Offshore drilling platform drilling pump valve steel and manufacturing method thereof

By optimizing specific chemical compositions and processes, the strength, toughness, and corrosion resistance issues of drilling pump and valve steel for offshore drilling platforms have been resolved, enabling the production of high-performance and green-manufacturing drilling pump and valve steel.

CN116219273BActive Publication Date: 2024-11-29JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211473636.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-29
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

Existing technologies struggle to produce drilling pump and valve steel for offshore drilling platforms that meets the requirements for high strength, toughness, and corrosion resistance, and the manufacturing methods suffer from material segregation and uneven microstructure.

Method used

By employing specific chemical composition design and process flow, including continuous casting, electroslag remelting, forging and quenching and tempering, combined with continuous furnace processing heated by natural gas, the uniformity and performance optimization of the steel are ensured. Water is used as the quenching medium, replacing traditional oil or soluble quenching liquid.

Benefits of technology

We produce drilling pump and valve steel with high strength, toughness, and excellent corrosion resistance. It has good microstructure uniformity, meets the requirements of offshore drilling platforms, and achieves green and low-carbon manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003955850890000061
    Figure BDA0003955850890000061
  • Figure BDA0003955850890000062
    Figure BDA0003955850890000062
  • Figure HDA0003955850900000011
    Figure HDA0003955850900000011
Patent Text Reader

Abstract

The invention relates to a drilling pump valve steel for an offshore drilling platform. The chemical composition thereof is calculated by mass percentage as follows: C: 0.28-0.36%, Si: 0.15-0.35%, Mn: 0.45-1.00%, P: ≤0.010%, S: ≤0.005%, Cr: 0.75-1.20%, Ni: 2.00-3.00%, Mo: 0.35-0.65%, Cu: ≤0.25%, V: 0.05-0.15%, Al: ≤0.035%, H: ≤0.00015%, O: ≤0.0015%, N: ≤0.0060%, As: ≤0.010%, Sn: ≤0.010%, Pb: ≤0.002%, Sb: ≤0.002%, Bi: ≤0.002%, and the balance is Fe and unavoidable impurity elements. The steel bars with the maximum size of 300mm are processed by KR pretreatment, BOF converter smelting, LF refining, RH vacuum degassing, CCM continuous casting (ESR electroslag remelting), rolling (forging), and tempering. The mechanical properties of the samples meet the following requirements: yield strength ≥153KSI, tensile strength ≥160KSI, elongation ≥13%, cross-sectional shrinkage ≥45%, 70℉ Charpy longitudinal impact energy ≥40ft-lbs, and surface and quarter-diameter hardness in the range of 352-390HBW.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical production of alloy structural steel bars, and in particular relates to a drilling pump valve steel for an offshore drilling platform and a manufacturing method thereof. Background Art

[0002] With the increasing depletion of land resources, countries around the world have all turned their attention to the exploitation of marine energy with rich oil and natural gas resources. Marine energy exploitation requires offshore drilling platform equipment, and the drilling pump is the heart of offshore drilling and exploitation activities. It is the source of continuous circulation of drilling fluid from the ground to the bottom of the well and then from the bottom of the well back to the ground. The drilling pump sucks the drilling fluid in the circulation tank and delivers it to the bottom of the well through the high-pressure manifold, hose, drill pipe, and drill nozzle on the ground at a pressure of 10 to 30 MPa and a delivery displacement of 20 to 60 liters per second. The drilling fluid flowing through the drill nozzle forms a high-pressure jet that breaks rocks, cleans the bottom of the well, and cools the drill bit. When drilling with a screw or turbine drill at the bottom of the well, the drilling fluid is the power source of the power drill. If the drilling pump does not work properly during the drilling process, the drilling fluid will not be able to maintain circulation, resulting in an underground drilling engineering accident, just like a person's heart stops beating. The working efficiency of the drilling pump directly affects the speed and progress of drilling. The drilling pump valve is the weakest part of the drilling pump accessories. Because it works in the drilling fluid containing fine sand for a long time, the working environment and conditions are very harsh, so the overall technical requirements for the material are very high.

[0003] Nowadays, whether a country can independently manufacture offshore drilling platforms reflects its marine equipment manufacturing strength. In the past decade, China's marine energy exploitation capabilities have been continuously improving. From raw materials to automatic control systems, it is not only able to manufacture independently, but many of its technologies are already leading the world.

[0004] The patent of the present invention discloses a drilling pump valve steel for an offshore drilling platform and a manufacturing method thereof. The drilling pump valve steel has the advantages of high pressure resistance, low temperature resistance, wear resistance, seawater corrosion resistance, low hydrogen, low non-metallic inclusions, and fine grains. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a drilling pump valve steel for an offshore drilling platform and a manufacturing method thereof in view of the above-mentioned prior art. The maximum diameter of the steel is 300 mm, and the macrostructure meets the following requirements according to the ASTM E381 standard: S, R, and C do not exceed level 1.5; the non-metallic inclusions meet the following requirements according to the ASTM E45 standard A method: A coarse, B coarse, and D coarse are all ≤0.5, A fine, B fine, and D fine are all ≤1.0, and C coarse and C fine are all level 0; the actual grain size meets the following requirements according to the ASTM E112 standard: ≥7.0; the ultrasonic flaw detection meets the ASTM The A388 standard stipulates that FBH=2.0mm; after quenching and tempering, the bars are sampled at the quarter diameter position for inspection and the mechanical properties meet the following requirements: yield strength ≥153KSI, tensile strength ≥160KSI, elongation ≥13%, cross-sectional shrinkage ≥45%, 70℉ Charpy longitudinal impact energy ≥40ft-lbs, surface and quarter diameter hardness in the range of 352-390HBW, which can be used to manufacture offshore oil drilling platform drilling pumps and valves, oil drilling tool connections, etc.

[0006] The technical solution adopted by the present invention to solve the above problems is: a drilling pump valve steel for an offshore drilling platform, wherein the chemical composition of the steel is, by mass percentage, C: 0.28-0.36%, Si: 0.15-0.35%, Mn: 0.45-1.00%, P: ≤0.010%, S: ≤0.005%, Cr: 0.75-1.20%, Ni: 2.00-3.00%, Mo: 0.35-0.65%, Cu: ≤0.25%, V: 0.05-0.15%, Al: ≤0.035%, H: ≤0.00015%, O: ≤0.0015%, N: ≤0.0060%, As: ≤0.010%, Sn: ≤0.010%, Pb: ≤0.002%, Sb: ≤0.002%, Bi: ≤0.002%, and the balance is Fe and unavoidable impurity elements.

[0007] The chemical composition of the drilling pump valve steel of the present invention is determined as follows:

[0008] C: Carbon increases the hardenability, strength and hardness of the material, but reduces the plasticity and impact toughness of the steel. A high carbon content is not good for welding performance and corrosion resistance. If the carbon content is too low, the strength and hardness of the steel are insufficient. In order to achieve a reasonable combination of comprehensive properties such as material strength and toughness, the C content of the present invention is 0.28-0.36%.

[0009] Si: Silicon has a good deoxidizing effect on molten steel and can improve the strength and hardness of ferrite and austenite. When the silicon content is too low, the deoxidation effect is poor. When the silicon content is high, the banded structure of the steel is serious and the toughness is reduced. The silicon content of the present invention is 0.15-0.35%.

[0010] Mn: Manganese and iron form a solid solution, which improves the strength and hardness of ferrite and austenite in steel. Manganese is second only to nickel in its ability to stabilize austenite structure, and strongly increases the hardenability of steel. However, manganese has a tendency to increase the grain coarsening of steel and is sensitive to temper brittleness. Too high manganese content increases the cracking sensitivity of steel. The manganese content of the present invention is controlled at 0.45-1.00%.

[0011] Cr: Chromium increases the hardenability of steel and has a secondary hardening effect. A certain amount of chromium is added to heat-treated steel to improve the strength and hardness of the steel after quenching and tempering. Higher chromium can form a passivation film on the steel surface to improve the corrosion resistance of the steel. In addition, chromium can combine with carbon to form a variety of carbides to increase the toughness of the material. The chromium content of the present invention is controlled at 0.75-1.20%.

[0012] Ni: Nickel is an element that improves the hardenability of steel and can significantly improve low-temperature toughness. It has a good effect on impact toughness and ductile-brittle transition temperature. Nickel can also improve the hardenability of steel, reduce the critical point and increase the stability of austenite. In addition, nickel can also improve the fatigue performance of steel. The nickel content of the present invention is controlled at 2.00-3.00%.

[0013] Mo: Molybdenum increases the hardenability of the material and can improve the tempering resistance of the steel. Molybdenum has a solid solution strengthening effect on ferrite and improves the stability of carbides, thereby increasing the strength of the steel. Molybdenum can also improve the ductility, toughness and wear resistance of the steel, and also has a beneficial effect on improving the corrosion resistance of the material. In addition, molybdenum improves the thermal strength of the steel. The present invention controls the molybdenum content to 0.35-0.65%.

[0014] Cu: Copper can improve the hardenability of steel and improve its atmospheric corrosion resistance, but too high a copper content can easily cause copper brittleness. The copper content of the present invention is controlled to be ≤0.25%.

[0015] V: Vanadium exists in the form of carbides in steel. Its main function is to refine the structure and grains of steel and improve the strength and toughness of steel. Vanadium can also increase the tempering stability of quenched steel, reduce overheating sensitivity, and increase tempering stability and wear resistance. The present invention controls the vanadium content to 0.05-0.15%.

[0016] Al: Aluminum is added to steel as a deoxidizer mainly for deoxidation. Its deoxidation ability is stronger than that of Si and Mn. In addition, it can refine the grains and fix the nitrogen in the steel, thereby improving the impact toughness of the steel. However, too high a content will damage the hot working properties of the steel and easily form large non-metallic inclusions that increase the brittleness of the steel. The aluminum content of the present invention is controlled at ≤0.035%.

[0017] S: Sulfur is a harmful element in steel, mainly existing in the form of MnS and FeS. It can cause hot brittleness of steel and reduce the mechanical properties of steel, especially the yield strength, plasticity and wear resistance. The presence of sulfur also has an adverse effect on the corrosion resistance and weldability of steel. The sulfur content of the present invention is controlled to be ≤0.005%.

[0018] P: Phosphorus is a harmful element in steel. It is easy to aggregate at the grain boundary to cause segregation, increase the temper brittleness of the steel, significantly reduce the plasticity and toughness of the grain boundary, make the steel easy to crack during cold working, and also have an adverse effect on weldability. The phosphorus content of the present invention is controlled to ≤0.010%.

[0019] H: Hydrogen is a harmful element in steel. Hydrogen dissolved in steel can cause defects such as hydrogen embrittlement and white spots. Hydrogen can sharply reduce the plasticity, toughness and fatigue strength of steel. In severe cases, it can cause hydrogen-induced cracking and brittle fracture. The hydrogen content of the present invention is controlled to be ≤0.00015%.

[0020] O: Oxygen is a harmful element in steel. Oxygen exists in steel in the form of FeO, MnO, SiO2, Al2O3 and other inclusions, which reduces the strength and plasticity of steel, especially has a serious impact on the fatigue strength and impact toughness of steel. The oxygen content of the present invention is controlled to ≤0.0015%.

[0021] Residual impurities and nitrogen elements: In order to improve the corrosion resistance and fatigue life of the final product, the gas and residual impurity elements in the steel must be strictly controlled. The nitrogen gas and residual element contents of the present invention are controlled as follows: N≤0.0060%, As≤0.010%, Sn≤0.010%, Pb≤0.002%, Sb≤0.002%, Bi≤0.002%.

[0022] The process flow adopted by the present invention for producing the above-mentioned offshore drilling platform drilling pump valve steel is: a process of continuous casting-(electroslag)-rolling (forging)-quenching and tempering to produce drilling pump valve steel, which specifically includes the following steps:

[0023] 1) Smelting and continuous casting: The smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter primary smelting, LF furnace refining, and RH vacuum degassing to produce molten steel. After RH degassing, the molten steel is treated with soft argon blowing. The molten steel is cast into Ф600mm continuous casting round billets with low superheat and full argon protection. After high temperature offline, the billet is slowly cooled in the pit. The pit temperature shall not be lower than 650℃, and the slow cooling time shall be greater than 60 hours. After the pit is removed, the billet is placed in the annealing furnace for stress relief annealing. The annealing temperature is 710±30℃, the annealing heating heating rate is ≤50℃ / h, the holding time is ≥15h, the cooling rate after holding is ≤30℃ / h, and it is cooled to ≤350℃ before being discharged from the furnace.

[0024] 2) Electroslag remelting: Ф800mm electroslag ingot is electroslag remelted with Ф600mm continuous casting electrode billet. The electroslag smelting is protected by argon throughout the process. The CaF2:Al2O3:CaO:SiO2 quaternary slag system is used. In order to fully remove the moisture in the slag, the pre-melted slag is baked for more than 15 hours. Mn powder and Al powder are added with the slag for deoxidation. Only Al powder is added for deoxidation during the remelting process. The electroslag remelting melting speed is controlled at 700-1250Kg / h. If the melting speed is too fast, the slag temperature is high and it is easy to absorb air, resulting in a high gas content in the molten steel. If the melting speed is too slow, it is easy to cause a thick slag skin on the contact surface between the ingot and the crystallizer, affecting the surface quality of the ingot. After demoulding, the steel ingot is placed in a furnace for annealing at 450±50℃. The temperature of the steel ingot is raised to 710±30℃ at a heating rate of ≤50℃ / h in the annealing furnace and kept warm for no less than 25 hours. The steel ingot is cooled to ≤300℃ at a furnace cooling rate of ≤30℃ / h before being taken out of the furnace.

[0025] 3) Forging: Ф800mm electroslag ingots are heated in a chamber furnace with a heating rate of ≤100℃ / h and a forging heating temperature of 1210-1280℃. The electroslag ingots need to be evenly burned through, the initial forging temperature is higher than 1180℃, and the final forging temperature is not lower than 880℃. After the continuous casting billet is taken out of the furnace, a 2000T fast forging machine is used to free forge bars of ≥Ф240mm. The scale is removed in time during the forging process. The initial billet is forged and drawn with a small reduction of 8-10% deformation rate, and the intermediate billet is drawn with a large reduction of 30-45% deformation rate to make the forging pressure penetrate into the core to improve the quality of the core of the bar, and then continue to draw the square and invert the outer circle to the finished product size; after the forging material is off the line, it is slowly cooled by high-temperature sand burying at ≥750℃, and air-cooled after the temperature drops below 200℃.

[0026] 4) Rolling: Ф600mm continuous casting billet is heated in a continuous furnace, the preheating temperature is 650-850℃, the rolling soaking temperature is 1210-1260℃, the total heating time is more than 7 hours, and the soaking time is more than 2 hours to ensure that the continuous casting billet is evenly burned through. The initial rolling temperature is higher than 1150℃. High-pressure water is used to descale and remove oxide skin before rolling. After the continuous casting billet is taken out of the furnace, a continuous rolling mill is used for multiple passes to roll bars of specification ≤Ф240mm, and the final rolling temperature is controlled to be not less than 880℃; after the rolled material comes off the line, it is cooled in a slow cooling pit at a high temperature of ≥650℃, and air-cooled after it is taken out of the pit after the temperature drops below 200℃.

[0027] 5) Bar quenching and tempering treatment: The steel is quenched and tempered in a continuous furnace, the austenitizing temperature is 860-920℃, the quenching medium is water, and the holding time is controlled to be more than 1.5h / mm of the bar diameter; the tempering temperature is 530-590℃, the holding time is controlled to be more than 2.0h / mm of the bar diameter, and air cooling is used.

[0028] 6) Inspection: Cut off the head and tail of each rod, and grade the macrostructure of each rod according to ASTM E381 standard: S, R, C not exceeding 1.5; grade the non-metallic inclusions according to ASTM E45 standard A method: A coarse, B coarse, D coarse are all ≤0.5, A fine, B fine, D fine are all ≤1.0, C coarse and C fine are all 0; the grain size is graded according to ASTM E112 standard and meets ≥7.0; ultrasonic flaw detection meets the FBH=2.0mm requirement of ASTM A388 standard; after quenching and tempering, the 1 / 4D position of the rod is sampled and tested for mechanical properties, which meet the following requirements: yield strength ≥153KSI, tensile strength ≥160KSI, elongation ≥13%, cross-sectional shrinkage ≥45%, 70℉ Charpy longitudinal impact energy ≥40ft-lbs, and the hardness of the surface and 1 / 4D position is in the range of 352-390HBW, which meets the requirements for the use of drilling pumps and valves and oil drilling tool connectors.

[0029] Compared with the prior art, the advantages of the present invention are:

[0030] 1) The present invention adopts a new composition design, starting from the influence on the heat treatment performance of steel, taking into account the steel's resistance to seawater corrosion, fatigue and other properties, while ensuring the hardenability of the steel, optimizing the ratio between the elements, so that the drilling pump valve steel not only has higher strength, hardness and toughness, but also has excellent corrosion resistance and fatigue performance.

[0031] 2) The rod of the present invention, in addition to conventional converter, refining, RH degassing, and continuous casting, adds an electroslag remelting process for large-sized rods, and adopts a forging processing technology, so that the final forged and rolled rods of all specifications have low segregation, uniform and dense steel structure, thereby obtaining higher comprehensive performance.

[0032] 3) The drilling pump valve steel manufactured by the present invention adopts natural gas heated continuous furnace tempering treatment, instead of the traditional electric heating box furnace or pit furnace quenching and tempering, and the combination of steel components can obtain a more stable and uniform tempering structure, and the product is safer to use; the quenching medium adopts water, instead of the traditional oil or soluble quenching liquid, to achieve green and low-carbon manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the tempering structure diagram of the Φ300mm round steel produced in Example 1 of the present invention.

[0034] Figure 2 This is the tempering diagram of Φ220mm round steel produced in Example 2 of the present invention. DETAILED DESCRIPTION

[0035] The present invention will be further described below with reference to examples.

[0036] Example 1

[0037] The drilling pump valve steel involved in this embodiment has a diameter of 300 mm, and its chemical element composition is calculated by mass percentage: C: 0.33%, Si: 0.22%, Mn: 0.70%, P: 0.007%, S: 0.002%, Cr: 1.05%, Ni: 2.51%, Mo: 0.56%, Cu: 0.02%, V: 0.013%, Al: 0.021%, H: 0.00008%, O: 0.0013%, N: 0.0043%, As: 0.0044%, Sn: 0.0017%, Pb: 0.001%, Sb: 0.001%, Bi: 0.001%, and the remainder is iron and unavoidable impurity elements.

[0038] The manufacturing process of the drilling pump valve steel is as follows: the smelting raw materials are configured according to the chemical composition of the above-mentioned steel products, and KR molten iron pretreatment, converter smelting, LF refining, RH vacuum degassing are carried out in sequence to obtain high-purity molten steel, the ingot is cooled in a slow cooling pit at high temperature, and stress relief annealing is performed after leaving the pit; then a 600mm Ф electrode round billet is continuously cast by a continuous casting machine; an 800mm Ф electroslag ingot is remelted by electroslag; the electroslag steel ingot is hot-transferred for annealing; then the electroslag ingot is heated and taken out of the furnace by a chamber furnace; 300mm round steel is freely forged by a 2000T fast forging machine, and the steel rod is forged and buried in sand for cooling, and then put into a continuous furnace heated by natural gas for quenching + high-temperature tempering and quenching treatment.

[0039] The steel bars produced by the above manufacturing process have high strength and toughness. The quenched and tempered mechanical properties are shown in Table 1 and the microstructure is shown in Table 2. Figure 1 .

[0040] Table 1 Quenched and tempered mechanical properties of steel in Example 1

[0041]

[0042] Example 2

[0043] The drilling pump valve steel involved in this embodiment has a diameter of 220 mm, and its chemical element composition is calculated by mass percentage: C: 0.31%, Si: 0.26%, Mn: 0.61%, P: 0.008%, S: 0.002%, Cr: 0.96%, Ni: 2.33%, Mo: 0.52%, Cu: 0.02%, V: 0.010%, Al: 0.025%, H: 0.00007%, O: 0.0012%, N: 0.0037%, As: 0.0048%, Sn: 0.0026%, Pb: 0.001%, Sb: 0.001%, Bi: 0.001%, and the remainder is iron and unavoidable impurity elements.

[0044] The manufacturing process of the drilling pump valve steel is to configure the smelting raw materials according to the chemical composition of the above-mentioned steel products and sequentially perform KR molten iron pretreatment, converter smelting, LF furnace refining, and RH vacuum degassing to obtain high-purity molten steel, and then continuously cast 600mm round billets by a continuous casting machine. The billets are cooled in a slow cooling pit at high temperature, and stress relief annealing is performed after exiting the pit; then the billets are heated in a continuous furnace and taken out of the furnace; after high-pressure water descaling, 220mm round steel is continuously rolled, and the steel bars are pit cooled after rolling off the line; and then quenching + high-temperature tempering and quenching and tempering treatment is performed in a continuous furnace heated by natural gas.

[0045] The drilling pump valve steel produced by the above manufacturing process has high strength and toughness. Its quenched and tempered mechanical properties are shown in Table 2, and its microstructure is shown in Table 2. Figure 2 .

[0046] Table 2 Quenched and tempered mechanical properties of steel in Example 2

[0047]

[0048] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing drilling pump valve steel for an offshore drilling platform, characterized in that: The chemical composition of the steel is C: 0.28-0.36%, Si: 0.15-0.35%, Mn: 0.45-1.00%, P: ≤0.010%, S: ≤0.005%, Cr: 0.75~1.20%, Ni: 2.00~3.00%, Mo: 0.35~0.65%, Cu: ≤0.25%, V: 0.05~0.15%, Al: ≤0.035%, H: ≤0.00015%, O: ≤0.0015%, N: ≤0.0060%, As: ≤0.010%, Sn: ≤0.010%, Pb: ≤0.002%, Sb: ≤0.002%, Bi: ≤0.002%, the balance is Fe and unavoidable impurity elements; the maximum diameter of the pump valve steel is Ф300mm; the macrostructure of the pump valve steel meets the following requirements according to ASTM E381 standard rating: S, R, C do not exceed level 1.5; non-metallic inclusions meet the following requirements according to ASTM The E45 standard A method rating meets the following requirements: A coarse, B coarse, and D coarse are all ≤0.5, A fine, B fine, and D fine are all ≤1.0, and C coarse and C fine are all 0; the actual grain size meets the ASTM E112 standard rating of ≥7.0; the ultrasonic flaw detection meets the ASTMA388 standard FBH=2.0mm requirement; the method comprises the following steps: 1) Smelting: The smelting raw materials are sequentially subjected to KR molten iron pretreatment, converter primary smelting, LF furnace refining, and RH vacuum degassing to produce molten steel, and then soft argon blowing treatment is performed after RH degassing; 2) Continuous casting: The molten steel is cast into continuous casting round billets with argon protection throughout the whole process at low superheat. The continuous casting round billets are put into the pit for slow cooling after being taken off the line at high temperature. After the pit is taken out, the billets are put into the annealing furnace for stress relief annealing. After annealing, they are cooled and taken out of the furnace at a temperature of 100°C. 3) Electroslag remelting: The continuous casting round billet is used as the electrode billet for electroslag remelting. The electroslag smelting is protected by argon gas throughout the whole process. Mn powder and Al powder are added with the slag for deoxidation. Only Al powder is added for deoxidation during the remelting process. The electroslag remelting melting speed is controlled at 700-1250Kg / h. After the ingot is demoulded, it is annealed in a warm furnace at 450±50℃. The ingot is heated to 710±30℃ in the annealing furnace at a heating rate of ≤50℃ / h and the insulation time shall not be less than 25 hours. It is cooled to ≤300℃ at a furnace cooling rate of ≤30℃ / h before being taken out of the furnace. 4) Forging: The electroslag ingot is heated in a chamber furnace, with a heating rate of ≤100℃ / h, a forging heating temperature of 1210-1280℃, a starting forging temperature higher than 1180℃, and a final forging temperature not lower than 880℃. After the continuous casting billet is taken out of the furnace, it is free forged by a fast forging machine to obtain a bar with a diameter of >Ф240mm. After the forged material is off the line, it is slowly cooled by sand burying at a high temperature of ≥750℃, and air-cooled after the temperature drops below 200℃; 5) Bar tempering treatment: The steel is tempered in a continuous furnace, the austenitizing temperature is 860-920℃, the quenching medium is water, and the holding time is controlled to be more than 1.5h / mm of the bar diameter; the tempering temperature is 530-590℃, the holding time is controlled to be more than 2.0h / mm of the bar diameter, and air cooling is used.

2. The method for manufacturing drilling pump valve steel for an offshore drilling platform according to claim 1, characterized in that: The mechanical properties of the quenched and tempered bars of the pump and valve steel are sampled and tested at the quarter diameter position, and the following are met: yield strength ≥153KSI, tensile strength ≥160KSI, elongation ≥13%, cross-sectional shrinkage ≥45%, 70℉ Charpy longitudinal impact energy ≥40ft-lbs, and surface and quarter diameter hardness are in the range of 352-390HBW.

3. The method for manufacturing drilling pump valve steel for an offshore drilling platform according to claim 1, characterized in that: In the step 2), the temperature of the furnace entering the furnace shall not be lower than 650°C, the slow cooling time shall be greater than 60 hours, the annealing temperature shall be 710±30°C, the annealing heating rate shall be ≤50°C / h, the holding time shall be ≥15h, the cooling rate after holding shall be ≤30°C / h, and the furnace shall be discharged after cooling to ≤350°C.

4. The method for manufacturing drilling pump valve steel for an offshore drilling platform according to claim 1, characterized in that: In the step 3), a quaternary slag system of CaF2:Al2O3:CaO:SiO2 is used, and the pre-melted slag baking time is more than 15 hours.

5. The method for manufacturing drilling pump valve steel for an offshore drilling platform according to claim 1, characterized in that: In the forging process of step 4), the oxide scale is removed in time, the initial blank is forged and drawn with a small reduction of 8-10% deformation rate, and the intermediate blank is drawn with a large reduction of 30-45% deformation rate so that the forging pressure penetrates into the core, and then the drawing is continued and the outer circle is inverted to the finished product size.

Citation Information

Patent Citations

  • Technology for producing LS-CrNiMo30C steel forging for subsea oil production wellhead device through continuous casting billet

    CN106591680A

  • Steel for main load-bearing piece of drilling exploitation hoisting equipment and preparation method of steel

    CN108048737A