A high temperature resistant titanium alcoholate hydrolysis organic base catalyst and its preparation method and application

By using a nitrogen-containing organic base-modified titanium alkoxide catalyst in polyester synthesis, the problems of poor hydrolysis stability and by-product generation of catalysts at high temperatures are solved, and efficient catalytic and high-quality polyester production are achieved.

CN116589670BActive Publication Date: 2024-11-05ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310793981.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-11-05
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

The catalyst is easy to hydrolyze during the existing polyester synthesis process, especially at high temperatures, which leads to problems such as decreasing catalytic activity, deteriorating polyester quality and equipment scaling, and it is difficult to effectively inhibit the formation of by-product tetrahydrofuran and reduce the polyester end carboxyl group. content.

Method used

Using a high-temperature hydrolysis titanium alkoxide organic base catalyst, the hydrolysis stability and solubility of the catalyst are improved by adding nitrogen-containing organic base to the titanium alkoxide catalyst, and the combination of titanium compounds with specific structures of diols and organic bases is formed. The stable six-membered ring structure enhances the catalyst's hydrolysis resistance.

Benefits of technology

It significantly improves the high-temperature hydrolysis stability of the catalyst, inhibits the formation of the by-product tetrahydrofuran, reduces the end carboxylic content of the polyester, and obtains polyester products with high intrinsic viscosity and low-end carboxylic content, solving the catalyst activity and quality problems .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589670B_ABST
    Figure CN116589670B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polyester catalysts, and discloses a high temperature resistant hydrolysis alcohol titanium organic base catalyst and its preparation method and application, the catalyst comprises a titanium compound, a diol containing an ortho-hydroxyl group and an organic base, the molar ratio of the titanium compound to the diol containing an ortho-hydroxyl group is 1:4-100; the molar ratio of the titanium compound to the organic base is 1:0.5-8. The preparation method is to react the titanium compound, the diol containing an ortho-hydroxyl group and the organic base under the conditions of 160-180°C nitrogen protection or 60-160°C and 10-0.2kPa. The catalyst of the present invention has excellent high temperature hydrolysis resistance and high catalytic activity, is applied to catalytic synthesis of polyester esters, especially polybutylene terephthalate and copolyesters thereof, can effectively inhibit the generation of byproduct THF, and the obtained polyester has a low content of terminal carboxyl groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester synthesis, and in particular to a high temperature resistant hydrolysis titanium alcoholate organic base catalyst and a preparation method and application thereof. Background Art

[0002] Thermoplastic polyesters such as polyethylene terephthalate (PET), polypropylene terephthalate (PPT), and polybutylene terephthalate (PBT) are widely used in the fields of automobile manufacturing, electronic and electrical manufacturing, optical fiber sleeves, office supplies, and fiber textiles due to their excellent heat resistance, chemical corrosion resistance, and insulation properties. Aliphatic-aromatic copolyesters are a widely used biodegradable material that combines the good biodegradability of aliphatic polyesters (such as polybutylene succinate, PBS) with the high melting point, fast crystallization rate, and excellent mechanical properties of aromatic polyesters (such as PBT). The copolyester synthesized by reacting terephthalic acid (TPA) which is an aromatic dibasic acid and succinic acid (SA) which is a fatty acid with 1,4-butanediol is poly(terephthalic acid-co-butylene succinate), referred to as PBST; the copolyester synthesized by reacting TPA and adipic acid (AA) which is a fatty acid with 1,4-butanediol is poly(terephthalic acid-co-butylene adipate), referred to as PBAT.

[0003] Catalysts commonly used in the synthesis of PBT and its copolyesters in the prior art include tin catalysts, titanium catalysts, etc. Among them, titanium catalysts show obvious advantages in the synthesis of polyesters such as PBT and copolyesters, such as low price, low toxicity, high activity, etc. Currently reported titanium polyester catalysts include inorganic titanium such as titanium dioxide and organic titanium such as alkoxy titanium and chelated titanium.

[0004] At present, titanium alkoxides such as tetrabutyl titanate (TBT), tetraisopropyl titanate (TPT) and other highly active titanium catalysts have been successfully used in the industrial production of PBT and its copolyesters. Since polyester raw materials contain a certain amount of water, especially diols are easy to absorb water, and the reaction process, especially the esterification process, will also produce water, so the esterification reaction system contains a certain amount of water. Compared with other catalysts, titanium alkoxides are prone to hydrolysis during the polyester synthesis process, especially the esterification process, to produce titanium dioxide and titanium polymers and precipitate and become inactive. The hydrolysis precipitate will not only remain in the PBT resin, causing quality problems such as deterioration of its fog value and increase of impurities, but also will be deposited on the inner surface of the equipment, gradually causing problems such as poor heat transfer effect and pipeline blockage.

[0005] In order to improve the hydrolysis resistance of titanate, major polyester companies have conducted a lot of research. For example, in order to inhibit the hydrolysis of catalysts in the polyester synthesis process, the British Imperial Chemical Company (CN1610580A) used hydroxycarboxylic acid as a complex to react with titanate. The modified titanium catalyst obtained was stable to water and could maintain catalytic activity well during the PET synthesis process. The American DuPont Company (CN1402653A) also proposed to react multifunctional organic matter (such as polyol amine, hydroxycarboxylic acid, polycarboxylic acid, condensed polycarboxylic acid) with titanate to improve the hydrolysis stability of titanate.

[0006] There are also studies that use ethylene glycol with bifunctional groups contained in the polymerization reaction system as a ligand to synthesize a new type of polyester catalyst with anti-hydrolysis performance - ethylene glycol titanium. Since ethylene glycol and titanium form a five-membered ring chelate structure with high thermodynamic stability, it will have good anti-hydrolysis properties and can show good catalytic effects in the polycondensation process. Patent CN1786044A uses ethylene glycol titanium to synthesize a PET copolyester product with a neutral tone, a characteristic viscosity of 0.65-0.85dL / g, and good transparency.

[0007] However, titanium glycolate is a solid catalyst with low solubility in alcohol and poor dispersibility, which is prone to catalyst agglomeration. For this reason, patent CN104327260A adopts the addition of IA group metal hydroxide to the titanium glycol catalyst, and the solubility of the catalyst in ethylene glycol is significantly improved. It has high catalytic activity for the depolymerization of ethylene glycol of polyesters such as PET and the copolymerization of the depolymerization products to synthesize PBAT, but the resulting polyester has poor color. Patent CN102924698A adds acetates of metal elements and phosphorus compounds to the synthesis process of titanium glycol catalyst to obtain a uniform liquid catalyst. When the catalyst is used to synthesize PBT, it has high activity, and the synthesized slices have excellent properties such as hue and thermal stability, but the tetrahydrofuran generated by the side reaction is too much.

[0008] Patents CN105085889A and CN103665349A use alkoxy titanium and 1,4-butanediol to prepare butanediol-coordinated chelated titanium catalysts. Unlike ethylene glycol titanium, butanediol titanium is liquid and has better hydrolysis stability than alkoxy titanium. The use of butanediol titanium to synthesize PBT shows high catalytic activity, but the resulting PBT intrinsic viscosity is still less than 1.0 dL / g.

[0009] Although the water resistance of the above-mentioned titanium alkoxide catalysts is better than that of titanium alkoxide at room temperature, there is no report on their hydrolysis stability at high temperature, i.e., the actual esterification or polycondensation reaction temperature. In fact, these titanium alkoxide catalysts produce white hydrolysis precipitates within 30 minutes of heating and reflux (about 210°C) in an aqueous BDO solution, indicating that the hydrolysis stability is still poor in the application environment of the catalyst, i.e., at the esterification temperature of 180-230°C, and a series of problems such as catalyst activity reduction, polyester quality deterioration, equipment fouling, etc. caused by catalyst hydrolysis still occur.

[0010] In the synthesis process of polyester or copolyester with the participation of 1,4-butanediol (BDO), especially in the esterification process, tetrahydrofuran (THF) is inevitably generated as a byproduct. At present, in the synthesis process of polyester or copolyester with the participation of 1,4-butanediol (BDO), the THF yield (calculated based on BDO) is often as high as 10% or even 15%. The generation of too much THF not only leads to the consumption of BDO raw materials, but also leads to a decrease in the actual alcohol-acid ratio, thereby reducing the esterification rate. Therefore, inhibiting the side reaction of THF generation is beneficial to the synthesis of polyester. At present, there is still a lack of polyester catalysts that have both high temperature hydrolysis stability and high catalytic activity and effectively inhibit THF generation (THF yield is less than 8%, or even less than 4%).

[0011] The polyester synthesized by esterification-polycondensation or transesterification-polycondensation of dibasic acid or its diester and excess diols is theoretically hydroxyl at its terminal groups. However, due to incomplete esterification, thermal decomposition at high temperature and other reasons (especially the latter), polyester products contain not only terminal hydroxyl groups but also a large number of terminal carboxyl groups. At present, the terminal carboxyl content of industrially produced polyesters is often high. For example, the national standards for PBT and PBAT stipulate that the terminal carboxyl content is below 50 mol / t, which is qualified. The actual terminal carboxyl content of commercial polyesters is mostly above 25 mol / t, or even above 30-40 mol / t. The presence of terminal carboxyl groups has an adverse effect on the processing stability, storage stability and durability of polyesters. At present, there is still a lack of polyester catalysts that have both high temperature hydrolysis stability and high catalytic activity and can effectively reduce the terminal carboxyl content of polyesters (below 15 mol / t, or even below 10 mol / t).

[0012] In summary, the development of a liquid titanium-based catalyst that has excellent hydrolysis stability, especially high-temperature hydrolysis stability, maintains high activity, can effectively inhibit the formation of THF, and effectively reduce the terminal carboxyl content of polyester is still a technical problem that needs to be solved. Summary of the invention

[0013] The present invention aims at the problem that the catalyst in the polyester synthesis process is easy to hydrolyze in the prior art, and provides a high-temperature resistant hydrolysis titanium alcoholate organic base catalyst. Compared with alkoxy titanium or titanium alcohol catalysts, the hydrolysis stability of the catalyst is greatly improved, especially the hydrolysis stability at high temperature. When used for synthesizing polyester, not only can a product with a high intrinsic viscosity be obtained, but also the generation of by-product THF can be effectively suppressed, and the acid value of the polyester product can be reduced.

[0014] To achieve the above object, the technical solution adopted by the present invention is:

[0015] A high temperature resistant titanium alcoholate hydrolysis organic base catalyst, comprising a titanium compound, an ortho-hydroxyl group-containing diol as shown in formula I, and an organic base;

[0016]

[0017] Wherein, R1 and R2 are independently selected from H, CH3, CH2CH3, CH2CH2CH3 or CH2CH2CH2CH3; the molar ratio of the titanium compound to the diol containing ortho-hydroxyl group is 1:4-100; the molar ratio of the titanium compound to the organic base is 1:0.5-8.

[0018] The present invention uses a nitrogen-containing organic base as a functional component and adds it to a titanium alcohol catalyst. It is found that the organic base can greatly improve the solubility of the titanium alcohol catalyst in the diol, and can significantly improve the hydrolysis stability of the catalyst while maintaining excellent catalytic activity. Polyesters with very excellent comprehensive properties can be synthesized by catalysis, especially PBT resins and copolyesters synthesized by catalysis have high intrinsic viscosity and low terminal carboxyl content, which overcomes the problem in the prior art that it is difficult to simultaneously achieve multiple properties such as high activity and hydrolysis stability, fluidity, selectivity (i.e., the ability to inhibit side reactions).

[0019] The chemical formula of the titanium compound is Ti(OR)4, wherein R is selected from a linear or branched alkyl group having 1 to 10 carbon atoms.

[0020] Preferably, the titanium compound includes one or more of tetramethyl titanate, tetraethyl titanate, tetraisopropyl titanate or tetrabutyl titanate.

[0021] Preferably, the diol containing adjacent hydroxyl groups includes any one or more of ethylene glycol, 1,2-propylene glycol, 1,2-butylene glycol, 1,2-pentanediol, 1,2-hexanediol, and 2,3-butylene glycol. The diol containing adjacent hydroxyl groups can form a stable six-membered ring structure with the titanium atom, and the side chain alkyl group can further improve the stability through the electron donation effect.

[0022] Further preferably, the diol containing ortho-hydroxyl groups includes ethylene glycol. The raw materials are easier to obtain and the cost is lower.

[0023] The organic base includes one or more of alcoholamine compounds, pyridine, amidine, and guanidine. In the present invention, it is found that the use of organic bases can form stronger titanium oxygen bonds or titanium nitrogen bonds, making the catalyst more difficult to hydrolyze. At the same time, the organic base can destroy the lattice structure of the diol titanium to a certain extent, making each unit smaller, with more hydroxyl groups and nitrogen atoms in the outer layer of the catalyst, and less oxygen being shared, and more lone pairs of electrons on oxygen, which are easy to form hydrogen bonds, so that the catalyst solubility is greatly improved compared with ethylene glycol titanium.

[0024] Preferably, the organic base includes one or more of ethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, diglycolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-methyldiethanolamine 1:4, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), 1,5,7-triazidobicyclo[4.4.0]dec-5-ene (TBD), hexacyclic bicyclic guanidine (MTBD), tetramethylguanidine (TMG), and 4-dimethylaminopyridine (DMAP). Using an organic base with stronger alkalinity can reduce the amount of organic base added, and a liquid catalyst with good hydrolysis stability can be obtained at a lower alkali-titanium ratio.

[0025] Further preferably, the organic base includes one or more of ethanolamine, triethanolamine, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), and 1,5,7-triazidobicyclo[4.4.0]dec-5-ene (TBD).

[0026] Preferably, the molar ratio of the titanium compound to the diol containing ortho-hydroxyl group is 1:20-100; such as 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, 1:55, 1:60, 1:65, 1:70, 1:75, 1:80, 1:85, 1:90, 1:95, or any value therebetween. Within the preferred composition range, the excess diol can react completely with the titanate raw material, and the titanium alcohol organic base catalyst maintains good fluidity while having a high titanium content.

[0027] Preferably, the molar ratio of the titanium compound to the organic base is 1:1-6, such as 1:1, 1:2, 1:3, 1:4, 1:5, 1:6 or any value therebetween.

[0028] The high temperature resistant hydrolysis titanium alcohol organic base catalyst also includes a phosphate compound; adding the phosphate compound can improve the color of the synthesized polyester.

[0029] Preferably, the phosphate compound includes at least one of trimethyl phosphate, triethyl phosphate, tripropyl phosphate, triisopropyl phosphate, tributyl phosphate, triphenyl phosphate, dibutyl phosphate and triethyl phosphoacetate;

[0030] The molar ratio of phosphorus in the phosphate compound to titanium in the titanium compound is 0.2-4:1, preferably 0.5-1.5:1.

[0031] The present invention also provides a method for preparing the high temperature resistant hydrolysis alcohol titanium organic base catalyst, comprising the steps of: mixing a titanium compound, a diol containing an ortho-hydroxyl group and an organic base for reaction at 160-180° C. for 0.5-4 hours to obtain the high temperature resistant hydrolysis alcohol titanium organic base catalyst.

[0032] The titanium alcohol organic base catalyst synthesized by the method of the present invention is a homogeneous transparent liquid, which avoids the problem that the heterogeneous catalyst is easy to precipitate during storage, and the low amount of catalyst used and the uneven state during use easily lead to the problem of inaccurate measurement of titanium element.

[0033] Preferably, the reaction is carried out under the protection of an inert gas.

[0034] Preferably, any two raw materials of the titanium compound, the diol containing an o-hydroxyl group and the organic base are first mixed and reacted at 160-180° C. for 0.5-4 h, and then the other raw material is added and mixed for another 0.5-4 h.

[0035] For example, in plan I:

[0036] 1) Mix the ortho-hydroxyl-containing diol and the organic base in a molar ratio of 160-180° C. and stir for 0.5-4 hours;

[0037] 2) adding the titanium compound to the reaction mixture obtained in 1), and continuously stirring and reacting at 160-180° C. for 0.5-4 hours to obtain the high temperature resistant hydrolysis alcohol titanium organic base catalyst.

[0038] Or, Option II:

[0039] 1) reacting an organic base with a titanium compound at 160-180° C. for 0.5-4 h;

[0040] 2) Adding the ortho-hydroxyl-containing diol to the reaction mixture obtained in 1), stirring and reacting for 0.5-4 hours at 160-180° C. under nitrogen protection, to obtain the high temperature resistant hydrolysis alcohol titanium organic base catalyst.

[0041] Or, Option III:

[0042] 1) mixing a diol containing an o-hydroxyl group with a titanium compound, and reacting the mixture at 160-180° C. for 0.5-4 h, or at 60-160° C. and 10 -0.2 kPa for 0.5-4 h;

[0043] 2) adding an organic base to the reaction mixture obtained in 1), and continuously stirring the reaction at 160-180° C. under nitrogen protection for 0.5-4 hours to obtain the high temperature resistant hydrolysis titanium alcohol organic base catalyst.

[0044] Preferably, in Scheme III, the ortho-hydroxyl-containing diol is reacted with the titanium compound at 160-180° C. for 0.5-4 h.

[0045] Preferably, a phosphate compound is also added to the raw material for reaction, which can further improve the color of the polyester product.

[0046] In the present invention, polyols and organic bases are used to coordinate titanium atoms together to improve the stability of the catalyst, especially its stability at high temperatures, so that it can still maintain good hydrolysis stability at high temperature reaction temperatures of esterification or ester exchange, and can inhibit or significantly reduce the generation of titanium dioxide or titanium polymer precipitation during polyester synthesis, while maintaining high catalytic activity.

[0047] The present invention also provides the use of the high temperature resistant hydrolysis alcohol titanium organic base catalyst in catalytic synthesis of polyester. For example, in the reaction process of synthesizing polyester from polyols and polyacids or polyacids, the catalyst can be used alone in the esterification or transesterification stage, the polycondensation stage, or in all stages.

[0048] The catalyst of the present invention is used for catalytic synthesis of polyester. It is found that the catalyst not only has the advantages of high temperature water stability, high catalytic activity, etc., but also can effectively inhibit the side reaction of generating tetrahydrofuran and reduce the terminal carboxyl content of polyester. When used for polymerization of PBT and its copolyester, the obtained polyester has high intrinsic viscosity, low terminal carboxyl content and low yield of by-product THF.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] (1) The present invention combines titanium compounds, diols with specific structures and organic bases to effectively improve the hydrolysis stability of the catalyst, especially the hydrolysis stability at high temperatures, effectively inhibit or reduce the generation of titanium dioxide or titanium polymer precipitation during the polyester synthesis process, and maintain high catalytic activity.

[0051] (2) The titanium-based catalyst of the present invention not only has high catalytic activity for synthesizing polyester, but also can effectively inhibit the side reaction of generating tetrahydrofuran and reduce the terminal carboxyl content of polyester. When used for the polymerization of PBT and its copolyester, the polyester obtained has high intrinsic viscosity, low terminal carboxyl content and low yield of by-product THF.

[0052] (3) The catalyst preparation method of the present invention is efficient, economical, and environmentally friendly. The raw materials are cheap and easily available, and the cost is low, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The following is the appearance of the catalysts prepared in Examples 1 and 2 and Comparative Examples 1 and 3 after being hydrolyzed at room temperature.

[0054] Figure 2 The following is the appearance of the catalysts prepared in Examples 1 and 2 and Comparative Examples 1 and 3 after high temperature hydrolysis. DETAILED DESCRIPTION

[0055] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0056] The raw materials used in the following specific embodiments are all purchased from the market and used directly without treatment. The test and analysis methods used are described as follows:

[0057] Intrinsic viscosity of polyester: The intrinsic viscosity of polyester samples was measured using a Hangzhou Zhongwang semi-automatic viscometer at a test temperature of 25°C. The solvent used for PBAT and PBST was chloroform. The solvent used for PET and PBT was phenol / tetrachloroethane (mass ratio w / w=3 / 2).

[0058] Esterification rate and THF yield: The refractive index of the effluent was tested at 25°C using an Abbe refractometer. The standard curve of mass concentration (c) and refractive index (n) (c = 11.2007n-14.9247, R 2 =0.9988) to calculate the contents of THF and water in the distillate, and then calculate the esterification rate (the degree of reaction of the carboxyl group) and the THF yield (expressed as the THF / BDO molar ratio).

[0059] Test of the catalyst's room temperature hydrolysis stability: Dissolve 2.5 g of the catalyst to be tested in 25 ml of anhydrous isopropanol, and add water to the solution with a dropper while stirring until the solution becomes significantly turbid, and record the mass of water added at this time.

[0060] High temperature hydrolysis stability test of catalyst: Add the catalyst to be evaluated, water and 1,4-butanediol (BDO) to a 50mL three-necked flask. The composition of the test solution is: the total amount is 25 grams, and the Ti content in the test solution is calculated to be 0.01wt% based on the Ti content in the catalyst, the mass fraction of water is 1wt%, and the rest is BDO. The flask is placed in an oil bath preheated to 210°C and heated, and nitrogen is introduced. A condenser is connected to the top of the flask to condense the refluxed rising steam. The time for the white precipitate to appear in the flask is compared to evaluate the high temperature hydrolysis resistance of the catalyst.

[0061] For convenience, in the present invention, the names of the chemicals used are replaced by English abbreviations. In the naming of the catalyst, simpler abbreviations are used to represent the chemicals used as catalyst components. The correspondence between the chemical names and abbreviations is listed in Table 1.

[0062] Table 1 Chemical names and abbreviations

[0063]

[0064] Note: In the naming of catalysts, in order to distinguish the components, the corresponding chemicals are abbreviated with only the first letter capitalized, as shown in brackets

[0065] Examples 1-10 Synthesis of Catalysts

[0066] Example 1 Synthesis of Catalyst TEEa

[0067] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0068] (ii) 1.27 g (20.83 mmol) of ethanolamine was added to the reaction mixture obtained in step (i), and the reaction was continued at 160° C. with continuous stirring. It was observed that the milky white suspension gradually disappeared, and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour, which was recorded as catalyst TEEa. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0069] Example 2 Synthesis of catalyst TETa

[0070] (i) In a 50 mL three-necked flask equipped with a stirring magnet, add 15.6 g (251.3 mmol) of ethylene glycol and 0.775 g (5.19 mmol) of triethanolamine. After the addition is complete, place the flask in a 160°C oil bath and stir for 1 h under nitrogen protection until the mixture is uniform and transparent.

[0071] (ii) 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the reaction mixture obtained in step (i). After the addition was completed, the mixture was stirred and reacted at 160° C. for 2 h. n-butanol was observed to be distilled out, and the reaction system remained a uniform and transparent liquid, which was recorded as catalyst TETa. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0072] Example 3 Synthesis of catalyst TEDga

[0073] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0074] (ii) 2.14 g (20.39 mmol) of diglycolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred and reacted at 160° C. It was observed that the milky white suspension gradually disappeared and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour, which was recorded as catalyst TEDga. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0075] Example 4 Synthesis of catalyst TED

[0076] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0077] (ii) 0.77 g (5.05 mmol) of DBU was added to the reaction mixture obtained in step (i), and the mixture was stirred and reacted at 160° C. It was observed that the milky white suspension gradually disappeared, and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour, which was recorded as catalyst TED. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0078] Example 5 Synthesis of Catalyst TEDbn

[0079] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0080] (ii) 0.666 g (5.35 mmol) of DBN was added to the reaction mixture obtained in step (i), and the reaction was continued at 160° C. with continuous stirring. It was observed that the milky white suspension gradually disappeared, and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour, which was recorded as catalyst TEDbn. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0081] Example 6 Synthesis of Catalyst TETbd

[0082] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0083] (ii) 0.704 g (4.56 mmol) of TBD was added to the reaction mixture obtained in step (i), and the mixture was stirred and reacted at 160° C. It was observed that the milky white suspension gradually disappeared and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour, which was recorded as catalyst TETbd. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0084] Example 7 Synthesis of Catalyst TETa-Tpp

[0085] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0086] (ii) 0.72 g (4.82 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred at 160° C. until the milky white suspension gradually disappeared and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour.

[0087] (iii) 1.24 g (3.79 mmol) of triphenyl phosphate was added to the reaction mixture obtained in step (ii), and the reaction was continued at 160° C. with stirring for about 1 hour. It was observed that the solid triphenyl phosphate gradually disappeared until the reaction system became a uniform transparent liquid, which was recorded as catalyst TETa-Tpp. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0088] Example 8 Synthesis of Catalyst TETa-Tepa

[0089] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0090] (ii) 0.72 g (4.82 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred at 160° C. until the milky white suspension gradually disappeared and the reaction system became a uniform transparent liquid. The reaction time was about 1 hour.

[0091] (iii) 1.06 g (4.72 mmol) of triethyl phosphoacetate was added to the reaction mixture obtained in step (ii), and the mixture was stirred and reacted at 160° C. for about 1 h. The reaction system remained a uniform transparent liquid, which was recorded as catalyst TETa-Tepa. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0092] Example 9 Synthesis of Catalyst TPeTa

[0093] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 26.1 g (250.6 mmol) of 1,2-pentanediol was added, and 3.41 g (10.02 mmol) of tetrabutyl titanate was slowly added dropwise to the 1,2-pentanediol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. The reaction system remained a uniform, clear and transparent solution, and n-butanol was distilled out.

[0094] (ii) 1.50 g (10.05 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the reaction was continued under nitrogen protection at 160° C. with stirring for about 1 hour. The reaction system remained a uniform, clear and transparent solution, which was recorded as catalyst TPeTa. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0095] Example 10 Synthesis of Catalyst TdmETa

[0096] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 22.50 g (249.67 mmol) of 2,3-butanediol was added, and 3.41 g (10.02 mmol) of tetrabutyl titanate was slowly added dropwise to the 2,3-butanediol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. The reaction system was observed to remain a uniform, clear and transparent solution, and n-butanol was distilled out.

[0097] (ii) 1.50 g (10.05 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the reaction was continued under nitrogen protection at 160° C. with stirring for about 1 hour. The reaction system remained a uniform, clear and transparent solution, which was recorded as the catalyst TdmETa. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0098] Application Example 1-10 Synthesis of Polyester

[0099] Application Example 1: Using TEEa to synthesize polyester PBT

[0100] 83g (0.5mol) of terephthalic acid and 90.1g (0.5mol) of 1,4-butanediol are added to a polymerization reactor, and the catalyst TEEa prepared in Example 1 is added, and the catalyst dosage is 50ppm (referring to the mass content of titanium element in the expected polymer, the same below). The temperature is controlled at 210-225°C, nitrogen is introduced, and an esterification reaction is carried out for 2 hours to obtain a prepolymer; then the pressure is gradually reduced, and a condensation reaction is carried out under vacuum conditions, the reaction temperature is controlled at 240-255°C, the pressure is controlled at less than 100Pa, and the reaction time is 1.25 hours; after cooling and pelletizing, PBT polyester is obtained, and its characteristic viscosity is 1.15dL / g. Application Example 2: Synthesis of copolyester PBST using TETa 50

[0101] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TETa prepared in Example 2 was added, with a catalyst dosage of 41 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 2 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 1.02dL / g.

[0102] Application Example 3: Synthesis of copolyester PBST using TEDga 50

[0103] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TEDga prepared in Example 3 was added, and the catalyst dosage was 35 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 2 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 1.15dL / g.

[0104] Application Example 4: Synthesis of copolyester PBST using TED 50

[0105] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TED prepared in Example 4 was added, with a catalyst dosage of 47 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 1.67 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester chips, the intrinsic viscosity is 1.07dL / g.

[0106] Application Example 5: Synthesis of copolyester PBAT using TEDbn 50

[0107] 41.5 g (0.25 mol) of terephthalic acid, 36.5 g (0.25 mol) of adipic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to the polymerization reactor, and the catalyst TEDbn prepared in Example 5 was added, and the catalyst dosage was 50 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and the esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 3.40 hours; after cooling and pelletizing, PBAT was obtained. 50 Polyester, its intrinsic viscosity is 1.03dL / g.

[0108] Application Example 6: Synthesis of copolyester PBST using TETbd 50

[0109] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TETbd prepared in Example 6 was added, and the catalyst dosage was 50 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 1.5 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 1.13dL / g.

[0110] Application Example 7: Synthesis of copolyester PBST using TETa-Tpp 50

[0111] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TETa-Tpp prepared in Example 7 was added, and the catalyst dosage was 50 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 2.5 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 1.06dL / g.

[0112] Application Example 8: Synthesis of copolyester PBST using TETa-Tepa 50

[0113] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TETa-Tepa prepared in Example 8 was added, and the catalyst dosage was 50 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 3 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 1.03dL / g.

[0114] Application Example 9: Synthesis of copolyester PBST using TPeTa 50

[0115] 41.5 g (0.25 mol) of terephthalic acid, 29.5 g (0.25 mol) of succinic acid and 90.1 g (0.5 mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TPeTa prepared in Example 9 was added, and the catalyst dosage was 50 ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100 Pa, and the reaction time was 2.5 hours; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 0.89dL / g.

[0116] Application Example 10: Using TETa to synthesize polyester PET

[0117] 83g (0.5mol) of terephthalic acid and 46.03g (0.75mol) of ethylene glycol were added to a polymerization reactor, and the catalyst TETa prepared in Example 2 was added, and the catalyst dosage was 50ppm. The temperature was controlled at 240-255°C, nitrogen was introduced, and an esterification reaction was carried out for 6 hours to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 270-290°C, the pressure was controlled at less than 100Pa, and the reaction time was 0.67h; after cooling and pelletizing, PET polyester was obtained, and its intrinsic viscosity was 0.83dL / g.

[0118] Comparative Example 1

[0119] The hydrolysis stability of commercial tetrabutyl titanate (TBT) catalyst was evaluated. Tetrabutyl titanate was purchased from Beijing Bailingwei Technology Co., Ltd. The results are shown in Table 2.

[0120] Comparative Example 2 Synthesis of Catalyst Titanium Ethylene Glycol (TE)

[0121] In a 50mL three-necked flask equipped with a stirring magnet, 55.86g (900mmol) of ethylene glycol was added, and 10.21g (30mmol) of tetrabutyl titanate was slowly added dropwise to the above solution. The mixed solution was placed in an oil bath at 160°C and reacted for 2h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0122] After cooling to room temperature, the white floccules were collected by centrifugation and then washed several times with deionized water and ethanol to remove excess ethylene glycol from the sample. Finally, the precipitate was dried in a vacuum oven at 50 °C for 4 hours to obtain a solid titanium ethylene glycol catalyst, which was recorded as TE.

[0123] Comparative Example 3 Synthesis of Catalyst TEP

[0124] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 15.6 g (251.3 mmol) of ethylene glycol was added, and 1.75 g (5.14 mmol) of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. After the addition was completed, the flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0125] (ii) 1.40 g (25 mmol) of potassium hydroxide was added to the reaction mixture obtained in step (i), and the mixture was stirred and reacted at 160° C. The milky white suspension gradually disappeared until the reaction system became a uniform transparent liquid. The reaction time was about 1 h, which was recorded as catalyst TEP. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0126] Comparative Example 4 Synthesis of Catalyst TB

[0127] 22.53 g of 1,4-butanediol was added to a 50 mL three-necked flask equipped with a stirring magnet, 1.70 g of tetrabutyl titanate was slowly added to the 1,4-butanediol, and mixed evenly. Then the flask was placed in a 160°C oil bath and reacted for 2 hours under nitrogen protection. It was observed that n-butanol was distilled out, and the reaction system remained uniform and transparent. The catalyst was recorded as TB. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0128] Comparative Example 5 Synthesis of Catalyst TBTa

[0129] 22.4 g of 1,4-butanediol was added to a 50 mL three-necked flask equipped with a stirring magnet, 1.72 g of tetrabutyl titanate was slowly added dropwise to the above solution, and mixed evenly. Then the flask was placed in a 160°C oil bath and reacted for 2 hours under nitrogen protection. It was observed that n-butanol was distilled out, and the reaction system remained uniform and transparent.

[0130] 0.75 g of triethanolamine was further added to the reaction mixture, mixed evenly, and stirred continuously at 160° C. for 1 hour. The reaction system remained uniform and transparent throughout. The catalyst was recorded as TBTa. The hydrolysis stability of the catalyst was evaluated. The results are shown in Table 2.

[0131] Comparative Example 6 Synthesis of Catalyst TETa-C at Room Temperature

[0132] 15.6 g of ethylene glycol was added to a 50 mL three-necked flask equipped with a stirring magnet, and 1.75 g of tetrabutyl titanate was slowly added dropwise to the ethylene glycol. The mixture was reacted for 2 h at room temperature under nitrogen protection. A light white precipitate was observed to form in the solution.

[0133] 0.775 g (5.19 mmol) of triethanolamine was further added to the reaction mixture, and stirring was continued at room temperature. The precipitate gradually disappeared until the reaction system became a uniform transparent liquid. The obtained catalyst was recorded as TETa-C. The hydrolysis stability of the catalyst was evaluated, and the results are shown in Table 2.

[0134] Comparative Example 7 Synthesis of Catalyst TPTa

[0135] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 19.0 g (249.70 mmol) of 1,3-propylene glycol was added, and 3.41 g (10.02 mmol) of tetrabutyl titanate was slowly added dropwise to ethylene glycol. The flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0136] (ii) 4.50 g (30.16 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred at 160° C. for 1 h. The solution was still a milky white thick suspension. The catalyst was recorded as TPTa.

[0137] Comparative Example 8 Synthesis of Catalyst TmPTa

[0138] (i) In a 50 mL three-necked flask equipped with a stirring magnet, 22.5 g (249.66 mmol) of 2-methyl-1,3-propanediol was added, and 3.41 g (10.02 mmol) of tetrabutyl titanate was slowly added dropwise to the 2-methyl-1,3-propanediol. The flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0139] (ii) 1.50 g (10.05 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred at 160° C. for 1 h. The solution was still a milky white thick suspension. The catalyst was recorded as TmPTa.

[0140] Comparative Example 9 Synthesis of Catalyst TGTa

[0141] (i) In a 50-mL three-necked flask equipped with a stirring magnet, 23.2 g (241.92 mmol) of propylene glycol was added, and 3.41 g (10.02 mmol) of tetrabutyl titanate was slowly added dropwise to the propylene glycol. The flask was placed in an oil bath at 160°C and reacted for 2 h under nitrogen protection. A milky white precipitate was observed in the solution, and the reaction system became a milky white thick suspension, and n-butanol was distilled out.

[0142] (ii) 4.50 g (30.16 mmol) of triethanolamine was added to the reaction mixture obtained in step (i), and the mixture was stirred at 160° C. for 1 h. The solution was still a milky white thick suspension. The catalyst was recorded as TGTa.

[0143] Application Comparative Example 1 Synthesis of copolyester PBST using titanium glycol catalysis 50

[0144] 41.5g (0.25mol) of terephthalic acid, 29.5g (0.25mol) of succinic acid and 90.1g (0.5mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst titanium glycolate prepared in Comparative Example 2 was added, and the catalyst dosage was 100ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2h to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100Pa, and the reaction time was 2h; after cooling and pelletizing, PBST was obtained. 50 Polyester, its intrinsic viscosity is 0.96dL / g.

[0145] Application Comparative Example 2 Synthesis of Copolyester PBST Using TEP Catalyst 50

[0146] 41.5g (0.25mol) of terephthalic acid, 29.5g (0.25mol) of succinic acid and 90.1g (0.5mol) of 1,4-butanediol were added to a polymerization reactor, and the catalyst TEP prepared in Comparative Example 3 was added, with a catalyst dosage of 54ppm. The temperature was controlled at 210-225°C, nitrogen was introduced, and an esterification reaction was carried out for 2h to obtain a prepolymer; then the pressure was gradually reduced, and a polycondensation reaction was carried out under vacuum conditions, the reaction temperature was controlled at 240-255°C, the pressure was controlled at less than 100Pa, and the reaction time was 3.25h; after cooling and pelletizing, PBST was obtained. 50 Polyester chips, the intrinsic viscosity is 0.97dL / g.

[0147] Application Comparative Example 3

[0148] The acid value of PBAT industrial products was measured. PBAT was purchased from Donghua Tianye.

[0149] The properties and hydrolysis stability evaluation results of the catalysts synthesized in each example and comparative example are summarized in Table 2.

[0150] Table 2 Catalyst properties and hydrolysis stability evaluation results prepared in Examples and Comparative Examples

[0151]

[0152]

[0153] a : refers to the time the catalyst is placed from synthesis to the hydrolysis stability test;

[0154] b : The mass of water added when turbidity appears in the test solution;

[0155] c : The mass ratio of water to titanium in the solution when turbidity appears in the test solution;

[0156] d : Mass percentage of titanium in the test solution;

[0157] e : The mass percentage of water in the test solution.

[0158] -: indicates that no experimental test was conducted or the test was conducted directly without placement

[0159] From the results of Comparative Examples 1 and 3, it can be seen that the hydrolysis stability of the existing catalyst tetrabutyl titanate and the catalyst TEP synthesized using an inorganic base are both very poor. The room temperature hydrolysis stability of TEP is improved compared to TBT, but at high temperatures, both hydrolyze and precipitate in less than 20 minutes, and the hydrolysis stability is worse than that of TBT. The TE catalyst synthesized in Comparative Example 2 has excellent hydrolysis resistance, but TE is a solid, not a liquid catalyst, which is not convenient for adding materials and is not conducive to uniform dispersion. This is also a defect of titanium glycolate.

[0160] It can be seen from the results of Examples 1-10 that according to the method of the present invention, the titanium-based catalyst synthesized from the titanium compound, the ortho-hydroxyl-containing diol shown in structural formula I and the organic base - the alcohol titanium organic base catalyst are all uniform, transparent and fluid liquid catalysts, not only showing excellent hydrolysis stability at room temperature, but also remaining non-hydrolyzed for at least two hours under high temperature, i.e., simulated esterification conditions (Note: the high-temperature hydrolysis test here was only carried out for 2 hours, so the result does not mean that it can only withstand 2 hours of hydrolysis; in fact, the TETa catalyst prepared in Example 2 remained clear and transparent after 10 hours of high-temperature hydrolysis); at the same time, the catalyst can remain hydrolytically stable after being placed for more than 6 months, such as the TETa obtained in Example 2 and the TED obtained in Example 4, after being placed for nearly 200 days, still showed the same hydrolysis stability as after being placed for 1 day.

[0161] The appearance of Comparative Example 1 (TBT), Comparative Example 3 (TEP), Example 1 (TEEa) and Example 2 (TETa) after the room temperature hydrolysis stability evaluation is as follows: Figure 1 As shown, the appearance after high temperature hydrolysis test is as follows Figure 2 It can be clearly seen that the catalysts of Example 1 and Example 2 are transparent and uniform, and no precipitation is produced after the high temperature hydrolysis test, and the stability is very good.

[0162] From the results of Comparative Examples 4 and 5, it can be seen that the room temperature hydrolysis stability of the titanium alkoxide catalyst TB and the titanium alkoxide organic base catalyst TBTa with 1,4-butanediol as the ligand is greatly improved compared with TBT, but the hydrolysis stability at high temperature is still not good enough. Under high temperature and water conditions, the TB catalyst will be obviously hydrolyzed within 30 minutes, and the TBTa catalyst will also have obvious hydrolysis turbidity within 1.5 hours. It can be seen that the structure of the diol is a key factor affecting the hydrolysis stability of the titanium alkoxide organic base catalyst.

[0163] Similarly, from the results of Comparative Examples 7, 8, and 9, it can be seen that the titanium alcoholate organic base catalysts TPTa, TmPTa, and TGTa with 1,3-propylene glycol, 2-methyl-1,3-propylene glycol, and glycerol as ligands, respectively, are still milky white thick suspensions, not liquid catalysts. It can be seen that the structure of the diol also has an important influence on the morphology of the titanium alcoholate organic base catalyst. The inventor unexpectedly found that the diol is preferably a structure containing ortho-hydroxyl groups, and the triol or a structure with two hydroxyl groups far apart is not ideal.

[0164] Comparing the TETa catalysts prepared in Example 2 and Comparative Example 6, the difference between the two is that the former is synthesized at a high temperature of 160°C, and the latter is synthesized at room temperature. However, surprisingly, the TETa catalyst prepared in Example 2 has excellent high-temperature hydrolysis stability, while the TETa-C catalyst prepared in Comparative Example 6, although having excellent room-temperature hydrolysis stability, has poor hydrolysis stability at a high temperature of 210°C, which is significantly inferior to the TETa catalyst prepared in Example 2, indicating that the performance of the catalyst depends not only on the formula, but also on the preparation conditions.

[0165] The conditions and results of the application of different catalysts in the synthesis of polyesters and copolyesters are summarized in Table 3.

[0166] Table 3 Synthesis conditions and results of homopolyester and copolyester prepared in application examples

[0167]

[0168] a : refers to the mass fraction of titanium element in the catalyst in the theoretical polyester yield;

[0169] b : The molar percentage of THF generated to the total amount of BDO added;

[0170] c : polycondensation time;

[0171] d : Intrinsic viscosity, test temperature is 25.0°C, the solvent used for PBAT and PBST is chloroform. The solvent used for PET and PBT is phenol / tetrachloroethane (mass ratio w / w=3 / 2).

[0172] e : The content of terminal carboxyl groups in polyester;

[0173] From the results of application examples 1-10, it can be seen that the titanium alcohol organic base catalyst synthesized by the present invention has a high catalytic activity for the synthesis of polyester and copolyester. For polyester and copolyester based on 1,4-butanediol, PBT and PBST with an intrinsic viscosity greater than 1.0 dL / g can be obtained when the Ti dosage is ≤50ppm and the polycondensation time is less than 3h. 50PBAT with an intrinsic viscosity greater than 1.0 dL / g can be obtained when the polycondensation time is less than 4 hours 50 ; For PET polyester, when the Ti dosage is 100ppm and the polycondensation time is less than 1h, the intrinsic viscosity of PET polyester can be obtained to be greater than 0.8dL / g. It can be seen that the titanium alcohol organic base catalyst synthesized by the present invention exhibits high catalyst activity for the synthesis of polyester or copolyester by the common diol and dibasic acid polycondensation method.

[0174] Comparative Example 1 uses titanium glycolate, which is a relatively mature catalyst in the prior art. The catalyst has good hydrolysis stability, but is not easy to disperse evenly. Under the condition that the Ti dosage is 100 ppm, the obtained PBST 50 The intrinsic viscosity is <1.0 dL / g. In contrast, in Application Examples 2-4 and 5-9, PBST is synthesized by using the titanium alcohol organic base catalyst of the present invention with the catalyst addition amount (in terms of Ti) being only half or less than half of that in Application Comparative Example 1. 50 Not only is the polycondensation time shorter than that of comparative example 1, but the obtained PBST 50 The intrinsic viscosity of polyester is higher. This shows that compared with titanium ethylene glycol, the titanium alcoholate organic base catalyst provided by the present invention has significantly higher catalytic activity.

[0175] Application of Comparative Example 2 Synthesis of PBST Using Titanium Alkoxide Inorganic Base Catalyst TEP 50 , melt polycondensation for 3.25 hours, the obtained PBST 50 The intrinsic viscosity is still less than 1.0 dL / g. Compared with the comparative example 2, the catalyst dosage (in terms of Ti) of the application examples 2-4 and 5-9 is equivalent to that of the comparative example 2. 50 When synthesized by , not only the polycondensation time is shorter, but also the intrinsic viscosity of the obtained polyester is higher. This shows that compared with the inorganic base catalyst of titanium alkoxide, the organic base of titanium alkoxide of the present invention has higher catalytic activity, which is obviously due to their excellent hydrolytic stability, especially high temperature hydrolytic stability. In contrast, TEP has poor high temperature hydrolytic stability.

[0176] It can also be seen from the results in Table 3 that when the polyester and copolyester based on butanediol are synthesized using the titanium alcohol organic base catalyst of the present invention, the amount of by-product THF generated is very small, only 2.45-7.51%, which is significantly lower than the THF generated when using titanium ethylene glycol (Comparative Example 1) and TEP (Comparative Example 2) catalysts.

[0177] It can also be seen from the results in Table 3 that the carboxyl content of the polyester synthesized using the titanium alcohol organic base catalyst of the present invention is very low, which is effective for PBT polyester or PBST 50 and PBAT 50For copolyester, the carboxyl content is only 7.2-12.8 mol / t, and for PET polyester, the carboxyl content is only 25.1 mol / t. In contrast, PBST synthesized using TEP catalyst in Comparative Example 2 50 The acid value of the copolyester is 14.84 mol / t, and the carboxyl content of the commercial PBAT is as high as 36.1 mol / t (Comparative Example 3). This shows that the use of the titanium alcohol organic base catalyst provided by the present invention to synthesize polyester is conducive to reducing the carboxyl content. Low carboxyl content is conducive to improving the processing stability and shelf life of polyester and copolyester.

[0178] In summary, the titanium alcohol organic base catalyst prepared by the present invention has an unexpected modification effect. The obtained catalyst has high catalytic activity, high temperature hydrolysis stability, good fluidity and solubility within a specific composition range. It is applied to the synthesis of various polyesters, especially PBT and its copolyesters to obtain products with high intrinsic viscosity. It also has the function of inhibiting the formation of by-product THF and terminal carboxyl groups, and the effect is very excellent.

[0179] The present invention is not limited to the above optional implementation modes. Anyone can derive other forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that fall within the scope defined by the claims of the present invention fall within the protection scope of the present invention.

Claims

1. A high temperature resistant titanium alcoholate hydrolysis organic base catalyst, characterized in that: It comprises a titanium compound, a diol containing an ortho-hydroxyl group as shown in formula I, and an organic base; Wherein, R1 and R2 are independently selected from H, CH3, CH2CH3, CH2CH2CH3 or CH2CH2CH2CH3; the molar ratio of the titanium compound to the diol containing ortho-hydroxyl group is 1:4-100; the molar ratio of the titanium compound to the organic base is 1:0.5-8; The chemical formula of the titanium compound is Ti(OR)4, wherein R is selected from a linear or branched alkyl group of 1 to 10 carbon atoms; The organic base includes one or more of ethanolamine, diethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, diglycolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-methyldiethanolamine, DBU, DBN, TBD, MTBD, TMG, and DMAP; The titanium compound and the diol containing ortho-hydroxyl group are mixed and reacted for 0.5-4h at 60-160°C and 10-0.2kPa; then an organic base is added and the mixture is mixed and reacted for 0.5-4h at 160-180°C to obtain the high temperature resistant hydrolysis alcohol titanium organic base catalyst.

2. The high temperature resistant hydrolysis titanium alcoholate organic base catalyst according to claim 1, characterized in that: The diol containing ortho-hydroxyl groups includes any one or more of ethylene glycol, 1,2-propylene glycol, 1,2-butylene glycol, 1,2-pentanediol, 1,2-hexanediol, and 2,3-butylene glycol.

3. The high temperature resistant hydrolysis titanium alcoholate organic base catalyst according to claim 1, characterized in that: The high temperature resistant hydrolysis titanium alcoholate organic base catalyst also includes a phosphate compound; The phosphate compound includes at least one of trimethyl phosphate, triethyl phosphate, tripropyl phosphate, triisopropyl phosphate, tributyl phosphate, triphenyl phosphate, dibutyl phosphate and triethyl phosphoacetate; The molar ratio of phosphorus in the phosphate compound to titanium in the titanium compound is 0.2-4:

1.

4. The method for preparing the high temperature resistant hydrolysis titanium alcoholate organic base catalyst according to claim 1, characterized in that: The titanium compound and the diol containing ortho-hydroxyl group are mixed and reacted for 0.5-4h at 60-160°C and 10-0.2kPa; then an organic base is added and the mixture is mixed and reacted for 0.5-4h at 160-180°C to obtain the high temperature resistant hydrolysis alcohol titanium organic base catalyst.

5. The method for preparing the high temperature resistant hydrolysis titanium alcoholate organic base catalyst according to claim 4, characterized in that: A phosphate compound is also added to the raw materials for reaction.

6. Use of the high temperature resistant hydrolysis alcohol titanium organic base catalyst according to any one of claims 1 to 3 in catalytic synthesis of polyester.