Coating composition containing chitosan
By treating chitosan in an acidic solution, small-grain chitosan compounds are formed and precipitated in paints or coatings, the dispersion problem in water-based paints and coatings is solved, and the elongation of the coating is improved and antifungal properties.
Patent Information
- Application Number
- CN202180062448.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-22
- Filing Date
- 2021-09-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-09-20
AI Technical Summary
The prior art is difficult to effectively disperse chitosan in water-based paints and coatings, resulting in its insoluble and instability in latex and other aqueous dispersion systems, affecting the quality and performance of the coatings.
By performing high-speed shearing treatment of chitosan compounds in acidic solution and precipitating after neutralization, the particle size is less than 30 microns, ensuring uniform dispersion in paint or coatings, and forming a stable membrane structure in the dry film .
The uniform dispersion of chitosan in paint or coating is achieved, the elongation, thermal cycle characteristics and anti-fungal staining of the coating are improved, and the dependence on traditional fungicides is reduced.
Smart Images

Figure CN116075564B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to paints and coatings containing chitosan which provide benefits over conventional coatings in the form of improved resistance to leaching, improved elongation and reduced susceptibility to fungal or mildew staining than conventional coatings, articles coated therewith, and methods of making the coatings or coated articles. Background Art
[0002] Paints and coatings typically contain three basic ingredients: a carrier fluid, a binder, and additives. Pigments are also commonly added to many paints and coatings. Each of these ingredients can include a single component or several different substances that are mixed into the paint or coating.
[0003] The carrier liquid is the fluid component of the paint that carries all the other paint components. The carrier liquid is part of the wet paint and typically evaporates as the paint forms a film and dries on the surface. In latex paints, the carrier liquid is typically water. In oil-based paints, the carrier liquid is typically an organic solvent. The amount and type of liquid is typically determined by the characteristics of the other paint components.
[0004] The binder component of a paint or coating is the substance that allows the paint or coating to form a film on a surface and adhere to the surface. In latex paints, the binder includes a latex resin, typically selected from acrylics, vinyl acrylics, styrene acrylics, or polyurethane dispersions ("PUDs"). In latex paints or coatings, the latex resin particles are typically in a dispersion with water as the carrier liquid.
[0005] Pigments provide both decorative and protective features to paints or coatings. Pigments are solid particles used to provide various qualities to paints or coatings, including but not limited to color, opacity, and durability. The paint or coating may also contain other solid particles, such as polyurethane beads or other solids. Pigments and other solids increase the volume of the paint or coating, and their content is related to the gloss or flatness of the paint or coating. Pigments may also impart color to the paint or coating.
[0006] A variety of additives may be included in paints or coatings. Additives are typically used in paint / coating formulations at relatively low levels but contribute to various properties of paints and coatings, including rheological properties, stability, paint performance, in-can preservation, dry film preservation or protection, and application quality.
[0007] Biocides are additives with mildew-proof, antibacterial and bactericidal properties. A variety of biocides are well known and used for a variety of purposes, including but not limited to preserving wet paint or coatings ("in-can" storage) and preserving or protecting dry films on coated articles. Such biocides include inorganic biocides, for example, those containing metal ions such as silver, zinc and copper. Other inorganic biocides include phosphates, metal ions, metals or other biocides containing zeolites or hydroxyapatites. There are also organic biocides, including organic acids, phenols, alcohols and quaternary ammonium compounds.
[0008] Some biocides are particularly effective, such as mildew or fungicides, which are additives with mildew or fungicidal properties. Mildew and fungicides are used to prevent, reduce or pre-prevent mildew from forming in cured paint or coating films. Zinc compounds (including zinc oxide) are common fungicides and mildew inhibitors, and the use of zinc compounds effectively prevents and / or reduces mildew, mold and fungi in cured films. Zinc oxide may have disadvantages and produce problems with the dispersibility of paints and coatings. Other known fungicides include iodopropynyl butylcarbamate (IPBC), 2-octyl-3 (2H)-isothiazolinone (OIT), thiophanate-methyl, etc.
[0009] Chitosan is a bio-based material that can be obtained in a renewable manner from sources such as chitin from crustaceans and, if dispersible, would be a useful additive or filler in paint formulations. In conventional practice, chitosan is not used in paints and coatings due to its water insolubility, adverse effects on the quality of paints and coatings, and difficulty in fully dispersing chitosan in latex and other aqueous dispersions used for paints and coatings, despite its relatively low cost and relative renewability. Providing a uniformly dispersed paint or coating is important not only for ease of preparation but also for providing a high quality paint that does not have grit or other defects in uniformity, application, appearance or feel.
[0010] Related art has sought to attempt alternative methods of dissolving or dispersing chitosan in water. One such method involves providing chitosan in an acidic solution. Acidic solutions are highly impractical for direct addition to water-based paints and coatings, the pH of which is substantially alkaline. Adding a significantly acidic solution to maintain acidity and therefore chitosan in solution will greatly interfere with the stability of the coating formulation and will require a thorough reformulation. Other methods require costly chemical modification of the chitosan polymer backbone with hydrophilic groups to provide water solubility before addition to the water-based paint or coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1aA Hegman gauge drawdown of a paint containing large particle size chitosan is shown; Figure 1b A Hegman gauge drawdown of an exemplary paint containing chitosan particles is shown.
[0012] Figure 2a shows a microscopic image of a painted panel, wherein the paint contains large particle size chitosan; Figure 2b Microscopic images of painted panels are shown, where an exemplary paint contains smaller particle size chitosan.
[0013] Figure 3a-3e An exemplary paint applied to a Hardie board substrate is shown after 19 weeks in a mold chamber.
[0014] Figure 4a-4e An exemplary paint applied to an aluminum panel is shown after 19 weeks in a mold chamber.
[0015] Figure 5a-5c An exemplary paint is shown applied to filter paper and tested for algae growth inhibition.
[0016] Figure 6a and Figure 6b A schematic diagram showing a portion of an exemplary method for preparing a paint or coating containing a chitosan compound is shown. Summary of the invention
[0017] In one embodiment, the present invention comprises a paint or coating composition comprising water, a latex binder resin and an additive, wherein such additives include but are not limited to chitosan compounds. In some embodiments, the chitosan compound additive has a particle size of less than 30 microns in the paint or coating, which is measured using ASTM D1210-05 "Standard Test Method for Fineness of Dispersion of Pigment-Vehicle Systems by Hegman-Type Gage". In another embodiment, the present invention comprises a coated article, which is formed by a paint or coating composition comprising water, a latex binder resin and an additive, wherein such additives include but are not limited to chitosan compounds, and wherein the paint or coating composition is dried to form a film on the coated article. The chitosan compound is distributed throughout the film on the coated article. In some embodiments, when dispersed in a paint or coating, the chitosan compound additive has a particle size of less than 30 microns, which is measured using ASTM D1210-05. Hegman gauge values below 30 microns also indicate that chitosan has adequate dispersibility. The dried paint or coating film exhibits improved elongation as measured according to ASTM D2370-16 "Standard Test Method for Tensile Properties", improved thermal cycling properties using a rating scale according to ASTM D714-02 "Standard Test Method for Evaluating Degree of Blistening of Paints" and ASTM D661-93 "Standard Test Method for Evaluating Degree of Cracking of Exterior Paints", and improved resistance to leaching of surfactants or other additives as measured according to the methods described herein.A modified version of the ASTM D5589-19 method "Standard Test Method for Determining the Resistance of Paint Films and Related Coatings to Algal Defacement" can be used to show reduced leaching of paint components in the exemplary compositions. The dried films may also be less susceptible to mold or fungal growth and fouling than the same paint or coating that does not include the chitosan compound. In some embodiments, coatings containing chitosan compounds may require reduced amounts of traditional fungicides such as zinc oxide.
[0018] In an embodiment of the invention, chitosan is incorporated into the paints and coatings, wherein the particle size of chitosan in the paints and coatings ranges from 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm or less than 16 μm.
[0019] In additional useful embodiments of the invention, chitosan is incorporated into the coating at 0.02% to 1.0%, 0.02% to 0.75%, 0.05% to 0.40%, or 0.02% to 0.30% by weight of dry coating solids.
[0020] In another embodiment, the paint or coating composition of the present invention may also include a pigment and an extender or filler. The paint or coating composition of this embodiment has one or more of the following features: a pigment volume concentration (PVC) of less than 60, about 25 wt% to about 65 wt% solids, at least 17 wt% binder polymer solids up to about 55 wt% binder polymer solids, and at least 10 wt% hiding pigment, such as titanium dioxide. In addition, the paint or coating composition may have one or more of the following qualities: improved dispersion of chitosan, wherein the chitosan particles have a particle size of 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm, or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm, or less than 16 μm and are uniformly distributed in the paint or coating, improved elongation in dry film form, improved thermal cycling properties, improved resistance to leaching of surfactants or other additives, and lower susceptibility to fungal fouling in dry film form.
[0021] In another embodiment, the coating includes a biocide additive. Such biocide additives can be selected by those skilled in the art to provide sufficient additional mildew or fungus resistance or other biocidal functions, including but not limited to in-can preservation or dry film preservation.
[0022] In another embodiment of the present invention, a preparation method is provided, by which a coating is prepared, the coating comprising water, a latex binder resin and additives, wherein such additives include but are not limited to chitosan compounds. The added chitosan has a relatively small particle size, less than 200 μm in some embodiments, and less than 100 μm in other embodiments. In certain other embodiments, small particle size chitosan is obtained from traditional sources of chitosan by applying high-speed shear (e.g., as applied to the pigment in the pigment grinding stage of paint preparation) to an aqueous acetic acid solution containing chitosan and adding a base (e.g., ammonium hydroxide) to neutralize the solution and precipitate chitosan from the solution. In certain embodiments of the preparation method, the coating also comprises a pigment, and chitosan is incorporated into the coating during the pigment grinding stage. In certain embodiments of the method, the coating is further applied to an article and dried. The wet coating has a pH above 7, while the dry coating has a pH below 7, 5 to 6 in certain embodiments. The deacetylated primary amines of chitosan are present in the film in their protonated state. DETAILED DESCRIPTION
[0023] In one embodiment, the present invention comprises a paint or coating composition comprising water, a latex binder resin and an additive, wherein such additives include but are not limited to chitosan compounds. In some embodiments, the chitosan compound additive has a particle size of less than 30 microns in the paint or coating, which is measured using ASTM D1210-05 "Standard Test Method for Fineness of Dispersion of Pigment-Vehicle Systems by Hegman-Type Gage". In another embodiment, the present invention comprises a coated article, which is formed by a paint or coating composition comprising water, a latex binder resin and an additive, wherein such additives include but are not limited to chitosan compounds, and wherein the paint or coating composition is dried to form a film on the coated article. The chitosan compound is distributed throughout the film on the coated article. In some embodiments, when dispersed in a paint or coating, the chitosan compound additive has a particle size of less than 30 microns, which is measured using ASTM D1210-05. Hegman gauge values below 30 microns also indicate that chitosan has adequate dispersibility. The dried paint or coating film exhibits improved elongation as measured according to ASTM D2370-16 "Standard Test Method for Tensile Properties", improved thermal cycling properties using a rating scale according to ASTM D714-02 "Standard Test Method for Evaluating Degree of Blistening of Paints" and ASTM D661-93 "Standard Test Method for Evaluating Degree of Cracking of Exterior Paints", and improved resistance to leaching of surfactants or other additives as measured according to the methods described herein.A modified version of the ASTM D5589-19 method "Standard Test Method for Determining the Resistance of Paint Films and Related Coatings to Algal Defacement" can be used to show reduced leaching of paint components in the exemplary compositions. The dried films may also be less susceptible to mold or fungal growth and fouling than the same paint or coating that does not include the chitosan compound. In some embodiments, coatings containing chitosan compounds may require reduced amounts of traditional fungicides such as zinc oxide.
[0024] In an embodiment of the invention, chitosan is incorporated into the paints and coatings, wherein the particle size of chitosan in the paints and coatings ranges from 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm or less than 16 μm.
[0025] In additional useful embodiments of the invention, chitosan is incorporated into the coating at 0.02% to 1.0%, 0.02% to 0.75%, 0.05% to 0.40%, or 0.02% to 0.30% by weight of dry coating solids.
[0026] In another embodiment, the paint or coating composition of the present invention may also include a pigment and an extender or filler. The paint or coating composition of this embodiment has one or more of the following features: a pigment volume concentration (PVC) of less than 60, about 25 wt% to about 65 wt% solids, at least 17 wt% binder polymer solids up to about 55 wt% binder polymer solids, and at least 10 wt% hiding pigment, such as titanium dioxide. In addition, the paint or coating composition may have one or more of the following qualities: improved dispersion of chitosan, wherein the chitosan particles have a particle size of 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm, or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm, or less than 16 μm and are uniformly distributed in the paint or coating, improved elongation in dry film form, improved thermal cycling properties, improved resistance to leaching of surfactants or other additives, and lower susceptibility to fungal fouling in dry film form.
[0027] In another embodiment, the coating includes a biocide additive. Such biocide additives can be selected by those skilled in the art to provide sufficient additional mildew or fungus resistance or other biocidal functions, including but not limited to in-can preservation or dry film preservation.
[0028] In another embodiment of the present invention, a preparation method is provided, by which a coating is prepared, the coating comprising water, a latex binder resin and additives, wherein such additives include but are not limited to chitosan compounds. The added chitosan has a relatively small particle size, less than 200 μm in some embodiments, and less than 100 μm in other embodiments. In certain other embodiments, small particle size chitosan is obtained from traditional sources of chitosan by applying high-speed shear (e.g., as applied to the pigment in the pigment grinding stage of paint preparation) to an aqueous acetic acid solution containing chitosan and adding a base (e.g., ammonium hydroxide) to neutralize the solution and precipitate chitosan from the solution. In certain embodiments of the preparation method, the coating also comprises a pigment, and chitosan is incorporated into the coating during the pigment grinding stage. In certain embodiments of the method, the coating is further applied to an article and dried. The wet coating has a pH above 7, while the dry coating has a pH below 7, 5 to 6 in certain embodiments. The deacetylated primary amines of chitosan are present in the film in their protonated state.
[0029] Chitosan Additives
[0030] As used herein, the term "chitosan" refers to a derivative of naturally occurring chitin having the following general chemical structure:
[0031]
[0032] Where n indicates the number of repeating structural units in a polymer or oligomer structure. Minor chemical variations in the structure are possible and will be recognized by those skilled in the art. Chitosan may also be obtained from other sources recognized by those skilled in the art.
[0033] Chitosan can be obtained from many sources by the deacetylation of naturally occurring chitin. The exemplary source of chitosan can be obtained with different molecular weights, and is usually provided by the following companies in acidic solution form: TidalVision Inc. (it is located in Bellingham, WA), Millipore Sigma (headquartered in Burlington, a subsidiary of MerkKGaA in VT), Qingdao Yunzhou Biochemistry Co. Ltd. (Qingdao, China), KitoZyme LLC (providing chitosan of pure plant origin, it is located in Herstal, Belgium) and Kimica Corporation (it is located in Chuo-ku). Chitosan can be obtained in dried flake form, acidic solution form or other forms. Chitosan of different molecular weights can be used for the present invention, and this molecular weight includes but is not limited to the molecular weight usually available.
[0034] When added to paint or coating formulations, chitosan from conventionally available sources and those used within the relevant art generally have particle sizes above 60 microns, as measured by Hegman gauge drawdown. These relatively large particle sizes result in a gritty-looking, poorly applied paint or coating that is unacceptable for commercial applications. In addition, larger particles have less available surface area per equivalent mass to interact with other components of the paint.
[0035] In embodiments of the invention, the chitosan compound added to the paint or coating of the invention has a particle size of 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm, or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm, or less than 16 μm, as measured by Hegman gauge drawdown. Without being bound by theory, it is believed that the smaller particle size of chitosan in the paints and coatings of the invention and the resulting larger surface area per equivalent mass allow for greater interaction with components such as surfactants, which potentially results in less leaching of the coating material. One particular theorized interaction may be hydrogen bonding between the chitosan and any polar monomers in the binder polymer of the paint or coating, which may allow for additional positive properties such as improved elongation and thermal cycling.
[0036] In embodiments of the present invention, it is believed that chitosan acts in a sense similar to filler or extender particles. Extenders or fillers can be used to reduce the amount of pigment required to achieve a desired hiding power, gloss, etc., but do not significantly affect the color of the paint or coating constructed from the pigment. Exemplary conventional fillers include, for example, sodium potassium aluminum silicate, such as 4 and 10 (sold by Unimin Corporation). When used, such fillers may be used in any desired amount.
[0037] Paint and coating compositions and methods for preparing the same
[0038] The paint or coating composition prepared according to the present invention may include chitosan in an amount of about 0.02% to 1.0% by weight, 0.02% to 0.75% by weight, 0.05% to 0.40% by weight, or 0.02% to 0.30% by weight of dry coating solids. According to the present disclosure, it will be understood by those skilled in the art that the amount of chitosan that can be added to a paint or coating formulation will vary based on the amount of other pigments or fillers / extenders in the paint or coating, which is represented by the base material name and / or gloss of the coating. In ultra-deep coatings, for example, additional chitosan that behaves like a filler when properly dispersed in a paint or coating formulation may be added, and its amount may be greater than the range provided above. As with other extenders or fillers, the maximum amount of chitosan that can be added to a paint or coating formulation is limited by the viscosity that increases when a threshold amount of chitosan is added.
[0039] Paint or coating composition according to the present invention generally comprises at least about 17% by weight, for example at least about 17.5% by weight to about 55% by weight of binder polymer solids. Binders that can be used in latex paint compositions are known in the art and include polymer binders, such as acrylic, vinyl acrylic or styrene acrylic binders. Other binders that are suitable for water-based paints and coating formulations can also be used, and other binders include but are not limited to polyurethane dispersions, water-based alkyd resins and their mixtures or modifiers. In one embodiment of the invention, paint or coating composition is formulated with a binder that does not cause component precipitation or forms grit. Paint and coating composition of the present invention may also include at least about 5% by weight of pigment. Such pigment may include inorganic pigments, such as titanium dioxide. Exemplary paint and coating compositions include at least about 11 weight %, also include, for example, at least about 12 weight %, also include, for example, at least about 13 weight %, also include, for example, at least about 14 weight %, also include, for example, at least about 15 weight %, also include, for example, at least about 16 weight %, also include, for example, at least about 17 weight %, also include, for example, at least about 18 weight %, also include, for example, at least about 19 weight %, and even also include, for example, at least about 20 weight % up to about 30 weight % of titanium dioxide. In another useful embodiment, the paint or coating composition includes greater than 10% titanium dioxide. Other colored pigments or dyes may also be added to the paint alone or in combination to produce a wide range of colored paints. Suitable additional pigments may include calcium carbonate, talcum, clay, silicate, aluminum silicate, calcium metasilicate, potassium aluminum silicate, magnesium silicate, barium sulfate, nepheline syenite, feldspar, zinc oxide or sulfide, or other pigments known to those skilled in the art. The content of such additional colored pigments may be up to about 30 weight %, for example, about 10 weight % to about 20 weight %. In some cases, "pigment" may also refer to a functional filler that is a non-water-soluble solid. Such functional fillers may include solids that provide additional functional properties to the paint, such as swelling ingredients, such as ammonium polyphosphate, melamine, pentaerythritol, and similar compounds. In a useful embodiment, the coating composition of the present invention is substantially free of or completely free of swelling ingredients, such as ammonium polyphosphate, melamine, and pentaerythritol and similar compounds. In another embodiment, the paint and coating contain no or substantially no pigment and are considered to be "clear coats" applied to various substrates.
[0040] The pigment volume concentration or PVC of a coating is the ratio of the volume of pigment (including functional fillers and fillers or extenders) present in the coating to the volume of total non-volatile materials (i.e., pigment and binder). The coating of the present invention preferably has a PVC of about 5 to about 60. In addition, the coating composition of the present invention also has a maximum solid content of less than 65% by weight, such as about 25% by weight to about 60% by weight, and also, for example, about 30% by weight to about 58% by weight. In certain embodiments, the PVC of the present invention can be zero.
[0041] The paints and coatings disclosed herein may also contain various other additives, including but not limited to thickeners, such as polyurethane thickeners and acrylic thickeners, in amounts up to about 10% by weight, for example, about 1% by weight to about 2% by weight. Synthetic organic materials may also be incorporated; these materials include plastic beads, hollow spheres, or other similar materials. Other optional components include glycols such as ethylene glycol and / or propylene glycol in amounts up to about 7%, and other solvents such as diethylene glycol dibenzoate and dipropylene glycol dibenzoate in amounts up to about 3%. The coating composition may also contain a pigment dispersant, which may be a solvent or a surfactant; a wet paint preservative; a dry film preservative; a foam control agent, such as oils, fatty acids, and siloxanes; a slip and wear additive; a tackifier, and / or other known paint additives.
[0042] The paint or coating compositions of the present invention may also contain a biocide, which includes, but is not limited to, metal ion-containing compounds, polymeric biocides, heterocyclic compounds, phenols, organometallic compounds, aldehydes, proteins, peroxides, alcohols, enzymes, polypeptides, cationic surfactants (including quaternary ammonium compounds), and halogen-releasing compounds.
[0043] Generally speaking, paints and coatings prepared according to the present invention are formulated to have a pH between 7 and 11 in the wet state (before being applied to a substrate and cured, "in the can"). In exemplary embodiments, the wet pH is 8-10, or in other embodiments, 9-10. Various pH adjusters can be used to adjust the wet pH. The pH of a paint or coating is very important to provide dispersibility and compatibility with all other components conventionally used in the preparation of paints and coatings. Conventional methods of incorporating chitosan into coatings involve providing the coating as an acidic solution that has a significantly lower pH in the wet state, which is friendly to the dissolution of chitosan in the wet coating. The present invention relates to dispersions of chitosan in traditional, higher pH wet coatings that allow formulation with other conventional materials; a formulation toolkit that is convenient and cost-effective for paint and coating formulators.
[0044] It should be noted that in order to prepare waterborne paints or coating formulations, a suitable dispersant / surfactant system is required in order to disperse the polymer and pigment in the paint or coating formulation. The method of selecting dispersants / surfactants for paint and coating formulations is well known to those of ordinary skill in the field of paint formulations. Those of ordinary skill in the art will be able to select dispersant / surfactant combinations in order to prepare desired paints or coating compositions having good stability characteristics.
[0045] Method for preparing coating composition
[0046] In some embodiments, the present invention encompasses methods for preparing coating compositions. Generally speaking, the methods for preparing coating compositions may include conventional preparation methods for forming a paint or coating and then adding a chitosan compound. Conventional preparation methods generally involve four or more stages, which include a pre-dilution stage, a grinding stage, a washing stage, and a dilution or dilution stage. In the pre-dilution stage, one or more binder resins may be blended with a carrier liquid in a dilution tank. Low shear mixing may be applied in a dilution tank to form a pre-dilution mixture. In the grinding stage, pigments and other additives that will not be homogenized under low shear mixing may be dispersed into the carrier liquid under high shear conditions. The grinding stage may be carried out in a high shear mixing device such as a mill. The high shear applied in the grinding stage breaks up agglomerates of particles and wet particles with liquid. The composition of the liquid added when diluting the grind may be the same or different from the composition of the carrier liquid used when preparing the grind. Next, in the washing stage, a washing liquid (which may have a composition that is the same or different from the composition of the carrier liquid) may be pumped into a high shear mixing device to move the grinding slurry into the dilution tank. Finally, in the dilution stage, the mill slurry, carrier liquid, wash liquid, and pre-diluted mixture including any other additional additives may be blended together under low shear conditions in a dilution tank. In this stage, the coating composition concentrate may be further diluted by the addition of further liquid, which may have the same composition as the carrier liquid or a different composition. The process may employ these conventional stages, or the coating composition may be prepared by other suitable methods. For example, the process may employ a continuous preparation using a slurry of components.
[0047] The one or more additives may be added at any suitable point during the preparation process, such as during the pre-dilution stage, the grinding stage, the washing stage, and the dilution or let-down stage.
[0048] The chitosan compound can be added to the paint or coating in the form of an acidic aqueous solution or other solution, and then neutralized by adding a base to precipitate the chitosan as a dispersion in the paint or coating. The chitosan must be added so that it is present and dispersed in the paint or coating with a particle size of 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm, or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm, or less than 16 μm. In a preferred embodiment, applying shear (such as the shear used in the pigment grinding stage of paint preparation) is sufficient to maintain a stable dispersion of the precipitated chitosan and allow the chitosan to have a particle size of 2 μm to 30 μm, 2 μm to 25 μm, 2 μm to 16 μm, or 4 μm to 16 μm, or less than 30 μm, less than 25 μm, less than 20 μm, or less than 16 μm in the paint. In certain embodiments, chitosan is added to the pigment grinding fluid during the pigment grinding stage. In a preferred embodiment, before being added to the grinding fluid, the chitosan compound is dissolved in acetic acid or other acid solutions. An acidic solution of chitosan (e.g., a high molecular weight chitosan acetate aqueous solution with 3 wt % chitosan and 6 wt % acetic acid purchased from Tidal Vision Inc.) can also be directly provided. Once the chitosan acidic solution is mixed into the grinding water by pouring or any suitable addition method, the chitosan is precipitated into the grinding water by adding alkali (e.g., ammonia), thereby forming a dispersion of chitosan and other grinding fluid components. In certain embodiments, the chitosan acidic solution can be added to the grinding water before adding any other grinding fluid components. In certain embodiments, the chitosan acidic solution is added together with other grinding components or added after other grinding components are added. In certain embodiments, alkali is slowly added under the shearing of the pigment grinding stage to allow sufficient mixing and avoid the rapid or local precipitation of chitosan. The dispersion remains throughout the paint or coating preparation process and the chitosan remains stably dispersed. Figure 6a and Figure 6b A portion of this embodiment is shown whereby the chitosan compound is incorporated into the paint or coating during a grinding stage beginning in an aqueous chitosan acetate solution. An exemplary aqueous chitosan-acid solution is a "high molecular weight" aqueous chitosan acetate solution (3 mass % chitosan, 6 mass % acetic acid) available from TidalVision Inc.
[0049] Once prepared, the coating composition can be dispensed into storage containers, such as paint cans. The coating composition can then be transported and stored, such as in a warehouse or on a storage rack.
[0050] Coated article having a dried paint film and method for providing a coated article
[0051] In certain embodiments, the article is coated with the above-mentioned paint and coating containing chitosan compound so that the coating forms a dry film on the article. The dried coating film shows characteristics superior to the same dry film without chitosan compound. One group of such improved characteristics is elongation. The film of the present invention can show an elongation improvement of 10% additional elongation to 50% additional elongation, 10% additional elongation to 40% additional elongation, 20% additional elongation to 50% additional elongation, or 15% additional elongation to 35% additional elongation, as compared with the same film without chitosan and measured according to ASTM D2370-16. Without being bound by theory, it is believed that hydrogen bonding can occur between any polar monomer in the binder polymer of the chitosan compound and the paint or coating to achieve improved elongation. The binder polymer with increasing polar monomers or increasing amounts of polar monomers can show increased elongation.
[0052] The dried films also showed improved resistance to leaching of the material. Resistance to leaching is indicated by testing using ASTM D5589-19, which is traditionally used to show resistance to algal fouling, but can be used in the present case to show reduced leaching by the absence of inhibition rings on exemplary samples. The dried films further appear to be less susceptible to fungal (including mold) fouling than the same films without the chitosan compound. Susceptibility to mold or fungal fouling can be determined using the methods described in the examples below or by any method acceptable to one of ordinary skill in the art.
[0053] The coating composition can be used for any suitable purpose. In some embodiments, the coating composition can be applied to interior or exterior building surfaces such as wood, dry wall, masonry, metal and plaster, or on a primer coating. In certain embodiments, the coating composition can be applied to metals, composite materials and other materials as a protective coating. In other embodiments, the coating composition can be applied to the surface to impart dry rubbing properties. For example, the surface can be a wall, which can have a paint or primer applied to the wall surface, on which a coating can be applied to form a dry rubbing surface. The coating composition can be applied with a brush, roller, sponge or spray gun or other conventional painting or coating tools. The cured coating can have any suitable thickness, such as a thickness range of 0.05mm-2mm, preferably about 0.1mm thick.
[0054] Implementation
[0055] Certain embodiments of the invention include:
[0056] Embodiment 1: A coating composition comprising: (a) a carrier liquid; (c) a binder polymer; and (d) a chitosan compound having a particle size of less than 30 μm in the coating composition.
[0057] Embodiment 2: The coating composition of Embodiment 1, wherein the carrier liquid comprises water.
[0058] Embodiment 3: The coating composition according to any one of Embodiments 1-2, wherein the coating composition further comprises a pigment.
[0059] Embodiment 4: The coating composition of any one of Embodiments 1-3, wherein the coating composition comprises 13 wt% to 30 wt% of the pigment, and the pigment is titanium dioxide.
[0060] Embodiment 5: The coating composition of any one of Embodiments 1-4, wherein the coating composition has a PVC of less than 60.
[0061] Embodiment 6: The coating composition of any of Embodiments 1-5, wherein the coating composition has from about 25 wt % to about 65 wt % solids.
[0062] Embodiment 7: The coating composition of any of Embodiments 1-6, wherein the coating composition has from about 30 wt % to about 60 wt % solids.
[0063] Embodiment 8: The coating composition of any one of Embodiments 1-7, wherein the coating composition comprises from about 0.02 wt % to about 1.0 wt % of the chitosan compound.
[0064] Embodiment 9: The coating composition of any one of Embodiments 1-8, wherein the chitosan compound has a particle size of less than 16 microns in the coating composition.
[0065] Embodiment 10: The coating composition of any of Embodiments 1-9, wherein the dried paint film has a Hegman scale rating of 5 or higher.
[0066] Embodiment 11: The coating composition of any of Embodiments 1-10, wherein the paint has a viscosity of less than 120 KU.
[0067] Embodiment 12: A coated article coated with the coating composition according to any one of Embodiments 1-11.
[0068] Embodiment 13: The coated article of Embodiment 12, wherein the coating composition forms a dried film on the article and the dried film exhibits improved elongation as measured by ASTM D2370-16 and compared to the same dried film without the chitosan compound.
[0069] Embodiment 14: The coated article of claim 12 or 13, wherein the coating composition forms a dried film on the article and the dried film exhibits improved thermal cycling properties as measured by ASTM D714-02 and ASTM D661-93 and compared to the same dried film without the deacetylated chitosan compound.
[0070] Embodiment 15: The coated article of any of Embodiments 12-14, wherein the coating composition forms a dried film on the article and the dried film exhibits resistance to leaching compared to the same dried film without the chitosan compound.
[0071] Embodiment 16: The coated article of any of Embodiments 12-15, wherein the coating composition forms a dried film on the article and the dried film exhibits reduced susceptibility to mold or fungal staining compared to the same dried film without the chitosan compound.
[0072] Embodiment 17: A method of preparing a coating composition, the method comprising providing a coating composition according to any one of Embodiments 1-11.
[0073] Embodiment 18: A method for preparing a coating composition, the method comprising: (a) providing a coating composition, the coating composition comprising a carrier liquid, a binder polymer and a pigment, wherein the coating composition is formed by a conventional preparation method including a grinding process and a dilution process; and (b) adding a deacetylated chitosan compound to the coating composition during a pigment grinding process, and applying shear to the deacetylated chitosan compound together with a grinding fluid during the grinding process.
[0074] Embodiment 19: A method according to Embodiment 18, wherein in step (b) the chitosan compound is provided in acetic acid and aqueous solution, and the grinding process further includes adding a base to neutralize the chitosan compound and precipitate the chitosan compound from the acetic acid and aqueous solution while applying shear during the grinding process.
[0075] Example
[0076] Comparative and Example Paint Compositions
[0077] Comparative (or "Control") and Example paint compositions were prepared according to the weight percent amounts shown in Table 1 below.
[0078] Table 1.
[0079]
[0080]
[0081] 1 021, obtained from Byk Chemie
[0082] 2Deacetylated chitosan powder, low molecular weight, purchased from Millipore Sigma
[0083] 3 Chitosan acetate aqueous solution (3 wt% chitosan, high molecular weight, 6 wt% acetic acid), purchased from Tidal Vision Inc.
[0084] 4. Ammonium hydroxide aqueous solution (19.7 wt%)
[0085] 5 Clay 40, purchased from BASF
[0086] 6 Zinc oxide (dry), purchased from Umicore Marketing
[0087] 7 663, purchased from Troy Corporation
[0088] 8-isothiazolinone and zinc pyrithione mixture
[0089] 9 ICEBERG TM Calcined kaolin clay, purchased from Burgess Pigments
[0090] 10 MINEX TM 4, purchased from Unimin Specialty Minerals
[0091] 11 021, purchased from Byk Chemie
[0092] As indicated in Table 1, different levels of biocides and extenders were added to different paints to show the effect of chitosan addition while maintaining PVC in various paint compositions. As will be appreciated by those skilled in the art, slight changes in the amount of dispersant and thickener were also made in the paints to maintain appropriate grinding fluid viscosity. The example and control paints were formed by mixing conventional paint components according to methods known in the art. Chitosan was incorporated into Example Paints 1, 2, and 3 by obtaining an aqueous chitosan acetate solution (3 wt % chitosan, 6 wt % acetic acid, high molecular weight solution, purchased from Tidal Vision Inc.) and incorporating it into the grinding water, and then adding the other grinding components by pouring. After incorporating the chitosan acetate solution, an aqueous ammonium hydroxide solution (19.7 wt %) was slowly added over 10 minutes for neutralization, and then the pH of the grinding fluid was brought to about 9 to precipitate the chitosan as a dispersion in the grinding water while applying high shear (typical shear applied when performing the grinding stage) by a Cowles blade. This step results in the use of about 77% by weight of the aqueous ammonium hydroxide solution shown in Table 1. The remaining grinding fluid components, including about 23% aqueous ammonium hydroxide solution shown in Table 1, were then added and each paint was formed by conventional mixing techniques using the materials in Table 1. Thus, the Example paints were formed.
[0093] A final control paint (Positive Control Paint 2) was also formed by dropping chitosan dry powder into the grinding water, using chitosan dry powder (low molecular weight chitosan powder, purchased from Millipore Sigma) added to the grinding water before adding the other grinding components. After adding the chitosan dry powder, an aqueous solution of ammonium hydroxide (19.7 wt %) was slowly added over 10 minutes for neutralization, and then the pH of the grinding fluid was brought to about 9 while high shear (typical shear applied when forming the grinding stage) was applied by a Cowles blade. This step resulted in the use of about 77 wt % of the aqueous solution of ammonium hydroxide shown in Table 1. The remaining grinding fluid components were then added, including about 23% aqueous solution of ammonium hydroxide shown in Table 1, and each paint was formed using the materials in Table 1 by conventional mixing techniques.
[0094] Particle size and paint quality determination
[0095] Hegman drawdowns of both Positive Control Paint 2 and Example Paint 1 were performed according to ASTM 1210-5 and the particle size was observed from the Hegman gauge drawdown. Figure 1a A drawdown of the positive control paint 2 is shown, and Figure 1bA Hegman drawdown of Example Paint 1 is shown. Positive Control Paint 2 shows that the chitosan particle size in Positive Control Paint 2 is in the range of 60 microns and larger. Example Paint 1 shows particle sizes of 12 microns to 16 microns and smaller. Of note, the average particle size of Attagel Clay 40 (available from BASF Catalyst LLC, the largest non-chitosan particle in either Positive Control Paint 2 or Example Paint 1) is 12 microns (as provided by the manufacturer). Figure 2a and Figure 2b The difference in appearance quality between the positive control paint 2 and the example paint 1 is further evident. Figure 2a Positive control paint 2 is shown at 80x magnification using a Keyence light microscope, and Figure 2b Example Paint 1 is shown at 80x magnification using a Keyence optical microscope. Drawdowns of both paints were made using a 4 mil bird bar on white Leneta paper (available from Leneta Co.).
[0096] Thermal Cycle Test
[0097] As shown in Table 2 below, positive control paint 1 and example paint 1 were subjected to thermal cycling testing. Cracking was evaluated and rated according to ASTM D661-93, and blistering was evaluated and rated according to ASTM D714-02. For each paint, a 1-inch wide paint brush (polyester / nylon blend or Chinese bristle) was used to apply the film to three types of substrates. Two coats were applied to each sample, each of which was dried at 40°F and 75% relative humidity for 24 hours before applying heat or cooling for testing. The samples were then frozen or heated according to the test method. The abbreviations in Table 2 correspond to the following substrates: GRA = bright red alkyd resin (alkyd paint applied to redwood in 6-inch × 18-inch sections); CLTX = chalk latex (latex paint applied to redwood; 6-inch × 18-inch sections); SYP = southern yellow pine (uncoated; 6-inch × 18-inch sections). Samples were prepared in triplicate and the measurements were averaged to obtain the following values.
[0098] Table 2.
[0099]
[0100] Elongation test
[0101] As shown in Table 3 below, positive control paint 1 and example paint 1 were tested for elongation. Percent elongation was evaluated according to ASTM D2370-16. Films were prepared by scraping wet paint on standard release paper using a 10 mil 8-path rod. The first coating was dried for 1 day at 23 ° C and 50% humidity. The second coating perpendicular to the first coating was scraped using the same 8-path rod, and it was dried for 7 days at 23 ° C and 50% humidity. The film was peeled off from the release paper and then cut into half an inch by 3 inch samples. Tension and elongation tests were performed on the sample film using an Instron tensiometer. Ten samples were produced from each paint, and five highest tensile strength samples were selected for each paint and the corresponding measurements were averaged to obtain the following values (± represents standard deviation).
[0102] Table 3.
[0103] paint Elongation % Tensile Strength (psi) Positive Control Paint 1 181.7±18.3 354.9±1.5 Example Paint 1 249.8±2.1 221.1±1.4
[0104] Leaching resistance test
[0105] In order to characterize the leaching of materials from the paint film formed by the comparative example paint and the exemplary paint, the positive control paint 1, the negative control paint and the example paint 1 were tested for algae fouling in general accordance with the method of ASTM D5589-19. The film was prepared by scraping each paint on #41 Whatman filter paper using a 4 mil bird-shaped rod. The film was allowed to dry for 24 hours and then cut into 1 inch by 1 inch squares. The sample was immersed in standard deionized water for 48 hours to remove any mobile ions or water-soluble components that may affect the test. The sample was then placed on a solidified B-11 agar plate. The sample was inoculated with 350 μL of an algae mixture, which included Chlorella vulgaris var viridis, Oscillatoria lutea, Scenedesmus quadricauda and UUlothrix gigas. The sample was then placed in a Percival incubator at a constant temperature (25°C) and growth was initiated with a fluorescent light source. Samples were observed 3 weeks after inoculation. Figure 5a Positive control paint 1 is shown at three weeks of inoculation. Figure 5b The negative control paint at three weeks of inoculation is shown, and Figure 5c Example Paint 1 is shown. Typically, ASTM D5589-19 is used to show resistance to algae fouling, but as will be appreciated by those skilled in the art, observation of samples subjected to this test also shows resistance to leaching. This may be absent. Figure 5c The "inhibition zone" around the painted filter paper substrate of Example Paint 1 shown in FIG. 1 and the presence of Positive Control Paint 1 ( Figure 5a ) and negative control paint ( Figure 5b ) were observed in both cases with inhibition zones.
[0106] Susceptibility to fungal / mold contamination
[0107] To illustrate the reduced susceptibility of exemplary dry paint films to fungal / mold stains, positive control paint 1 and experimental paint 1 were applied to aluminum panels (purchased from Q-Lab, Westlake, OH) and Hardie board substrates. Each paint was applied to the aluminum panel using a 10 mil 8-path rod to obtain a final coating thickness of approximately 5 mils wet. The paint was applied to the Hardie panel by a brush (2 coats) to obtain a similar final topcoat of 5 mils wet. Two sets of samples were prepared in triplicate and allowed to fully cure for 1 week under ambient conditions and then placed in a mold cabinet with environmental control. Throughout the experiment, the mold cabinet was maintained at 90 ° F (± 2 ° F) and 95-98% humidity. Vermiculite chips were inoculated with Aspergillus niger, Penicillium Sp., and Aureobasidium pullans fungal spores and placed on the mold cabinet floor. The painted aluminum panels and Hardie boards were randomly hung on racks in the mold cabinet where the panels or boards were not in contact with each other or directly in contact with the inoculated vermiculite. Measurements were made by rating each panel or board according to the scale provided in Table 4 below and then averaging the triplicate results for each paint after 19 weeks of exposure. Figure 3a A Hardie panel coated with positive control paint 1 is shown. Figure 3b A Hardie plate coated with a negative control paint is shown. Figure 3c A Hardie board coated with Example Paint 1 is shown. Figure 3d A Hardie board coated with Example Paint 2 is shown, and Figure 3e A Hardie panel coated with Example Paint 3 is shown. Figure 3a An aluminum panel coated with positive control paint 1 is shown, Figure 3b An aluminum panel coated with a negative control paint is shown. Figure 3c An aluminum panel coated with Example Paint 1 is shown. Figure 3d An aluminum panel coated with Example Paint 2 is shown, and Figure 3e Shown is an aluminum panel coated with Example Paint 3. When rated, all boards and panels are shown after 19 weeks in the mold chamber.
[0108] Table 4.
[0109] Rating Relative mold growth 0 0% plates covered with growth 3 30% of the plates are covered with growth 5 50% of the plate is covered with growth 7 70% of the board is covered with growth 10 100% of the board is covered with growth
[0110] The rating results are provided below in Table 5. The ratings reported are the average of triplicate samples of each coating run on each substrate.
[0111] Table 5.
[0112] paint Hardie board substrate Aluminum sheet substrate Positive Control Paint 1 1 1 Negative control paint 4 5 Example Paint 1 0 1 Example Paint 2 2 1 Example Paint 3 3 1
Claims
1. A coating composition, comprising: (a) a carrier liquid; (c) a binder polymer; and (d) chitosan, which is precipitated from an acidic solution of chitosan; wherein the coating composition has a pH greater than 7, in, The coating composition is formed by a method of preparing a coating composition, the method comprising: (a) adding chitosan in the form of acidic chitosan to a grinding fluid during a pigment grinding process; (b) adding a base to the grinding fluid during the pigment grinding process to precipitate the chitosan and apply shear to the grinding fluid; (c) blending the grinding fluid with a carrier fluid and a binder polymer to form the coating composition.
2. The coating composition of claim 1, wherein the base is ammonia.
3. The coating composition of claim 1, wherein the carrier liquid comprises water.
4. The coating composition according to claim 1, wherein the coating composition further comprises a pigment.
5. The coating composition of claim 1, wherein the coating composition comprises 13 to 30 weight percent of a pigment, and the pigment is titanium dioxide.
6. The coating composition of claim 1, wherein the coating composition has a PVC of less than 60.
7. The coating composition of claim 1, wherein the coating composition has 25 to 65 weight percent solids.
8. The coating composition of claim 7, wherein the coating composition has 30 to 60 wt% solids.
9. The coating composition of claim 1, wherein the coating composition comprises 0.02 wt% to 1.0 wt% chitosan.
10. The coating composition of claim 1 wherein the precipitated chitosan has a particle size in the coating composition of less than 16 microns.
11. The coating composition of claim 1, wherein a film formed from the dried coating composition has a Hegman scale rating of 5 or greater.
12. The coating composition of claim 1, wherein the coating has a viscosity of less than 120 KU.
13. A coated article coated with the coating composition according to claim 1.
14. A method for preparing a coating composition, the method comprising: (a) adding chitosan in the form of acidic chitosan to a grinding fluid during a pigment grinding process; (b) adding a base to the grinding fluid during the pigment grinding process to precipitate the chitosan and apply shear to the grinding fluid; (c) blending the grinding fluid with a carrier fluid and a binder polymer to form a coating composition.