Corrugated plate type flue gas denitration catalyst and preparation method thereof
Through the improved preparation method, the active components are uniformly precipitated and dispersed, and the problems of uneven dispersion and high-altitude rapid forming of the active components of corrugated plate flue gas denitrification catalyst are solved, the denitrification efficiency and wear resistance are improved, and the production cost is reduced.
Patent Information
- Application Number
- CN202111681468.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The active components of the existing corrugated plate flue gas denitrogenation catalyst are unevenly dispersed, resulting in low denitrification efficiency, low molding rate and insufficient mechanical strength under high airspeed conditions, which increases production costs.
By mixing the titanium source precursor solution with the aluminum source precursor solution, adjusting the pH precursor value, and then mixing with the alkali and tungsten source precursor solution to dry and calcining to form an intermediate powder, and then with the vanadium source precursor solution and nano SiO2 The sol and polymer dispersant are mixed into a slurry, sprayed on the surface of the corrugated plate and dried and calcined to form a corrugated plate-type denitrification catalyst with uniform active components and high external specific surface area.
The denitrification activity and wear resistance of the catalyst are improved, the outer specific surface area is increased, the forming rate and mechanical strength are improved, and the production cost and transportation damage rate are reduced.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a corrugated plate type flue gas denitration catalyst and a preparation method thereof. Background Art
[0002] Nitrogen oxides (NO x ) is one of the main air pollutants, and emission requirements are becoming increasingly stringent. According to the applicable requirements of relevant standards, gas boilers in the petrochemical industry implement the "Emission Standards for Air Pollutants from Thermal Power Plants" (GB 13223-2011), and the NOx emission concentration of gas boilers is less than 100mg / m 3 , and some areas have implemented NOx<50mg / m 3 Ultra-low concentration emission standards. Natural gas is the main fuel for gas boilers. Its combustion has the advantages of low nitrogen, low sulfur and low dust emissions. However, due to the large amount of combustion air injected, nitrogen in the air will produce a large amount of NOx under high temperature conditions. Gas boilers are important energy equipment for industrial production and are indispensable in the oil refining process. With the continuous improvement of the scale and process level of refining equipment, gas boilers are required to meet the standards. Therefore, under the dual pressure of technical requirements and environmental protection standards, more stable and reliable flue gas denitrification technology must be equipped to ensure the stable and standard operation of gas boilers.
[0003] Among the many flue gas denitrification technologies, the selective catalytic reduction (SCR) method is still the international mainstream technology, and its NOx removal rate can reach 80% to 90%. Among them, the denitrification catalyst is the core of the SCR technology. Many scientific research institutions and enterprises in my country have also conducted a series of studies on the flue gas and refining flue gas conditions of fuel boilers in my country, and developed some denitrification catalysts, most of which are honeycomb SCR catalysts; due to the special requirements of flue gas denitrification conditions, most gas boilers need to use corrugated plate SCR catalysts, but most of the corrugated plate denitrification catalysts are foreign technology products.
[0004] CN106732709 B proposes a preparation process of a corrugated plate denitration catalyst, firstly, under a constant temperature of 60-80°C, vanadium pentoxide, molybdenum trioxide and tungsten trioxide are added to a mixed solution of citric acid and hydrochloric acid, stirred until dissolved, and then carbon nitride, acidic silica sol and titanium dioxide are added, and stirred to obtain an active sol; then the active sol is evenly sprayed on the upper and lower surfaces of the inorganic fiberboard, and dried at 40-80°C for 5-30 minutes to obtain a plate catalyst; then the plate catalyst is rolled into a corrugated shape, and dried and calcined in a nitrogen atmosphere to obtain a corrugated plate denitration catalyst. This method has a simple process and low cost, but the raw materials used, such as vanadium pentoxide, molybdenum trioxide, tungsten trioxide, carbon nitride, titanium dioxide, etc., are not mixed at the atomic level, and the active substances are unevenly dispersed, which affects the performance of the catalyst.
[0005] CN103143396B proposes a method for preparing a corrugated plate denitration catalyst, wherein titanium dioxide, silicon dioxide, and an active substance are mixed into a slurry, and then a binder, glass fiber, etc. are added, and finally extrusion molding is performed. The method is simple in process, but the active substance is not well dispersed, resulting in a low denitration efficiency of the catalyst.
[0006] CN 107138150 B discloses a honeycomb denitration catalyst, which is prepared from the following components in parts by weight: 70-90 parts of titanium dioxide, 2-16 parts of tungsten trioxide, 1.0-3 parts of vanadium pentoxide, and 0.5-3 parts of pore-forming agent. The denitration catalyst of the invention has the advantages of high catalytic efficiency, small amount of catalyst and low cost. CN 107096524 B discloses a honeycomb low-temperature denitration catalyst and a preparation method thereof, which uses a honeycomb denitration catalyst including titanium dioxide, tungsten trioxide, ammonium metavanadate and the like as components and a preparation method thereof, resists heavy metal and sulfide poisoning, and prolongs service life, but these catalysts are currently generally suitable for preparing honeycomb catalysts with no more than 50 holes to meet denitration sites with lower air velocity requirements. In order to meet the actual needs of denitrification with higher space velocity requirements, the catalyst needs to be processed into a honeycomb catalyst with more pores to increase its external specific surface area. Honeycomb catalysts with more pores are prone to cracks or stick to the mold during extrusion, and have low molding rate and mechanical strength, resulting in a waste of production resources and increased costs.
[0007] Therefore, those skilled in the art still need to conduct further research on the corrugated plate flue gas denitrification catalyst with high space velocity requirements. Summary of the invention
[0008] The main purpose of the present invention is to provide a corrugated plate flue gas denitration catalyst and a preparation method thereof, so as to overcome the defects of the prior art such as uneven dispersion of active components of the denitration catalyst and low denitration efficiency of the catalyst.
[0009] In order to achieve the above object, the present invention provides a method for preparing a corrugated plate type flue gas denitration catalyst, comprising the following steps:
[0010] Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7 to 12, and precipitating;
[0011] Step 2, mixing the precipitate obtained in step 1 with an alkali solution, stirring, and obtaining a secondary precipitate;
[0012] Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder;
[0013] Step 4, mixing the intermediate powder with the vanadium source precursor solution, nano-SiO2 sol, polymer dispersant, and pore-forming agent into a slurry, spraying it on the surface of the corrugated plate, drying, and calcining to form a corrugated plate type denitrification catalyst.
[0014] In one embodiment of the method for preparing the corrugated plate flue gas denitration catalyst of the present invention, the alkali solution in step 2 is an alkali metal hydroxide solution or an alkaline earth metal hydroxide solution, and the concentration of the alkali solution is 0.5 to 5 mol / L; the mass of the alkali solution is 1 to 5 times the mass of the precipitate obtained in step 1.
[0015] In the preparation method of the corrugated plate flue gas denitration catalyst described in the present invention, in one embodiment, the tungsten source precursor solution is at least one of ammonium paratungstate solution and ammonium metatungstate solution; the tungsten source precursor solution is calculated as tungsten trioxide, and the titanium source precursor solution is calculated as TiO2, and the mass ratio of the tungsten source precursor solution to the titanium source precursor solution is 0.5-6.0:100.
[0016] In the preparation method of the corrugated plate flue gas denitration catalyst described in the present invention, in one embodiment, the vanadium source precursor solution is at least one of ammonium metavanadate solution and ammonium vanadate solution, the vanadium source precursor solution is calculated as V2O5, and the titanium source precursor solution is calculated as TiO2, and the mass ratio of the vanadium source precursor solution to the titanium source precursor solution is 0.2 to 5.0:100.
[0017] In the preparation method of the corrugated plate flue gas denitration catalyst described in the present invention, in one embodiment, the pH adjustment reagent in step 1 is ammonia water, and the pH value is adjusted to 7-12; the mixing method in step 4 is stirring or ultrasonic oscillation, and the mixing time is 0.1-8h; the water mass content of the slurry in step 4 is 40-90%.
[0018] In one embodiment of the method for preparing the corrugated plate flue gas denitrification catalyst of the present invention, the polymer dispersant is at least one of polyethylene glycol, polyacrylamide, and polyvinyl pyrrolidone; the titanium source precursor solution is calculated as TiO2, and the mass ratio of the polymer dispersant to the titanium source precursor solution is 0.1 to 2.0:100.
[0019] Wherein, the calcination temperature in step 3 and step 4 is both 450-680° C., and the calcination time is both 2-40 hours.
[0020] In step 4, the drying and calcining process is carried out according to the following procedures: the slurry sprayed on the surface of the corrugated plate is heated from room temperature to 50-105°C, the heating rate is controlled to be no more than 1°C / min, the humidity is controlled to be 50-98%, and after reaching the predetermined temperature, the temperature is kept constant for 3-20 days to form a catalyst dry embryo; the catalyst dry embryo is calcined according to the following process: the temperature is increased from 50-105°C to 450-680°C, the heating rate is controlled to be no more than 1°C / min, after the temperature reaches the predetermined temperature, the temperature is kept constant for 2-40 hours, and then the temperature is cooled, the cooling rate is no more than 4°C / min, and the temperature is cooled to below 50°C to obtain a corrugated plate denitrification catalyst; wherein the humidity of the drying process is preferably 75-95%.
[0021] In step 4, the pore-forming agent is at least one of polyethylene oxide and sesbania powder, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the pore-forming agent to the titanium source precursor solution is 0.1 to 2.0:100.
[0022] In one embodiment of the preparation method of the corrugated plate flue gas denitrification catalyst described in the present invention, the nano-SiO2 sol is in liquid state, the mass content of the effective ingredient SiO2 is 5.0-50%, the nano-SiO2 particle size is 5-80nm, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the nano-SiO2 sol to the titanium source precursor solution is 0.3-5.0:100.
[0023] In one embodiment of the method for preparing the corrugated plate flue gas denitrification catalyst of the present invention, the pore-forming agent is at least one of polyethylene oxide and sesbania powder, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the pore-forming agent to the titanium source precursor solution is 0.1 to 2.0:100.
[0024] In order to achieve the above object, the present invention also provides a corrugated plate type flue gas denitration catalyst obtained by the above preparation method.
[0025] Beneficial effects of the present invention:
[0026] The present invention utilizes a strong alkali to dissolve aluminum atoms in a titanium-aluminum lattice, thereby greatly increasing the lattice defects of the titanium substrate. The lattice defects of aluminum dissolved by the strong alkali are at the surface position that is easy to contact with flue gas in a flue gas atmosphere. After being supplemented by the catalytic promoter component, the SCR catalytic activity can be more effectively exerted, thereby improving the denitration effect under the same conditions. Tungsten element is added to the titanium substrate after the aluminum element is dissolved. Since there are more lattice defects, the tungsten element is supplemented, and the lattice defects of the hybrid substrate are more stable after calcination. At the same time, the crystal form of the titanium substrate can remain in the anatase type without crystallization during high-temperature calcination, which is more conducive to the catalyst maintaining a high denitration activity.
[0027] The invention adds nano-SiO2 sol before the finished catalyst product is roasted, and after dispersion or penetration, the anti-wear performance of the corrugated plate catalyst can be improved after roasting.
[0028] DeNOx catalysts with large external specific surface areas have certain technical difficulties in preparation. The catalysts are prone to cracks or stick to the mold during extrusion, and have low molding rates and mechanical strength, resulting in high production costs and high transportation damage rates. Corrugated plate catalysts have larger external specific surface areas, high molding rates, low production costs, and are easy to transport and have low damage rates. They reduce catalyst loading space and reduce device investment costs. Corrugated plate deNOx catalysts have overcome this problem better. DETAILED DESCRIPTION
[0029] The following is a detailed description of the embodiments of the present invention. The embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and processes are given. However, the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments where specific conditions are not specified are usually based on conventional conditions.
[0030] The present invention provides a method for preparing a corrugated plate type flue gas denitration catalyst, comprising the following steps:
[0031] Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7-12, and precipitating;
[0032] Step 2, mixing the precipitate obtained in step 1 with an alkali solution, stirring, and obtaining a secondary precipitate;
[0033] Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder;
[0034] Step 4, mixing the intermediate powder with the vanadium source precursor solution, nano-SiO2 sol, polymer dispersant, and pore-forming agent into a slurry, spraying it on the surface of the corrugated plate, drying, and calcining to form a corrugated plate type denitrification catalyst.
[0035] In one embodiment, the titanium source precursor is a soluble titanium-containing compound, such as a titanium-containing compound soluble in water. In another embodiment, the titanium source precursor is at least one of titanyl sulfate and metatitanic acid, and the titanium source precursor solution is a solution formed by the titanium source precursor. Further, the titanium source precursor solution is a solution formed by dissolving the titanium source precursor in water, and the solution contains an acid solution, such as sulfuric acid. In another embodiment, the concentration of the titanium source precursor solution in terms of TiO2 is 15 to 40 g / L.
[0036] In one embodiment, the aluminum source precursor is a soluble aluminum-containing compound, such as an aluminum-containing compound soluble in water. In another embodiment, the aluminum source precursor is aluminum sulfate, and the aluminum source precursor solution is a solution formed by the aluminum source precursor, and further, the aluminum source precursor solution is a solution formed by dissolving the aluminum source precursor in water.
[0037] In one embodiment, the titanium source precursor solution is calculated as TiO2, the aluminum source precursor solution is calculated as Al2O3, and the mass ratio of the titanium source precursor solution to the aluminum source precursor solution is 100:0.3-5.0.
[0038] After the titanium source precursor solution and the aluminum source precursor solution are mixed, the pH value of the mixed solution is adjusted to 7 to 12, and then precipitated, washed, and filtered. In one embodiment, the pH value of the mixed solution is adjusted to 7.5 to 10. The present invention does not particularly limit the reagent used to adjust the pH value, for example, it can be ammonia water.
[0039] The present invention utilizes an in-situ mixing method to mix titanium atoms and aluminum atoms at the molecular level, so that crystals with lattice defects are generated in the subsequent titanium-aluminum co-precipitation process, and the particle size of the metal oxide in the precipitate is small and uniform.
[0040] Step 2 is to mix the precipitate obtained in step 1 with an alkali solution, and stir to obtain a secondary precipitate.
[0041] In one embodiment, the alkali solution is a strong alkali solution; in another embodiment, the alkali solution is an alkali metal hydroxide solution or an alkaline earth metal hydroxide solution, such as a sodium hydroxide solution, a potassium hydroxide solution, etc. In another embodiment, the concentration of the alkali solution is 0.5 to 5 mol / L, and the amount of the alkali solution used is 1 to 5 times the mass of the precipitate obtained in step 1.
[0042] The present invention utilizes a strong base to dissolve the aluminum atoms in the titanium-aluminum lattice, which greatly increases the lattice defects of the titanium substrate. The lattice defects of the aluminum dissolved by the strong base are easily exposed to the surface position of the flue gas in the flue gas atmosphere. After being supplemented by the co-catalytic components, the SCR catalytic activity can be more effectively exerted, thereby enhancing the denitrification effect under the same conditions.
[0043] Step 3 is to mix the secondary precipitate with the tungsten source precursor solution, dry, roast and grind to obtain an intermediate powder.
[0044] In one embodiment, the tungsten source precursor is a soluble tungsten-containing compound, such as a tungsten-containing compound soluble in water. In another embodiment, the tungsten source precursor is at least one of an ammonium paratungstate solution and an ammonium metatungstate solution, and the tungsten source precursor solution is a solution formed by the tungsten source precursor, and further, the tungsten source precursor solution is a solution formed by dissolving the tungsten source precursor in water. In another embodiment, the tungsten source precursor solution is calculated as tungsten trioxide, and the titanium source precursor solution is calculated as TiO2, and the mass ratio of the tungsten source precursor solution to the titanium source precursor solution is 0.5 to 6.0:100.
[0045] In one embodiment, the calcination temperature in step 3 is preferably 450-680° C., and the calcination time is preferably 2-40 hours.
[0046] The present invention supplements tungsten element on the titanium substrate after the aluminum element is dissolved. Since there are more lattice defects, the tungsten element fills the position. After roasting, the lattice defects of the hybrid substrate are more stable. At the same time, the crystal form of the titanium substrate can remain in the anatase type without crystal transformation during high-temperature roasting, which is more conducive to the catalyst maintaining a high denitrification effect.
[0047] Step 4 is to mix the intermediate powder with the vanadium source precursor solution, nano-SiO2 sol, polymer dispersant and pore-forming agent into slurry, spray it on the surface of the corrugated plate, dry it and bake it to form a corrugated plate type denitrification catalyst.
[0048] In one embodiment, the vanadium source precursor is a soluble vanadium-containing compound, such as a vanadium-containing compound soluble in water. In another embodiment, the vanadium source precursor is at least one of an ammonium metavanadate solution and an ammonium vanadate solution, and the vanadium source precursor solution is a solution formed by a vanadium source precursor, and further, the vanadium source precursor solution is a solution formed by dissolving the vanadium source precursor in water. In another embodiment, the vanadium source precursor solution is calculated as V2O5, and the titanium source precursor solution is calculated as TiO2, and the mass ratio of the vanadium source precursor solution to the titanium source precursor solution is 0.2 to 5.0:100.
[0049] Under the action of the polymer dispersant, the vanadium source of the catalyst of the present invention can be fully dispersed on the hybridized substrate. At the same time, due to the influence of the co-catalyst component tungsten on the substrate with larger lattice defects, vanadium penetrates deeper into the surface of the titanium-tungsten particles, connects more tightly, and disperses more evenly. After calcination, the catalyst activity is higher and more stable.
[0050] In addition, the present invention adds nano-SiO2 sol before the catalyst product is roasted, and after dispersion or penetration, the wear resistance of the corrugated plate catalyst can be improved after roasting. In one embodiment, the nano-SiO2 sol is liquid, the SiO2 mass content is 5.0-50%, the nano-SiO2 particle size is 5-80nm, the titanium source precursor solution is calculated in terms of TiO2, and the mass ratio of the nano-SiO2 sol to the titanium source precursor solution is 0.3-5.0:100.
[0051] In step 4, the pore-forming agent is at least one of polyethylene oxide and sesbania powder, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the pore-forming agent to the titanium source precursor solution is 0.1 to 2.0:100.
[0052] In one embodiment, the polymer dispersant is at least one of polyethylene glycol, polyacrylamide, and polyvinyl pyrrolidone. The mass ratio of the titanium source precursor solution is 0.1 to 2.0:100 based on TiO2. In another embodiment, the water mass content of the slurry in step 4 is 40 to 90%.
[0053] In one embodiment, the mixing method in step 4 is stirring or ultrasonic oscillation, the mixing time is 0.1 to 8 hours, the roasting temperature is 450 to 680° C., and the roasting time is 2 to 40 hours.
[0054] In step 4, the drying and calcining process is carried out according to the following procedures: the slurry sprayed on the surface of the corrugated plate is heated from room temperature to 50-105°C, the heating rate is controlled to be no more than 1°C / min, the humidity is controlled to be 50-98%, and after reaching the predetermined temperature, the temperature is kept constant for 3-20 days to form a catalyst dry embryo; the catalyst dry embryo is calcined according to the following process: the temperature is increased from 50-105°C to 450-680°C, the heating rate is controlled to be no more than 1°C / min, after the temperature reaches the predetermined temperature, the temperature is kept constant for 2-40 hours, and then the temperature is cooled, the cooling rate is no more than 4°C / min, and the temperature is cooled to below 50°C to obtain a corrugated plate denitrification catalyst; wherein the humidity of the drying process is preferably 75-95%.
[0055] In one embodiment, the total thickness of the slurry sprayed on the surface of the corrugated plate in step 4 is 0.2-0.6 mm, the corrugation width of the corrugated plate is 4-8 mm, and the corrugation height is 4-10 mm. The corrugated plate is an inorganic fiber board, which can be boron fiber, glass fiber, quartz fiber, ceramic fiber, etc., preferably ceramic fiber. The inorganic ceramic fiber board is used as the catalyst substrate, the substrate has high strength, strong high temperature resistance, and convenient processing and molding, which is conducive to its modular assembly and long-term stable operation on the industrial denitration device.
[0056] Therefore, the present invention provides a method for preparing a corrugated plate type flue gas denitration catalyst. The active components of the corrugated plate type flue gas denitration catalyst obtained by the method are evenly dispersed, the catalyst has high catalytic denitration activity and strong wear resistance.
[0057] The technical solution of the present invention will be further described below through specific embodiments.
[0058] Evaluation method:
[0059] NOx conversion rate evaluation conditions: air velocity 10000h-1 , reaction temperature 370℃, intake NOx 600mg / Nm 3 、SO2: 500mg / Nm 3 , the ammonia nitrogen volume ratio is 1, and the water content is 5%.
[0060] NOx and SO2 concentration determination method: flue gas continuous online analyzer, Siemens ULTRAMAT23.
[0061] SO2 / SO3 conversion rate determination method: Limestone-gypsum wet flue gas desulfurization unit performance acceptance test specification (DL / T998-2006).
[0062] Embodiment 1:
[0063] Titanyl sulfate containing 100 g of TiO2 was dissolved in sulfuric acid to form a solution; aluminum sulfate containing 5 g of Al2O3 was dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 9 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 4 mol / L sodium hydroxide solution, stirred for 5 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 50% with deionized water, 3g of ammonium paratungstate solution calculated as WO3 is added, and after stirring for 3 hours, it is dried, roasted at 600°C for 6 hours, and ground into powder; the roasted powder is then mixed with 1.0g of ammonium metavanadate solution calculated as V2O5 to make a slurry with a water content of 50%, stirred and added with 2.0g of nano-SiO2 sol, 0.5g of polyethylene oxide and 0.5g of polyvinyl pyrrolidone, stirred for 100 minutes to form a slurry with a water content of 80%, and evenly sprayed on the upper and lower sides of the ceramic fiber board with a total spraying thickness of 0.4mm. After drying, it is roasted at 630°C for 10 hours to obtain a corrugated board denitrification catalyst.
[0064] The catalyst obtained above was evaluated. Evaluation results: Catalyst NO x The conversion rate is 98.1%, and the SO2 / SO3 conversion rate is 0.65.
[0065] Example 2
[0066] Titanyl sulfate containing 100 g of TiO2 was dissolved in sulfuric acid to form a solution; aluminum sulfate containing 3 g of Al2O3 was dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 9.5 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 4 mol / L sodium hydroxide solution, stirred for 3 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 60% with deionized water, 1 g of ammonium paratungstate solution calculated as WO3 is added, and after stirring for 2 hours, it is dried, calcined at 510°C for 10 hours, and ground into powder; the calcined powder is then mixed with 0.5 g of ammonium vanadate solution calculated as V2O5 to make a slurry with a water content of 50%, stirred and 1.0 g of nano-SiO2, 0.5 g of polyethylene oxide and 1.0 g of polyethylene glycol are added, stirred for 2 hours to form a slurry with a water content of 60%, and evenly sprayed on the upper and lower sides of the ceramic fiber board with a total spraying thickness of 0.2 mm, and dried and calcined at 600°C for 7 hours to obtain a corrugated board denitrification catalyst.
[0067] The catalyst NO x Conversion rate: 97.0%, SO2 / SO3 conversion rate: 0.70.
[0068] Example 3
[0069] Titanyl sulfate containing 100 g of TiO2 was dissolved in sulfuric acid to form a solution; aluminum sulfate containing 2 g of Al2O3 was dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 8.5 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 3 mol / L sodium hydroxide solution, stirred for 10 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 70% with deionized water, 5 g of ammonium paratungstate solution calculated as WO3 is added, and after stirring for 10 hours, it is dried, roasted at 550°C for 3 hours, and ground into powder; the roasted powder is then mixed with 1.5 g of ammonium vanadate solution calculated as V2O5 to make a slurry with a water content of 35%, and after stirring, 2.0 g of nano-SiO2, 0.3 g of sesbania powder and 1.0 g of polyacrylamide are added, and after stirring for 5 hours, a slurry with a water content of 60% is formed and evenly sprayed on the upper and lower sides of the ceramic fiber board, with a total spraying thickness of 0.5 mm, and then dried and roasted at 630°C for 8 hours to obtain a denitration catalyst.
[0070] The fresh catalyst obtained above was evaluated. Evaluation results: Catalyst NO x The conversion rate is 98.5%, and the SO2 / SO3 conversion rate is 0.77.
[0071] Example 4
[0072] Titanic acid containing 100 g of TiO2 is dissolved in sulfuric acid to form a solution; aluminum sulfate containing 0.5 g of Al2O3 is dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 8.5 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 4 mol / L sodium hydroxide solution, stirred for 12 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 40% with deionized water, 6 g of ammonium paratungstate solution calculated as WO3 is added, and after stirring for 3 hours, it is dried, calcined at 450°C for 5 hours, and ground into powder; the calcined powder is then mixed with 2 g of ammonium metavanadate solution calculated as V2O5 to make a slurry with a water content of 40%, and after stirring, 2 g of nano-SiO2, 0.5 g of sesbania powder and 2 g of polyvinyl pyrrolidone are added, and after stirring for 5 hours, a slurry with a water content of 60% is formed, which is evenly sprayed on the upper and lower sides of the ceramic fiber board with a total spraying thickness of 0.5 mm, and a denitrification catalyst is obtained after drying and calcining at 600°C for 5 hours.
[0073] The catalyst NO x The conversion rate is 99.1%, and the SO2 / SO3 conversion rate is 0.83.
[0074] Example 5
[0075] Titanyl sulfate containing 100 g of TiO2 was dissolved in sulfuric acid to form a solution; aluminum nitrate containing 1.0 g of Al2O3 was dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 9 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 4.0 mol / L sodium hydroxide solution, stirred for 7 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 40% with deionized water, 5g of ammonium metatungstate solution calculated as WO3 is added, and after stirring for 3 hours, it is dried, calcined at 550°C for 4 hours, and ground into powder; the calcined powder is then mixed with 3g of ammonium metavanadate solution calculated as V2O5 to make a slurry with a water content of 50%, and after stirring, 0.5g of nano-SiO2, 2.0g of sesbania powder and 1.0g of polyvinyl pyrrolidone are added, and after stirring for 2 hours, a slurry with a water content of 70% is formed, which is evenly sprayed on the upper and lower sides of the ceramic fiber board with a total spraying thickness of 0.6mm, and a denitrification catalyst is obtained after drying and calcining at 580°C for 3 hours.
[0076] The catalyst NO x The conversion rate is 98.9%, and the SO2 / SO3 conversion rate is 0.80.
[0077] Example 6
[0078] Titanyl sulfate containing 100 g of TiO2 was dissolved in sulfuric acid to form a solution; aluminum nitrate containing 2 g of Al2O3 was dissolved in deionized water to form a solution. After the above two solutions are uniformly mixed, the pH value is adjusted to 10 with ammonia water. After complete precipitation, it is filtered and washed; the washed material is placed in a 3 mol / L sodium hydroxide solution, stirred for 2 hours, fully washed and filtered; the washed material is made into a slurry with a water content of 50% with deionized water, 4 g of ammonium metatungstate solution calculated as WO3 is added, and after stirring for 2 hours, it is dried, calcined at 450°C for 11 hours, and ground into powder; the calcined powder is then mixed with 3 g of ammonium metavanadate solution calculated as V2O5 to make a slurry with a water content of 70%, and after stirring, 1.5 g of nano-SiO2, 2.0 g of sesbania powder and 1.0 g of polyacrylamide are added, and after stirring for 5 hours, a slurry with a water content of 70% is formed, which is evenly sprayed on the upper and lower sides of the ceramic fiber board with a total spraying thickness of 0.6 mm, and the corrugated board structure monomer is immersed in the slurry, and a denitrification catalyst is obtained after drying and calcining at 600°C for 8 hours.
[0079] The catalyst obtained above was evaluated. The evaluation results showed that the fresh catalyst NO x The conversion rate is 99.4%, and the SO2 / SO3 conversion rate is 0.89.
[0080] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a corrugated plate flue gas denitration catalyst, characterized in that: The steps include: Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7-12, and precipitating; Step 2, mixing the precipitate obtained in step 1 with an alkali solution, stirring, and obtaining a secondary precipitate; Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder; Step 4, mixing the intermediate powder with the vanadium source precursor solution, nano-SiO2 sol, polymer dispersant, and pore-forming agent into a slurry, spraying it on the surface of the corrugated plate, drying, and calcining to form a corrugated plate type denitration catalyst; Wherein, the alkali solution in step 2 is an alkali metal hydroxide solution or an alkaline earth metal hydroxide solution.
2. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: In step 3 and step 4, the calcination temperature is 450-680° C., and the calcination time is 2-40 hours.
3. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: In step 4, the drying and calcining process is carried out according to the following procedure: the slurry sprayed on the surface of the corrugated plate is heated from room temperature to 50-105° C., the heating rate is controlled to be no more than 1° C. / min, the humidity is controlled to be 50-98%, and after reaching the predetermined temperature, the temperature is kept constant for 3-20 days to form a catalyst dry embryo; The catalyst dry body is calcined according to the following process: the temperature is increased from 50-105°C to 450-680°C, and the heating rate is controlled to be no more than 1°C / min. After the temperature reaches the predetermined temperature, it is calcined at a constant temperature for 2-40 hours, and then cooled at a rate of no more than 4°C / min to below 50°C to obtain a corrugated plate deNOx catalyst.
4. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 3, characterized in that: The humidity during the drying process is controlled at 75-95%.
5. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: The concentration of the alkali solution in step 2 is 0.5-5 mol / L; the mass of the alkali solution is 1-5 times the mass of the precipitate obtained in step 1.
6. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: The tungsten source precursor solution is at least one of ammonium paratungstate solution and ammonium metatungstate solution; the tungsten source precursor solution is calculated as tungsten trioxide, and the titanium source precursor solution is calculated as TiO2, and the mass ratio of the tungsten source precursor solution to the titanium source precursor solution is 0.5-6.0:
100.
7. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: The vanadium source precursor solution is at least one of ammonium metavanadate solution and ammonium vanadate solution. The vanadium source precursor solution is calculated as V2O5, and the titanium source precursor solution is calculated as TiO2. The mass ratio of the vanadium source precursor solution to the titanium source precursor solution is 0.2 to 5.0:
100.
8. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: In step 1, the pH adjusting reagent is ammonia water, and the pH value is adjusted to 7.5-10; in step 4, the mixing method is stirring or ultrasonic oscillation, and the mixing time is 0.1-8 hours; the water mass content of the slurry in step 4 is 40-90%.
9. The method for preparing a corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: The polymer dispersant is at least one of polyethylene glycol, polyacrylamide and polyvinyl pyrrolidone; the titanium source precursor solution is calculated as TiO2, and the mass ratio of the polymer dispersant to the titanium source precursor solution is 0.1 to 2.0:
100.
10. The method for preparing the corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: In step 4, the nano-SiO2 sol is in liquid state, the SiO2 mass content is 5.0-50%, the nano-SiO2 particle size is 5-80nm, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the nano-SiO2 sol to the titanium source precursor solution is 0.3-5.0:
100.
11. The method for preparing a corrugated plate type flue gas denitration catalyst according to claim 1, characterized in that: In step 4, the pore-forming agent is at least one of polyethylene oxide and sesbania powder, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the pore-forming agent to the titanium source precursor solution is 0.1 to 2.0:
100.
12. The corrugated plate type flue gas denitration catalyst obtained by the preparation method according to any one of claims 1 to 10.
Citation Information
Patent Citations
Honeycomb flue gas denitrification catalyst and preparation method thereof
CN103143396B
A preparation process for a corrugated plate denitrification catalyst
CN106732709B
A method for preparing a honeycomb denitration catalyst with increased specific surface area
CN107096524B
A honeycomb denitrification catalyst with improved strength and its preparation method
CN107138150B
Honeycomb denitration catalyst with increased specific surface area and preparation method
CN107321344A