of time, blow dry, and roll press to obtain the negative electrode sheet 4-1.

[0321] The positive electrode slurry C3 is coated on the aluminum foil, and the surface capacity of the control electrode is 5 mAh / cm 2 , blow drying and roller pressing to obtain the positive electrode sheet 4-1.

[0322] The negative electrode sheet 4-1, the positive electrode sheet 4-1 and the separator S1 containing the battery material are stacked and baked to obtain a dry battery cell, and then the electrolyte E4 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 4-1 containing battery materials.

[0323] Experimental Example 4-2

[0324] Preparation method of negative electrode sheet 4-2 and battery 4-2:

[0325] The preparation method of the negative electrode sheet 4-2 is substantially the same as the preparation method of the negative electrode sheet 4-1, except that the monomers A4 and B4 are replaced by the monomer A4, and the remaining steps are the same to obtain the negative electrode sheet 4-2;

[0326] The preparation method of battery 4-2 is substantially the same as that of battery 4-1, except that negative electrode plate 4-1 is replaced by negative electrode plate 4-2, and the remaining steps are the same to obtain battery 4-2.

[0327] Experimental Example 5-1

[0328] Monomer A5: Monomer B5:

[0329] Monomer A5 is an existing substance, CAS: 869483-26-1, MS (ESI) m / z 284.10 (MH) + .

[0330] Monomer B5 is an existing substance, CAS: 18133-42-1, MS (ESI) m / z 111.99 (MH) + .

[0331] Preparation method of positive electrode sheet 5-1 and battery 5-1:

[0332] According to the data listed in Table 5, under the condition of dew point ≤ -30°C, monomers A5, B5 (molar ratio of B5 to A5 is 0.5) and initiator BPO are mixed into the prepared positive electrode slurry C3 and mixed evenly, and coated on aluminum foil to control the surface capacity of the electrode to 5 mA h / cm 2 , control the coating speed, polymerize in situ at a certain temperature for a period of time, blow dry, and roll press to obtain the positive electrode sheet 5-1.

[0333] The negative electrode slurry F3 was coated on the copper foil, and the surface capacity of the control electrode was 5.3 mAh / cm 2 The negative electrode sheet 5-1 is obtained by air drying and roller pressing.

[0334] The positive electrode sheet 5-1, negative electrode sheet 5-1 and separator S1 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E5 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 5-1 containing battery materials.

[0335] Experimental Example 5-2

[0336] Preparation method of positive electrode sheet 5-2 and battery 5-2:

[0337] The preparation method of the positive electrode sheet 5-2 is substantially the same as the preparation method of the positive electrode sheet 5-1, except that the monomers A5 and B5 are replaced by the monomer A5, and the remaining steps are the same to obtain the positive electrode sheet 5-2;

[0338] The preparation method of battery 5-2 is substantially the same as that of battery 5-1, except that the positive electrode sheet 5-1 is replaced by the positive electrode sheet 5-2, and the remaining steps are the same to obtain battery 5-2.

[0339] Comparative Example 5-3

[0340] Preparation method of positive electrode sheet 5-3 and battery 5-3:

[0341] The preparation method of the positive electrode sheet 5-3 is substantially the same as the preparation method of the positive electrode sheet 5-1, except that the monomers A5, B5 and BPO are not added, and the remaining steps are the same to obtain the positive electrode sheet 5-3;

[0342] The preparation method of battery 5-3 is roughly the same as that of battery 5-1, except that the positive electrode plate 5-1 is replaced by the positive electrode plate 5-3, and monomers A5, B5 and initiator BPO are added to the electrolyte E5; the positive electrode plates, negative electrode plates and separators are stacked and baked to obtain a dry battery cell, the above-mentioned electrolyte is injected into the battery cell, and the monomers are initiated to polymerize in situ at 60°C. The remaining steps are the same to obtain battery 5-3.

[0343] Comparative Example 5-4

[0344] Preparation method of positive electrode sheet 5-4 and battery 5-4:

[0345] The preparation method of the positive electrode sheet 5-4 is substantially the same as the preparation method of the positive electrode sheet 5-2, except that the monomer A5 and BPO are not added, and the remaining steps are the same to obtain the positive electrode sheet 5-4;

[0346] The preparation method of battery 5-4 is substantially the same as that of battery 5-3, except that positive electrode plate 5-3 is replaced by positive electrode plate 5-4, and A5 and B5 added to electrolyte E5 are replaced by A5. The remaining steps are the same to obtain battery 5-4.

[0347] Experimental Example 6-1

[0348] Monomer A6: Monomer B6:

[0349] Preparation method: Monomer A6 is an existing substance, CAS 191105-63-2, MS (ESI) m / z 368.14 (MH) + .

[0350] Monomer B6: Pass The intermediate was obtained by fluorination Under nitrogen protection, 0.2 mmol of the intermediate was added to a 25 mL Schlenk tube. 2mL dry dichloromethane, 0.2mmol NBS, after adding, heat to 40℃ and stir to react for 8h, terminate the reaction, evaporate under reduced pressure, and obtain the intermediate by column chromatography

[0351] Add 0.2 mmol of intermediate into a 25 mL reaction tube 100 μL (3M) NaOH, stir at room temperature for 8 h, terminate the reaction, add 5 mL of dichloromethane and 5 mL of water, extract with 3×5 mL of dichloromethane, combine the organic phases, wash the organic phases with saturated NaCl, dry with anhydrous sodium sulfate, filter, distill under reduced pressure, and obtain the intermediate by column chromatography

[0352] Under nitrogen protection, 0.2 mmol of the intermediate was added to a 25 mL Schlenk tube. 2mL dichloromethane, cooled to 0℃, added 0.2mmol acryloyl chloride dropwise, reacted for 1h after addition, returned to room temperature for 1h, added 5mL water, extracted with 3×5mL dichloromethane, combined the organic phases, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, distilled under reduced pressure, and column chromatography to obtain the intermediate

[0353] Under nitrogen protection, add 0.2 mmol of intermediate 5 and 2 mL of dry tetrahydrofuran to a 25 mL Schlenk tube, cool to -78 °C, dropwise add 0.2 mmol of n-butyl lithium (n-hexane solution), react for 30 minutes after addition, return to room temperature, and distill under reduced pressure to obtain monomer B6. MS (ESI) m / z 188.02 (MH) + .

[0354] Preparation method of positive electrode sheet 6-1 and battery 6-1:

[0355] According to the data listed in Table 5, under the condition of dew point ≤ -30°C, monomers A6, B6 (molar ratio of B6 to A6 is 0.8) and initiator BPO are mixed into the prepared positive electrode slurry C3 and mixed evenly, and coated on aluminum foil to control the surface capacity of the electrode to 5 mAh / cm 2 , control the coating speed, polymerize in situ at a certain temperature for a period of time, blow dry, and roll press to obtain the positive electrode sheet 6-1.

[0356] The negative electrode slurry F3 was coated on the copper foil, and the surface capacity of the control electrode was 5.3 mAh / cm 2 The negative electrode sheet 6-1 is obtained by air drying and roller pressing.

[0357] The positive electrode sheet 6-1, negative electrode sheet 6-1 and separator S2 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E6 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 6-1 containing battery materials.

[0358] Experimental Example 6-2

[0359] Preparation method of positive electrode sheet 6-2 and battery 6-2:

[0360] The preparation method of the positive electrode sheet 6-2 is substantially the same as the preparation method of the positive electrode sheet 6-1, except that the monomers A6 and B6 are replaced by the monomer A6, and the remaining steps are the same to obtain the positive electrode sheet 6-2;

[0361] The preparation method of battery 6-2 is substantially the same as that of battery 6-1, except that positive electrode sheet 6-1 is replaced by positive electrode sheet 6-2, and the remaining steps are the same to obtain battery 6-2.

[0362] Comparative Example 6-3

[0363] Preparation method of positive electrode sheet 6-3 and battery 6-3:

[0364] The preparation method of the positive electrode sheet 6-3 is substantially the same as the preparation method of the positive electrode sheet 6-1, except that the monomers A6 and B6 are replaced by the monomer B6, and the remaining steps are the same to obtain the positive electrode sheet 6-3;

[0365] The preparation method of battery 6-3 is substantially the same as that of battery 6-1, except that positive electrode sheet 6-1 is replaced by positive electrode sheet 6-3, and the remaining steps are the same to obtain battery 6-3.

[0366] Comparative Example 6-4

[0367] Preparation method of positive electrode sheet 6-4 and battery 6-4:

[0368] Monomers A6 and B6 are in situ polymerized at 60°C under the action of initiator BPO to obtain polymer material G6-4, and then polymer material G6-4 is mixed into positive electrode slurry C3 and mixed evenly. The remaining steps are the same as the preparation method of positive electrode sheet 6-1 to obtain positive electrode sheet 6-4.

[0369] The preparation method of battery 6-4 is substantially the same as that of battery 6-1. The positive electrode sheet 6-1 is replaced with the positive electrode sheet 6-4. The remaining steps are the same to obtain battery 6-4.

[0370] Experimental Example 7

[0371] Monomer A7: Monomer B7:

[0372] Preparation method: Monomer A7 is an existing substance, CAS: 2429914-94-1, the nuclear magnetic resonance hydrogen spectrum of monomer A7 1 H NMR (300MHz, DMSO, δppm): 7.72(d, 2H), 7.40(d, 2H), 7.48(d, 1H), 4.51(d, 2H), 4.31(m , 2H), 4.19(m, 4H), 4.47(d, 2H), 1.36(t, 6H), 6.12(dd, 1H), 6.41(d, 1H), 5.83(d, 1H).

[0373] Monomer B7: First and Amidation reaction occurs to obtain (For the specific synthesis route, see Nature Communications, 12(1), 930; 2021.DOI: 10.1038 / s41467-021-21190-8), and then bromine is obtained at the benzyl position by NBS free radical reaction. (For the specific synthetic route, see Malaria Journal, 13, 190 / 1-190 / 26, 26; 2014.DOI: 10.1186 / 1475-2875-13-190), then use n-butyl lithium to extract hydrogen from the α-C of the sulfur of sulfonyl lactone, and then react with the substrate of benzyl bromide to undergo nucleophilic substitution to obtain monomer B7 (For the specific synthetic route, see Chemical Communications, 47 (41), 11465-11467; 2011.DOI: 10.1039 / c1cc14435a.). H NMR spectrum of monomer B7 1 H NMR (300MHz, DMSO, δppm): 9.54(s, 1H), 3.57(m, 1H), 4.32(m, 1H), 4.22(m, 1H), 2.50(m, 1H), 2.25(m , 1H), 7.69(d, 2H), 7.17(d, 2H), 2.94(dd, 1H), 2.69(dd, 1H), 1.98(s, 3H), 5.79(s, 1H), 5.72(s, 1H).

[0374] Preparation method of positive electrode sheet 7 and battery 7:

[0375] According to the data listed in Table 5, under the condition of dew point ≤-30°C, monomers A7, B7 (the molar ratio of B7 to A7 is 0.025) and initiator AIBN are mixed into the prepared positive electrode slurry C4 and mixed evenly, and coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm 2, control the coating speed, polymerize in situ at a certain temperature, blow dry, and roll press to obtain the positive electrode sheet 7.

[0376] Metal lithium F4 is used as the negative electrode plate to obtain the negative electrode plate 7.

[0377] The positive electrode sheet 7, negative electrode sheet 7 and separator S2 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E4 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 7 containing battery materials.

[0378] Experimental Example 8

[0379] Monomer A8: Monomer B8:

[0380] Preparation method: Monomer A8 is an existing substance, CAS 2230541-46-3. MS (ESI) m / z 286.08 (MH) + .

[0381] Monomer B8:

[0382] In the first step, n-butyl lithium is used to extract hydrogen from sulfonyl lactone, and then a nucleophilic addition reaction occurs with cyclohexanone to hydrolyze the sulfonyl lactone to obtain an alcohol. In the second step, it is subjected to esterification reaction with acrylic acid to obtain monomer B8. (Ref 1: Journal of Organic Chemistry, 46 (1), 101-6; 1981. DOI: 10.1021 / jo00314a022), Ref 2: Azerbaidzhanskii Khimicheskii Zhurna l, (2), 131-134; 2009). MS (ESI) m / z 274.09 (MH) + .

[0383] Preparation method of positive electrode sheet 8 and battery 8:

[0384] According to the data listed in Table 5, under the condition of dew point ≤ -30°C, monomers A8, B8 (molar ratio of B8 to A8 is 0.08) and initiator BPO are mixed into the prepared positive electrode slurry C5 and mixed evenly, and coated on aluminum foil to control the surface capacity of the electrode to 5 mA h / cm 2 , control the coating speed, polymerize in situ at a certain temperature, blow dry, and roll press to obtain the positive electrode sheet 8.

[0385] The negative electrode slurry F1 was coated on the copper foil, and the surface capacity of the control electrode was 5.3 mAh / cm 2 The negative electrode sheet 8 is obtained by air drying and roller pressing.

[0386] The positive electrode sheet 8, negative electrode sheet 8 and separator S1 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E4 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 8 containing battery materials.

[0387] Experimental Example 9-1

[0388] Monomer A9: MS (ESI) m / z 305.06 (MH) +

[0389] Monomer B9: MS (ESI) m / z 194.03 (MH) + , Monomer B9 is an existing substance, CAS: 63411-25-6

[0390] Monomer A9 preparation method:

[0391] The intermediate is obtained by esterification and hydrolysis of glutaric anhydride and vinyl alcohol. Pyridine phosphate is then used to prepare lithium alcoholate, which is then esterified with an equivalent amount of the intermediate prepared previously to form monomer A9 (Ref: Zhurnal Obshchei Khimii, 65 (11), 1924-5; 1995).

[0392] Preparation method of positive electrode sheet 9-1, negative electrode sheet 9-1 and battery 9-1:

[0393] As shown in Table 5, under the condition of dew point ≤ -30°C, monomers A9, B9 (molar ratio of B9 to A9 is 0.6) and initiator BPO are mixed into the prepared positive electrode slurry C6 and mixed evenly, and coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm 2 , controlling the coating speed, in-situ polymerization at a certain temperature, air drying, and roller pressing to obtain a positive electrode sheet 9-1;

[0394] As shown in Table 5, monomers A9, B9 (the molar ratio of B9 to A9 is 0.6) and initiator BPO are mixed into the negative electrode slurry F1 and mixed evenly, and coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , controlling the coating speed to 0.5 m / min to 70 m / min, in-situ polymerization at 50° C. for 6 h, air drying, and roller pressing to obtain a negative electrode sheet 9-1;

[0395] The positive electrode sheet 9-1, negative electrode sheet 9-1 and separator S1 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E5 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 9-1 containing battery materials.

[0396] Experimental Example 9-2

[0397] Preparation method of positive electrode sheet 9-2, negative electrode sheet 9-2 and battery 9-2:

[0398] The preparation method of the positive electrode sheet 9-2 is substantially the same as the preparation method of the positive electrode sheet 9-1, except that the monomers A9 and B9 are replaced by the monomer A9, and the remaining steps are the same to obtain the positive electrode sheet 9-2;

[0399] The preparation method of the negative electrode sheet 9-2 is substantially the same as the preparation method of the negative electrode sheet 9-1, except that the monomers A9 and B9 are replaced by the monomer A9, and the remaining steps are the same to obtain the negative electrode sheet 9-2;

[0400] The preparation method of battery 9-2 is roughly the same as that of battery 9-1, except that the positive electrode sheet 9-1 is replaced by the positive electrode sheet 9-2, and the negative electrode sheet 9-1 is replaced by the negative electrode sheet 9-2. The remaining steps are the same to obtain battery 9-2.

[0401] Comparative Example 9-3

[0402] Preparation method of positive electrode sheet 9-3, negative electrode sheet 9-3 and battery 9-3:

[0403] The preparation method of the positive electrode sheet 9-3 is substantially the same as the preparation method of the positive electrode sheet 9-1, except that the monomers A9 and B9 are replaced by the monomer B9, and the remaining steps are the same to obtain the positive electrode sheet 9-3;

[0404] The preparation method of the negative electrode sheet 9-3 is substantially the same as the preparation method of the negative electrode sheet 9-1, except that the monomers A9 and B9 are replaced by the monomer B9, and the remaining steps are the same to obtain the negative electrode sheet 9-3;

[0405] The preparation method of battery 9-2 is roughly the same as that of battery 9-1, except that the positive electrode sheet 9-1 is replaced by the positive electrode sheet 9-3, and the negative electrode sheet 9-1 is replaced by the negative electrode sheet 9-3. The remaining steps are the same to obtain battery 9-3.

[0406] Experimental Example 9-4

[0407] Preparation method of positive electrode sheet 9-4, negative electrode sheet 9-4 and battery 9-4:

[0408] The preparation method of the positive electrode sheet 9-4 is substantially the same as the preparation method of the positive electrode sheet 9-2, except that the monomer A9 is not added, and the remaining steps are the same to obtain the positive electrode sheet 9-4;

[0409] The preparation method of the negative electrode sheet 9-4 is exactly the same as the preparation method of the negative electrode sheet 9-2, and the negative electrode sheet 9-4 can be obtained;

[0410] The preparation method of battery 9-4 is roughly the same as that of battery 9-2, except that the positive electrode sheet 9-2 is replaced by the positive electrode sheet 9-4, and the negative electrode sheet 9-2 is replaced by the negative electrode sheet 9-4. The remaining steps are the same to obtain battery 9-4.

[0411] Experimental Example 9-5

[0412] Preparation method of positive electrode sheet 9-5, negative electrode sheet 9-5 and battery 9-5:

[0413] The preparation method of the positive electrode sheet 9-5 is exactly the same as the preparation method of the positive electrode sheet 9-2, and the positive electrode sheet 9-5 can be obtained;

[0414] The preparation method of the negative electrode sheet 9-5 is substantially the same as the preparation method of the negative electrode sheet 9-2, except that the monomer A9 is not added, and the remaining steps are the same to obtain the negative electrode sheet 9-5;

[0415] The preparation method of battery 9-5 is roughly the same as that of battery 9-2, except that the positive electrode sheet 9-2 is replaced by the positive electrode sheet 9-5, and the negative electrode sheet 9-2 is replaced by the negative electrode sheet 9-5. The remaining steps are the same to obtain battery 9-5.

[0416] Experimental Example 10-1

[0417] Monomer A10: MS (ESI) m / z 334.11 (MH) + (Monomer A10 is an existing substance, CAS: 2542065-61-0)

[0418] Monomer B10: MS (ESI) m / z 190.11 (MH) + (Monomer B10 is an existing substance, CAS: 35836-29-4)

[0419] Preparation method of positive electrode sheet 10-1, negative electrode sheet 10-1 and battery 10-1:

[0420] As shown in Table 5, under the condition of dew point ≤ -30°C, monomers A10, B10 (the molar ratio of B10 to A10 is 0.3) and initiator AIBN are mixed into the prepared positive electrode slurry C1 and mixed evenly, and coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm2 , control the coating speed, polymerize in situ at a certain temperature, blow dry, and roll press to obtain the positive electrode sheet 10-1.

[0421] As shown in Table 5, monomers A10, B10 (the molar ratio of B10 to A10 is 0.3) and initiator AIBN are mixed into the prepared negative electrode slurry F1 and mixed evenly, and then coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , controlling the coating speed to 0.5 m / min to 70 m / min, in-situ polymerization at 50° C. for 6 h, air drying, and roller pressing to obtain a negative electrode sheet 10-1;

[0422] The positive electrode sheet 10-1, negative electrode sheet 10-1 and separator S1 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E1 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 10-1 containing battery materials.

[0423] Experimental Example 10-2

[0424] Preparation method of positive electrode sheet 10-2, negative electrode sheet 10-2 and battery 10-2:

[0425] The preparation method of the positive electrode sheet 10-2 is substantially the same as the preparation method of the positive electrode sheet 10-1, except that the monomers A10 and B10 are replaced by the monomer A10, and the remaining steps are the same to obtain the positive electrode sheet 10-2;

[0426] The preparation method of the negative electrode sheet 10-2 is substantially the same as the preparation method of the negative electrode sheet 10-1, except that the monomers A10 and B10 are replaced by the monomer A10, and the remaining steps are the same to obtain the negative electrode sheet 10-2;

[0427] The preparation method of battery 10-2 is substantially the same as that of battery 10-1, except that the positive electrode sheet 10-1 is replaced by the positive electrode sheet 10-2, and the negative electrode sheet 10-1 is replaced by the negative electrode sheet 10-2. The remaining steps are the same to obtain battery 10-2.

[0428] Experimental Example 11

[0429] Monomer A11: MS (ESI) m / z 705.25 (MH) + (A11 is an existing substance, CAS: 68397-51-3)

[0430] Monomer B11: MS (ESI) m / z 187.08 (MH) +

[0431] Preparation method of monomer B11: Obtained by hydrolysis Obtained by oxidation with manganese dioxide (DCM, 80°C) Prepared by coupling reaction of CuCN with bromoalkane

[0432] Br2 addition and then NaF substitution preparation. Under nitrogen protection, 0.2mmol was added to a 25mL reaction tube. 2mL dry dichloromethane, cooled to 0℃, 0.2mmol liquid bromine was added dropwise, after addition, reacted at room temperature for 1h, 1mL saturated sodium thiosulfate aqueous solution was added until colorless, 2mL water was added, extracted with 3×5mL dichloromethane, the organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, and distilled under reduced pressure to obtain a crude product. This crude product was added to a 25mL reaction tube, 2mL dry dichloromethane, 0.1mmol benzyltriethylammonium chloride (TEBAC), 0.2mmol NaF were added, stirred at 40℃ for 8h, cooled to room temperature, quenched with water, extracted with dichloromethane, the organic phases were combined, dried, and distilled under reduced pressure to obtain of crude product.

[0433] Hydrolyze under alkaline conditions. Under nitrogen protection, The crude product was added to a 25 mL reaction tube, 2 mL of 1,4-dioxane and 100 μL of 3M NaOH were added, the temperature was raised to 90 °C for reaction for 8 h, cooled to room temperature, 5 mL of water was added, and the mixture was extracted with 3 × 5 mL of dichloromethane. The organic phases were combined, washed with saturated NaCl, dried over anhydrous sodium sulfate, filtered, evaporated under reduced pressure, and column chromatography was performed to obtain

[0434] Under nitrogen protection, 0.2 mmol of Add to a 25 mL reaction tube, add 1 mL of acetic anhydride, heat to 120 ° C for 8 h, cool and distill under reduced pressure, and purify by column chromatography to obtain

[0435] Preparation by low temperature hydrogen extraction of n-butyl lithium and nucleophilic substitution. Under nitrogen protection, 0.2 mmol Add to a 25mL Schlenk reaction tube, add 2mL dry tetrahydrofuran, cool to -78°C, add n-butyl lithium dropwise, react for 1h, add isopentyl bromide dropwise, react for 1h, return to room temperature and react for 1h, add water to quench, add 5mL water, extract with 3×5mL dichloromethane, combine the organic phases, wash the organic phases with saturated NaCl, dry over anhydrous sodium sulfate, filter, distill under reduced pressure, and obtain monomer B11 by column chromatography.

[0436] Preparation method of positive electrode sheet 11, negative electrode sheet 11 and battery 11:

[0437] According to the data listed in Table 5, under the condition of dew point ≤ -30°C, monomers A11, B11 (the molar ratio of B11 to A11 is 0.7) and initiator BPO are mixed into the prepared positive electrode slurry C5 and mixed evenly, and coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm 2 , controlling the coating speed, in-situ polymerization at a certain temperature, air drying, and roller pressing to obtain a positive electrode sheet 11;

[0438] As shown in Table 5, monomers A11, B11 (the molar ratio of B11 to A11 is 0.7) and initiator BPO are mixed into the negative electrode slurry F2 and mixed evenly, and coated on copper foil to control the electrode surface capacity to 5.3 mAh / cm 2 , controlling the coating speed, in-situ polymerization at a certain temperature, air drying, and roller pressing to obtain a negative electrode sheet 11;

[0439] The positive electrode sheet 11, the negative electrode sheet 11 and the separator S2 containing the battery material are stacked and baked to obtain a dry battery cell, and then the electrolyte E6 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 11 containing battery materials.

[0440] Experimental Example 12-1

[0441] Monomer A12: MS (ESI) m / z 334.11 (MH) + (Monomer A12 is an existing substance, CAS: 936752-22-6)

[0442] Monomeric B12: B12 is an existing substance, CAS: 1686096-69-4, MS (ESI) m / z 189.98 (MH) +

[0443] Preparation method of positive electrode sheet 12-1, negative electrode sheet 12-1 and battery 12-1:

[0444] As shown in Table 5, under the condition of dew point ≤ -30°C, monomers A12, B12 (the molar ratio of B12 to A12 is 1) and initiator BPO are mixed into the positive electrode slurry C1 and mixed evenly, and then coated on aluminum foil to control the electrode surface capacity to 5 mAh / cm 2 , control the coating speed, polymerize in situ at a certain temperature, blow dry, and roll press to obtain the positive electrode sheet 12-1.

[0445] As shown in Table 5, monomers A12, B12 (the molar ratio of B12 to A12 is 1) and initiator BPO were mixed into the prepared negative electrode slurry F1 and mixed evenly, and coated on copper foil to control the electrode surface capacity to be 5.3 mAh / cm2 , controlling the coating speed, in-situ polymerization at a certain temperature, air drying, and roller pressing to obtain a negative electrode sheet 12-1;

[0446] The positive electrode sheet 12-1, negative electrode sheet 12-1 and separator S1 containing battery materials are stacked and baked to obtain a dry battery cell, and then the electrolyte E6 is injected, the battery is packaged, and left to stand at room temperature for 12 hours to allow the battery cell to be fully soaked, thereby obtaining a solid-state battery 12-1 containing battery materials.

[0447] Experimental Example 12-2

[0448] Preparation method of positive electrode sheet 12-2, negative electrode sheet 12-2 and battery 12-2:

[0449] The preparation method of the positive electrode sheet 12-2 is substantially the same as the preparation method of the positive electrode sheet 12-1, except that the monomers A12 and B12 are replaced by the monomer A12, and the remaining steps are the same to obtain the positive electrode sheet 12-2;

[0450] The preparation method of the negative electrode sheet 12-2 is substantially the same as the preparation method of the negative electrode sheet 12-1, except that the monomers A12 and B12 are replaced by the monomer A12, and the remaining steps are the same to obtain the negative electrode sheet 12-2;

[0451] The preparation method of battery 12-2 is substantially the same as that of battery 12-1, except that the positive electrode sheet 12-1 is replaced by the positive electrode sheet 12-2, and the negative electrode sheet 12-1 is replaced by the negative electrode sheet 12-2. The remaining steps are the same to obtain battery 12-2.

[0452] Table 5-1 Experimental example battery configuration

[0453]

[0454]

[0455]

[0456] Table 5-2 Preparation parameters of batteries in experimental examples and comparative examples

[0457]

[0458]

[0459] Battery Test

[0460] After the secondary battery was completely cured in situ, the first-week discharge capacity, first-week efficiency, and 400-cycle capacity retention rate of the battery were tested at room temperature. The test voltage range was 2.75 to 4.2 V, and the cycle mode was 0.5C / 0.5C (C represents the rate). The test results are shown in Table 6.

[0461] Table 6 Battery test results

[0462]

[0463]

[0464] The capacity retention rates of battery 7 and blank battery 5 in Table 6 are the capacity retention rates after 50 cycles of the battery, and the capacity retention rates of the remaining batteries are the capacity retention rates after 400 cycles.

[0465] The present application provides an electrode sheet for a lithium battery, which is coated on a current collector by mixing a phosphorus-based monomer containing a ring structure with an electrode slurry, and then polymerized in situ to generate an electrode sheet for a lithium battery containing a phosphorus-based polymer material. The solid-state battery prepared by using the electrode sheet for a lithium battery greatly improves the cycle stability and safety of the battery and prolongs the battery life. As can be seen from Table 6, in a solid-state battery system with high nickel ternary (Ni83, NCA), lithium cobalt oxide as the positive electrode, and graphite, silicon carbon, silicon oxygen carbon, and metallic lithium as the negative electrode, compared with a blank battery, the energy density of the solid-state battery prepared by the present invention is only slightly reduced, but the cycle stability of the battery is significantly improved.

[0466] The negative electrode sheet was prepared by mixing monomers A and B in the negative electrode slurry and initiating in-situ polymerization of the monomers. The solid-state batteries (battery 1-1, battery 2-1, battery 3-1, battery 4-1) prepared from the negative electrode sheet had a battery capacity of 10.18 to 10.24 Ah and a capacity retention rate of 93.24% to 93.37% after 400 cycles. The solid-state batteries (battery 1-2, battery 2-2, battery 3-2, battery 4-2, battery 9-4) prepared by mixing monomer A in the negative electrode slurry and initiating in-situ polymerization of the monomers had a battery capacity of 9.96 to 10.05 Ah and a capacity retention rate of 92.12% to 92.32% after 400 cycles, which were slightly higher than the electrical performance of the corresponding blank batteries 1 to 3 (battery capacity of 9.88 to 9.99 Ah and a capacity retention rate of 91.16% to 91.34% after 400 cycles). The electrical performance of the solid-state batteries in which monomers A and B are in situ polymerized (battery 1-1, battery 2-1, battery 3-1, battery 4-1) is better than that of the solid-state batteries in which only monomer A is polymerized in situ (battery 1-2, battery 2-2, battery 3-2, battery 4-2), indicating that the solid-state batteries prepared by simultaneously mixing monomers A and B in the negative electrode slurry and initiating in situ polymerization of the monomers have higher cycle stability.

[0467] The positive electrode sheet is prepared by simultaneously mixing monomers A and B into the positive electrode slurry and in-situ polymerization of the monomers is initiated. The solid-state batteries prepared from the positive electrode sheet (battery 5-1, battery 6-1, batteries 7-8) have a battery capacity of 10.21-10.29 Ah, a capacity retention rate of 93.25%-93.36% after 400 cycles, and a capacity retention rate of 92.78% after 50 cycles of battery 7. The solid-state batteries prepared by mixing monomer A into the positive electrode slurry and initiating in-situ polymerization of the monomer (battery 5-2, battery 6-2, battery 9-5) have a battery capacity of 9.99-10.05 Ah and a capacity retention rate of 92.21%-92.29% after 400 cycles, which are slightly higher than the electrical performance of the corresponding blank battery Battery 3 and blank battery 5 (battery capacity 9.88-9.95 Ah, blank battery Battery 3 has a capacity retention rate of 91.16% after 400 cycles, and blank battery 5 has a capacity retention rate of 84.32% after 50 cycles). The cyclability of Battery 7 is significantly better than that of Blank Battery 5 because the present invention can inhibit lithium dendrites and improve the cyclability of the battery. The electrical performance of the solid-state batteries in which monomers A and B are polymerized in situ (battery 5-1, battery 6-1, batteries 7 to 8) is better than that of the solid-state batteries in which only monomer A is polymerized in situ (battery 5-2, battery 6-2, battery 9-5), indicating that the solid-state batteries prepared by simultaneously mixing monomers A and B in the positive electrode slurry and initiating in situ polymerization of the monomers have higher cycle stability.

[0468] Battery 9-1, battery 10-1, battery 11, and battery 12-1 are prepared by mixing monomer A and monomer B into positive and negative electrode slurries at the same time, and in-situ polymerization of the monomers is initiated to prepare electrode plates. The solid-state battery prepared from the electrode plates has a capacity of 10.17Ah to 10.31Ah, and a capacity retention rate of 93.15% to 93.67% after 400 cycles. The solid-state batteries (battery 9-2, battery 10-2, battery 12-2) prepared by simultaneously mixing monomer A into the positive and negative electrode slurries and initiating in-situ polymerization of the monomers have a battery capacity of 9.94 to 10.14 Ah and a capacity retention rate of 92.25% to 92.88% after 400 cycles, which are slightly higher than the corresponding blank batteries 1, blank batteries 4 and blank batteries 6 (battery capacity of 9.97 to 9.99 Ah, and a capacity retention rate of 91.23% to 91.28% after 400 cycles), but far lower than the electrical performance of the solid-state batteries (battery 9, battery 10-1, battery 11, battery 12-1), indicating that the solid-state batteries prepared by simultaneously mixing monomers A and B in the positive and negative electrode slurries and initiating in-situ polymerization of the monomers have higher cycle stability.

[0469] From the above comparison, it can be seen that the electrode sheet for lithium battery is prepared by mixing monomers A and B in the electrode slurry and initiating in-situ polymerization of the monomers. The solid-state batteries (battery 1-1, battery 2-1, battery 3-1, battery 4-1, battery 5-1, battery 6-1, batteries 7 to 9, battery 10-1, battery 11, battery 12-1) prepared from the electrode sheet have a higher capacity retention rate after 400 cycles than the solid-state batteries (battery 1-2, battery 2-2, battery 3-2, battery 4-2, battery 5-2, battery 6-2, battery 9-2, battery 9-4, battery 9-5, battery 10-2, battery 12-2) prepared by only mixing monomer A in the electrode slurry and initiating in-situ polymerization. This shows that the solid-state battery prepared by simultaneously mixing monomers A and B in the electrode slurry and initiating in-situ polymerization of the monomers has higher cycle stability.

[0470] Battery 9-2 is prepared by in-situ mixing of monomer A into both positive and negative electrode slurries. The battery capacity is 10.14Ah and the capacity retention rate after 400 cycles is 92.88%. Battery 9-4 and battery 9-5 are prepared by in-situ mixing of monomer A into only the positive electrode slurry or the negative electrode slurry. Battery 9-2 is much better than batteries 9-4 and batteries 9-5 in terms of first-week efficiency, capacity, cyclability and other electrical properties (battery capacity is 10.02Ah~10.05Ah, and the capacity retention rate after 400 cycles is 92.27%~92.29%), indicating that the battery prepared by simultaneously mixing monomers into positive and negative electrode slurries is better than the battery prepared only in positive electrode slurry or negative electrode slurry in its electrical performance, indicating that mixing in both positive and negative electrode slurries has higher cycle stability.

[0471] In battery 1-11, monomer A is mixed in electrolyte and injected into the battery cell to initiate in-situ polymerization of the monomer; in battery 1-16, solid electrolyte is prepared by in-situ polymerization of monomer, and then solid-state battery is assembled. Battery 1-11 (battery capacity 9.85Ah, capacity retention rate of 91.44% after 400 cycles) and battery 1-16 (battery capacity 9.76Ah, capacity retention rate of 91.08% after 400 cycles) are much smaller than battery 1-2 (battery capacity 10.01Ah, capacity retention rate of 92.12% after 400 cycles) in terms of first-week efficiency, capacity, cyclability and other electrical properties, indicating that the in-situ polymerization after mixing in the electrode slurry of the present application has certain advantages.

[0472] Battery 1-12 is a battery in which monomer A is only coated on the surface of the negative electrode plate and then polymerized in situ, battery 1-13 is a battery in which monomer A is coated on the surface of the diaphragm and then polymerized in situ, and battery 1-14 is a battery in which monomer A is coated on the surface of the positive electrode plate and then polymerized in situ. In the above batteries, monomers are not polymerized in situ in the electrode slurry. In terms of electrical properties such as the first cycle efficiency, capacity, and cyclability of the battery (battery capacity 9.83Ah~9.85Ah, capacity retention rate 91.32%~91.45% after 400 cycles), they are far less than battery 1-2 (monomer A is prepared by mixing in the negative electrode slurry). All of these illustrate that only the order of mixing the monomer with the electrode slurry, then polymerizing in situ to generate the electrode sheet and then preparing the battery in this application will not reduce the electrical performance of the battery, but will instead improve the first efficiency, capacity retention rate, etc. to a certain extent.

[0473] Battery 1-15 first prepares a polymer material by in-situ polymerization of monomers and then mixes the polymer material into the negative electrode slurry, which is different from the order of battery 1-2. However, the first-week efficiency, capacity, cyclability and other electrical performance data of battery 1-15 (battery capacity 9.81Ah, capacity retention rate of 91.19% after 400 cycles) are lower than those of battery 1-2. Battery 6-4 also first prepares a polymer material by in-situ polymerization of monomers and then mixes the polymer material into the positive electrode slurry, and its electrical performance is far lower than that of battery 6-1. This shows that the order of preparing electrode sheets in the present application has certain advantages, and only by following the preparation method of electrode sheets in the present application can good results be obtained.

[0474] Although the monomers A and B are mixed in the negative electrode slurry in Comparative Example 1-9, no initiator is added, and the monomers A and B cannot be polymerized (battery capacity 9.76Ah, capacity retention rate of 89.87% after 400 cycles), its performance in terms of the first cycle efficiency, capacity, cyclability and other electrical properties of the battery is far less than that of the solid-state battery prepared by mixing monomers A and B in the electrode slurry and initiating in-situ polymerization. In addition, battery 1-10 (battery capacity 9.78Ah, capacity retention rate of 89.76% after 400 cycles) does not add an initiator, and monomer A cannot be polymerized. Its performance in terms of the first cycle efficiency, capacity, cyclability and other electrical properties of the battery is far less than that of the solid-state battery prepared by mixing monomer A in the electrode slurry and initiating in-situ polymerization. In batteries 1-8, 6-3 and 9-3, only monomer B was polymerized in situ, and the battery capacity was between 9.77 and 9.81 Ah, and the capacity retention rate after 400 cycles was 91.11% to 91.24%, which was much lower than the electrical performance of battery 1-1.

[0475] K3 in battery 1-7 represents the acrylate of the prior art. The solid-state battery 1-7 is prepared by mixing monomers A and K3 in the electrode slurry and initiating in-situ polymerization to prepare the electrode sheet. The battery capacity is 9.87Ah and the capacity retention rate after 400 cycles is 91.26%, which is much smaller than the solid-state battery prepared by mixing monomers A and B in the electrode slurry and initiating in-situ polymerization. This shows that the monomer A+B in the present invention has higher cycle stability than A and acrylate.

[0476] The solid-state batteries (battery 1-5, battery 1-6) prepared using only monomer D have a battery capacity between 9.43Ah and 9.51Ah, and a capacity retention rate of 88.48% to 88.85% after 400 cycles; the solid-state batteries (battery 1-3, battery 1-4) prepared using monomers K1 and K2 have a battery capacity between 9.71Ah and 9.75Ah, and a capacity retention rate of 90.28% to 90.46% after 400 cycles.

[0477] Among them, the substituents connected to the P atom in monomers K1 and K2 do not contain a ring structure, while the substituents connected to the P atom in monomers A used in the batteries in other experimental examples all contain at least one ring structure. By comparing the electrochemical performance of the above batteries in terms of first efficiency and capacity retention, it can be seen that when the substituent connected to P in monomer A contains a ring structure, the battery has better electrochemical performance.

[0478] In the monomer A used in battery 1-17, there is an ester group between P and the double bond; in the monomer A used in battery 10-2 and battery 12-2, there is no ester group between P and the double bond. From the electrochemical performance of battery 1-17, battery 10-2 and battery 12-2 in terms of first efficiency and capacity retention rate, it can be seen that in the structure of monomer A, the structure containing an ester group between P and the double bond can make the battery have better electrochemical performance.

[0479] Battery 1-18 adds the phosphorus-based flame retardant TPP to the electrolyte, and its performance in terms of first efficiency and capacity retention rate is lower than that of battery 1-1 and battery 1-2, which further shows that the present invention enables the electrode to have good capacity utilization and cycle stability. This is mainly because the present invention adopts an in-situ mixing method in the electrode slurry, so that the surface of the electrode active material particles is coated with a thin layer of phosphorus-containing polymer material. The polymer layer can maintain a low interfacial impedance during the battery cycle, while homogenizing the ion flow, thereby ensuring the electrochemical performance of the battery.

[0480] It can be seen from batteries 1-2 and 1-20 that if the content of phosphorus-based polymer material is too high, the battery's electrical properties such as energy density and cycle performance will be significantly reduced.

[0481] Depend on Figure 1It can be seen that the capacity retention rate of battery 1-1 is much higher than that of comparative battery 1-5 and blank battery 1, indicating that the present application can significantly improve the electrochemical performance of the battery by in-situ mixing of the electrode sheet prepared by the cyclic phosphorus-based monomer in the electrode slurry and applying the electrode sheet to the battery. The capacity retention rate of battery 1-1 is higher than that of battery 1-2, indicating that the solid-state battery prepared by mixing monomers A+B in the electrode slurry and initiating in-situ polymerization has better cyclability than the solid-state battery prepared by mixing only monomer A and initiating in-situ polymerization.

[0482] Battery safety performance test

[0483] The batteries prepared in the above experimental examples, the batteries prepared in the comparative examples and blank batteries 1-5 were subjected to acupuncture safety tests according to safety requirements and test methods for power batteries for electric vehicles in GB-T31485-2015 for lithium-ion batteries.

[0484] 1. Needle penetration test: The battery is charged at 1C constant current and constant voltage, with a cut-off current of 0.05C; a φ8mm high-temperature resistant steel needle is used to penetrate the battery plate at a speed of 25mm / s from a direction perpendicular to the battery plate. The penetration position should be close to the geometric center of the punctured surface, and the steel needle stays in the battery; observe for 1h, monitor the changes in the surface temperature of the battery cell during the process, and record whether the battery cell catches fire or explodes. The results are shown in Table 7.

[0485] Table 7 Cell acupuncture result record

[0486]

[0487]

[0488] The present application provides an electrode sheet for a lithium battery. A phosphorus-based monomer containing a ring structure is mixed with an electrode slurry and then coated on a current collector. After in-situ polymerization, an electrode sheet for a lithium battery containing a phosphorus-based polymer material is generated. The solid-state battery prepared using the electrode sheet greatly improves the safety of the battery.

[0489] As shown in Table 7, the electrode sheet is prepared by mixing monomers A and B in the negative electrode slurry and initiating in-situ polymerization of the monomers. The solid-state batteries (battery 1-1, battery 2-1, battery 3-1, battery 4-1) prepared from the electrode sheet do not catch fire or explode during the needle puncture test. The surface temperature of the battery cell during the needle puncture is 29.9-30.3°C, which is much lower than the surface temperature of blank batteries 1-3 (620.7-624.5°C), which significantly improves the battery safety. The solid-state batteries (battery 1-2, battery 2-2, battery 3-2, battery 4-2, battery 9-4) did not catch fire or explode during the puncture test. The surface temperature of the battery cell during puncture was 37.7-38.1°C, which was much lower than the surface temperature of the blank batteries, but higher than the surface temperature of the solid-state batteries in which monomers A and B were in situ polymerized (battery 1-1, battery 2-1, battery 3-1, battery 4-1). This shows that the solid-state batteries prepared by simultaneously mixing monomers A and B in the negative electrode slurry and initiating in-situ polymerization of the monomers have higher safety.

[0490] The electrode sheet is prepared by mixing monomers A and B in the positive electrode slurry and initiating in-situ polymerization of the monomers. The solid-state batteries prepared from the electrode sheet (battery 5-1, battery 6-1, batteries 7-8) do not catch fire or explode during the needle puncture test. The surface temperature of the battery cell during the needle puncture is 30.3-30.7°C, which is much lower than the surface temperature of blank battery 3 and blank battery 5 (624.5°C and 633.1°C), which significantly improves the battery safety. The solid-state batteries prepared by only mixing monomer A in the positive electrode slurry and initiating in-situ polymerization (battery 5-2, battery 6-2, battery 9- 5). The battery did not catch fire or explode during the puncture test. The surface temperature of the battery cell during puncture was 38.3-38.7°C, which was much lower than the surface temperature of the blank battery, but higher than the surface temperature of the solid-state batteries (battery 5-1, battery 6-1, batteries 7-8) prepared by in-situ mixing of monomers A and B in the positive electrode slurry. This indicates that the safety of the solid-state batteries (battery 5-1, battery 6-1, batteries 7-8) prepared by in-situ mixing of monomers A and B in the positive electrode slurry is better than that of the solid-state batteries (battery 5-2, battery 6-2, battery 9-5) prepared by in-situ mixing of monomers A and B in the positive electrode slurry.

[0491] Battery 9-1, Battery 10-1, Battery 11, and Battery 12-1 are prepared by simultaneously mixing monomer A and monomer B in the positive and negative electrode slurries and initiating in-situ polymerization of the monomers. The batteries do not catch fire or explode during the puncture test. The surface temperature of the battery cell during puncture is 27.2-30.3°C, which is much lower than the surface temperature of the blank battery, significantly improving the battery safety. The solid-state batteries (Battery 9-2, Battery 10-2, and Battery 12-2) prepared by mixing only monomer A in the positive and negative electrode slurries and in-situ polymerization do not catch fire or explode during the puncture test. The surface temperature of the battery cell during puncture is 34.5-36 .8℃, which is also much lower than the surface temperature of the blank battery, but higher than the surface temperature of the solid-state batteries (battery 9-1, battery 10-1, battery 11, battery 12-1) prepared by in-situ mixing monomers A and B in the positive and negative electrode slurries at the same time, indicating that the solid-state batteries (battery 9-1, battery 10-1, battery 11, battery 12-1) prepared by in-situ mixing monomers A and B in the positive and negative electrode slurries at the same time are safer than the solid-state batteries (battery 9-2, battery 10-2, battery 12-2) prepared by in-situ mixing monomer A in the positive and negative electrode slurries, and are better than the blank batteries 1 to 6 without monomer A mixed.

[0492] From the above comparison, it can be seen that the electrode sheet is prepared by mixing monomers A and B in the electrode slurry and initiating in-situ polymerization of the monomers. The needle-punctured surface temperature of the solid-state batteries (battery 1-1, battery 2-1, battery 3-1, battery 4-1, battery 5-1, battery 6-1, batteries 7 to 9, battery 10-1, battery 11, battery 12-1) prepared from the electrode sheet is lower than that of the solid-state batteries (battery 1-2, battery 2-2, battery 3-2, battery 4-2, battery 5-2, battery 6-2, battery 9-2, battery 9-4, battery 9-5, battery 10-2, battery 12-2) prepared by only mixing monomer A in the electrode slurry and initiating in-situ polymerization. This shows that the solid-state battery prepared by simultaneously mixing monomers A and B in the electrode slurry and initiating in-situ polymerization of the monomers has higher safety.

[0493] Battery 9-2 is prepared by in-situ mixing of monomer A into the positive and negative electrode slurries, while batteries 9-4 and 9-5 are prepared by in-situ mixing of monomer A into only the positive electrode slurry or the negative electrode slurry. The surface temperature of battery 9-2 is 34.5°C, which is lower than that of batteries 9-4 and 9-5 (38.3~38.5°C), indicating that the battery prepared by in-situ mixing of monomers into the positive and negative electrode slurries is better in safety performance than the battery prepared by in-situ mixing of cyclic phosphorus-based monomers into only the positive electrode slurry or the negative electrode slurry, indicating that simultaneous mixing in the positive and negative electrode slurries has higher safety and can reduce the surface activity of the positive and negative electrode particles at the same time.

[0494] In battery 1-11, monomer A is mixed in electrolyte and injected into the battery cell to initiate in-situ polymerization of the monomer; in battery 1-16, the monomer is firstly initiated to polymerize in situ to prepare a solid electrolyte and then a solid-state battery is assembled. The surface temperature of the battery cells of battery 1-11 and battery 1-16 after acupuncture is much higher than that of battery 1-2, indicating that the in-situ polymerization after mixing in the electrode slurry can significantly reduce the temperature of the electrode sheet and has a protective effect.

[0495] Battery 1-12 is a battery in which monomer A is only coated on the surface of the negative electrode plate and then polymerized in situ, battery 1-13 is a battery in which monomer A is coated on the surface of the diaphragm and then polymerized in situ, and battery 1-14 is a battery in which monomer A is coated on the surface of the positive electrode plate and then polymerized in situ. In none of the above batteries are monomers polymerized in situ in the electrode slurry, and the battery safety is far less than that of battery 1-2 (prepared by mixing monomer A in the negative electrode slurry). It is shown that only the sequence of mixing monomers with electrode slurry and then polymerizing in situ to generate electrode sheets and then to generate batteries in this application can protect the battery, significantly reduce the surface temperature of the battery cell, suppress the temperature rise of the battery, and avoid the danger of fire and explosion of the battery.

[0496] Battery 1-15 first prepares a polymer material by in-situ polymerization of monomers and then mixes the polymer material into the negative electrode slurry, which is different from the order of battery 1-2, but the surface temperature of battery 1-15 is 384.7°C, which is much higher than that of battery 1-2; battery 6-4 also first prepares a polymer material by in-situ polymerization of monomers and then mixes the polymer material into the positive electrode slurry, and its surface temperature is much higher than that of battery 6-1; this shows that the order of preparing electrode sheets in the present application has certain advantages, and only by following the preparation method of electrode sheets in the present application can better safety be obtained.

[0497] In Comparative Example 1-9, although monomers A and B were mixed in the electrode slurry, no initiator was added, and monomers A and B could not be polymerized. During the needle puncture test, the battery caught fire and exploded, and the surface temperature of the battery cell during the needle puncture was 456.3° C. In addition, since no initiator was added to battery 1-10, monomer A could not be polymerized either. During the needle puncture test, the battery caught fire and exploded, and the surface temperature of the battery cell during the needle puncture was 474.4° C.

[0498] In batteries 1-8, 6-3 and 9-3, only monomer B underwent in-situ polymerization. The batteries caught fire and exploded when punctured. The surface temperature of the battery cells was 545.1-563.5°C during puncture. Although the surface temperature of the battery cells was lower than that of the blank batteries, it was much higher than that of the batteries in the experimental examples of this application.

[0499] Battery 1-18 added a phosphorus-containing flame retardant to the electrolyte. The battery caught fire and exploded when punctured. The surface temperature of the battery cell was 489.3°C during puncture, indicating that adding the same amount of flame retardant as the monomer of the present invention to the electrolyte has no flame retardant effect at all, and the flame retardant cannot fundamentally suppress the temperature rise of the battery. This further shows that the solid-state battery prepared by in-situ blending of cyclic phosphorus-based monomers in the electrode slurry of the present invention can significantly improve the safety of the battery.

[0500] K3 in battery 1-7 represents the acrylate of the prior art. The solid-state battery 1-7 prepared by mixing monomers A and K3 in the electrode slurry and initiating in-situ polymerization to prepare the electrode sheet has a cell surface temperature of 44.4°C during acupuncture, which is much higher than the solid-state battery (battery 1-1) prepared by mixing monomers A and B in the electrode slurry and initiating in-situ polymerization, indicating that the monomer A+B in the present invention has higher safety performance than A and acrylate. The solid-state batteries (batteries 1-5 and 1-6) prepared only with monomer D caught fire and exploded during acupuncture, and the cell surface temperature during acupuncture was 587.4 to 598.8°C.

[0501] The solid-state batteries (battery 1-3, battery 1-4) prepared with monomers K1 and K2 did not catch fire or explode when punctured, and the surface temperature of the battery cell was 79.9-80.1°C during puncture. The substituents connected to the P atom in monomers K1 and K2 do not contain ring structures, indicating that although the introduction of K1 and K2 has improved the battery safety to a certain extent, the ability to suppress the temperature rise of the battery is insufficient. In the monomer A used in the battery in other experimental examples, the substituents connected to the P atom all contain at least one ring structure. It can be seen from the safety performance data that the battery has better safety performance when the monomer A contains a phosphorus group and the substituent connected to P contains a ring structure. In the monomer A used in battery 1-17, there is an ester group between P and the double bond, and the surface temperature of the battery cell after puncture is 34.3°C; in the monomer A used in batteries 10-2 and 12-2, there is no ester group between P and the double bond, and the surface temperature of the battery cell after puncture is 36.6-36.8°C, which is higher than the surface temperature of battery 1-2. It can be seen that in the structure of monomer A, the structure containing an ester group between P and the double bond can make the battery have better safety performance.

[0502] It can be seen from batteries 1-2, 1-19 and 1-20 that if the content of phosphorus-based polymer material is too little, it is difficult to coat a thin layer of polymer material containing phosphorus groups on the surface of the electrode active material particles, and the battery will catch fire or explode when punctured, and the improvement in battery safety is not obvious. If the content of phosphorus-based polymer material is too much, the battery will not catch fire or explode when punctured, and although the safety of the battery can be greatly improved, the battery's electrical properties such as energy density and cycle performance will be reduced.

[0503] It can be seen from batteries 1-2 and batteries 1-11 to 1-16, batteries 2-1 and batteries 2-3, batteries 5-1 and batteries 5-3, batteries 5-2 and 5-4 that the solid-state batteries prepared by monomer A or A+B using the following methods all caught fire and exploded when punctured. These methods include: 1. directly adding monomers and initiators to the electrolyte and then injecting them into the battery cell to initiate in-situ polymerization of the monomers to prepare a solid-state battery; 2. preparing the monomers and initiators into a precursor solution, coating it on the surface of the positive electrode, negative electrode or diaphragm, and then initiating in-situ polymerization of the monomers; 3. first initiating monomer polymerization in vitro to prepare a polymer material, and then mixing it into the electrode slurry; 4. initiating in-situ polymerization of monomers to prepare a solid electrolyte and then assembling a solid-state battery. The present invention prepares an electrode sheet containing a phosphorus-based polymer material by mixing the monomer into the electrode slurry and initiating in-situ polymerization of the monomer. The solid-state battery prepared by the electrode sheet does not catch fire or explode when punctured. The above phenomenon further shows that the electrode sheet containing a phosphorus-based polymer material prepared by the in-situ mixing method in the electrode slurry in the present application has higher safety. This is because the present application adopts the method of in-situ mixing in the electrode slurry, so that the surface of the electrode active material particles is coated with a thin layer of polymer material containing phosphorus groups. Compared with general polymer electrolytes, the polymer layer has higher thermal stability and electrochemical stability, which can effectively reduce the surface activity of the electrode particles, reduce the direct contact between the active material particles and the electrolyte, inhibit the side reaction between the active material and the electrolyte, and improve the safety performance of the battery; in addition, the polymer layer can maintain a low interface impedance during the battery cycle, and at the same time homogenize the ion flow, so that the electrode has good capacity play and cycle stability, and ensures the electrochemical performance of the battery.

[0504] from Figure 2 It can be seen more intuitively that the solid-state battery prepared by introducing monomer A or simultaneously introducing monomers A+B into the electrode slurry and initiating in-situ polymerization of the monomers in the present invention remains in good condition after puncture, while the blank battery 1 and batteries 1-11 and 1-15 caught fire and exploded after the puncture test and were severely damaged. This shows that the electrode sheet containing phosphorus-based polymer materials prepared by adding monomers to the electrode slurry and initiating in-situ polymerization provided in the present application can be applied to solid-state batteries, which can significantly improve the safety performance of the battery.

[0505] 2. Battery Thermal Shock Safety Test

[0506] The battery was charged at 1C constant current and constant voltage, with a cut-off current of 0.05C; heated at 180℃ for 2h: the heating rate was 5℃ / s, heated to 180℃ and kept warm for 2h, and observed for 1h; and recorded whether the battery caught fire or exploded. If it did not catch fire or explode, it passed, otherwise it failed. The changes in the surface temperature of the battery cell were monitored during the process. The test results are shown in Table 8.

[0507] Table 8 Battery thermal shock safety results record

[0508]

[0509]

[0510] The present application provides an electrode sheet for a lithium battery, which is prepared by mixing a phosphorus-based monomer containing a ring structure with an electrode slurry and coating the mixture on a current collector, and then subjecting the mixture to in-situ polymerization to generate an electrode sheet containing a phosphorus-based polymer material. The solid-state battery prepared using the electrode sheet greatly improves the safety of the battery.

[0511] As shown in Table 8, the electrode sheet is prepared by mixing monomers A and B or monomer A in the electrode slurry and initiating in-situ polymerization of the monomer. The solid-state batteries prepared from the electrode sheet all passed the thermal shock test. The solid-state battery prepared by mixing monomer B in the electrode slurry to initiate in-situ polymerization, the battery containing monomer A or containing monomers A and B at the same time but not polymerized, the solid-state battery containing only D1 and D2 and the blank battery did not pass the thermal shock test; and the battery did not pass the thermal shock test when monomer A or A+B was introduced into the solid-state battery in the following ways: first, the monomer and the initiator were directly added to the electrolyte and then injected into the battery cell to initiate the in-situ polymerization of the monomer to prepare the solid-state battery; second, the monomer and the initiator were prepared into a precursor solution and coated on the surface of the positive electrode, the negative electrode or the diaphragm, and then the monomer was polymerized in situ; third, the monomer polymerization was initiated in vitro to prepare a polymer material, and then mixed into the electrode slurry; fourth, the solid electrolyte was prepared by in-situ polymerization of the monomer and then the solid-state battery was assembled; further indicating that the present invention improves the safety of the battery. Moreover, if the content of phosphorus-based polymer material is too little, it is difficult to coat a thin layer of polymer material containing phosphorus groups on the surface of the electrode active material particles, and the battery will catch fire and explode during the thermal shock test, and the improvement of battery safety is not obvious; if the content of phosphorus-based polymer material is too much, the battery will not catch fire or explode during the thermal shock test, although it can greatly improve the safety of the battery, it will reduce the battery's energy density and cycle performance and other electrical properties. Mainly because the present application adopts the method of in-situ blending in the electrode slurry, so that the surface of the electrode active material particles is coated with a thin layer of polymer material containing phosphorus groups. Compared with general polymer electrolytes, this polymer layer has higher thermal stability and electrochemical stability, which can effectively reduce the surface activity of the electrode particles, reduce the direct contact between the active material particles and the electrolyte, inhibit the side reaction between the active material and the electrolyte, and improve the battery safety performance; in addition, the polymer layer can maintain a low interface impedance during the battery cycle, and at the same time homogenize the ion flow, so that the electrode has good capacity play and cycle stability, and ensures the electrochemical performance of the battery. 3. Extrusion test: After fully charging the battery, place it in two planes and squeeze it perpendicular to the plate at a rate of 2mm / s. Stop squeezing when the voltage reaches 0V or the battery deformation reaches 50%. The battery passes the squeezing process if it does not catch fire or explode.

[0512] Table 9 Comparison of extrusion test results

[0513]

[0514]

[0515] The present application provides an electrode sheet for a lithium battery, which is prepared by mixing a phosphorus-based monomer containing a ring structure with an electrode slurry and coating the mixture on a current collector, and then subjecting the mixture to in-situ polymerization to generate an electrode sheet containing a phosphorus-based polymer material. The solid-state battery prepared using the electrode sheet greatly improves the safety of the battery.

[0516] As shown in Table 9, the electrode sheets prepared by mixing monomers A and B or monomer A in the electrode slurry and initiating in-situ polymerization of the monomers all passed the extrusion test. The solid-state batteries prepared by mixing monomer B in the electrode slurry and initiating in-situ polymerization, the batteries containing monomer A or containing monomers A and B but not polymerized, the solid-state batteries containing only D1 and D2 and the blank batteries did not pass the extrusion test; and the batteries introduced with monomers A or A+B into the solid-state battery in the following ways also did not pass the extrusion test: first, the monomers and initiators were directly added to the electrolyte and then injected into the battery core to initiate in-situ polymerization of the monomers to prepare the solid-state battery; second, the monomers and initiators were prepared into a precursor solution and coated on the surface of the positive electrode, the negative electrode or the diaphragm to initiate in-situ polymerization of the monomers; third, the monomers were first polymerized in vitro to prepare a polymer material, and then mixed into the electrode slurry; fourth, the solid electrolyte was prepared by in-situ polymerization of the monomers and then the solid-state battery was assembled; further indicating that the present invention improves the safety of the battery.

[0517] In the puncture test, thermal shock safety test, and extrusion test, monomer A or monomer A and B are mixed in the electrode slurry and the monomers are polymerized in situ to prepare the electrode sheet. The solid-state batteries prepared from the electrode sheet all passed the test, and the solid-state batteries prepared by polymerizing both monomers A and B have better safety and better electrochemical performance. However, the monomers introduced into the solid-state battery by other means did not pass the safety test, such as directly adding the monomers and initiators to the electrolyte and then injecting them into the battery core to initiate the in-situ polymerization of the monomers, preparing the monomers and initiators into precursor liquids and coating them on the positive electrode, negative electrode or diaphragm surface and then initiating the in-situ polymerization of the monomers, first initiating the polymerization of the monomers in vitro to prepare a polymer material, then mixing it into the electrode slurry, initiating the in-situ polymerization of the monomers to prepare a solid electrolyte, and then assembling the solid-state battery; while the solid-state batteries and blank batteries in which monomer A or A+B is mixed into the electrode slurry but polymerization is not initiated, or monomer B is mixed into the electrode slurry and in-situ polymerization is initiated, the flame retardant of the same content of the present invention is added to the electrolyte, or only D1 or D2 is mixed, all failed to pass the safety test. Moreover, if the content of phosphorus-based polymer material is too little, the battery cannot pass the safety test because it is difficult to coat a thin layer of polymer material containing phosphorus groups on the surface of the electrode active material particles; if the content of phosphorus-based polymer material is too much, although the safety of the battery can be greatly improved, it will reduce the battery's energy density and cycle performance and other electrical properties. This shows that the phosphorus-based monomer containing a ring structure in the present application is mixed with the electrode slurry and then coated on the current collector. After in-situ polymerization, an electrode sheet containing a phosphorus-based polymer material is generated. The solid-state battery prepared using the electrode sheet greatly improves the safety of the battery. Moreover, for the same monomer, the positive and negative electrode slurries are simultaneously in-situ mixed, and the safety and electrical performance of the battery are also due to the in-situ mixing of the separate electrodes. It should be noted that the monomer A in this patent, or the mixture of monomer A and monomer B, can also be directly matched with commercial electrolytes and used, and excellent results can still be obtained, indicating that the monomers used to prepare polymer materials in this application have good compatibility with various electrolytes.

[0518] Based on previous research findings, the safety performance of lithium-ion batteries can be significantly improved by introducing the monomers involved in the present invention into the battery cell through a general application method. For example, the monomers are injected into the battery cell to initiate in-situ polymerization, and the monomers are coated on the surface of the positive and negative electrodes or the diaphragm to initiate in-situ polymerization. Although these solutions have been verified to improve the safety of battery cells in 250-280Wh / kg battery cell samples, and the corresponding battery cells can successfully pass tests such as puncture, extrusion, collision, and 150°C thermal shock, the safety performance of battery cells with higher specific energy (300Wh / kg) is not significantly improved. In order to obtain a battery with a specific energy of 300Wh / kg, the present invention further increases the proportion of active substances in the battery cell, especially increases the surface capacity of the electrode (the positive electrode is 5mAh / cm 2 ; The negative electrode is 5.3mAh / cm2 ), and these improvements will make the chain reaction of thermal runaway in the battery cell more likely to occur, making it more difficult to ensure the safety performance of the battery, and higher requirements need to be placed on the polymer monomers and application methods. The technical solution provided by the present invention can further significantly improve the safety of the battery cell, so that the 300Wh / kg high-energy-density battery can also successfully pass safety tests such as needle puncture; compared with the prior art, the technical solution of the present invention can ensure the safety performance of the battery cell with a higher energy-density (300Wh / kg).

[0519] In summary, the solid-state battery prepared by the present invention can not only significantly improve the battery safety performance, but also extremely well maintain the electrochemical performance of the battery, and is suitable for large-scale promotion and application.

[0520] In the present invention, only some structures are selected as representatives in the experimental examples to illustrate the preparation method and effects of the present application, and other structures not listed have similar effects.

[0521] The monomers used in the experimental examples can all be purchased or prepared simply, and the preparation processes are all existing technologies, so they are not described in detail in the specification.

[0522] It should also be noted that the applicant has conducted a large number of tests on this series of structures. Sometimes, in order to better compare with the existing system, the same structure and system have been tested more than once. Therefore, there may be certain errors in different tests.

[0523] Finally, it should be noted that the above-described embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

[0524] The preferred specific implementation modes and embodiments of the present application are described in detail above in conjunction with the accompanying drawings, but the present application is not limited to the above implementation modes, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present application.

Claims

1. An electrode sheet for a lithium battery, comprising a current collector and an electrode material covering the current collector, wherein the electrode material comprises an electrode active material, a conductive agent and a binder, and the electrode sheet is a positive electrode sheet or a negative electrode sheet, It is characterized in that The electrode material also includes a phosphorus-based polymer material formed by polymerization of monomers; The mass percentage of the phosphorus-based polymer material in the electrode material is 0.06-15%; The monomers include monomer A; The monomer A is at least one of the compounds shown in formula I, Among them, M 1 Any one selected from C, N, P, S, Si; R 1 ~R 4 Independantly selected from any one of a chain or a ring having no, a substituent or no substituent, in R 1 In the case of a chain selected from a chain containing or not containing a substituent, the chain is a pure carbon chain, or a carbon chain containing only one heteroatom; Indicates a ring structure; A 1 It means that any position of the ring structure can be substituted with a substituent.

2. The lithium battery electrode sheet according to claim 1, It is characterized in that R 1 contains at least one unsaturated bond and / or at least one heteroatom; the heteroatom includes N, O, P, S, Si, and F; R 3 ~R 4 Independently selected from none, a saturated carbon chain consisting of 1 to 10 carbon atoms, or an unsaturated carbon chain.

3. The lithium battery electrode sheet according to claim 1, It is characterized in that R 3 Selected from Or -OR, R is selected from any one of H, Li, halogen, a chain or a ring with or without a substituent.

4. The lithium battery electrode sheet according to claim 3, It is characterized in that The OR is OLi.

5. The lithium battery electrode sheet according to claim 3, It is characterized in that The chain or ring containing or not containing a substituent is a chain or ring consisting of 1 to 8 atoms.

6. The lithium battery electrode sheet according to claim 1, It is characterized in that The monomers also include monomer B; The monomer B is selected from at least one of the compounds shown in formula II, Among them, M 3 Selected from C, N, P, S, Si; R 12 ~R 14 Independently selected from any one of a chain or a ring with no substituent, with substituent or without substituent.

7. The lithium battery electrode sheet according to claim 6, It is characterized in that R 14 It is selected from a ring or a chain containing at least one heteroatom, and any position of the ring or the chain can be substituted by a substituent.

8. The lithium battery electrode sheet according to claim 6, It is characterized in that The molar ratio of the monomer B to the monomer A is α, wherein 0<α≤1.

9. The lithium battery electrode sheet according to claim 1, It is characterized in that The monomer and the initiator are added during the slurry mixing process of the electrode material, and in-situ polymerization is performed to form the phosphorus-based polymer material.

10. The lithium battery electrode sheet according to claim 1, It is characterized in that The weight proportions of the components in the electrode material are: 80-99 parts of electrode active material, 0.5-10 parts of conductive agent, 0.5-10 parts of binder, and 0.1-15 parts of monomer.

11. A method for preparing an electrode sheet for a lithium battery as claimed in any one of claims 1 to 10, It is characterized in that The method for preparing the electrode sheet for lithium battery comprises: (1) taking an electrode active material, a conductive agent, a binder, a monomer, and an initiator, and mixing them uniformly to prepare a mixed slurry; (2) coating the mixed slurry on a current collector and polymerizing the mixed slurry in situ to obtain the electrode sheet for a lithium battery; In-situ polymerization conditions: in-situ polymerization temperature is 55-125°C, and in-situ polymerization time is 0.1-30 min; The mass of the initiator is 0.1% to 2% of the mass of the monomer; the coating condition is: the coating speed is 0.5 m / min to 70 m / min.

12. A battery, It is characterized in that It comprises the electrode sheet for lithium battery according to any one of claims 1 to 10 or the electrode sheet for lithium battery obtained according to the preparation method according to claim 11.