Light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber and preparation method thereof
By introducing modified nano-tungsten bronze into cellulose and coating it with zirconium phosphate and polyethylene glycol, a three-layer composite structure is formed, which solves the problems of insufficient heat storage capacity and powder loss in heat-generating viscose fibers, improves the fiber's heating efficiency, antibacterial properties and color lightness, and extends its service life.
Patent Information
- Application Number
- CN202211649806.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing heat-generating viscose fibers have problems such as insufficient heat storage capacity, powder loss due to acid and alkali insensitivity, uneven spinning solution, and dark color affecting the fashionability and service life of clothing.
Modified nano-tungsten bronze was introduced into cellulose, and a three-layer composite structure was formed by coating its surface with zirconium phosphate and polyethylene glycol. This improved its acid and alkali resistance and compatibility, enhanced its heat generation and heat storage performance, and improved the dispersibility and phase change heat storage function of the system by controlling the mass ratio of zirconium phosphate to polyethylene glycol to be (1-5):1.
It effectively improves the heat generation and heat storage efficiency of viscose fiber, reduces powder loss, ensures the service life and heating effect of the fiber, and enhances antibacterial and flame retardant properties and color lightness.
Smart Images

Figure BDA0004009890130000111 
Figure BDA0004009890130000121
Abstract
Description
Technical Field
[0001] The invention relates to the D01F field, and in particular to a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber and a preparation method thereof. Background Art
[0002] Thermal fibers are used in cold-resistant clothing and have a wide range of uses. Existing thermal fibers are given certain heating and warmth properties by post-finishing or adding functional materials. At present, traditional heating viscose fibers focus on their heating function, but ignore their insufficient heat storage capacity and poor warmth retention in cold weather. At the same time, the heating viscose fibers on the market are darker in color, which affects the fashionability and wide application of clothing. In addition, heating viscose fibers generally have the problem that the powder is not resistant to acid and alkali when preparing the fiber, and the powder has a large density, which makes the spinning solution prone to powder deposition, and then makes the spinning solution uneven, which not only causes serious loss of powder, but also affects the service life and heating effect of the fiber.
[0003] Existing products such as heat-storage viscose fiber fabrics, such as a Chinese patent application (authorization announcement number CN103498208B), disclose a heat-storage fiber and a preparation method thereof. Specifically, the heat-storage fiber is prepared by dispersing heat-storage powder of a specific particle size in acrylonitrile and vinyl acetate blended fibers. However, the functional material inside the fiber is prone to leakage when undergoing a solid-liquid phase change, thereby affecting the comfort of the fabric surface and even causing harm to the environment. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber and a preparation method thereof. In the presence of an auxiliary agent, modified nano tungsten bronze is introduced into cellulose to prepare a viscose fiber with antibacterial and flame-retardant properties. The system has high compatibility, which can effectively improve the heating and heat storage efficiency of the viscose fiber while reducing the loss of the effective ingredient powder due to acid and alkali intolerance, thereby ensuring the heating and heat storage effects and service life of the viscose fiber.
[0005] On one hand, the present invention provides a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, the preparation raw materials of which include 0.1-30 parts of modified nano tungsten bronze, 40-100 parts of cellulose solution, 0.05-5 parts of additives and 20-50 parts of water.
[0006] As a preferred technical solution, the modified nano tungsten bronze is a three-layer composite structure, including a surface polyethylene glycol grafted layer, an intermediate zirconium phosphate coating layer and an inner metal-doped tungsten bronze. The structural formula of the metal-doped tungsten bronze is M x WO3.
[0007] As a preferred technical solution, the M xIn WO3, M is any one of alkali metals, alkaline earth metal elements, and rare earth metal elements, preferably cesium; x is 0.01 to 0.4, preferably 0.1 to 0.33.
[0008] Preferably, the M x M in WO3 is cesium. The radius of the cesium ion is slightly larger than the radius of the hexagonal channel in the tungsten oxide octahedron. When lattice distortion occurs, the doping efficiency of the cesium ion in the tungsten oxide octahedron is higher and more stable, and due to the increase in surface defects, the infrared absorption capacity can be greatly improved.
[0009] As a preferred technical solution, the preparation method of the modified nano tungsten bronze at least includes the following preparation steps:
[0010] (1) Preparing metal-doped tungsten bronze powder using a metal source, a tungsten source and tungsten trioxide;
[0011] (2) Weigh the zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 20-30 minutes to fully dissolve them, obtain a solution, then add ammonia water with a mass concentration of 15% dropwise, adjust the solution pH to 8.5-9.5, then slowly add metal-doped tungsten bronze powder, continue stirring for 3-8 hours, collect the powder by suction filtration, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixed gas, heat it to 300-400°C at a heating rate of 5-10°C / min, keep it warm for 1-2 hours, and naturally cool it to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate;
[0012] (3) Add metal-doped tungsten bronze powder coated with zirconium phosphate and oxalic acid into redistilled tetrahydrofuran and stir for 30 minutes, add N,N'-dicyclohexylcarboximide and 4-dimethylaminopyridine under nitrogen protection, add polyethylene glycol after stirring for 12 hours and stir for 48-72 hours, filter, rinse with solvent, and dry to obtain modified nano tungsten bronze.
[0013] Preferably, in step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is (0.5-1.5): 1; preferably, the zirconium source is one of zirconium nitrate, zirconium oxide, and zirconium oxychloride.
[0014] In the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to polyethylene glycol is (1-5):1.
[0015] Based on the system of the present invention, by coating zirconium phosphate on the surface of the inner metal-doped tungsten bronze, especially controlling the mass ratio of zirconium phosphate-coated cesium tungsten bronze powder to polyethylene glycol to (1-5):1, the acid and alkali resistant surface modification of nano tungsten bronze is achieved, and the loss of effective ingredient powder due to acid and alkali resistance is reduced, while giving viscose fiber antibacterial and flame retardant functions, thereby improving its heating and heat storage efficiency. The inventor analyzed that the reason may be that by controlling the mass ratio of zirconium phosphate-coated cesium tungsten bronze powder to polyethylene glycol to (1-5):1, the thermal conductivity effect and the heating and heat storage effect of the zirconium phosphate coating layer are effectively balanced, thereby improving the heating and heat storage efficiency.
[0016] As a preferred technical solution, the polyethylene glycol is at least one of polyethylene glycol 400, polyethylene glycol 600, polyethylene glycol 800, polyethylene glycol 1000, polyethylene glycol 1200, polyethylene glycol 1500, and polyethylene glycol 2000; preferably, the polyethylene glycol is one of polyethylene glycol 600, polyethylene glycol 800, and polyethylene glycol 1000.
[0017] As a preferred technical solution, the density of polyethylene glycol grafted in the polyethylene glycol grafted layer is 0.1 to 0.8 g / cm 3 The graft thickness is 10-25 nm. Preferably, the density of the polyethylene glycol graft is 0.2-0.6 g / cm 3 The grafting thickness is 15 to 20 nm.
[0018] In the present invention, the outer layer of the modified nano tungsten bronze is grafted with polyethylene glycol, which improves its compatibility and dispersibility with the organic system and realizes the function of phase change heat storage. The inventors found in the process of exploration that, in particular, the mass ratio of zirconium phosphate-coated cesium tungsten bronze powder to polyethylene glycol is controlled to be (1-5): 1. On the one hand, the problem of sedimentation of the modified nano tungsten bronze in the production process is solved through hydrogen bond interaction in the system, thereby ensuring the subsequent spinning effect, while ensuring the thermal insulation effect and heat storage efficiency.
[0019] As a preferred technical solution, the auxiliary agent is one or a combination of dimethyl nylonate, propylene glycol methyl ether acetate, dimethyl carbonate, diethyl carbonate, 1,4-butyrolactone, ethylene glycol tert-butyl ether, propylene glycol methyl ether, D-limonene, ethylene carbonate, and ethylene glycol diacetate.
[0020] As a preferred technical solution, the method for preparing the cellulose solution is: dissolving cellulose at low temperature in an aqueous solution containing urea and alkali and then subjecting the solution to freeze-thaw cycles to obtain a colorless and transparent cellulose solution.
[0021] As a preferred technical solution, the cellulose ((C6H 10 O5) n) has a degree of polymerization (number of D-glucoside) n=200-1200. Preferably, the degree of polymerization of the cellulose is n=500-1000. The inventors found in the process of exploration that by controlling the degree of polymerization of cellulose to 200-1200, especially when the degree of polymerization of cellulose is 500-1000, the viscosity of the system is within a suitable range, which is conducive to the dispersion of the modified nano tungsten bronze, while ensuring that the fracture strength, elongation and fatigue resistance of the prepared viscose are within a good range.
[0022] Preferably, the alkali is sodium hydroxide or lithium hydroxide; the mass concentration of urea in the aqueous solution containing urea and alkali is 3-10wt%, and the mass concentration of alkali is 0.1-2wt%.
[0023] Preferably, the mass concentration of cellulose in the cellulose solution is 50-80wt%.
[0024] Preferably, the temperature range of the freeze-thaw cycle is -40°C-80°C, and the number of freeze-thaw cycles is 5 times.
[0025] Another aspect of the present invention provides a method for preparing light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, which comprises at least the following steps:
[0026] S1, mixing and grinding the modified nano tungsten bronze, additives and water to obtain a mixture;
[0027] S2, mixing the mixed material with the cellulose solution and stirring to obtain a spinning solution;
[0028] S3, filtering the spinning solution and adding it into a spinning box, metering, filtering, spinning, and coagulation to obtain the primary spun yarn, which is then stretched, shaped, cleaned, dried, and wound.
[0029] Preferably, the sanding time in step (1) is 24-36 hours.
[0030] Preferably, the mixing and stirring in step (2) is mechanical stirring, and the stirring rate of the mechanical stirring is 500 to 1000 rpm.
[0031] Beneficial effects:
[0032] 1. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber provided by the present invention introduces modified nano tungsten bronze into cellulose in the presence of an auxiliary agent to prepare a viscose fiber with antibacterial and flame-retardant properties. The system has high compatibility, which effectively improves the heating and heat storage efficiency of the viscose fiber while reducing the loss of the effective ingredient powder due to acid and alkali intolerance, thereby ensuring the heating and heat storage effects and service life of the viscose fiber.
[0033] 2. Based on the system of the present invention, by coating zirconium phosphate on the surface of the inner metal-doped tungsten bronze, especially controlling the mass ratio of zirconium phosphate-coated cesium tungsten bronze powder to polyethylene glycol to (1-5):1, the acid and alkali resistant surface modification of nano tungsten bronze is achieved, and the loss of effective ingredient powder due to acid and alkali resistance is reduced, while giving viscose fiber antibacterial and flame retardant functions, thereby improving its heating and heat storage efficiency.
[0034] 3. The outer layer of the modified nano tungsten bronze in the present invention is grafted with polyethylene glycol, which improves its compatibility and dispersibility with the organic system and realizes the function of phase change heat storage.
[0035] 4. The present invention controls the mass ratio of zirconium phosphate-coated cesium tungsten bronze powder to polyethylene glycol to (1-5): 1. On the one hand, the problem of sedimentation of modified nano tungsten bronze during the production process is solved through hydrogen bond interaction in the system, thereby ensuring the subsequent spinning effect and at the same time ensuring the thermal insulation effect and heat storage efficiency.
[0036] 5. Based on the system of the present invention, by controlling the degree of polymerization of cellulose to 200-1200, especially when the degree of polymerization of cellulose is 500-1000, the viscosity of the system is within a suitable range, which is beneficial to the dispersion of modified nano tungsten bronze and ensures that the fracture strength, elongation and fatigue resistance of the prepared viscose are within a good range. DETAILED DESCRIPTION
[0037] Example 1
[0038] Embodiment 1 of the present invention provides a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, the raw materials for preparing the fiber include 15 parts of modified nano tungsten bronze, 75 parts of cellulose solution, 3 parts of an auxiliary agent and 35 parts of water.
[0039] The modified nano tungsten bronze is a three-layer composite structure, including a surface polyethylene glycol grafted layer, an intermediate zirconium phosphate coating layer and an inner metal-doped tungsten bronze. The structural formula of the metal-doped tungsten bronze is M x WO3.
[0040] The M x In WO3, M is cesium and x is 0.2.
[0041] The preparation method of the modified nano tungsten bronze comprises the following preparation steps:
[0042] (1) The metal source (cesium carbonate), tungsten source (tungstic acid) and tungsten trioxide were mixed and calcined at 600°C in vacuum for 5 hours to prepare metal-doped tungsten bronze powder, with the molar ratio of cesium to tungsten being 1:5;
[0043] (2) Weigh the zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them, obtain a solution, then add ammonia water with a mass concentration of 15% dropwise, adjust the solution pH to 9, and then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, filter and collect the powder, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixed gas, heat to 380°C at a heating rate of 8°C / min, keep warm for 1.5 hours, and naturally cool to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate;
[0044] (3) The metal-doped tungsten bronze powder coated with zirconium phosphate was added to redistilled tetrahydrofuran and stirred for 30 minutes. N,N'-dicyclohexylcarboximide and 4-dimethylaminopyridine were added under nitrogen protection. After stirring for 12 hours, polyethylene glycol was added and stirred for 72 hours. After the end, the modified nano tungsten bronze was filtered, washed with solvent, and dried to obtain the modified nano tungsten bronze.
[0045] In the step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is 1:1; the zirconium source is zirconium oxide.
[0046] In the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to polyethylene glycol is 3:1.
[0047] The polyethylene glycol is polyethylene glycol 800.
[0048] The auxiliary agent is a combination of dimethyl nylonate and propylene glycol methyl ether acetate, and the mass ratio of the dimethyl nylonate to propylene glycol methyl ether acetate is 2:1.
[0049] The preparation method of the cellulose solution comprises the following steps: dissolving cellulose at low temperature with an aqueous solution containing urea and alkali, and then performing freeze-thaw cycles to obtain a colorless and transparent cellulose solution.
[0050] The cellulose ((C6H 10 O5) n ) has a degree of polymerization (number of D-glucosides) of n=800.
[0051] The alkali is lithium hydroxide; the mass concentration of urea in the aqueous solution containing urea and alkali is 8wt%, and the mass concentration of the alkali is 1wt%.
[0052] The mass concentration of cellulose in the cellulose solution is 60 wt %.
[0053] The temperature range of the freeze-thaw cycle is -40°C-80°C, and the number of freeze-thaw cycles is 5 times.
[0054] Embodiment 1 of the present invention provides a method for preparing light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, comprising the following steps:
[0055] S1, mixing and grinding the modified nano tungsten bronze, additives and water to obtain a mixture;
[0056] S2, mixing the mixed material with the cellulose solution and stirring to obtain a spinning solution;
[0057] S3, filtering the spinning solution and adding it into a spinning box, metering, filtering, spinning, and coagulation to obtain primary silk, which is then stretched, shaped, cleaned, dried, and wound.
[0058] The sanding time in step (1) is 36 hours.
[0059] The mixing and stirring in step (2) is mechanical stirring, and the stirring rate of the mechanical stirring is 1000 rpm.
[0060] Example 2
[0061] Embodiment 2 of the present invention provides a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, the raw materials for preparing the fiber include 30 parts of modified nano tungsten bronze, 100 parts of cellulose solution, 5 parts of additives and 50 parts of water.
[0062] The modified nano tungsten bronze is a three-layer composite structure, including a surface polyethylene glycol grafted layer, an intermediate zirconium phosphate coating layer and an inner metal-doped tungsten bronze. The structural formula of the metal-doped tungsten bronze is M x WO3.
[0063] The M x In WO3, M is cesium and x is 0.1.
[0064] The preparation method of the modified nano tungsten bronze comprises the following preparation steps:
[0065] (1) The metal source (cesium carbonate), tungsten source (tungstic acid) and tungsten trioxide were mixed and calcined at 800°C in vacuum for 1.5 hours to prepare metal-doped tungsten bronze powder, with the molar ratio of cesium to tungsten being 1:10;
[0066] (2) Weigh the zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them, obtain a solution, then add ammonia water with a mass concentration of 15% dropwise, adjust the solution pH to 9, and then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, filter and collect the powder, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixed gas, heat to 400°C at a heating rate of 8°C / min, keep warm for 2 hours, and naturally cool to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate;
[0067] (3) The metal-doped tungsten bronze powder coated with zirconium phosphate was added to redistilled tetrahydrofuran and stirred for 30 minutes. N,N'-dicyclohexylcarboximide and 4-dimethylaminopyridine were added under nitrogen protection. After stirring for 12 hours, polyethylene glycol was added and stirred for 72 hours. After the end, the modified nano tungsten bronze was filtered, washed with solvent, and dried to obtain the modified nano tungsten bronze.
[0068] In the step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is 1.5:1; the zirconium source is zirconium oxide.
[0069] In the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to the polyethylene glycol is 1:1.
[0070] The polyethylene glycol is polyethylene glycol 800.
[0071] The auxiliary agent is a combination of dimethyl nylonate and propylene glycol methyl ether acetate, and the mass ratio of the dimethyl nylonate to propylene glycol methyl ether acetate is 2:1.
[0072] The preparation method of the cellulose solution comprises the following steps: dissolving cellulose at low temperature with an aqueous solution containing urea and alkali, and then performing freeze-thaw cycles to obtain a colorless and transparent cellulose solution.
[0073] The cellulose ((C6H 10 O5) n ) has a degree of polymerization (number of D-glucosides) of n=800.
[0074] The alkali is lithium hydroxide; the mass concentration of urea in the aqueous solution containing urea and alkali is 8wt%, and the mass concentration of the alkali is 1wt%.
[0075] The mass concentration of cellulose in the cellulose solution is 60 wt %.
[0076] The temperature range of the freeze-thaw cycle is -40°C-80°C, and the number of freeze-thaw cycles is 5 times.
[0077] Embodiment 2 of the present invention provides a method for preparing light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, comprising the following steps:
[0078] S1, mixing and grinding the modified nano tungsten bronze, additives and water to obtain a mixture;
[0079] S2, mixing the mixed material with the cellulose solution and stirring to obtain a spinning solution;
[0080] S3, filtering the spinning solution and adding it into a spinning box, metering, filtering, spinning, and coagulation to obtain primary silk, which is then stretched, shaped, cleaned, dried, and wound.
[0081] The sanding time in step (1) is 36 hours.
[0082] The mixing and stirring in step (2) is mechanical stirring, and the stirring rate of the mechanical stirring is 1000 rpm.
[0083] Example 3
[0084] Embodiment 3 of the present invention provides a light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, the raw materials for preparing the fiber include 5 parts of modified nano tungsten bronze, 40 parts of cellulose solution, 1 part of auxiliary agent and 20 parts of water.
[0085] The modified nano tungsten bronze is a three-layer composite structure, including a surface polyethylene glycol grafted layer, an intermediate zirconium phosphate coating layer and an inner metal-doped tungsten bronze. The structural formula of the metal-doped tungsten bronze is M x WO3.
[0086] The M x In WO3, M is cesium and x is 0.33.
[0087] The preparation method of the modified nano tungsten bronze comprises the following preparation steps:
[0088] (1) The metal source (cesium carbonate), tungsten source (tungstic acid) and tungsten trioxide were mixed and calcined at 400°C in vacuum for 9 hours to prepare metal-doped tungsten bronze powder, with the molar ratio of cesium to tungsten being 1:3;
[0089] (2) Weigh the zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them, obtain a solution, then add ammonia water with a mass concentration of 15% dropwise, adjust the solution pH to 9, and then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, filter and collect the powder, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixed gas, heat to 350°C at a heating rate of 8°C / min, keep warm for 1 hour, and naturally cool to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate;
[0090] (3) The metal-doped tungsten bronze powder coated with zirconium phosphate was added to redistilled tetrahydrofuran and stirred for 30 minutes. N,N'-dicyclohexylcarboximide and 4-dimethylaminopyridine were added under nitrogen protection. After stirring for 12 hours, polyethylene glycol was added and stirred for 72 hours. After the end, the modified nano tungsten bronze was filtered, washed with solvent, and dried to obtain the modified nano tungsten bronze.
[0091] In the step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is 0.5:1; the zirconium source is zirconium oxide.
[0092] In the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to polyethylene glycol is 5:1.
[0093] The polyethylene glycol is polyethylene glycol 800.
[0094] The auxiliary agent is a combination of dimethyl nylonate and propylene glycol methyl ether acetate, and the mass ratio of the dimethyl nylonate to propylene glycol methyl ether acetate is 2:1.
[0095] The preparation method of the cellulose solution comprises the following steps: dissolving cellulose at low temperature with an aqueous solution containing urea and alkali, and then performing freeze-thaw cycles to obtain a colorless and transparent cellulose solution.
[0096] The cellulose ((C6H 10 O5) n ) has a degree of polymerization (number of D-glucosides) of n=800.
[0097] The alkali is lithium hydroxide; the mass concentration of urea in the aqueous solution containing urea and alkali is 8wt%, and the mass concentration of the alkali is 1wt%.
[0098] The mass concentration of cellulose in the cellulose solution is 60 wt %.
[0099] The temperature range of the freeze-thaw cycle is -40°C-80°C, and the number of freeze-thaw cycles is 5 times.
[0100] Embodiment 3 of the present invention provides a method for preparing light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber, comprising the following steps:
[0101] S1, mixing and grinding the modified nano tungsten bronze, additives and water to obtain a mixture;
[0102] S2, mixing the mixed material with the cellulose solution and stirring to obtain a spinning solution;
[0103] S3, filtering the spinning solution and adding it into a spinning box, metering, filtering, spinning, and coagulation to obtain the primary spun yarn, which is then stretched, shaped, cleaned, dried, and wound.
[0104] The sanding time in step (1) is 36 hours.
[0105] The mixing and stirring in step (2) is mechanical stirring, and the stirring rate of the mechanical stirring is 1000 rpm.
[0106] Example 4
[0107] Example 4 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that x is 0.01.
[0108] Example 5
[0109] Example 5 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof, and its specific implementation method is the same as that of Example 1, except that the M x M in WO3 is sodium, that is, the metal source used to prepare metal-doped tungsten bronze powder is sodium carbonate.
[0110] Example 6
[0111] Embodiment 6 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation manner is the same as that of Embodiment 1, except that in step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is 0.1:1.
[0112] Example 7
[0113] Embodiment 7 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation manner is the same as that of Embodiment 1, except that in step (2), the mass ratio of the zirconium source to the metal-doped tungsten bronze powder is 3:1.
[0114] Example 8
[0115] Example 8 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the polyethylene glycol is polyethylene glycol 2000.
[0116] Example 9
[0117] Embodiment 9 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation manner is the same as that of Embodiment 1, except that in step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to the polyethylene glycol is 0.5:1.
[0118] Example 10
[0119] Comparative Example 1 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that in the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to the polyethylene glycol is 8:1.
[0120] Embodiment 11
[0121] Comparative Example 11 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the step (2) is specifically as follows: weigh a zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them to obtain a solution, then dropwise add ammonia water with a mass concentration of 15%, adjust the solution pH to 9, then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, collect the powder by suction filtration, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixture, heat to 300°C at a heating rate of 8°C / min, keep warm for 1.5 hours, and naturally cool to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate.
[0122] Example 12
[0123] Comparative Example 12 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the step (2) is specifically as follows: weigh a zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them to obtain a solution, then dropwise add ammonia water with a mass concentration of 15%, adjust the solution pH to 9, then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, collect the powder by suction filtration, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixture, heat to 500°C at a heating rate of 8°C / min, keep warm for 1.5 hours, and naturally cool to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate.
[0124] Embodiment 13
[0125] Comparative Example 21 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that the step (2) is specifically as follows: weigh a zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 25 minutes to fully dissolve them to obtain a solution, then dropwise add ammonia water with a mass concentration of 15%, adjust the solution pH to 9, and then slowly add metal-doped tungsten bronze powder, continue stirring for 5 hours, collect the powder by suction, wash, dry, and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixture, heat to 380°C at a heating rate of 8°C / min, keep warm for 3 hours, and naturally cool to room temperature to obtain zirconium phosphate-coated metal-doped tungsten bronze powder.
[0126] Comparative Example 1
[0127] Comparative Example 1 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the step (3) is specifically as follows: the metal-doped tungsten bronze powder coated with zirconium phosphate is stirred and mixed with polyethylene glycol for 72 hours, and then filtered, rinsed with solvent, and dried to obtain the modified nano tungsten bronze.
[0128] Comparative Example 2
[0129] Comparative Example 2 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified nano tungsten bronze has no polyethylene glycol grafting layer.
[0130] Comparative Example 3
[0131] Comparative Example 3 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the zirconium source is replaced by magnesium oxide.
[0132] Comparative Example 4
[0133] Comparative Example 4 of the present invention provides a light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the metal-doped tungsten bronze powder coated with zirconium phosphate is replaced by a mixture of metal-doped tungsten bronze powder (prepared in step (1) of Example 1) and zirconium phosphate (zirconium phosphate modified by step (3) of Example 1) powder in a mass ratio of 1:1.5.
[0134] Performance Testing
[0135] (1) Powder loss rate: The W (tungsten) content in the spinning solution before spinning and the light-absorbing, heat-storing, antibacterial viscose fiber after spinning and finalization in the examples and comparative examples was determined by ICP spectral emission method. Powder loss rate (%) = (tungsten content in spinning solution - tungsten content in viscose fiber) / tungsten content in spinning solution. The results are shown in Table 1.
[0136] (2) L value (color difference value): The light-absorbing, heat-generating, heat-storing and antibacterial viscose fibers provided in the examples and comparative examples were tested for L value using a colorimeter. The results are shown in Table 1.
[0137] (3) Heating effect: The maximum temperature of the light-absorbing, heat-generating, heat-storing, antibacterial viscose fibers provided in the examples and comparative examples was tested. The results are shown in Table 1.
[0138] (4) Heat preservation rate: The light-absorbing, heat-generating, heat-storing, antibacterial viscose fibers provided in the examples and comparative examples are made into fibers with a gram weight of 220-230 g / m 2 The thermal insulation rate of the fabric is measured according to method A specified in GB / T11048-1989. The results are shown in Table 1.
[0139] (5) Breaking strength: Referring to the standard GB / T 3923.1-2013, the breaking strength of the light-absorbing, heat-storing, antibacterial viscose fibers provided in the examples and comparative examples was tested. The results are shown in Table 1.
[0140] Table 1
[0141]
[0142]
[0143] Under the technical solutions provided in Examples 1-3 of the present invention, the viscose fibers prepared have a lower powder loss rate, a higher L value, a light fiber color, excellent thermal insulation and heating properties, and at the same time ensure the breaking strength of the fiber.
[0144] In Example 4 of the present invention, the cesium doping amount is too small, and in Example 5, the cesium doping is replaced by sodium doping, both of which lead to a decrease in the number of surface defects of the metal-doped tungsten bronze powder and a decrease in the infrared absorption rate, so the thermal insulation rate and heating effect of the fiber finally prepared are reduced.
[0145] In Example 6, the amount of zirconium source added was too low, resulting in a decrease in the acid and alkali resistance of the composite powder and an increase in the powder loss rate, which resulted in a decrease in the fiber thermal insulation rate and a decrease in the fracture strength. In Example 7, the amount of zirconium source added was too high, resulting in an excessively thick outer coating layer of the metal-doped tungsten bronze powder, which affected the infrared absorption effect, and ultimately reduced the heating effect and thermal insulation rate of the prepared fiber.
[0146] In Example 8, the molecular weight of polyethylene glycol is too high, and the longer hydrophobic chain will lead to a decrease in the dispersibility of the modified composite powder, thereby reducing the thermal insulation and heat generation properties of the prepared fiber, and will affect the breaking strength of the fiber.
[0147] In Example 9, the amount of polyethylene glycol added was increased, resulting in an excessively thick graft layer of the modified composite powder, which affected the thermal insulation and heat generation properties of the fiber. In Example 10, the amount of polyethylene glycol added was reduced, resulting in poor dispersibility of the modified composite powder, and a decrease in heat storage capacity, which reduced the thermal insulation, heat generation and breaking strength of the fiber.
[0148] In Example 11, the sintering temperature was low, and part of the metal-doped tungsten bronze powder was not coated by zirconium phosphate, resulting in an increase in the powder loss rate during the fiber preparation process, a darker color of the prepared fiber, and decreased heat generation, thermal insulation performance, and fracture strength. In Example 12, the sintering temperature was increased to 500°C, and in Example 13, the sintering time was increased to 3h at 380°C, both of which resulted in an excessively thick grafted layer of the modified composite powder, affecting the heat generation and thermal insulation performance of the final prepared fiber.
[0149] The comparative test results of Example 1 and Comparative Example 1 show that the modified nano tungsten bronze prepared by directly mixing zirconium phosphate-coated cesium tungsten bronze powder with polyethylene glycol is used to prepare viscose fiber. The composite powder has poor dispersion effect and polyethylene glycol is easily lost during the phase change process, which significantly reduces the heat generation and thermal insulation performance of the fiber, and also reduces the breaking strength of the fiber.
[0150] The comparative test results of Example 1 and Comparative Example 2 show that the composite powder without the grafted polyethylene glycol layer has poor dispersibility, and the heat generation performance, thermal insulation performance and breaking strength of the prepared fiber are significantly reduced.
[0151] The comparative test results of Example 1 and Comparative Example 3 show that replacing zirconium phosphate with magnesium phosphate leads to a decrease in the acid and alkali resistance of the powder, an increase in the powder loss rate, and a significant decrease in the thermal insulation and heating properties.
[0152] The comparative test results of Example 1 and Comparative Example 4 show that directly blending the modified zirconium phosphate with tungsten bronze cannot improve the acid and alkali resistance, whiteness and dispersibility of tungsten bronze, resulting in a high powder loss rate, and the heating performance, thermal insulation performance and breaking strength of the fiber will be affected and reduced.
Claims
1. A light-absorbing, heat-generating, heat-storing, antibacterial viscose fiber, characterized in that: The raw materials for its preparation include 0.1-30 parts of modified nano tungsten bronze, 40-100 parts of cellulose solution, 0.05-5 parts of additives, and 20-50 parts of water; The preparation method of the modified nano tungsten bronze at least comprises the following preparation steps: (1) Metal-doped tungsten bronze powder is prepared using metal source, tungsten source and tungsten trioxide; (2) Weigh the zirconium source and diammonium dihydrogen phosphate in deionized water, stir for 20-30 minutes to fully dissolve them, obtain a solution, then add ammonia water with a mass concentration of 15% dropwise, adjust the solution pH to 8.5-9.5, then slowly add metal-doped tungsten bronze powder, continue stirring for 3-8 hours, collect the powder by suction filtration, wash, dry and sieve to obtain a precursor; sinter the precursor in a nitrogen-hydrogen mixed gas, heat it to 300-400°C at a heating rate of 5-10°C / min, keep it warm for 1-2 hours, and naturally cool it to room temperature to obtain metal-doped tungsten bronze powder coated with zirconium phosphate; (3) Add metal-doped tungsten bronze powder coated with zirconium phosphate and oxalic acid to redistilled tetrahydrofuran and stir for 30 minutes, add N,N'-dicyclohexylcarboximide and 4-dimethylaminopyridine under nitrogen protection, add polyethylene glycol after stirring for 12 hours and stir for 48-72 hours, filter, rinse with solvent, and dry to obtain modified nano tungsten bronze; In the step (3), the mass ratio of the metal-doped tungsten bronze powder coated with zirconium phosphate to the polyethylene glycol is (1-5): 1; The preparation method of the cellulose solution comprises: dissolving cellulose at low temperature in an aqueous solution containing urea and alkali and then performing freeze-thaw cycles to obtain a colorless and transparent cellulose solution; the polymerization degree of the cellulose is n=200-1200.
2. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to claim 1, characterized in that: The modified nano tungsten bronze is a three-layer composite structure, including a surface polyethylene glycol grafted layer, an intermediate zirconium phosphate coating layer and an inner metal-doped tungsten bronze. The structural formula of the metal-doped tungsten bronze is M x WO3.
3. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to claim 2, characterized in that: The M x In WO3, M is any one of alkali metal, alkaline earth metal element and rare earth metal element, and x is 0.01~0.
4.
4. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to claim 3, characterized in that: The M x In WO3, x is 0.1-0.
33.
5. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to claim 1, characterized in that: The mass ratio of the zirconium source to the metal-doped tungsten bronze powder in step (2) is (0.5-1.5):
1.
6. The light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to claim 1, characterized in that: The polyethylene glycol is at least one of polyethylene glycol 400, polyethylene glycol 600, polyethylene glycol 800, polyethylene glycol 1000, polyethylene glycol 1200, polyethylene glycol 1500, and polyethylene glycol 2000.
7. A method for preparing the light-absorbing, heat-generating, heat-storing and antibacterial viscose fiber according to any one of claims 1 to 6, characterized in that: At least the following steps are included: S1, mixing and grinding the modified nano tungsten bronze, additives and water to obtain a mixture; S2, mixing the mixed material with the cellulose solution and stirring to obtain a spinning solution; S3, filtering the spinning solution and adding it into a spinning box, metering, filtering, spinning, and coagulation to obtain the primary spun yarn, which is then stretched, shaped, cleaned, dried, and wound.
Citation Information
Patent Citations
Heat storage fiber and preparation method thereof
CN103498208B
Hexagonal crystal tungsten bronze short rod nanoparticles and preparation method thereof
CN105502503A
Variable valency metal catalyzed and doped tungsten bronze nano-short rod particle and preparation method thereof
CN105668632A
High-efficiency thermochromic nano composite powder with core-shell structure and preparation method thereof
CN108659812A
Liquid phase dispersoid containing multi-layer-structure nano composite particles and preparation method of liquid phase dispersoid