Exhaust purification catalyst device
By optimizing the configuration and concentration distribution of the catalyst coating in the exhaust purification catalyst device, using multi-layer structure and precious metal catalysts, the problem of poor reduction of hot NOx and cold HC in the prior art is solved, and the exhaust purification efficiency is achieved The improvement meets strict environmental protection standards.
Patent Information
- Application Number
- CN202180074874.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-06
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-21
AI Technical Summary
The existing exhaust gas purification catalyst device is insufficient in reducing hot NOx and cold HC simultaneously, especially in reducing cold HC.
An exhaust purification catalyst device was designed, and its catalyst coating was arranged on the upstream and downstream sides of the exhaust stream. Using precious metal catalysts such as Pt, Pd and Rh, the upstream side was ensured by optimizing the concentration and distribution of the catalyst. The catalyst concentration relationship between the coating and the downstream side coating realizes a three-way catalytic effect, promoting the oxidation of HC and the reduction of NOx.
It achieves a simultaneous reduction of hot NOx and cold HC, significantly reduces emissions, improves exhaust purification efficiency, and meets strict environmental protection standards such as LEV III and Euro6 regulations.
Smart Images

Figure CN116419797B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an exhaust gas purification catalyst device. Background Art
[0002] Exhaust gas emitted from internal combustion engines such as automobile engines contains nitrogen oxides (NO x ), carbon monoxide (CO), hydrocarbons (HC), etc. These exhaust gases are purified by an exhaust purification catalyst that oxidizes CO and HC and reduces NOx, and then released into the atmosphere.
[0003] With respect to the three components of CO, HC, and NOx contained in exhaust gas, the emission weight per unit distance traveled by automobiles is regulated in various countries from the viewpoint of alleviating air pollution.
[0004] Exhaust regulations are becoming more stringent year by year. Currently, LEV III regulations apply in the United States and Euro 6 regulations apply in Europe. In Europe, it is expected that the transition to Euro 7 regulations will take place in the near future.
[0005] Under such circumstances, for example, Patent Document 1 describes a layered catalyst composite device comprising a substrate, a first layer containing Pd deposited on the substrate, a second layer containing Rh deposited on the first layer, and a third layer containing Pd deposited on the second layer, and exemplifies a method in which the third layer is deposited only on the upstream side portion of the substrate to generate a high Pd-containing region.
[0006] Prior Art Literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application No. 2010-501337 Summary of the invention
[0009] In the above regulations, an operation mode including a cold start is adopted as a test mode, and achieving a high degree of reduction in both cold HC emission (cold HC) and hot NOx emission (hot NOx) is an urgent issue.
[0010] Among them, cold HC accounts for a large proportion of the total exhaust amount, and therefore Patent Document 1 above proposes an exhaust gas purification catalyst device designed with emphasis on reducing cold HC.
[0011] However, conventional exhaust gas purification catalyst devices including the layered catalyst composite device described in Patent Document 1 are insufficient in achieving both the reduction of hot NOx and the reduction of cold HC.
[0012] Therefore, an object of the present invention is to provide an exhaust gas purification catalyst device that achieves both a reduction in hot NOx and a reduction in cold HC at a high level.
[0013] The present invention is as follows.
[0014] [Mode 1] An exhaust gas purification catalyst device comprising a substrate and a catalyst coating layer on the substrate,
[0015] The catalyst coating layer comprises an upstream coating layer arranged on the upstream side of the exhaust flow and a downstream coating layer arranged on the downstream side of the exhaust flow.
[0016] The upstream coating layer comprises an upstream lower coating layer disposed on the substrate and an upstream upper coating layer disposed on the upstream lower coating layer.
[0017] The downstream coating layer comprises a downstream lower coating layer disposed on the substrate and a downstream upper coating layer disposed on the downstream lower coating layer.
[0018] The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer, and the downstream upper coating layer each contain a catalyst noble metal selected from Pt, Pd, and Rh,
[0019] Satisfying both (i) and (ii) below,
[0020] (i) the concentration of one or both selected from Pt and Pd in the upstream upper coating layer and the downstream lower coating layer is higher than the concentration of one or both selected from Pt and Pd in the upstream lower coating layer, and higher than the concentration of one or both selected from Pt and Pd in the downstream upper coating layer;
[0021] (ii) The concentrations of Rh in the upstream lower coating layer and the downstream upper coating layer are both higher than the concentration of Rh in the upstream upper coating layer and higher than the concentration of Rh in the downstream lower coating layer.
[0022] [Aspect 2] The exhaust gas purification catalyst device according to aspect 1,
[0023] At least the downstream lower coating layer comprises ceria,
[0024] The ceria concentration in the upstream lower coating layer, the ceria concentration in the upstream upper coating layer, and the ceria concentration in the downstream upper coating layer are all 70% or less of the ceria concentration in the downstream lower coating layer.
[0025] [Mode 3] The exhaust gas purification catalyst device according to Mode 1 or 2,
[0026] The amount of cerium dioxide in the upstream lower coating layer is 10 g / L or less relative to 1 L of the substrate on which the upstream lower coating layer is formed.
[0027] The amount of ceria in the downstream-side upper coating layer is 10 g / L or less relative to 1 L of the substrate in the portion where the downstream-side upper coating layer is formed.
[0028] [Aspect 4] The exhaust gas purification catalyst device according to any one of aspects 1 to 3,
[0029] The upstream side upper coating layer and the downstream side lower coating layer each contain Pd,
[0030] (The amount of Pd in the upstream upper coating) / (the substrate 1L of the upstream upper coating forming part) is at least 2.0 times (the amount of Pd in the downstream lower coating) / (the substrate 1L of the downstream lower coating forming part).
[0031] [Aspect 5] The exhaust gas purification catalyst device according to any one of aspects 1 to 4,
[0032] The total length of the upstream side lower coating layer and the downstream side upper coating layer is at least 80% of the length of the substrate.
[0033] [Aspect 6] The exhaust gas purification catalyst device according to any one of aspects 1 to 5,
[0034] There is no region in the vicinity of the end portion on the upstream side of the exhaust gas flow where the upstream upper coating layer is directly disposed on the substrate without interposing the upstream lower coating layer therebetween.
[0035] [Aspect 7] The exhaust gas purification catalyst device according to any one of aspects 1 to 6,
[0036] The length of the upstream coating layer is not less than 20% and not more than 50% of the length of the substrate.
[0037] [Aspect 8] The exhaust gas purification catalyst device according to any one of aspects 1 to 7,
[0038] The coating amount of the upstream coating layer is 240 g / L or less relative to 1 L of the substrate at the upstream coating layer forming portion.
[0039] [Aspect 9] The exhaust gas purification catalyst device according to any one of aspects 1 to 8,
[0040] The coating amount of the upstream-side upper coating layer is 160 g / L or less relative to 1 L of the substrate at the upstream-side upper coating layer forming portion.
[0041] According to the present invention, it is possible to provide an exhaust gas purification catalyst device which achieves both a high degree of reduction in hot NOx and a high degree of reduction in cold HC. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram showing an example of the configuration of the exhaust gas purification catalyst device of the present invention.
[0043] Figure 2 It is a schematic diagram showing another example of the configuration of the exhaust gas purification catalyst device of the present invention.
[0044] Figure 3 It is a schematic diagram showing still another example of the configuration of the exhaust gas purification catalyst device of the present invention.
[0045] Figure 4 It is a schematic diagram showing still another example of the configuration of the exhaust gas purification catalyst device of the present invention.
[0046] Figure 5 It is a schematic diagram showing the configuration of exhaust gas purification catalyst devices manufactured in Example 1 and Comparative Examples 1 to 5, respectively.
[0047] Figure 6 It is a schematic diagram showing the configuration of the exhaust gas purification catalyst device manufactured in Examples 1, 9, and 10, respectively.
[0048] Figure 7 It is a schematic diagram showing the configuration of the exhaust gas purification catalyst device manufactured in each of Examples 11 to 16. DETAILED DESCRIPTION
[0049] The exhaust gas purification catalyst device of the present invention is an exhaust gas purification catalyst device having a substrate and a catalyst coating layer on the substrate.
[0050] The catalyst coating layer comprises an upstream coating layer arranged on the upstream side of the exhaust flow and a downstream coating layer arranged on the downstream side of the exhaust flow.
[0051] The upstream coating layer comprises an upstream lower coating layer disposed on the substrate and an upstream upper coating layer disposed on the upstream lower coating layer.
[0052] The downstream coating layer comprises a downstream lower coating layer disposed on the substrate and a downstream upper coating layer disposed on the downstream lower coating layer.
[0053] The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer, and the downstream upper coating layer each contain a catalyst noble metal selected from Pt, Pd, and Rh,
[0054] Satisfying both (i) and (ii) below,
[0055] (i) the concentration of one or both selected from Pt and Pd in the upstream upper coating layer and the downstream lower coating layer is higher than the concentration of one or both selected from Pt and Pd in the upstream lower coating layer, and higher than the concentration of one or both selected from Pt and Pd in the downstream upper coating layer;
[0056] (ii) The concentrations of Rh in the upstream lower coating layer and the downstream upper coating layer are both higher than the concentration of Rh in the upstream upper coating layer and higher than the concentration of Rh in the downstream lower coating layer.
[0057] Hereinafter, a typical configuration of the exhaust gas purification catalyst device of the present invention will be described with reference to the drawings.
[0058] Figure 1 to Figure 4 Each of them is a schematic diagram showing a configuration example of the exhaust gas purification catalyst device of the present invention.
[0059] Figure 1 The exhaust gas purification catalyst device (100) is an exhaust gas purification catalyst device having a substrate (110) and a catalyst coating on the substrate (110). The catalyst coating of the exhaust gas purification catalyst device (100) has an upstream coating (120) arranged on the upstream side of the exhaust gas flow and a downstream coating (130) arranged on the downstream side of the exhaust gas flow.
[0060] The upstream coating layer comprises an upstream lower coating layer (121) disposed on a substrate (110) and an upstream upper coating layer (122) disposed on the upstream lower coating layer (121). The downstream coating layer comprises a downstream lower coating layer (131) disposed on the substrate (110) and a downstream upper coating layer (132) disposed on the downstream lower coating layer (131).
[0061] The upstream side lower coating layer (121), the upstream side upper coating layer (122), the downstream side lower coating layer (131) and the downstream side upper coating layer (132) respectively contain a catalyst noble metal selected from Pt, Pd and Rh.
[0062] Furthermore, the exhaust gas purification catalyst device (100) satisfies both of the following (i) and (ii):
[0063] (i) the concentration of one or both selected from Pt and Pd in the upstream upper coating layer (122) and the downstream lower coating layer (131) is higher than the concentration of one or both selected from Pt and Pd in the upstream lower coating layer (121), and higher than the concentration of one or both selected from Pt and Pd in the downstream upper coating layer (132);
[0064] (ii) The concentration of Rh in the upstream lower coating layer (121) and the downstream upper coating layer (132) is higher than the concentration of Rh in the upstream upper coating layer (122), and higher than the concentration of Rh in the downstream lower coating layer (131).
[0065] The above elements (i) and (ii) show that:
[0066] In the upstream side coating layer, the upper layer contains one or two selected from Pt and Pd at a high concentration, the lower layer contains Rh at a high concentration, and,
[0067] In the downstream side coating layer, the upper layer contains Rh at a high concentration, and the lower layer contains one or two selected from Pt and Pd at a high concentration.
[0068] Figure 1 The exhaust gas purification catalyst device (100) can achieve a high degree of simultaneous reduction of hot NOx and cold HC by such a structure.
[0069] That is, the upper layer of the upstream side coating layer of the exhaust gas flow that is preheated first contains one or both of the catalyst precious metals selected from Pt and Pd at a high concentration. Therefore, the oxidation purification of HC is promoted, and the cold HC is greatly reduced. In addition, the lower layer of the upstream side coating layer contains Rh at a high concentration. Therefore, in the upstream side coating layer, while the oxidation reaction caused by the catalyst precious metal in the upper layer proceeds, the reduction reaction caused by the Rh in the lower layer also proceeds, so that the overall three-way catalytic action can be promoted, thereby helping to reduce the cold HC and further reducing the cold HC.
[0070] On the other hand, for the downstream coating, the upper layer that is easily in contact with the exhaust gas contains Rh at a high concentration. This can effectively reduce thermal NOx. In addition, the lower layer of the downstream coating contains one or both of the catalyst precious metals selected from Pt and Pd at a high concentration, which helps reduce thermal HC.
[0071] Figure 2 The exhaust gas purification catalyst device (200) shown in FIG. 1 is another configuration example of the exhaust gas purification catalyst device of the present invention.
[0072] Figure 2 The exhaust gas purification catalyst device (200) comprises a substrate (210) and a catalyst coating on the substrate (210),
[0073] The catalyst coating layer comprises an upstream coating layer (220) arranged on the upstream side of the exhaust flow and a downstream coating layer (230) arranged on the downstream side of the exhaust flow.
[0074] The upstream coating layer comprises an upstream lower coating layer (221) disposed on a substrate (210) and an upstream upper coating layer (222) disposed on the upstream lower coating layer (221).
[0075] The downstream coating layer comprises a downstream lower coating layer (231) disposed on a substrate (210) and a downstream upper coating layer (232) disposed on the downstream lower coating layer (231).
[0076] The relationship between the type and concentration of the catalytic noble metal contained in each coating layer is Figure 1 The exhaust gas purification catalyst device (100) is the same.
[0077] However, in Figure 2 In the exhaust gas purification catalyst device (200), the upstream side lower coating layer (221) and the downstream side upper coating layer (232) are connected to form an integral body, thereby forming an Rh layer (240) that exists continuously in the exhaust gas flow direction.
[0078] In the exhaust gas purification catalyst device (200) as well:
[0079] The upstream coating layer contains one or both of a catalyst noble metal selected from Pt and Pd in the upper layer, and contains Rh in a high concentration in the lower layer;
[0080] The downstream coating layer contains Rh at a high concentration in the upper layer, and contains one or both of catalytic noble metals selected from Pt and Pd at a high concentration in the lower layer.
[0081] therefore, Figure 2 The exhaust gas purification catalyst device (200) is provided by Figure 1 The exhaust gas purification catalyst device (100) uses the same mechanism to significantly reduce cold HC, promote three-way catalysis, and reduce hot NOx and hot HC.
[0082] Figure 3 The exhaust gas purification catalyst device (300) shown in is another configuration example of the exhaust gas purification catalyst device of the present invention.
[0083] Figure 3 The exhaust gas purification catalyst device (300) comprises a substrate (310) and a catalyst coating on the substrate (310),
[0084] The catalyst coating layer comprises an upstream coating layer (320) arranged on the upstream side of the exhaust flow and a downstream coating layer (330) arranged on the downstream side of the exhaust flow.
[0085] The upstream coating layer comprises an upstream lower coating layer (321) disposed on a substrate (310) and an upstream upper coating layer (322) disposed on the upstream lower coating layer (321).
[0086] The downstream coating layer comprises a downstream lower coating layer (331) disposed on a substrate (310) and a downstream upper coating layer (332) disposed on the downstream lower coating layer (331).
[0087] The relationship between the type and concentration of the catalytic noble metal contained in each coating layer is Figure 1 The exhaust gas purification catalyst device (100) is the same.
[0088] However, in Figure 3 In the exhaust gas purification catalyst device (300), the length of the upstream side upper coating layer (322) is different from the length of the upstream side lower coating layer (321). Specifically, the length of the upstream side upper coating layer (322) is shorter than the length of the upstream side lower coating layer (321), so that a part of the upstream side lower coating layer (321) is directly in contact with the exhaust gas.
[0089] In the exhaust gas purification catalyst device (300) as well:
[0090] The upstream coating layer contains one or both of a catalyst noble metal selected from Pt and Pd in the upper layer, and contains Rh in a high concentration in the lower layer.
[0091] The downstream coating layer contains Rh at a high concentration in the upper layer, and contains one or both of catalytic noble metals selected from Pt and Pd at a high concentration in the lower layer.
[0092] therefore, Figure 3 The exhaust gas purification catalyst device (300) is Figure 1 The exhaust gas purification catalyst device (100) uses the same mechanism to significantly reduce cold HC, promote three-way catalysis, and reduce hot NOx and hot HC.
[0093] Figure 4 The exhaust gas purification catalyst device (400) shown in FIG. 1 is another configuration example of the exhaust gas purification catalyst device of the present invention.
[0094] Figure 4 The exhaust gas purification catalyst device (400) comprises a substrate (410) and a catalyst coating on the substrate (410),
[0095] The catalyst coating layer comprises an upstream coating layer (420) arranged on the upstream side of the exhaust flow and a downstream coating layer (430) arranged on the downstream side of the exhaust flow.
[0096] The upstream coating layer comprises an upstream lower coating layer (421) disposed on a substrate (410).
[0097] The downstream coating layer comprises a downstream lower coating layer (431) disposed on a substrate (410) and a downstream upper coating layer (432) disposed on the downstream lower coating layer (431).
[0098] Regarding the above, Figure 1 The exhaust gas purification catalyst device (100) is the same.
[0099] However, in Figure 4 In the exhaust purification catalyst device (400), the upstream side upper coating (422) includes: an upstream side upper coating downstream portion (422(b)) which further extends from the upstream side upper coating upstream portion (422(a)) arranged on the upstream side lower coating (421) to the downstream side and covers a portion of the upstream side of the downstream side upper coating (432).
[0100] In this Figure 4 In the exhaust gas purification catalyst device (400), the type and concentration of the catalyst precious metal contained in each coating layer are also related to Figure 1 The exhaust gas purification catalyst device (100) is the same as that of Figure 1 The exhaust gas purification catalyst device (100) uses the same mechanism to significantly reduce cold HC, promote three-way catalysis, and reduce hot NOx and hot HC.
[0101] Hereinafter, each element constituting the exhaust gas purification catalyst device of the present invention will be described in detail one by one.
[0102] Exhaust purification catalyst device
[0103] As described above, the exhaust gas purification catalyst device of the present invention has a substrate and a catalyst coating layer on the substrate.
[0104] Substrate
[0105] As the substrate in the exhaust gas purification catalyst device of the present invention, a substrate commonly used as a substrate for exhaust gas purification catalyst devices can be used, for example, a monolithic honeycomb substrate of a direct current type made of cordierite, SiC, stainless steel, inorganic oxide particles, etc.
[0106] Catalyst coating
[0107] The catalyst coating layer exists on the substrate. Specifically, the catalyst coating layer may exist as a layer protruding toward the cell side on the surface of the cell wall that normalizes the cells communicating from the upstream end to the downstream end of the exhaust gas flow in the substrate.
[0108] The catalyst coating layer includes an upstream coating layer arranged on the upstream side of the exhaust flow and a downstream coating layer arranged on the downstream side of the exhaust flow.
[0109] 〈Upstream coating〉
[0110] The upstream coating layer is disposed on the substrate at the upstream side of the exhaust gas flow and includes an upstream lower coating layer and an upstream upper coating layer.
[0111] The upstream side lower coating layer is directly disposed on the substrate at the upstream side of the exhaust gas flow on the substrate. The upstream side upper coating layer is disposed on the upstream side lower coating layer.
[0112] 〈Downstream coating〉
[0113] The downstream coating layer is disposed on the substrate at the downstream side of the exhaust gas flow and includes a downstream lower coating layer and a downstream upper coating layer.
[0114] The downstream side lower coating layer is directly disposed on the substrate at the downstream side of the exhaust gas flow on the substrate. The downstream side upper coating layer is disposed on the downstream side lower coating layer.
[0115] (Length of catalyst coating)
[0116] From the viewpoint of effectively reducing cold HC, the length of the upstream side coating can be more than 20%, more than 22%, more than 25%, more than 27%, more than 30%, or more than 32% of the length of the substrate; from the viewpoint of ensuring the manifestation of the three-way catalytic effect of the downstream side coating, the length of the substrate can be less than 50%, less than 48%, less than 45%, less than 43%, less than 40%, less than 38%, or less than 35%.
[0117] Typically, the length of the upstream coating layer may be not less than 20% and not more than 50% of the length of the substrate.
[0118] The length of the upstream coating layer mentioned above is also appropriate even if it is the length of the upstream lower coating layer and the length of the upstream upper coating layer. Here, the length of the upstream lower coating layer and the length of the upstream upper coating layer may be the same or different. The length of the upstream upper coating layer may be independently of the length of the upstream lower coating layer and may be more than 25%, more than 30%, more than 35%, or more than 40% of the length of the substrate, and may be less than 75%, less than 70%, less than 65%, less than 60%, less than 55%, or less than 50% of the length of the substrate.
[0119] Typically, the length of the upstream upper coating layer can be 30% or more and 60% or less of the length of the substrate independently of the length of the upstream lower coating layer.
[0120] When the length of the upstream lower coating layer is different from the length of the upstream upper coating layer, the length of the upstream coating layer in this specification is defined as the length of the portion where the upstream lower coating layer and the upstream upper coating layer are stacked on the substrate.
[0121] In addition, in order to ensure the effect of reducing cold HC brought by the three-way catalytic action, the exhaust purification catalyst device of the present invention may not have an area near the end on the upstream side of the exhaust flow where the upstream upper coating is directly arranged on the substrate without passing through the upstream lower coating.
[0122] From the viewpoint of ensuring the manifestation of the three-way catalytic effect, the length of the downstream side coating can be more than 50%, more than 52%, more than 55%, more than 60%, more than 62%, or more than 65% of the substrate length; from the viewpoint of effectively reducing the cold HC caused by the upstream side coating, the length of the substrate can be less than 80%, less than 78%, less than 75%, less than 73%, less than 70%, or less than 68%.
[0123] Typically, the length of the downstream coating layer may be not less than 50% and not more than 80% of the length of the substrate.
[0124] The length of the downstream coating layer mentioned above is also appropriate even if it is the length of the downstream lower coating layer and the length of the downstream upper coating layer. Here, the length of the downstream lower coating layer and the length of the downstream upper coating layer may be the same or different. In the case where the length of the downstream lower coating layer is different from the length of the downstream upper coating layer, the length of the downstream coating layer in this specification is defined as the length of the portion where the downstream lower coating layer and the downstream upper coating layer are stacked on the substrate.
[0125] In addition, from the viewpoint of ensuring the configuration length of the layer containing Rh as a catalytic noble metal at a high concentration so as to effectively reduce thermal NOx, the total length of the upstream side lower coating layer and the downstream side upper coating layer can be more than 70%, more than 75%, more than 80%, more than 85%, more than 90%, or more than 95% of the substrate length, or it can be 100% of the substrate length.
[0126] As described above, the method in which the length of the upper coating layer on the upstream side is longer than the length of the lower coating layer on the upstream side and the upper coating layer on the upstream side covers a part of the coating layer on the downstream side is also included in the exhaust gas purification catalyst device of the present invention. In this case, in order to effectively reduce thermal NOx, at least a part of the coating layer on the downstream side, especially the upper coating layer on the downstream side, can be configured to be not covered by the upper coating layer on the upstream side and can be in direct contact with the exhaust gas.
[0127] From this viewpoint, the downstream upper coating layer may be not covered by the upstream upper coating layer and directly contact the exhaust gas within a range of 30%, 35%, 40%, 45%, or 50% or more of the substrate length.
[0128] (Amount of catalyst coating applied)
[0129] In order to reduce cold HC, it is desirable to set the heat capacity of the exhaust gas purification catalyst device, especially the upstream side of the exhaust gas flow, low to improve the temperature rise. From this point of view, the coating amount of the upstream side coating can be less than 250g / L, less than 240g / L, less than 230g / L, less than 220g / L, less than 210g / L, less than 200g / L, less than 190g / L, or less than 180g / L relative to the substrate 1L of the upstream side coating forming part. On the other hand, from the point of view of ensuring the effect of reducing cold HC brought by the upstream side coating, the coating amount of the upstream side coating can be more than 160g / L, more than 170g / L, more than 180g / L, more than 190g / L, or more than 200g / L relative to the substrate 1L of the upstream side coating forming part.
[0130] Similarly, from the viewpoint of improving the temperature rise property on the upstream side of the exhaust gas flow, the coating amount of the upstream upper coating layer may be 160 g / L or less, 150 g / L or less, 140 g / L or less, 120 g / L or less, 110 g / L or less, 100 g / L or less, or 90 g / L or less relative to 1L of the substrate where the upstream upper coating layer is formed. On the other hand, from the viewpoint of ensuring the cold HC reduction effect brought about by the upstream upper coating layer, the coating amount of the upstream upper coating layer may be 60 g / L or more, 70 g / L or more, 80 g / L or more, 90 g / L or more, 100 g / L or more, or 110 g / L or more relative to 1L of the substrate where the upstream upper coating layer is formed.
[0131] Furthermore, from the viewpoint of improving the temperature rise of the upstream side of the exhaust gas flow, the coating amount of the upstream side lower coating layer can be 140 g / L or less, 130 g / L or less, 120 g / L or less, 110 g / L or less, 100 g / L or less, or 90 g / L or less relative to the substrate 1L of the upstream side lower coating layer forming portion. On the other hand, in order to ensure the cold HC reduction effect brought about by the three-way catalytic action, the coating amount of the upstream side lower coating layer can be 60 g / L or more, 65 g / L or more, 70 g / L or more, or 75 g / L or more relative to the substrate 1L of the upstream side lower coating layer forming portion.
[0132] In addition, from the viewpoint of avoiding a useless increase in exhaust back pressure and ensuring the three-way catalytic effect brought about by the downstream side coating to achieve a reduction in hot HC and thermal NOx, the coating amount of the downstream side upper coating can be less than 120 g / L, less than 110 g / L, less than 100 g / L, or less than 90 g / L relative to 1L of the substrate where the downstream side upper coating is formed, and can be more than 60 g / L, more than 65 g / L, more than 70 g / L, more than 75 g / L, more than 80 g / L, or more than 85 g / L.
[0133] From the same point of view, the coating amount of the downstream side lower layer coating can be less than 200 g / L, less than 190 g / L, less than 185 g / L, or less than 180 g / L relative to 1L of the substrate where the downstream side lower layer coating is formed, and can be more than 150 g / L, more than 160 g / L, more than 170 g / L, or more than 175 g / L.
[0134] 〈Composition of Catalyst Coating〉
[0135] (Catalyst precious metals)
[0136] The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer, and the downstream upper coating layer each contain a catalyst noble metal selected from Pt, Pd, and Rh, and satisfy both of the following (i) and (ii),
[0137] (i) the concentration of one or both selected from Pt and Pd in the upstream upper coating layer and the downstream lower coating layer is higher than the concentration of one or both selected from Pt and Pd in the upstream lower coating layer, and higher than the concentration of one or both selected from Pt and Pd in the downstream upper coating layer;
[0138] (ii) The concentrations of Rh in the upstream side lower coating layer and the downstream side upper coating layer are both higher than the concentration of Rh in the upstream side upper coating layer, and higher than the concentration of Rh in the downstream side lower coating layer.
[0139] Specifically, the above-mentioned requirement (i) may be that the concentration of one or both selected from Pt and Pd in the upstream upper coating layer and the downstream lower coating layer is more than 2 times, more than 5 times, more than 10 times, more than 50 times, more than 100 times, more than 500 times, or more than 1000 times the concentration of one or both selected from Pt and Pd in the upstream lower coating layer and the concentration of one or both selected from Pt and Pd in the downstream upper coating layer, respectively; or, the upstream lower coating layer and the downstream upper coating layer do not contain one or both selected from Pt and Pd, so the ratio may be infinite.
[0140] Specifically, the above-mentioned requirement (ii) may be that the concentration of Rh in the upstream lower coating layer and the downstream upper coating layer is more than 2 times, more than 5 times, more than 10 times, more than 50 times, more than 100 times, more than 500 times, or more than 1000 times the concentration of Rh in the upstream upper coating layer and the concentration of Rh in the downstream lower coating layer, respectively; or, the upstream upper coating layer and the downstream lower coating layer do not contain Rh, so the ratio may be infinite.
[0141] As stated above, these (i) and (ii) elements mean that:
[0142] For the upstream coating layer, the upper layer contains one or two selected from Pt and Pd at a high concentration, the lower layer contains Rh at a high concentration, and,
[0143] For the downstream side coating layer, the upper layer contains Rh at a high concentration, and the lower layer contains one or two selected from Pt and Pd at a high concentration.
[0144] Here, the concentration of the catalytic noble metal in each coating layer refers to the mass ratio (g / L) of the amount of the catalytic noble metal in the coating layer relative to 1 L of the substrate in the portion where the coating layer is formed.
[0145] The upstream upper coating layer and the downstream lower coating layer may each contain one or both selected from Pt and Pd, and may particularly contain Pd. In this case, these coating layers may not contain Pt.
[0146] In the case where the upstream-side upper coating layer and the downstream-side lower coating layer contain Pd and do not contain Pt, the contents of Pd in these coating layers can be as follows.
[0147] The amount of Pd in the upstream upper coating layer can be greater than 1.0 g / L, greater than 2.0 g / L, greater than 3.0 g / L, or greater than 4.0 g / L, and can be less than 8.0 g / L, less than 7.0 g / L, less than 6.0 g / L, less than 5.5 g / L, less than 5.0 g / L, less than 4.5 g / L, or less than 4.0 g / L, relative to 1 L of the substrate where the upstream upper coating layer is formed.
[0148] The amount of Pd in the upstream side lower coating layer can be greater than 0.25 g / L, greater than 0.50 g / L, greater than 0.75 g / L, or greater than 1.00 g / L, and can be less than 2.00 g / L, less than 1.75 g / L, less than 1.50 g / L, less than 1.25 g / L, or less than 1.00 g / L, relative to 1 L of the substrate where the upstream side lower coating layer is formed.
[0149] In order to effectively reduce cold HC through the upstream upper coating layer and thereby reduce the total HC amount, it is desirable to centrally configure Pd in the upstream upper coating layer among the upstream upper coating layer and the downstream lower coating layer. On the other hand, it is also necessary to ensure the three-way catalytic effect of the downstream coating layer to reduce hot HC.
[0150] From the above viewpoints, (the amount of Pd in the upper coating on the upstream side) / (the substrate 1L of the upstream upper coating forming part) can be more than 1.5 times, more than 2.0 times, more than 2.5 times, more than 3.0 times, more than 3.5 times, or more than 4.0 times the (amount of Pd in the lower coating on the downstream side) / (the substrate 1L of the downstream lower coating forming part), and can be less than 10.0 times, less than 8.0 times, less than 7.0 times, less than 6.0 times, or less than 5.0 times.
[0151] The upstream upper coating layer and the downstream lower coating layer may be substantially free of Rh. These coating layers substantially free of Rh means that the amount of Rh in these coating layers is 0.020 g / L or less, 0.010 g / L or less, 0.005 g / L or less, 0.003 g / L or less, or 0.001 g / L or less relative to 1 L of the substrate of the coating layer forming portion, and may be completely free of Rh.
[0152] The upstream side lower coating layer and the downstream side upper coating layer may each contain Rh.
[0153] The amount of Rh in these coatings, calculated as (the amount of Rh in each coating) / (1L of the substrate forming the portion of each coating), can be greater than 0.05 g / L, greater than 0.10 g / L, greater than 0.15 g / L, or greater than 0.20 g / L, and can be less than 0.40 g / L, less than 0.35 g / L, less than 0.30 g / L, less than 0.25 g / L, or less than 0.20 g / L.
[0154] The ratio (weight ratio) of (the amount of Rh in the lower coating layer on the upstream side) / (the substrate 1L of the portion forming the lower coating layer on the upstream side) to (the amount of Rh in the upper coating layer on the downstream side) / (the substrate 1L of the portion forming the upper coating layer on the downstream side) can be in the range of 1.0:2.0 to 2.0:1.0, in the range of 1.0:1.5 to 1.5:1.0, or in the range of 1.0:1.2 to 1.2:1.0.
[0155] The upstream lower coating layer and the downstream upper coating layer may be substantially free of Pt and Pd, respectively. These coating layers substantially free of Pt and Pd means that the total amount of Pt and Pd in these coating layers is 0.020 g / L or less, 0.010 g / L or less, 0.005 g / L or less, 0.003 g / L or less, or 0.001 g / L or less relative to 1 L of the substrate of the coating-forming portion, and may be completely free of Pt and Pd.
[0156] The catalytic noble metal in each coating layer may be supported on one or two or more inorganic oxides described below. Typically, the catalytic noble metal in the coating layer may be supported on one or two or more inorganic oxide particles in the form of fine particles.
[0157] (Optional ingredient)
[0158] The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer and the downstream upper coating layer may each contain any component other than the catalyst noble metal, such as inorganic oxides, promoters, binders and the like.
[0159] Inorganic oxides
[0160] The inorganic oxide may be an oxide of one or more elements selected from, for example, Al, Si, Ti, Zr, Ce, La, Pr, Nd, Y, etc. When the inorganic oxide is an oxide of two or more elements, it may be a mixture of multiple inorganic oxides, a composite oxide containing multiple elements, or an inorganic oxide in a form containing both. Specifically, for example, it may be aluminum oxide, silicon dioxide, titanium dioxide, silicon dioxide-alumina composite oxide, ceria, zirconium oxide, ceria-zirconia composite oxide (CZ), etc. These inorganic oxides may be composite oxides doped with rare earth elements (La, Pr, Nd, Y, etc.) other than Ce.
[0161] Each coating layer may contain a material having oxygen storage capacity (OSC material). When the coating layer contains the OSC material, the OSC material's atmosphere moderation capability enables catalytic purification of HC even when the gas is rich, and in particular contributes to the reduction of hot HC.
[0162] The OSC material is typically ceria. Ceria can be contained in each coating layer in the form of ceria alone or in the form of a composite oxide containing ceria. The composite oxide containing ceria can be, for example, CZ, or CZ doped with a rare earth element.
[0163] At least the downstream lower coating layer may contain ceria. If the downstream lower coating layer contains ceria, the atmosphere can be moderated without hindering the metallization of Rh in the downstream upper coating layer, thereby promoting the three-way catalytic effect brought about by the downstream coating layer and contributing to the reduction of hot HC and hot NOx.
[0164] In order to fully exert the atmosphere moderation ability, the amount of cerium dioxide in the downstream lower coating layer can be more than 10 g / L, 20 g / L or more, 30 g / L or more, 40 g / L or more, 45 g / L or more, 50 g / L or more, or 55 g / L or more relative to 1L of the substrate where the downstream lower coating layer is formed. On the other hand, in order to maintain the effective pore volume of the substrate and avoid the useless increase of the exhaust back pressure, the amount of cerium dioxide in the downstream lower coating layer can be less than 100 g / L, less than 90 g / L, less than 80 g / L, less than 75 g / L, less than 70 g / L, or less than 65 g / L relative to 1L of the substrate where the downstream lower coating layer is formed.
[0165] In order not to hinder the metallization of Rh present in the downstream upper coating layer, the amount of ceria in the downstream upper coating layer may be 12 g / L or less, 10 g / L or less, 9 g / L or less, or 8 g / L or less relative to 1 L of the substrate where the downstream upper coating layer is formed. On the other hand, in order to maintain the reduction purification activity of Rh even in dilute conditions, and for the purpose of imparting a certain atmosphere mitigation capability to the downstream upper coating layer, the amount of ceria in the downstream upper coating layer may be 1 g / L or more, 2 g / L or more, 3 g / L or more, 4 g / L or more, or 5 g / L or more relative to 1 L of the substrate where the downstream upper coating layer is formed.
[0166] In order to improve the atmosphere moderation ability of the downstream side coating without hindering the metallization of Rh present in the upper coating on the downstream side, the total amount of cerium dioxide in the upper and lower layers on the downstream side can be 12 g / L or more, 20 g / L or more, 30 g / L or more, 40 g / L or more, 50 g / L or more, 55 g / L or more, 60 g / L or more, or 65 g / L or more, and can be 110 g / L or less, 100 g / L or less, 90 g / L or less, 80 g / L or less, 75 g / L or less, or 70 g / L or less.
[0167] In order not to hinder the metallization of Rh present in the upstream lower coating layer, and to maintain the oxidation activity of the upstream coating layer, and in particular to effectively reduce cold emissions, the amount of cerium dioxide in the upstream lower coating layer may be 10 g / L or less, 9 g / L or less, or 8 g / L or less relative to 1L of the substrate where the upstream lower coating layer is formed. On the other hand, in order to exert the reduction purification activity of Rh in dilute conditions, and for the purpose of also imparting a certain atmosphere mitigation capability to the upstream lower coating layer, the amount of cerium dioxide in the upstream lower coating layer may be 1 g / L or more, 2 g / L or more, 3 g / L or more, 4 g / L or more, or 5 g / L or more relative to 1L of the substrate where the upstream lower coating layer is formed.
[0168] In order to give the upstream coating layer an atmosphere moderating capability, the upstream upper coating layer may also contain ceria. However, in order to maintain the oxidation activity of the upstream coating layer and seek effective reduction of cold emissions, the amount of ceria in the upstream upper coating layer may also be limited, for example, relative to 1L of the substrate forming the upstream upper coating layer, it may be 60g / L or less, 50g / L or less, 40g / L or less, 30g / L or less, 20g / L or less, 15g / L or less, 10g / L or less, 5g / L or less, 3g / L or less, or 1g / L or less, or the upstream upper coating layer may not contain ceria.
[0169] In order not to hinder the metallization of Rh present in the downstream upper coating layer and the upstream lower coating layer, and to maintain the oxidation activity of the upstream coating layer, and to effectively reduce cold HC, the concentration of cerium dioxide in the upstream lower coating layer, the concentration of cerium dioxide in the upstream upper coating layer, and the concentration of cerium dioxide in the downstream upper coating layer can be independently 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 25% or less, 20% or less, 15% or less, or 10% or less of the concentration of cerium dioxide in the downstream lower coating layer. In particular, the concentration of cerium dioxide contained in the upstream upper coating layer can be 8% or less, 5% or less, 3% or less, 1% or less, or 0.5% or less of the concentration of cerium dioxide in the downstream lower coating layer, or can also be 0%. In the above, the concentration of cerium dioxide in the coating layer refers to the mass ratio of the amount of cerium dioxide in the coating layer relative to the substrate 1L of the coating layer forming portion.
[0170] In order to maintain the oxidation activity of the upstream coating and seek effective reduction of cold HC, the concentration of ceria in the upstream coating can be 65% or less, 60% or less, 50% or less, 40% or less, 25% or less, 30% or less, 20% or less, or 15% or less relative to the concentration of ceria in the downstream coating. On the other hand, in order to impart the required atmospheric oxidation capacity to the upstream coating so that the upstream coating can contribute to the reduction of cold HC through the three-way catalytic function, the concentration of ceria in the upstream coating can be 1% or more, 3% or more, 5% or more, 7% or more, or 10% or more of the concentration of ceria in the downstream coating. In the above, the concentration of ceria in the coating refers to the mass ratio of the total amount of ceria in the upper and lower layers of the coating relative to the substrate 1L of the coating forming part.
[0171] The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer, and the downstream upper coating layer may each contain aluminum oxide. Aluminum oxide may be contained in each coating layer in the form of aluminum oxide alone or in the form of a composite oxide containing aluminum oxide. The composite oxide containing aluminum oxide may be, for example, a silicon dioxide-aluminum oxide composite oxide or aluminum oxide doped with a rare earth element. The rare earth element doped in aluminum oxide may be, for example, La, Pr, Nd, Y, etc., and may be La in particular.
[0172] The catalytic noble metal contained in each coating layer may be supported on one or two or more of the above-mentioned inorganic oxides. Typically, the catalytic noble metal may be supported on the surface of one or two or more particles of the inorganic oxides in the form of fine particles.
[0173] Catalyst
[0174] Each coating may also contain a promoter.
[0175] The promoter contained in the coating layer of the exhaust gas purification catalyst device of the present invention may be, for example, an alkali metal compound, an alkaline earth metal compound, etc. Typically, it may be a strong acid salt of an alkali metal or an alkaline earth metal, for example, barium sulfate.
[0176] Adhesives
[0177] The binder contained in the coating layer of the exhaust gas purification catalyst device of the present invention may be, for example, a sol of an inorganic oxide, typically an alumina sol, a zirconia sol, a titania sol or the like.
[0178] Method for manufacturing exhaust gas purification catalyst device
[0179] The exhaust gas purification device of the present invention can be manufactured by a known method, a method obtained by appropriately modifying a known method by a person skilled in the art, or a method combining these methods.
[0180] The following Figure 1 The exhaust gas purification catalyst device (100) shown in Figure 2 A specific example of the manufacturing method thereof will be described by taking the exhaust gas purification catalyst device (200) shown in FIG. 1 as an example. However, the method of manufacturing the exhaust gas purification device of the present invention is not limited thereto.
[0181] In manufacturing Figure 1 In the case of the exhaust gas purification catalyst device (100) shown in , first, a substrate (110) corresponding to a substrate of a desired exhaust gas purification catalyst device (100) is prepared.
[0182] Next, an upstream lower coating layer (121) and a downstream lower coating layer (131) are formed on the substrate (110). The order in which the upstream lower coating layer (121) and the downstream lower coating layer (131) are formed can be any order. Next, the desired exhaust purification catalyst device (100) is obtained by forming an upstream upper coating layer (122) on the upstream lower coating layer (121) and forming a downstream upper coating layer (132) on the downstream lower coating layer (131). The order in which the upstream upper coating layer (122) and the downstream upper coating layer (132) are formed can be any order.
[0183] In order to form each coating layer, the following method can be used: apply each coating layer forming coating liquid on the substrate or the lower coating layer in a prescribed coating range, dry it as needed, and then sinter it. Each coating layer forming coating liquid can be a catalyst metal precursor, an inorganic oxide, or any other component, such as an aqueous dispersion, containing a prescribed type and amount. The catalyst noble metal precursor can be appropriately selected from the desired catalyst noble metal nitrate, sulfate, chloride, complex, etc., which is soluble in a solvent (such as water).
[0184] The firing may be performed in one go after the coating liquids for all the layers are applied, or may be performed in multiple steps such that the coating liquids for some layers are applied and fired, and then the coating liquids for other layers are applied and fired.
[0185] In manufacturing Figure 2 In the case of the exhaust gas purification catalyst device (200) shown in , first, a substrate (210) corresponding to a substrate of a desired exhaust gas purification catalyst device (200) is prepared.
[0186] Next, a downstream side lower layer coating (231) is formed on the substrate (210).
[0187] Next, an Rh layer (240) is formed on the substrate on which the downstream side lower coating layer (231) is formed. The Rh layer (240) is a coating layer formed by connecting an upstream side lower coating layer (221) formed directly on the substrate (210) on the upstream side of the exhaust flow and a downstream side upper coating layer (232) formed on the downstream side lower coating layer (231) on the downstream side of the exhaust flow.
[0188] Then, an upstream upper coating layer (222) is formed on the upstream lower coating layer (221) located on the upstream side of the exhaust gas flow in the Rh layer (240), thereby obtaining Figure 2 An exhaust gas purification catalyst device (200) is provided.
[0189] The formation of each coating can be made with Figure 1 The process is carried out in the same manner as the exhaust gas purification catalyst device (100) shown in FIG. 1 , or by adopting a method to which appropriate changes have been made by a person skilled in the art.
[0190] Example
[0191] In the following Examples and Comparative Examples, a cylindrical cordierite direct current type honeycomb substrate having a capacity of about 1 L was used as a substrate.
[0192] The components used in the preparation of the coating liquid are as follows.
[0193] Rh precursor: rhodium chloride
[0194] Pd precursor: palladium nitrate
[0195] Alumina: Composite Al2O3 containing La
[0196] OSC material A: CZ composite oxide containing La, Pr, Nd and Y (cerium dioxide content of 60 mass%)
[0197] OSC material B: CZ composite oxide containing La, Pr, Nd and Y (cerium dioxide content is 20 mass%)
[0198] Co-catalyst: barium sulfate
[0199] Binder: Alumina sol
[0200] Example 1
[0201] 1.Manufacture of exhaust gas purification catalyst device
[0202] (1) Preparation of coating liquid
[0203] A coating liquid for forming a downstream lower Pd layer was prepared by mixing 1.45 g of palladium nitrate (equivalent to 0.67 g in terms of metal Pd), 40.20 g of alumina, 67.00 g of OSC material A (equivalent to 40.20 g of cerium dioxide), 6.70 g of barium sulfate and 3.35 g of alumina sol in distilled water and performing wet grinding using a bead mill.
[0204] The types and amounts of the components used were set to the types and amounts described in Table 1, respectively. In addition, the coating liquid for forming the upstream lower Rh layer, the coating liquid for forming the downstream upper Rh layer, and the coating liquid for forming the upstream upper Pd layer were prepared respectively by the same method as the preparation of the coating liquid for forming the downstream lower Pd layer mentioned above.
[0205] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0206] At the downstream end of the exhaust flow of the substrate, the coating liquid for forming the downstream lower Pd layer obtained in the above process was arranged, and the coating liquid for forming the downstream lower Pd layer was sucked from the upstream end by a suction device to apply the coating liquid to a region of 67% of the length of the substrate from the downstream end of the substrate. Next, at the upstream end of the exhaust flow of the substrate after the coating liquid for forming the downstream lower Pd layer was applied, the coating liquid for forming the upstream lower Rh layer was arranged, and the coating liquid for forming the upstream lower Rh layer was sucked from the downstream end by a suction device to apply the coating liquid to a region of 33% of the length of the substrate from the upstream end of the substrate. Then, the coated substrate was calcined at 500° C. for 2 hours in the atmosphere, thereby forming a lower layer consisting of the downstream Pd layer and the upstream Rh layer on the substrate.
[0207] At the downstream end of the exhaust flow of the substrate after the lower layer is formed, the coating liquid for forming the downstream upper Rh layer obtained in the above is arranged, and the coating liquid for forming the downstream upper Rh layer is sucked from the upstream end by a suction device to apply the coating liquid for forming the downstream upper Rh layer to an area of 67% of the length of the substrate from the downstream end of the substrate having the lower layer. Next, at the upstream end of the exhaust flow of the substrate after the coating liquid for forming the downstream upper Rh layer is applied, the coating liquid for forming the upstream upper Pd layer is arranged, and the coating liquid for forming the upstream upper Pd layer is sucked from the downstream end by a suction device to apply the coating liquid for forming the upstream upper Pd layer to an area of 33% of the length of the substrate from the upstream end of the substrate. Then, by firing the coated substrate at 500° C. for 2 hours in the atmosphere, an upper layer consisting of the downstream Rh layer and the upstream Pd layer is formed on the lower layer on the substrate, thereby obtaining the exhaust gas purification catalyst device of Example 1.
[0208] In the exhaust purification catalyst device obtained here, the Pd density of the upper layer (upstream upper Pd layer) in the upstream side region (the region of 33% of the substrate length from the upstream end) of the catalyst coating (the amount of Pd in the upstream upper Pd layer / 1L of the substrate forming the upstream upper Pd layer) is 4.00g / L-region.
[0209] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 5 (A).
[0210] (3) Evaluation of exhaust gas purification catalyst device
[0211] The exhaust gas purification catalyst device obtained in the above was subjected to a durability test under rich and lean alternating conditions for a duration equivalent to 150,000 miles.
[0212] The exhaust gas purification catalyst device after durability was installed in a vehicle compliant with the ULEV70 standard equipped with a gasoline engine with an exhaust volume of 2000 mL, and a test was carried out in the FTP75 driving mode to measure the NMOG (non-methane organic gas) and NOx emissions in each stage of Bag 1 to Bag 3.
[0213] The exhaust gas purification catalyst device samples were mounted just below the engine, and no underfloor catalyst was mounted in order to facilitate comparison of the samples.
[0214] In addition, Bag 1 is a cold start phase, Bag 2 is a transient phase, and Bag 3 is a hot start phase. Therefore, NMOG emissions in Bag 1 are equivalent to cold HC emissions, and the sum of NOx emissions in Bag 2 and Bag 3 is equivalent to hot NOx emissions.
[0215] Table 2 shows the evaluation results of the exhaust gas purification catalyst device.
[0216] Comparative Example 1 and Comparative Example 2
[0217] (1) Preparation of coating liquid
[0218] A lower layer forming coating liquid and an upper layer forming coating liquid were prepared in the same manner as in Example 1 except that the types and amounts of the components used were those shown in Table 1, respectively.
[0219] The coating liquid for forming the lower layer prepared here is a coating liquid for forming the lower Pd layer in Comparative Example 1, and is a coating liquid for forming the lower Rh layer in Comparative Example 2;
[0220] The coating liquid for forming the upper layer is the coating liquid for forming the upper Rh layer in Comparative Example 1, and is the coating liquid for forming the upper Pd layer in Comparative Example 2.
[0221] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0222] The coating liquid for forming the lower layer obtained in the above process was placed at the downstream end of the exhaust gas flow of the substrate, and the coating liquid for forming the lower layer was applied to 100% of the length of the substrate by sucking it from the upstream end with a suction device. Then, the coated substrate was calcined at 500° C. for 2 hours in the atmosphere, thereby forming the lower layer on the substrate.
[0223] The coating liquid for forming the upper layer obtained in the above was arranged at the downstream end of the exhaust gas flow of the substrate after the lower layer was formed, and the coating liquid for forming the upper layer was applied to the area of 100% of the length of the substrate from the downstream end of the substrate having the lower layer by sucking it from the upstream end with an aspirator. Then, the coated substrate was calcined at 500° C. for 2 hours in the atmosphere to form the upper layer on the lower layer on the substrate, thereby obtaining the exhaust gas purification catalyst devices of Comparative Examples 1 and 2, respectively.
[0224] The structures of the catalyst coating layers of the exhaust gas purification catalyst device obtained here are shown in Figure 5 (B) and Figure 5 (C).
[0225] (3) Evaluation of exhaust gas purification catalyst device
[0226] Using each of the exhaust gas purification catalyst devices obtained as described above, evaluation was performed in the same manner as in Example 1. Table 2 shows the evaluation results.
[0227] Comparative Example 3
[0228] (1) Preparation of coating liquid
[0229] The types and amounts of the components used were set to the types and amounts described in Table 1, respectively. In addition, the coating liquid for forming the downstream lower Pd layer, the coating liquid for forming the upstream lower Pd layer, and the coating liquid for forming the upper Rh layer were prepared in the same manner as in Example 1.
[0230] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0231] At the downstream end of the exhaust flow of the substrate, the coating liquid for forming the downstream lower Pd layer obtained in the above was arranged, and the coating liquid for forming the downstream lower Pd layer was sucked from the upstream end by an aspirator to apply the coating liquid for forming the downstream lower Pd layer to an area of 67% of the length of the substrate from the downstream end of the substrate. Next, at the upstream end of the exhaust flow of the substrate after the coating liquid for forming the downstream lower Pd layer was applied, the coating liquid for forming the upstream lower Pd layer was arranged, and the coating liquid for forming the upstream lower Pd layer was sucked from the downstream end by an aspirator to apply the coating liquid for forming the upstream lower Pd layer to an area of 33% of the length of the substrate from the upstream end of the substrate. Then, by calcining the coated substrate at 500°C for 2 hours in the atmosphere, a lower layer consisting of the downstream Pd layer and the upstream Pd layer was formed on the substrate.
[0232] The coating liquid for forming the upper Rh layer obtained in the above was placed at the downstream end of the exhaust gas flow of the substrate after the lower layer was formed, and the coating liquid for forming the upper Rh layer was applied to the area of 100% of the length of the substrate from the downstream end of the substrate having the lower layer by sucking it from the upstream end with a sucker. Then, the coated substrate was calcined at 500° C. for 2 hours in the atmosphere to form the upper Rh layer on the lower layer on the substrate, thereby obtaining the exhaust gas purification catalyst device of Comparative Example 3.
[0233] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 5 (D).
[0234] (3) Evaluation of exhaust gas purification catalyst device
[0235] Using the exhaust gas purification catalyst device obtained as described above, evaluation was carried out in the same manner as in Example 1. Table 2 shows the evaluation results.
[0236] Comparative Example 4
[0237] (1) Preparation of coating liquid
[0238] The types and amounts of the components used were set to the types and amounts described in Table 1, respectively. In addition, the coating liquid for forming the lower Pd layer, the coating liquid for forming the downstream upper Rh layer, and the coating liquid for forming the upstream upper Pd layer were prepared in the same manner as in Example 1.
[0239] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0240] The coating liquid for forming the lower Pd layer obtained in the above process was placed at the downstream end of the exhaust gas flow of the substrate, and the coating liquid for forming the lower Pd layer was applied to the area of 100% of the length of the substrate by sucking it from the upstream end with an aspirator. Then, the coated substrate was fired at 500° C. for 2 hours in the atmosphere, thereby forming a lower layer on the substrate, which was a Pd layer.
[0241] At the downstream end of the exhaust flow of the substrate after the lower layer is formed, the coating liquid for forming the downstream upper Rh layer obtained in the above is arranged, and the coating liquid for forming the downstream upper Rh layer is sucked from the upstream end by a suction device to apply the coating liquid for forming the downstream upper Rh layer to an area of 67% of the length of the substrate from the downstream end of the substrate having the lower layer. Next, at the upstream end of the exhaust flow of the substrate after the coating liquid for forming the downstream upper Rh layer is applied, the coating liquid for forming the upstream upper Pd layer is arranged, and the coating liquid for forming the upstream upper Pd layer is sucked from the downstream end by a suction device to apply the coating liquid for forming the upstream upper Pd layer to an area of 33% of the length of the substrate from the upstream end of the substrate. Then, by calcining the coated substrate at 500°C for 2 hours in the atmosphere, an upper layer consisting of the downstream Rh layer and the upstream Pd layer is formed on the lower layer on the substrate, thereby obtaining the exhaust gas purification catalyst device of Comparative Example 4.
[0242] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 5 (E).
[0243] (3) Evaluation of exhaust gas purification catalyst device
[0244] Using the exhaust gas purification catalyst device obtained as described above, evaluation was carried out in the same manner as in Example 1. Table 2 shows the evaluation results.
[0245] Comparative Example 5
[0246] (1) Preparation of coating liquid
[0247] The types and amounts of the components used were set to the types and amounts described in Table 1, and the coating liquid for forming the lower Pd layer, the coating liquid for forming the upper Rh layer, and the coating liquid for forming the uppermost Pd layer on the upstream side were prepared in the same manner as in Example 1.
[0248] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0249] Using the coating liquid for forming the lower Pd layer and the coating liquid for forming the upper Rh layer obtained above, a lower layer and an upper layer were sequentially formed on a substrate in the same manner as in Comparative Example 1. The lower layer was a Pd layer, and the upper layer was a Rh layer.
[0250] At the exhaust gas flow upstream end of the substrate after the lower layer and the upper layer were formed, a coating liquid for forming the uppermost Pd layer on the upstream side was arranged, and the coating liquid for forming the uppermost Pd layer on the upstream side was applied to a region of 33% of the length of the substrate from the upstream end of the substrate by sucking it with an aspirator. Then, the coated substrate was fired at 500° C. for 2 hours in the atmosphere to form the uppermost Pd layer on the upper layer on the substrate, thereby obtaining the exhaust gas purification catalyst device of Comparative Example 5.
[0251] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 5 (F).
[0252] (3) Evaluation of exhaust gas purification catalyst device
[0253] Using the exhaust gas purification catalyst device obtained as described above, evaluation was carried out in the same manner as in Example 1. Table 2 shows the evaluation results.
[0254]
[0255] Table 1 (continued)
[0256]
[0257]
[0258] In the exhaust purification catalyst device of Comparative Example 1 in which the catalyst coating has a two-layer structure of a lower Pd layer and an upper Rh layer, and the components of the catalyst coating are uniformly arranged over 100% of the length of the substrate, the effect of reducing hot NOx emissions in post-durable emissions was confirmed, but the reduction in cold HC emissions was insufficient.
[0259] In addition, in the exhaust gas purification catalyst device of Comparative Example 2, in which the catalyst coating layer has a two-layer structure of a lower Rh layer and an upper Pd layer, and the components of the catalyst coating layer are uniformly arranged over 100% of the length of the substrate, cold HC emissions are reduced compared to the device of Comparative Example 1, but hot NOx emissions are greatly increased. This is believed to be caused by: the heat of the catalytic reaction causes the exhaust gas flow downstream side of the catalyst coating layer to become hotter, causing the Pd layer with low heat resistance to thermally deteriorate; and because the Rh layer having NOx reduction purification activity is arranged in the lower layer, the contact efficiency with the exhaust gas becomes poor, and the reaction efficiency becomes low.
[0260] The exhaust gas purification catalyst device of Comparative Example 3 has a structure in which the Pd layer of the lower layer is divided into the upstream side and the downstream side of the exhaust gas flow based on the device of Comparative Example 1, and the Pd concentration on the upstream side is increased. For this exhaust gas purification device, it is expected to maintain the effect of reducing hot NOx emissions of the device of Comparative Example 1 and reduce cold HC emissions. However, in the device of Comparative Example 3, the effect of reducing cold HC emissions is not sufficient. It is believed that this is because the reaction efficiency of Pd arranged in the lower layer and HC is low.
[0261] The exhaust gas purification catalyst device of Comparative Example 4 has a structure in which the upper layer is divided based on the device of Comparative Example 1, and a Pd layer is arranged on the upstream side of the exhaust gas flow. By arranging the Pd layer on the upstream side, the length of the upper Rh layer is shortened. In the device of Comparative Example 4, cold HC emissions are reduced to some extent by arranging Pd in the upper layer on the upstream side. However, compared with the device of Comparative Example 1, hot NOx emissions increase. It is believed that this is due to the shortening of the length of the upper Rh layer.
[0262] The exhaust gas purification catalyst device of Comparative Example 5 has a structure in which a Pd layer is added as the uppermost layer on the upstream side based on the device of Comparative Example 1. In the device of Comparative Example 5, cold HC emissions are reduced to some extent. However, hot NOx emissions are increased compared with the device of Comparative Example 1. It is believed that this is because the heat capacity of the catalyst coating is increased by additionally configuring the Pd layer as the uppermost layer on the upstream side, and the temperature rise performance is impaired.
[0263] Compared with these comparative examples, in the exhaust gas purification catalyst device of Example 1 having the configuration specified by the present invention, both cold HC emissions and hot NOx emissions are intentionally reduced. In addition, by reducing these emissions, the total emission of NMOG and NOx is also greatly reduced.
[0264] Embodiments 2 to 5
[0265] (1) Preparation of coating liquid
[0266] The coating liquids for forming each layer were prepared in the same manner as in Example 1 except that the amount of the OSC material A contained in the coating liquid for forming the upstream upper Pd layer was changed to the amount described in Table 3.
[0267] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0268] Using the coating liquid for forming each layer obtained above, a lower layer consisting of a downstream side Pd layer and an upstream side Rh layer, and an upper layer consisting of a downstream side Rh layer and an upstream side Pd layer are sequentially formed on a substrate in the same manner as in Example 1, thereby obtaining exhaust purification catalyst devices of Examples 2 to 5, respectively.
[0269] (3) Evaluation of exhaust gas purification catalyst device
[0270] Using each exhaust gas purification catalyst device obtained as described above, evaluation was performed in the same manner as in Example 1. The evaluation results of cold HC emissions (NMOG emissions in the Bag 1 stage) are shown in Table 4 together with the evaluation results of Example 1.
[0271]
[0272]
[0273] From the results of Table 3 and Table 4, the cold HC emission of the exhaust gas purification catalyst device of Examples 1 to 5 generally shows a low value. Among them, the following tendency is seen: the smaller the ratio of the ceria concentration in the upper layer on the upstream side to the ceria concentration in the lower layer on the downstream side, the lower the cold HC emission. In particular, in the exhaust gas purification catalyst devices of Examples 1 to 3 in which the ratio of the ceria concentration in the upper layer on the upstream side to the ceria concentration in the lower layer on the downstream side is less than 0.45, the cold HC emission is extremely low. It is believed that this is due to the following situation: since the amount of OSC material in the upstream side region, especially in the upper Pd layer on the upstream side, is reduced, the oxygen absorption caused by the OSC material is limited, so that the oxidation catalytic activity of Pd is maintained at a high state even when it is rich.
[0274] Embodiments 6 to 8
[0275] (1) Preparation of coating liquid
[0276] The coating liquids for forming each layer were prepared in the same manner as in Example 1 except that the amount of aluminum oxide contained in the coating liquid for forming the upstream upper Pd layer was changed to the amount described in Table 5.
[0277] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0278] Using the coating liquid for forming each layer obtained above, a lower layer consisting of a downstream side Pd layer and an upstream side Rh layer, and an upper layer consisting of a downstream side Rh layer and an upstream side Pd layer are sequentially formed on the substrate in the same manner as in Example 1, thereby obtaining the exhaust purification catalyst devices of Examples 6 to 8, respectively.
[0279] (3) Evaluation of exhaust gas purification catalyst device
[0280] Using each exhaust gas purification catalyst device obtained as described above, evaluation was performed in the same manner as in Example 1. The evaluation results of cold HC emissions (NMOG emissions in the Bag 1 stage) are shown in Table 6 together with the evaluation results of Example 1.
[0281]
[0282]
[0283] From the results of Table 5 and Table 6, the cold HC emissions of the exhaust gas purification catalyst devices of Example 1 and Examples 6 to 8 generally show low values. Among them, the following tendency is seen: the less the coating amount (total solid content) of the catalyst layer on the upper layer on the upstream side is, the lower the cold HC emissions are. In particular, in the exhaust gas purification catalyst devices of Example 1 and Example 6, in which the catalyst coating on the upper layer on the upstream side is less than 130 g / L, the cold HC emissions are extremely low. It is believed that this is due to the following situation: since the coating amount of the catalyst coating on the upper layer on the upstream side is reduced, the heat capacity is reduced, which becomes particularly advantageous in terms of the preheating properties of the Pd layer as the upper layer on the upstream side.
[0284] Example 9
[0285] (1) Preparation of coating liquid
[0286] The types and amounts of the components used were set to the types and amounts described in Table 7, and the coating liquid for forming the downstream lower Pd layer, the coating liquid for forming the Rh layer, and the coating liquid for forming the upstream upper Pd layer were prepared in the same manner as in Example 1.
[0287] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0288] The downstream side lower Pd layer forming coating liquid obtained in the above process was placed at the downstream end of the exhaust flow of the substrate, and the downstream side lower Pd layer forming coating liquid was sucked from the upstream end by a suction device to apply the downstream side lower Pd layer forming coating liquid to a region of 67% of the length of the substrate from the downstream end of the substrate. Next, the Rh layer forming coating liquid was placed at the upstream end of the exhaust flow of the substrate after the downstream side lower Pd layer forming coating liquid was applied, and the Rh layer forming coating liquid was sucked from the downstream end by a suction device to apply the Rh layer forming coating liquid to a region of 80% of the length of the substrate from the upstream end of the substrate. Furthermore, the upstream side upper Pd layer forming coating liquid was placed at the upstream end of the exhaust flow of the substrate after the downstream side lower Pd layer forming coating liquid and the Rh layer forming coating liquid were applied, and the upstream side upper Pd layer forming coating liquid was sucked from the downstream end by a suction device to apply the upstream side upper Pd layer forming coating liquid to a region of 33% of the length of the substrate from the upstream end of the substrate. Then, by sintering the coated substrate at 500°C for 2 hours in the atmosphere, an exhaust purification catalyst device of Example 9 is obtained, which has a downstream lower Pd layer, an Rh layer with a length of 80% of the substrate length from the upstream end, and an upstream upper Pd layer on the substrate in sequence.
[0289] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 6 (B).
[0290] (3) Evaluation of exhaust gas purification catalyst device
[0291] Using the exhaust gas purification catalyst device obtained as described above, evaluation was performed in the same manner as in Example 1. The evaluation results are shown in Table 8 together with the evaluation results of Example 1.
[0292] Example 10
[0293] (1) Preparation of coating liquid
[0294] In the same manner as in Example 9, coating liquids for forming each layer described in Table 7 were prepared.
[0295] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0296] The configuration position of the coating liquid for forming the Rh layer is set to the downstream end of the exhaust flow, and then the coating liquid for forming the Rh layer is applied to an area of 80% of the length of the substrate from the downstream end of the substrate by sucking it from the upstream end with an aspirator. Otherwise, the same procedure as in Example 9 is performed to obtain an exhaust purification catalyst device of Example 10 having, in sequence, a downstream side lower Pd layer, a Rh layer of 80% of the length of the substrate from the downstream end, and an upstream side upper Pd layer on the substrate.
[0297] The structure of the catalyst coating layer of the exhaust gas purification catalyst device obtained here is shown in Figure 6 (C).
[0298] (3) Evaluation of exhaust gas purification catalyst device
[0299] Using the exhaust gas purification catalyst device obtained as described above, evaluation was performed in the same manner as in Example 1. The evaluation results are shown in Table 8 together with the evaluation results of Example 1.
[0300]
[0301]
[0302] From the results of Tables 7 and 8, the following contents were found.
[0303] The exhaust gas purification catalyst device of Example 9, in which the Rh layer exists in the region of 80% of the substrate length from the upstream end of the substrate, has both NMOG and NOx emissions equivalent to those of the device of Example 1. Regarding the exhaust gas purification catalyst device of Example 9, it is considered that the amount of thermal NOx emissions increases because the Rh layer is not present in the region of 20% of the substrate length from the downstream end of the substrate. However, if the Rh layer exists in a length of about 80% of the substrate length, the influence of not having the Rh layer on the downstream side is small.
[0304] On the other hand, in the exhaust gas purification catalyst device of Example 10 in which the Rh layer exists in the region of 80% of the length of the substrate from the downstream end of the substrate, in particular, cold HC emissions and cold NOx emissions increase. The exhaust gas purification catalyst device of Example 10 does not have an Rh layer in the region of 20% of the length of the substrate from the upstream end of the substrate. It is considered that this leads to an increase in cold HC emissions and an increase in cold NOx emissions.
[0305] Examples 11 to 16
[0306] (1) Preparation of coating liquid
[0307] A coating liquid for forming a downstream lower Pd layer, a coating liquid for forming an upstream lower Rh layer, a coating liquid for forming an upstream upper Rh layer, and a coating liquid for forming an upstream upper Pd layer having the same compositions as the corresponding coating liquids in Example 1 were prepared respectively.
[0308] (2) Formation of Catalyst Coating (Manufacturing of Exhaust Gas Purification Catalyst Device)
[0309] Using the coating liquid for forming the downstream side lower Pd layer and the coating liquid for forming the upstream side lower Rh layer prepared above, a lower layer consisting of a downstream side Pd layer and an upstream side Rh layer was formed on the substrate in the same manner as in Example 1. Furthermore, using the coating liquid for forming the downstream side upper Rh layer, the coating liquid for forming the downstream side upper Rh layer was applied to the lower layer on the substrate in the same manner as in Example 1.
[0310] After the coating liquid for forming the upper Rh layer on the downstream side was applied to the lower layer, the coating liquid for forming the upper Pd layer on the upstream end of the exhaust gas flow of the substrate was placed, and the coating liquid for forming the upper Pd layer on the upstream side was sucked from the upstream end by an aspirator. At this time, the degree of suction was adjusted so that the coating length (d (%)) of the coating liquid for forming the upper Pd layer on the upstream side relative to the length of the substrate became the lengths recorded in Table 9. Then, the coated substrate was calcined at 500° C. for 2 hours in the atmosphere, thereby obtaining the exhaust gas purification catalyst devices of Examples 11 to 16, respectively.
[0311] The structures of the catalyst coating layers of the exhaust gas purification catalyst device obtained here are shown in Figure 7 (A)~(C).
[0312] (3) Evaluation of exhaust gas purification catalyst device
[0313] Using the exhaust gas purification catalyst device obtained as described above, evaluation was performed in the same manner as in Example 1. The evaluation results are shown in Table 9 together with the evaluation results of Example 1.
[0314] In Table 9, the coating length of the upstream upper Pd layer and the length of the portion of the downstream upper Rh layer that is not covered by the upstream upper Pd layer and can directly contact the exhaust are shown together as ratios relative to the substrate length ("to substrate length (%)").
[0315]
[0316] The following trends are seen from the results in Table 9.
[0317] The exhaust gas purification catalyst devices of Example 1 and Examples 11 to 16 are all excellent in reducing cold HC and hot NOx.
[0318] In particular, in the case of Example 1 and Examples 12 to 14 where the length of the upstream upper Pd layer is greater than 30% and less than 60% of the length of the substrate (therefore, the length of the portion of the downstream upper Rh layer that is not covered by the upstream upper Pd layer and can directly contact the exhaust gas is greater than 40% and less than 70% of the length of the substrate), the emissions of cold HC and hot NOx are greatly reduced.
[0319] Description of Reference Numerals
[0320] 100, 200, 300, 400: Exhaust purification catalyst device
[0321] 110, 210, 310, 410: Base material
[0322] 120, 220, 320, 420: Upstream side coating
[0323] 121, 221, 321, 421: Upstream side lower coating
[0324] 122, 222, 322, 422: Upstream side upper coating
[0325] 130, 230, 330, 430: Downstream coating
[0326] 131, 231, 331, 431: Downstream side lower coating
[0327] 132, 232, 332, 432: Downstream upper coating
[0328] 240: Rh layer
[0329] 422(a): Upstream part of the upper coating on the upstream side
[0330] 422(b): Downstream part of the upper coating on the upstream side
Claims
1. An exhaust gas purification catalyst device comprising a substrate and a catalyst coating on the substrate, The catalyst coating layer comprises an upstream coating layer arranged on the upstream side of the exhaust flow and a downstream coating layer arranged on the downstream side of the exhaust flow. The upstream coating layer comprises an upstream lower coating layer disposed on the substrate and an upstream upper coating layer disposed on the upstream lower coating layer. The downstream coating layer comprises a downstream lower coating layer disposed on the substrate and a downstream upper coating layer disposed on the downstream lower coating layer. The upstream lower coating layer, the upstream upper coating layer, the downstream lower coating layer, and the downstream upper coating layer each contain a catalyst noble metal selected from Pt, Pd, and Rh, Satisfying both (i) and (ii) below, (i) the concentration of one or both selected from Pt and Pd in the upstream upper coating layer and the downstream lower coating layer is higher than the concentration of one or both selected from Pt and Pd in the upstream lower coating layer, and higher than the concentration of one or both selected from Pt and Pd in the downstream upper coating layer; (ii) The concentrations of Rh in the upstream lower coating layer and the downstream upper coating layer are both higher than the concentration of Rh in the upstream upper coating layer and higher than the concentration of Rh in the downstream lower coating layer.
2. The exhaust gas purification catalyst device according to claim 1, At least the downstream lower coating layer comprises ceria, The ceria concentration in the upstream lower coating layer, the ceria concentration in the upstream upper coating layer, and the ceria concentration in the downstream upper coating layer are all 70% or less of the ceria concentration in the downstream lower coating layer.
3. The exhaust gas purification catalyst device according to claim 1, The amount of cerium dioxide in the upstream lower coating layer is 10 g / L or less relative to 1 L of the substrate of the upstream lower coating layer forming portion. The amount of ceria in the downstream-side upper coating layer is 10 g / L or less relative to 1 L of the substrate in the portion where the downstream-side upper coating layer is formed.
4. The exhaust gas purification catalyst device according to claim 1, The upstream side upper coating layer and the downstream side lower coating layer each contain Pd, The amount of Pd in the upstream upper coating layer relative to the upstream upper coating layer forming portion of the substrate 1L is 2.0 times or more the amount of Pd in the downstream lower coating layer relative to the downstream lower coating layer forming portion of the substrate 1L.
5. The exhaust gas purification catalyst device according to claim 2, The upstream side upper coating layer and the downstream side lower coating layer each contain Pd, The amount of Pd in the upstream upper coating layer relative to the upstream upper coating layer forming portion of the substrate 1L is 2.0 times or more the amount of Pd in the downstream lower coating layer relative to the downstream lower coating layer forming portion of the substrate 1L.
6. The exhaust gas purification catalyst device according to claim 3, The upstream side upper coating layer and the downstream side lower coating layer each contain Pd, The amount of Pd in the upstream upper coating layer relative to the upstream upper coating layer forming portion of the substrate 1L is 2.0 times or more the amount of Pd in the downstream lower coating layer relative to the downstream lower coating layer forming portion of the substrate 1L.
7. The exhaust gas purification catalyst device according to any one of claims 1 to 6, The total length of the upstream side lower coating layer and the downstream side upper coating layer is at least 80% of the length of the substrate.
8. The exhaust gas purification catalyst device according to any one of claims 1 to 6, There is no region in the vicinity of the end portion on the upstream side of the exhaust gas flow where the upstream upper coating layer is directly disposed on the substrate without interposing the upstream lower coating layer therebetween.
9. The exhaust gas purification catalyst device according to any one of claims 1 to 6, The length of the upstream coating layer is not less than 20% and not more than 50% of the length of the substrate.
10. The exhaust gas purification catalyst device according to any one of claims 1 to 6, The coating amount of the upstream coating layer is 240 g / L or less relative to 1 L of the substrate at the upstream coating layer forming portion.
11. The exhaust gas purification catalyst device according to any one of claims 1 to 6, The coating amount of the upstream-side upper coating layer is 160 g / L or less relative to 1 L of the substrate at the upstream-side upper coating layer forming portion.