Adhesive layer, laminated sheet, adhesive composition, and optical semiconductor device

By using a binder layer with high haze value and low light transmittance in an optical semiconductor device, combining colorant and light diffusing particles to form anti-glare and anti-reflective laminates, the anti-reflective in the prior art is solved The excellent appearance and sealing performance of optical semiconductor devices are achieved.

CN117801715BActive Publication Date: 2024-12-03NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410034629.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-10-11
Filing Date
2023-02-14
Publication Date
2024-12-03
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The existing adhesive layer has shortcomings in preventing reflection and suppressing uneven brightness, and it is impossible to achieve excellent anti-reflectivity and uniform light transmission brightness at the same time.

Method used

Adhesive layer with haze value of more than 61% and total light transmittance of less than 69%, combined with colorant and light diffusing particles, forming a laminated sheet with anti-glare and anti-reflective properties for sealing optical semiconductor components. , ensure the anti-reflectivity and brightness uniformity of the substrate surface.

Benefits of technology

Excellent anti-reflective properties during bonding and the effect of suppressing uneven transmission light brightness during bonding, thereby improving the appearance and sealing performance of the optical semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801715B_ABST
    Figure CN117801715B_ABST
Patent Text Reader

Abstract

The present invention relates to an adhesive layer, a laminated sheet, an adhesive composition and an optical semiconductor device. An adhesive layer is provided which has excellent anti-reflection properties when attached to an adherend and can suppress uneven brightness of transmitted light. The laminated sheet (1) comprises at least an adhesive layer (21). The haze value of the adhesive layer (21) is greater than 61% and the total light transmittance is less than 69%. The laminated sheet (1) may have a layer (42) having anti-glare properties and / or anti-reflection properties on one surface. The laminated sheet (1) preferably has a thickness of less than 500 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of February 14, 2023, an application number of 202310112194.3, and an invention name of Adhesive layer, laminated sheet, adhesive composition, and optical semiconductor device. Technical Field

[0002] The present invention relates to an adhesive layer. More specifically, the present invention relates to an adhesive layer suitable for sealing optical semiconductor elements such as mini / micro LEDs. Background Art

[0003] In recent years, self-luminous display devices represented by mini / micro LED display devices (Mini / Micro Light Emitting Diode Display) have been designed as a new generation of display devices. Mini / micro LED display devices, as a basic structure, use a substrate with a large number of tiny optical semiconductor elements (LED chips) arranged at a high density as a display panel, the optical semiconductor elements are sealed by a sealing material, and a covering member such as a resin film and a glass plate is stacked on the outermost layer.

[0004] In a display body having a self-luminous display device such as a mini / micro LED display device, wiring (metal wiring) of metal oxides such as metal and ITO is arranged on the substrate of the display panel. For example, such a display device has the following problems: when it is turned off, light is reflected by the above-mentioned metal wiring, etc., the beauty of the screen deteriorates, and the appearance is poor. Therefore, as a sealing material for sealing the optical semiconductor element, a technology using an anti-reflection layer for preventing reflection caused by the metal wiring is adopted.

[0005] In addition, in displays using self-luminous display devices, there is a problem of uneven brightness (brightness unevenness) caused by the light source of the optical semiconductor element. When uneven brightness occurs, a phenomenon called "color shift" occurs in which the color tone changes when the display is viewed from the front and when it is viewed from an oblique angle.

[0006] Patent Document 1 discloses an adhesive film having an adhesive layer dispersed with carbon black on one side of a transparent substrate. Patent Document 2 discloses an adhesive sheet having an adhesive layer containing light-diffusing fine particles. In addition, Patent Document 3 discloses a colored adhesive sheet having a colored adhesive layer having a haze value of 1% or more and 60% or less.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 11-335639

[0010] Patent Document 2: Japanese Patent Application Publication No. 2021-138825

[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-164702 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] However, although the adhesive layer in the adhesive sheet of Patent Documents 1 and 3 can be expected to prevent reflection caused by metal wiring when sealing the optical semiconductor element, it does not suppress uneven brightness. In addition, although the adhesive layer in the adhesive sheet of Patent Document 2 can be expected to suppress uneven brightness, it does not have anti-reflective properties. Therefore, an adhesive layer that has excellent anti-reflective properties when attached to an adherend and can suppress uneven brightness of transmitted light is required.

[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a pressure-sensitive adhesive layer which has excellent antireflection properties when attached to an adherend and can suppress uneven brightness of transmitted light.

[0015] Solutions for solving problems

[0016] The present inventors have conducted intensive research to achieve the above-mentioned object and have found that a pressure-sensitive adhesive layer having a specific haze value and total light transmittance can provide excellent antireflection properties when attached to an adherend and can suppress uneven brightness of transmitted light. The present invention has been completed based on these findings.

[0017] That is, the present invention provides an adhesive layer having a haze value of 61% or more and a total light transmittance of 69% or less.

[0018] The present invention also provides a laminate sheet comprising the above-mentioned adhesive layer.

[0019] The laminated sheet may include an anti-glare and / or anti-reflection layer on one surface.

[0020] The thickness of the laminated sheet is preferably 500 μm or less.

[0021] The present invention also provides an adhesive composition comprising a colorant and light diffusing fine particles, wherein the adhesive composition has a haze value of 61% or more and a total light transmittance of 69% or less when forming an adhesive layer.

[0022] The present invention also provides an optical semiconductor device including: a substrate; an optical semiconductor element disposed on the substrate; and the laminate sheet or a cured product thereof for sealing the optical semiconductor element.

[0023] Effects of the Invention

[0024] The adhesive layer of the present invention has excellent anti-reflection properties when attached to an adherend and can suppress uneven brightness of transmitted light. Therefore, when a laminated sheet having the adhesive layer of the present invention is used to seal an optical semiconductor element, the substrate surface has excellent anti-reflection properties and is less likely to cause uneven brightness caused by light emitted by the optical semiconductor element. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a cross-sectional view of a sheet for sealing an optical semiconductor element according to one embodiment of the present invention.

[0026] Figure 2 This is a cross-sectional view of a sheet for sealing an optical semiconductor element according to another embodiment of the present invention.

[0027] Figure 3 To show the use of Figure 1 A partial cross-sectional view of one embodiment of an optical semiconductor device of the optical semiconductor element sealing sheet shown.

[0028] Figure 4 To show the use of Figure 2 A partial cross-sectional view of one embodiment of an optical semiconductor device of the optical semiconductor element sealing sheet shown.

[0029] Figure 5 To show the use of Figure 2 A partial cross-sectional view of another embodiment of an optical semiconductor device of the optical semiconductor element sealing sheet shown.

[0030] Description of Reference Numerals

[0031] 1Sheet for sealing optical semiconductor elements

[0032] 2 Sealing resin layer

[0033] 21 Adhesive layer of the present invention

[0034] 22 Non-diffusion functional layer

[0035] 3 Release liner

[0036] 4 Base material

[0037] 41. Substrate film

[0038] 42 functional layers

[0039] 5 substrates

[0040] 6 Optical semiconductor devices

[0041] 7 Sealing resin layer

[0042] 71 Diffusion Function Coloring Layer

[0043] 72 Non-diffusion functional layer

[0044] 10 Optical semiconductor devices DETAILED DESCRIPTION

[0045] [Adhesive layer]

[0046] The adhesive layer of the present invention has a haze value of 61% or more and a total light transmittance of 69% or less. The adhesive layer of the present invention is a single-layer adhesive layer. The adhesive layer of the present invention is preferably a resin layer composed of a resin.

[0047] The haze value (initial haze value) of the adhesive layer of the present invention is 61% or more, preferably 70% or more, more preferably 80% or more, further preferably 90% or more, 95% or more, 97% or more, and even near 99.9%. By making the haze value 61% or more, it is possible to suppress uneven brightness of light passing through the adhesive layer when it is attached to an adherend. It should be noted that the upper limit of the haze value is not particularly limited, that is, it can be 100%.

[0048] The total light transmittance of the adhesive layer of the present invention is 69% or less, preferably 60% or less, more preferably 50% or less, further preferably 40% or less, further preferably 30% or less. In addition, from the viewpoint of ensuring light transmittance, the total light transmittance is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, further preferably 2% or more, further preferably 2.5% or more, and particularly preferably 3% or more.

[0049] The haze value and total light transmittance are values ​​for a single layer and can be measured by the method specified in JIS K7136 and JIS K7361-1, and can be controlled by the type and thickness of the adhesive layer, the colorant, the type and amount of light diffusing fine particles, etc.

[0050] The adhesive layer of the present invention may be a resin layer having a property of being cured by radiation irradiation (radiation-curable resin layer), or a resin layer not having a property of being cured by radiation irradiation (non-radiation-curable resin layer). Examples of the radiation include electron beams, ultraviolet rays, α rays, β rays, γ rays, or X-rays.

[0051] The adhesive layer of the present invention preferably contains a colorant. As long as the colorant can be dissolved or dispersed in the adhesive layer of the present invention, it can be a dye or a pigment. From the aspect that there is no sedimentation like a pigment and it is easy to be evenly distributed, a dye is preferred. In addition, from the aspect that the color development is high even if a small amount is added, a pigment is also preferred. When a pigment is used as a colorant, it is preferably low in conductivity or no conductivity. The above-mentioned colorant can be used only one, or two or more can be used.

[0052] As the colorant, a black colorant is preferred. As the black colorant, a known and commonly used colorant (pigment, dye, etc.) for presenting black can be used, for example, carbon black (furnace black, channel black, acetylene black, thermal black, lamp black, pine smoke, etc.), graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite (non-magnetic ferrite, magnetic ferrite, etc.), magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex, anthraquinone colorant, zirconium nitride, etc. In addition, a colorant that is combined and mixed to present a color other than black and acts as a black colorant can also be used.

[0053] When the pressure-sensitive adhesive layer of the present invention is a radiation-curable resin layer, the colorant is preferably a colorant that absorbs visible light and has a transmittance to light of a wavelength at which the radiation-curable resin layer can be cured.

[0054] About the containing ratio of the colorant in the adhesive layer of the present invention, from the viewpoint of giving appropriate anti-reflection ability to the adherend, relative to the total amount 100 mass % of the adhesive layer of the present invention, preferably more than 0.04 mass %, more preferably more than 0.1 mass %, also can be more than 0.2 mass %, more than 0.4 mass %. In addition, the containing ratio of the above-mentioned colorant is, for example, less than 10 mass %, preferably less than 5 mass %, more preferably less than 3 mass %, further preferably less than 1 mass %, also can be less than 0.8 mass %, less than 0.1 mass %. The above-mentioned containing ratio is appropriately set according to the type of colorant, the color tone and the transmittance of the adhesive layer. The colorant can be added to the composition in the form of a solution or dispersion formed by dissolving or dispersing in an appropriate solvent.

[0055] The adhesive layer of the present invention preferably contains light diffusing fine particles. The adhesive layer of the present invention particularly preferably contains light diffusing fine particles dispersed in a resin layer. The light diffusing fine particles may be used alone or in combination of two or more.

[0056] The above-mentioned light diffusible particles have a suitable refractive index difference with the resin that can constitute the adhesive layer of the present invention, and the adhesive layer of the present invention is given diffusion performance. As light diffusible particles, inorganic particles, polymer particles, etc. can be listed. As the material of inorganic particles, for example, silicon dioxide, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, metal oxides, etc. can be listed. As the material of polymer particles, for example, silicone resin, acrylic resin (for example, comprising polymethacrylate resins such as polymethyl methacrylate), polystyrene resin, polyurethane resin, melamine resin, polyethylene resin, epoxy resin, etc. can be listed.

[0057] As the polymer particles, particles composed of silicone resin are preferred. In addition, as the inorganic particles, particles composed of metal oxides are preferred. As the metal oxides, titanium oxide and barium titanate are preferred, and titanium oxide is more preferred. By having such a structure, the light diffusion property of the adhesive layer of the present invention is more excellent, and the uneven brightness is further suppressed. As the polymer particles, particles composed of silicone resin are preferred. In this case, the color tone of the colorant based on the adhesive layer is not easy to change, and it is stably exerted, and the transparency is more excellent.

[0058] The shape of the light diffusing fine particles is not particularly limited, and may be, for example, a true spherical shape, a flat shape, or an irregular shape.

[0059] From the viewpoint of imparting appropriate light diffusion performance, the average particle size of the light diffusing particles is preferably 0.1 μm or more, more preferably 0.15 μm or more, further preferably 0.2 μm or more, and particularly preferably 0.25 μm or more. In addition, from the viewpoint of preventing the haze value from becoming too high and displaying a high-definition image, the average particle size of the light diffusing particles is preferably 12 μm or less, more preferably 10 μm or less, and further preferably 8 μm or less. The average particle size can be measured, for example, using a Coulter counter.

[0060] The refractive index of the light diffusing fine particles is preferably 1.2 to 5, more preferably 1.25 to 4.5, further preferably 1.3 to 4, and particularly preferably 1.35 to 3.

[0061] From the viewpoint of more efficiently reducing uneven brightness, the absolute value of the refractive index difference between the light diffusing particles and the adhesive constituting the adhesive layer of the present invention (for example, in the adhesive layer of the present invention, the resin layer excluding various additives such as colorants and light diffusing particles) is preferably 0.001 or more, more preferably 0.01 or more, further preferably 0.02 or more, particularly preferably 0.03 or more, and may also be 0.04 or more, or 0.05 or more. In addition, from the viewpoint of preventing the haze value from becoming too high and displaying a high-definition image, the absolute value of the refractive index difference between the light diffusing particles and the resin is preferably 5 or less, more preferably 4 or less, and further preferably 3 or less.

[0062] Regarding the content of the light diffusing particles in the adhesive layer of the present invention, from the viewpoint of imparting appropriate light diffusing properties to the adhesive layer of the present invention, relative to 100 parts by mass of the adhesive constituting the adhesive layer of the present invention, it is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, further preferably 0.1 parts by mass or more, further preferably 0.15 parts by mass or more, further preferably 0.6 parts by mass or more, further preferably 1 parts by mass or more, and may also be 2 parts by mass or more, 5 parts by mass or more, and particularly preferably 10 parts by mass or more. In addition, from the viewpoint of preventing the haze value from becoming too high, the content of the light diffusing particles is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, further preferably 50 parts by mass or less, and may also be 40 parts by mass or less, 30 parts by mass or less, and particularly preferably 20 parts by mass or less, relative to 100 parts by mass of the resin constituting the adhesive layer of the present invention.

[0063] When the adhesive layer of the present invention is the above-mentioned resin layer, the resin constituting the above-mentioned resin layer may include known and commonly used resins, such as acrylic resins, urethane acrylate resins, urethane resins, rubber resins, epoxy resins, epoxy acrylate resins, oxetane resins, silicone resins, silicone acrylic resins, polyester resins, polyether resins (polyvinyl ether, etc.), polyamide resins, fluorine resins, vinyl acetate / vinyl chloride copolymers, modified polyolefins, etc. The above-mentioned resins may be used alone or in combination of two or more.

[0064] In addition, as the resin, a known and commonly used pressure-sensitive adhesive can be used. As the adhesive, for example, acrylic adhesives, rubber adhesives (natural rubber adhesives, synthetic rubber adhesives, mixed systems thereof, etc.), silicone adhesives, polyester adhesives, urethane adhesives, polyether adhesives, polyamide adhesives, fluorine adhesives, etc. can be listed. The adhesives can be used alone or in combination of two or more.

[0065] The acrylic resin is a polymer containing a structural unit derived from an acrylic monomer (a monomer component having a (meth)acryloyl group in a molecule) as a structural unit of the polymer. The acrylic resin may be used alone or in combination of two or more.

[0066] The acrylic resin is preferably a polymer containing the largest number of structural units derived from (meth)acrylate in terms of mass ratio. It should be noted that in this specification, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid" (either or both of "acrylic acid" and "methacrylic acid"), and the same applies to the others.

[0067] Examples of the (meth)acrylate include hydrocarbon group-containing (meth)acrylates. Examples of the (meth)acrylates include (meth)acrylate alkyl esters having a linear or branched aliphatic hydrocarbon group, (meth)acrylates having alicyclic hydrocarbon groups such as (meth)acrylate cycloalkyl esters, and (meth)acrylates having aromatic hydrocarbon groups such as (meth)acrylate aryl esters. The hydrocarbon group-containing (meth)acrylates may be used alone or in combination of two or more.

[0068] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0069] As the alkyl (meth)acrylate, preferably, one having a linear or branched aliphatic hydrocarbon group having a carbon number of 1 to 20 (preferably 1 to 14, more preferably 2 to 10). When the carbon number is within the above range, the glass transition temperature of the acrylic resin can be easily adjusted, and the adhesiveness of the resin layer can be easily made more appropriate.

[0070] Examples of the (meth)acrylate having an alicyclic hydrocarbon group include: (meth)acrylate having a monocyclic aliphatic hydrocarbon ring such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylate having a dicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; (meth)acrylate having a tricyclic aliphatic hydrocarbon ring such as dicyclopentyl (meth)acrylate, dicyclopentyloxyethyl (meth)acrylate, tricyclopentyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate; and the like.

[0071] As the (meth)acrylate having an aromatic hydrocarbon group, for example, phenyl (meth)acrylate, benzyl (meth)acrylate, etc. can be mentioned.

[0072] As the hydrocarbon group-containing (meth)acrylate, preferably, a (meth)acrylate alkyl ester having a linear or branched aliphatic hydrocarbon group is included, and more preferably, a (meth)acrylate having an alicyclic hydrocarbon group is included. In this case, the resin layer has a good balance of adhesiveness and excellent conformability to the unevenness of the adherend.

[0073] In order to properly show the basic characteristics such as adhesiveness and adhesion to the adherend brought by the hydrocarbon group-containing (meth)acrylate in the resin layer, the ratio of the hydrocarbon group-containing (meth)acrylate in all the monomer components constituting the acrylic resin is preferably 40% by mass or more, more preferably 50% by mass or more, and further preferably 60% by mass or more relative to the total amount (100% by mass) of all the monomer components. In addition, from the viewpoint of being able to copolymerize with other monomer components and obtain the effects of the other monomer components, the above ratio is preferably 95% by mass or less, and more preferably 80% by mass or less.

[0074] The ratio of the (meth)acrylic acid alkyl ester having a linear or branched aliphatic hydrocarbon group in all the monomer components constituting the acrylic resin is preferably 30% by mass or more, more preferably 40% by mass or more, relative to the total amount (100% by mass) of all the monomer components. In addition, the ratio is preferably 90% by mass or less, more preferably 70% by mass or less.

[0075] The ratio of the (meth)acrylate having an alicyclic hydrocarbon group in all the monomer components constituting the acrylic resin is preferably 1% by mass or more, more preferably 5% by mass or more, relative to the total amount (100% by mass) of all the monomer components. In addition, the ratio is preferably 30% by mass or less, more preferably 20% by mass or less.

[0076] For the purpose of introducing the first functional group described later, or for the purpose of modifying cohesion, heat resistance, etc., the acrylic resin may contain a structural unit derived from other monomer components copolymerizable with the hydrocarbon-containing (meth)acrylate. Examples of the other monomer components include polar group-containing monomers such as carboxyl-containing monomers, acid anhydride monomers, hydroxyl-containing monomers, glycidyl-containing monomers, sulfonic acid-containing monomers, phosphoric acid-containing monomers, and nitrogen-containing monomers. Each of the other monomer components may be used alone or in combination of two or more.

[0077] Examples of the carboxyl group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Examples of the acid anhydride monomer include maleic anhydride, itaconic anhydride, etc.

[0078] Examples of the hydroxyl-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0079] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and methylglycidyl (meth)acrylate.

[0080] Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0081] As said phosphoric acid group-containing monomer, 2-hydroxyethyl acryloyl phosphate etc. are mentioned, for example.

[0082] Examples of the nitrogen atom-containing monomer include morpholine group-containing monomers such as (meth)acryloylmorpholine, cyano group-containing monomers such as (meth)acrylonitrile, and amide group-containing monomers such as (meth)acrylamide.

[0083] As the above-mentioned polar group-containing monomer constituting the above-mentioned acrylic resin, it is preferable to contain a hydroxyl-containing monomer. By using a hydroxyl-containing monomer, the introduction of the first functional group described later is easy. In addition, the acrylic resin and the above-mentioned resin layer have excellent water resistance, are not easy to fog even when used in a high humidity environment, and have excellent whitening resistance.

[0084] As the hydroxyl group-containing monomer, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.

[0085] In order to appropriately express the basic characteristics such as adhesiveness and adhesion to the adherend brought about by the hydrocarbon group-containing (meth)acrylate in the resin layer, the ratio of the polar group-containing monomer in the total monomer components (100% by mass) constituting the acrylic resin is preferably 5 to 50% by mass, more preferably 10 to 40% by mass. In particular, from the viewpoint of making the resin layer more water-resistant, the ratio of the hydroxyl-containing monomer is preferably within the above range.

[0086] As the above-mentioned other monomer components, it can further include vinyl monomers such as caprolactone adducts of (meth)acrylic acid, vinyl acetate, vinyl propionate, styrene, α-methylstyrene, etc.; diol acrylate monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, etc.; acrylate monomers such as tetrahydrofurfuryl (meth)acrylate, fluoro (meth)acrylate, silicone (meth)acrylate, alkoxy-substituted hydrocarbon group-containing (meth)acrylate (2-methoxyethyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, etc.), etc.

[0087] The ratio of the above-mentioned other monomer components in the total monomer components (100 mass %) constituting the above-mentioned acrylic resin is, for example, about 3 to 50 mass %, or may be 5 to 40 mass %, or 10 to 30 mass %.

[0088] The acrylic resin may contain a structural unit derived from a multifunctional (meth)acrylate copolymerizable with the monomer components constituting the acrylic resin in order to form a crosslinked structure in its polymer backbone. Examples of the multifunctional (meth)acrylate include hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. The multifunctional monomer may be used alone or in combination of two or more.

[0089] In order to properly express the basic properties such as adhesiveness and close adhesion to the adherend brought about by the above-mentioned hydrocarbon group-containing (meth)acrylate in the above-mentioned resin layer, the ratio of the above-mentioned multifunctional monomer in the total monomer components (100% by mass) constituting the above-mentioned acrylic resin is preferably 40% by mass or less, more preferably 30% by mass or less.

[0090] When the above-mentioned resin layer is a radiation-curable resin layer, examples of the above-mentioned resin layer include: a layer containing a base polymer and a radiation-polymerizable monomer component or oligomer component having functional groups such as radiation-polymerizable carbon-carbon double bonds; a layer containing a polymer having radiation-polymerizable functional groups (especially an acrylic resin) as a base polymer, etc.

[0091] As the radiation polymerizable functional group, radiation free radical polymerizable groups such as groups containing carbon-carbon unsaturated bonds such as olefinic unsaturated groups, radiation cation polymerizable groups, etc. can be listed. As the group containing carbon-carbon unsaturated bonds, for example, vinyl, propenyl, isopropenyl, acryloyl, methacryloyl, etc. can be listed. As the radiation cation polymerizable group, epoxy, oxetanyl, oxacyclopentyl, etc. can be listed. Among them, preferably a group containing carbon-carbon unsaturated bonds, more preferably acryloyl, methacryloyl. The radiation polymerizable functional group can be only one type, or it can be more than two types. The position of the radiation polymerizable functional group can be any one of the polymer side chain, the polymer main chain, and the end of the polymer main chain.

[0092] The polymer having radiation polymerizable functional groups can be prepared, for example, by reacting a polymer having a reactive functional group (first functional group) with a functional group (second functional group) capable of reacting with the first functional group to form a bond and a compound having the radiation polymerizable functional group while maintaining the radiation polymerizability of the radiation polymerizable functional group. Therefore, the polymer having radiation polymerizable functional groups preferably includes a structural part derived from the polymer having the first functional group and a structural part derived from the compound having the second functional group and the radiation polymerizable functional group.

[0093] As the combination of the above-mentioned first functional group and the above-mentioned second functional group, for example, carboxyl and epoxy, epoxy and carboxyl, carboxyl and aziridine radicals, aziridine radicals and carboxyl, hydroxyl and isocyanate, isocyanate and hydroxyl etc. can be listed. Among these, from the viewpoint of the ease of reaction tracking, preferably the combination of hydroxyl and isocyanate, the combination of isocyanate and hydroxyl. The above-mentioned combination can be only one, or it can be two or more.

[0094] Examples of the compound having a radiation polymerizable functional group and an isocyanate group include methacryloyl isocyanate, 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate (MOI), m-isopropenyl-α,α-dimethylbenzyl isocyanate, etc. These compounds may be used alone or in combination of two or more.

[0095] The content of the structural part derived from the compound having the second functional group and the radiation polymerizable functional group in the acrylic resin having the radiation polymerizable functional group is preferably 0.5 mol or more, more preferably 1 mol or more, further preferably 3 mol or more, and particularly preferably 10 mol or more, relative to 100 mol of the total amount of the structural part derived from the acrylic resin having the first functional group, from the viewpoint of being able to further promote the curing of the radiation curable resin layer. The above content is, for example, 100 mol or less.

[0096] The molar ratio of the second functional group to the first functional group in the acrylic resin having a radiation polymerizable functional group [second functional group / first functional group] is preferably 0.01 or more, more preferably 0.05 or more, further preferably 0.2 or more, and particularly preferably 0.4 or more, from the viewpoint of further promoting the curing of the radiation curable resin layer. In addition, from the viewpoint of further reducing low molecular weight substances in the radiation curable resin layer, the molar ratio is preferably less than 1.0, more preferably 0.9 or less.

[0097] The acrylic resin is obtained by polymerizing the above-mentioned various monomer components. The polymerization method is not particularly limited, and examples thereof include solution polymerization, emulsion polymerization, bulk polymerization, polymerization by active energy ray irradiation (active energy ray polymerization), etc. In addition, the obtained acrylic resin may be any one of a random copolymer, a block copolymer, a graft copolymer, etc.

[0098] The above-mentioned acrylic resin having a radiation-polymerizable functional group can be produced, for example, by the following method: after polymerizing (copolymerizing) a raw material monomer containing a monomer component having a first functional group to obtain an acrylic resin having a first functional group, the above-mentioned compound having a second functional group and a radiation-polymerizable functional group is subjected to a condensation reaction or an addition reaction with the acrylic resin while maintaining the radiation polymerizability of the radiation-polymerizable functional group.

[0099] Various common solvents can be used in the polymerization of the monomer components. Examples of the above-mentioned solvents include organic solvents such as esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone. The above-mentioned solvents may be used alone or in combination of two or more.

[0100] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the free radical polymerization of the monomer components are not particularly limited and can be appropriately selected for use. It should be noted that the weight average molecular weight of the acrylic polymer can be controlled by the amount of the polymerization initiator and chain transfer agent used and the reaction conditions, and the appropriate amount can be adjusted according to their types.

[0101] As the polymerization initiator used for polymerization of the monomer components, a thermal polymerization initiator, a photopolymerization initiator (photoinitiator), etc. can be used depending on the type of polymerization reaction. The above-mentioned polymerization initiator may be used alone or in combination of two or more.

[0102] The thermal polymerization initiator is not particularly limited, and examples thereof include azo polymerization initiators, peroxide polymerization initiators, redox polymerization initiators, etc. The amount of the thermal polymerization initiator used is preferably 1 part by mass or less, more preferably 0.005 to 1 part by mass, and further preferably 0.02 to 0.5 part by mass, relative to 100 parts by mass of the total amount of all monomer components constituting the acrylic resin having the first functional group.

[0103] Examples of the photopolymerization initiator include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, and titanocene-based photopolymerization initiators. Among them, acetophenone-based photopolymerization initiators are preferred.

[0104] Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, 4-(tert-butyl)dichloroacetophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, and methoxyacetophenone.

[0105] The amount of the photopolymerization initiator used is preferably 0.005 to 1 part by mass, more preferably 0.01 to 0.7 part by mass, and still more preferably 0.18 to 0.5 part by mass relative to 100 parts by mass of the total amount of all monomer components constituting the acrylic resin. If the amount used is 0.005 part by mass or more (particularly 0.18 part by mass or more), there is a tendency that the molecular weight of the acrylic resin can be easily controlled to be relatively small, and the unevenness followability of the resin layer becomes better.

[0106] The reaction of the acrylic resin having the first functional group and the compound having the second functional group and the radiation polymerizable functional group can be carried out by stirring in a solvent in the presence of a catalyst. As the solvent, the above-mentioned solvents can be listed. The catalyst is appropriately selected according to the combination of the first functional group and the second functional group. The reaction temperature in the reaction is, for example, 5 to 100° C., and the reaction time is, for example, 1 to 36 hours.

[0107] The acrylic resin may have a structural part derived from a crosslinking agent. For example, the acrylic resin may be crosslinked to further reduce the low molecular weight substances in the resin layer. In addition, the weight average molecular weight of the acrylic resin may be increased. It should be noted that when the acrylic resin has a radiation polymerizable functional group, the crosslinking agent is a substance that crosslinks the functional groups other than the radiation polymerizable functional group (e.g., the first functional groups, the second functional groups, or the first functional group and the second functional group). The crosslinking agent may be used alone or in combination of two or more.

[0108] Examples of the crosslinking agent include isocyanate crosslinking agents, epoxy crosslinking agents, melamine crosslinking agents, peroxide crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, amine crosslinking agents, silicone crosslinking agents, and silane crosslinking agents. Among the crosslinking agents, isocyanate crosslinking agents and epoxy crosslinking agents are preferred, and isocyanate crosslinking agents are more preferred, from the viewpoint of excellent adhesion to optical semiconductor elements and a small amount of impurity ions.

[0109] Examples of the isocyanate crosslinking agent (polyfunctional isocyanate compound) include lower aliphatic polyisocyanates such as 1,2-ethylene diisocyanate, 1,4-butylene diisocyanate, and 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated xylene diisocyanate; aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate. Examples of the isocyanate crosslinking agent include trimethylolpropane / toluene diisocyanate adducts, trimethylolpropane / hexamethylene diisocyanate adducts, and trimethylolpropane / xylylene diisocyanate adducts.

[0110] The content of the structural part derived from the crosslinking agent is not particularly limited, but is preferably 5 parts by mass or less, more preferably 0.001 to 5 parts by mass, and further preferably 0.01 to 3 parts by mass, based on 100 parts by mass of the total amount of the acrylic resin excluding the structural part derived from the crosslinking agent.

[0111] The resin layer may contain other components other than the above components within the scope of not damaging the effect of the present invention. As the above other components, curing agent, crosslinking accelerator, tackifying resin (rosin derivatives, polyterpene resins, petroleum resins, oil-soluble phenols, etc.), oligomers, anti-aging agents, fillers (metal powder, organic fillers, inorganic fillers, etc.), antioxidants, plasticizers, softeners, surfactants, antistatic agents, surface lubricants, leveling agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, granular materials, foil-like materials, etc. can be listed. The above other components can be used only one, or two or more.

[0112] The L value of the adhesive layer of the present invention when it is bonded to an aluminum foil is measured from the adhesive layer side with a 10° field of view and a light source of D65. * a * b * L in (SCI) * (SCI), and / or, L * a * b * L in (SCE) * (SCE) is preferably 70 or less, more preferably 60 or less, and still more preferably 50 or less. * (SCE) is more preferably 40 or less. When the light reflected by the object includes regular reflected light and diffuse reflected light, the regular reflected light is light that is difficult to be recognized by the naked eye. * (SCE) is the value measured for reflected light excluding regular reflected light, L * When (SCE) is 70 or less, the appearance of the image display device when viewed with the naked eye is excellent. * (SCI) is a value measured for reflected light including regular reflected light. Although it has a low correlation with the visibility of the naked eye, it can measure a color tone close to the true color tone of the object. * When (SCI) is 70 or less, the image display device has excellent visibility and appearance even under the influence of the environment. * (SCI) is called "Reflection L * (SCI)”, the above L * (SCE) is called "Reflection L * (SCE)". Reflection L *(SCI) and Reflection L * (SCE) can be specifically measured by the method described in the Examples. * (SCI) and Reflection L * (SCE) can also be measured in a state where a transparent layer such as a release liner is provided on the surface of the pressure-sensitive adhesive layer opposite to the aluminum foil.

[0113] For the adhesive layer of the present invention, the circular diameter measured by the following light diffusion effect confirmation test using a measurement sample bonded to a glass plate is preferably 60 mm or more (especially higher than 60 mm), more preferably 65 mm or more, further preferably 70 mm or more, and particularly preferably 80 mm or more. When the circular diameter is 60 mm or more, brightness unevenness is further suppressed.

[0114] <Light diffusion effect confirmation test>

[0115] An LED light is set on the screen, and the glass plate is closely attached to the LED light. When the LED light irradiates the screen through the glass plate, the position of a circular light with a diameter of 16 mm appears on the screen as the position of the LED light. Then, in a state where the glass plate side of the measurement sample obtained by attaching the adhesive layer of the present invention to the glass plate is closely attached to the LED light, the diameter of the circular light that appears when the LED light irradiates the screen through the glass plate and the adhesive layer is measured. It should be noted that the measurement can also be performed in a state where a transparent layer such as a release liner is provided on the surface of the adhesive layer on the opposite side of the glass plate.

[0116] The adhesive layer of the present invention may be in any form, for example, an emulsion type, a solvent type (solution type), an active energy ray curable type, a heat-melting type (hot melt type), etc. As the above-mentioned active energy ray, for example, ionizing radiation such as α-ray, β-ray, γ-ray, neutron ray, electron ray, ultraviolet ray, etc. can be listed, and ultraviolet ray is particularly preferred. That is, the above-mentioned active energy ray curable adhesive layer is preferably an ultraviolet curable adhesive layer.

[0117] The adhesive layer of the present invention can be manufactured, for example, by applying (coating) an adhesive composition for forming an adhesive layer on a release liner, and drying and curing the obtained adhesive composition layer; or by applying (coating) the above-mentioned adhesive composition on a release liner, and irradiating the obtained adhesive composition layer with active energy rays to cure it. In addition, it can also be further heated and dried as needed.

[0118] The adhesive composition forming the adhesive layer of the present invention contains, for example, the above-mentioned colorant, the above-mentioned light diffusing particles, and other components as required. When the adhesive layer of the present invention is the above-mentioned resin layer, the above-mentioned adhesive composition may contain a resin forming the above-mentioned resin layer, a monomer component as a constituent component of the resin, an oligomer of the monomer component, a partial polymer, and other binder components. As an adhesive composition containing a resin, for example, a so-called solvent-based adhesive composition can be listed. In addition, as an adhesive composition containing a monomer component, an oligomer component, or a partial polymer, for example, a so-called active energy ray-curable adhesive composition can be listed.

[0119] The adhesive layer of the present invention is preferably used in a sheet for sealing one or more optical semiconductor elements arranged on a substrate. When the optical semiconductor element is sealed using a sheet including the adhesive layer of the present invention, the antireflection property of the substrate surface is excellent, and brightness unevenness caused by light emitted by the optical semiconductor element is unlikely to occur. In addition, color shift is unlikely to occur.

[0120] [Laminated Sheet]

[0121] The adhesive layer of the present invention can be stacked with other layers to form a laminated sheet. As the above-mentioned other layers, other adhesive layers, resin layers, substrate portions described later, layers with anti-glare properties, layers with anti-reflective properties, etc., except the adhesive layer of the present invention can be listed. In addition, the above-mentioned laminated sheet can directly or indirectly have multiple layers of the adhesive layer of the present invention. At this time, multiple adhesive layers of the present invention can be layers with the same thickness, composition, physical properties, etc., or different layers.

[0122] The laminated sheet is preferably a sheet for sealing one or more optical semiconductor elements arranged on a substrate (sometimes referred to as an "optical semiconductor element sealing sheet"). The optical semiconductor element sealing sheet at least comprises a sealing resin layer. It should be noted that, in this specification, "sealing an optical semiconductor element" means burying at least a portion of the optical semiconductor element in the sealing resin layer, or following and covering it with the sealing resin layer. The sealing resin layer has such flexibility that at least a portion of the optical semiconductor element can be buried, or followed and covered with the sealing resin layer.

[0123] When the adhesive layer of the present invention is used as a constituent element of a sheet for sealing an optical semiconductor element, it functions as a layer having both the performance of diffusing light and the performance of preventing light reflection caused by metal wiring etc. provided on a substrate. Therefore, by using the adhesive layer of the present invention, compared with the case where two layers, a light diffusing functional layer for the purpose of diffusing light and a coloring layer for the purpose of preventing light reflection caused by metal wiring etc. provided on a substrate, are used as constituent elements of the sheet for sealing an optical semiconductor element, a thickness equivalent to that of one layer can be achieved, so that it can be made thinner, which contributes to the downsizing of optical semiconductor devices.

[0124] When the laminated sheet is the optical semiconductor element sealing sheet, the adhesive layer of the present invention is preferably a layer constituting the sealing resin layer. The sealing resin layer may include a non-diffusion functional layer not intended to exert a light diffusion function as the other layer.

[0125] The non-diffusion functional layer is a non-colored layer different from the colored layer described later. The non-diffusion functional layer may be a colorless layer or slightly colored. The non-diffusion functional layer may be transparent or non-transparent.

[0126] The haze value (initial haze value) of the non-diffusing functional layer is not particularly limited. From the viewpoint of improving the light transmittance of the laminated sheet, it is preferably less than 30%, more preferably less than 10%, further preferably less than 5%, particularly preferably less than 1%, and may also be less than 0.5%. It should be noted that the lower limit of the haze value of the non-diffusing functional layer is not particularly limited.

[0127] The total light transmittance of the non-diffusing functional layer is not particularly limited, and from the viewpoint of improving the light transmittance of the laminated sheet, it is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and particularly preferably 90% or more. In addition, the upper limit of the total light transmittance of the non-diffusing functional layer is not particularly limited, and may be less than 100%, or less than 99.9%, or less than 99%.

[0128] The haze value and total light transmittance of the non-diffusing functional layer are values ​​of a single layer and can be measured by the method specified in JIS K7136 and JIS K7361-1, and can be controlled by the type and thickness of the non-diffusing functional layer.

[0129] The non-diffusion functional layer is preferably the resin layer. In this case, the constituent monomers of the resin in the non-diffusion functional layer and the resin that can be contained in the adhesive layer of the present invention and the composition ratio thereof may be the same or different.

[0130] From the viewpoint of improving the light transmittance of the laminated sheet, the content of the colorant and / or light diffusing fine particles in the non-diffusing functional layer is preferably less than 0.01 parts by mass, more preferably less than 0.005 parts by mass based on 100 parts by mass of the resin constituting the non-diffusing functional layer.

[0131] When the sealing resin layer comprises the adhesive layer of the present invention and the non-diffusion functional layer, the non-diffusion functional layer is preferably located on the opposite side to the adherend compared to the adhesive layer of the present invention, and more preferably located on the surface of the sealing resin layer. When the non-diffusion functional layer is provided at the above position, when the optical semiconductor element sealing sheet is attached, even if the surface of the adhesive layer of the present invention has a concave-convex shape, the surface of the adhesive layer of the present invention is prevented from being exposed on the surface of the sealing resin layer on the opposite side to the optical semiconductor element, and the surface of the sealing resin layer on the front side is easy to become flat, and is not easy to cause random reflection of external light, and the appearance of the optical semiconductor device is improved both when it is turned off and when it is lit.

[0132] The above-mentioned sealing resin layer may have other layers except the adhesive layer of the present invention and the above-mentioned non-diffusion functional layer. As the above-mentioned other layers, a colored layer, a diffusion functional layer, etc. can be listed. The above-mentioned colored layer and the above-mentioned diffusion functional layer are layers that do not belong to the adhesive layer of the present invention. The above-mentioned colored layer is a layer for the purpose of preventing the reflection of light caused by the metal wiring etc. arranged on the substrate, and is not for the purpose of exerting the function of diffusing light. In addition, the above-mentioned diffusion functional layer is a non-colored layer for the purpose of exerting the function of diffusing light, and is not for the purpose of preventing the reflection of light caused by the metal wiring etc. arranged on the substrate. The above-mentioned diffusion functional layer can be a colorless layer, and can also be slightly colored. The above-mentioned diffusion functional layer can be transparent or non-transparent.

[0133] The total number of layers constituting the sealing resin layer is not particularly limited, and may be 2 or more, or 3 or more. From the viewpoint of reducing the thickness of the optical semiconductor device, the total number of layers may be, for example, 10 or less, 5 or less, or 4 or less.

[0134] The coloring layer contains at least the colorant. The coloring layer is preferably the resin layer. The content of the colorant in the coloring layer is preferably 0.2% by mass or more, more preferably 0.4% by mass or more, relative to the total amount of the coloring layer (100% by mass). In addition, the content of the colorant is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 3% by mass or less.

[0135] The haze value (initial haze value) of the colored layer is preferably 50% or less, more preferably 40% or less, further preferably 30% or less, and particularly preferably 20% or less. In addition, the haze value of the colored layer is preferably 1% or more, more preferably 3% or more, further preferably 5% or more, particularly preferably 8% or more, and may be 10% or more.

[0136] The total light transmittance of the coloring layer is preferably 40% or less, more preferably 30% or less, further preferably 25% or less, and particularly preferably 20% or less. In addition, the total light transmittance of the coloring layer is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and may be 2.5% or more, or 3% or more.

[0137] The haze value and total light transmittance of the colored layer are values ​​of a single layer, and can be measured by the method specified in JIS K7136 and JIS K7361-1, and can be controlled by the type, thickness, type and blending amount of the colorant.

[0138] The diffusion function layer preferably contains the light diffusing particles. The diffusion function layer is preferably the resin layer. The diffusion function layer may be transparent or non-transparent. The content ratio of the colorant in the diffusion function layer is preferably less than 0.2% by mass, more preferably less than 0.1% by mass, further preferably less than 0.05% by mass, and may also be less than 0.01% by mass or less than 0.005% by mass relative to the total amount 100% by mass of the diffusion function layer.

[0139] The content of the light diffusing fine particles in the diffusion functional layer is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, further preferably 0.1 parts by mass or more, and particularly preferably 0.15 parts by mass or more relative to 100 parts by mass of the resin constituting the diffusion functional layer. In addition, the content of the light diffusing fine particles is preferably 80 parts by mass or less, more preferably 70 parts by mass or less relative to 100 parts by mass of the resin constituting the diffusion functional layer.

[0140] The haze value (initial haze value) of the diffusion functional layer is preferably 30% or more, more preferably 40% or more, further preferably 50% or more, particularly preferably 60% or more, and may be 70% or more, 80% or more, 90% or more, 95% or more, 97% or more, and further preferably around 99.9%. It should be noted that the upper limit of the haze value of the diffusion functional layer may be 100%.

[0141] The total light transmittance of the diffusion function layer is preferably 40% or more, more preferably 60% or more, further preferably 70% or more, and particularly preferably 80% or more. In addition, the total light transmittance of the diffusion function layer may be less than 100%, or less than 99.9%, or less than 99%.

[0142] The haze value and total light transmittance of the diffusion function layer are values ​​of a single layer and can be measured by the method specified in JIS K7136 and JIS K7361-1, and can be controlled by the type and thickness of the diffusion function layer and the type and amount of light diffusing fine particles.

[0143] Each layer constituting the above-mentioned laminated sheet may or may not have adhesiveness and / or adhesion independently. It is particularly preferred that each layer constituting the above-mentioned sealing resin layer has adhesiveness and / or adhesion. By having such a structure, the above-mentioned sealing resin layer can easily seal the optical semiconductor element. In addition, the closeness and / or adhesion between the layers are excellent, and the sealing of the optical semiconductor element is more excellent. It is particularly preferred that at least the layer in contact with the optical semiconductor element has adhesiveness and / or adhesion. By having such a structure, the tracking and embedding properties of the optical semiconductor element based on the sealing resin layer are excellent. As a result, the appearance is excellent even in the case of a high height difference caused by the optical semiconductor element. It should be noted that the layers other than the layers in contact with the optical semiconductor element may not have adhesiveness and / or adhesion. At this time, the adhesion between adjacent sealing resin layers in a flat state is low, and when adjacent small-sized stacks (stacks in which the sealing resin layers seal the optical semiconductor elements arranged on the substrate) are pulled apart, it is not easy to cause damage to the sheets or adhesion of adjacent sealing resin layers.

[0144] Each layer constituting the sealing resin layer may be independently a radiation-curable resin layer or a non-radiation-curable resin layer.

[0145] The sealing resin layer may be a single-layer structure formed by a single layer of the adhesive layer of the present invention, or a laminated structure including the adhesive layer of the present invention. Examples of the laminated structure of the sealing resin layer include: a structure consisting of two layers of the adhesive layer of the present invention; a structure consisting of two layers, one of which is the adhesive layer of the present invention, and the other is the adhesive layer of the present invention, a coloring layer, a diffusion function layer, or a non-diffusion function layer (in different order); a structure consisting of three layers, one of which is the adhesive layer of the present invention, and the other two layers are respectively the adhesive layer of the present invention, a coloring layer, a diffusion function layer, or a non-diffusion function layer (in different order); a structure consisting of four layers, one of which is the adhesive layer of the present invention, and the other three layers are respectively the adhesive layer of the present invention, a coloring layer, a diffusion function layer, or a non-diffusion function layer (in different order), etc. More specifically, for example, [the adhesive layer of the present invention], [the adhesive layer of the present invention / non-diffusion function layer], [the adhesive layer of the present invention / diffusion function layer], [the adhesive layer of the present invention / non-diffusion function layer / diffusion function layer] (the above is the order from the optical semiconductor element side), etc.

[0146] <Base Material>

[0147] The laminated sheet may include a substrate portion. In addition, in the optical semiconductor element sealing sheet, the sealing resin layer may be provided on at least one surface of the substrate portion. When the substrate portion is provided on the side of the sealing resin layer opposite to the optical semiconductor element side in the optical semiconductor element sealing sheet, the surface of the sealing resin layer can be made flat, thereby making it less likely to produce random reflections of light, and improving the appearance of the optical semiconductor device both when it is extinguished and when it is illuminated. In addition, by forming the anti-glare layer and anti-reflection layer described later on the substrate portion, the optical semiconductor device can be given anti-glare and anti-reflection properties. In addition, the support body of the adhesive layer of the present invention in the laminated sheet is provided with the substrate portion, so that the laminated sheet has excellent handleability. It should be noted that the substrate portion may not necessarily be provided.

[0148] The substrate part may be a single layer or a plurality of layers having the same or different compositions, thicknesses, etc. When the substrate part is a plurality of layers, each layer may be bonded together by other layers such as an adhesive layer. It should be noted that the substrate layer used in the substrate part is a part that is bonded to the adherend together with the adhesive layer and the sealing resin layer of the present invention, and the release liner that is peeled off when the laminate is used (when bonded) and the surface protection film that is only used to protect the surface of the substrate part are not included in the "substrate part".

[0149] Examples of the substrate layer constituting the substrate portion include glass, plastic substrates (particularly plastic films), etc. Examples of the resin constituting the plastic substrate include low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, ultra-low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolymer polypropylene, polybutene, polymethylpentene, ionomers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylate (random, alternating) copolymers, ethylene-vinyl acetate copolymers (EVA), ethylene-propylene copolymers, cyclic olefin polymers, ethylene-butene copolymers, ethylene-hexene copolymers, and the like. Polyolefin resins such as olefin copolymers; polyurethane; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT); polycarbonate; polyimide resins; polyetheretherketone; polyetherimide; polyamides such as aramid and wholly aromatic polyamide; polyphenylene sulfide; fluororesin; polyvinyl chloride; polyvinylidene chloride; cellulose resins such as triacetyl cellulose (TAC); silicone resin; acrylic resins such as polymethyl methacrylate (PMMA); polysulfone; polyarylate; polyvinyl acetate, etc. The above resins may be used alone or in combination of two or more. The above substrate layer may also be various optical films such as anti-reflection (AR) films, polarizing plates, and phase difference plates.

[0150] The thickness of the plastic film is preferably 20 to 300 μm, more preferably 40 to 250 μm. When the thickness is 20 μm or more, the support and handling properties of the laminated sheet are further improved. When the thickness is 300 μm or less, the overall thickness when attached to an adherend can be further reduced.

[0151] For the purpose of improving adhesion and retention, the surface of the substrate having the adhesive layer or the sealing resin layer may be subjected to physical treatments such as corona discharge treatment, plasma treatment, sandblasting treatment, ozone exposure treatment, flame exposure treatment, high voltage electric shock exposure treatment, ionizing radiation treatment, etc.; chemical treatments such as chromic acid treatment; and surface treatments such as easy-adhesion treatment based on a coating agent (primer). The surface treatment for improving adhesion is preferably applied to the entire surface of the adhesive layer side or the sealing resin layer side of the substrate.

[0152] From the viewpoint of excellent function as a support and surface scratch resistance, the thickness of the substrate is preferably 5 μm or more, more preferably 10 μm or more, and from the viewpoint of better transparency, the thickness of the substrate is preferably 300 μm or less, more preferably 250 μm or less.

[0153] <Laminated Sheet>

[0154] The above-mentioned laminated sheet may have a layer with anti-glare and / or anti-reflection properties. By having such a structure, the gloss and reflection of light can be suppressed when the optical semiconductor element is sealed, making the appearance better. As the above-mentioned layer with anti-glare properties, an anti-glare treatment layer can be listed. As the above-mentioned layer with anti-reflection properties, an anti-reflection treatment layer can be listed. The anti-glare treatment and the anti-reflection treatment can be implemented by well-known and commonly used methods, respectively. The above-mentioned layer with anti-glare properties and the above-mentioned layer with anti-reflection properties can be the same layer or different layers. The above-mentioned layer with anti-glare and / or anti-reflection properties can have only one layer or more than two layers. In addition, the above-mentioned layer with anti-glare and / or anti-reflection properties is preferably provided on one surface of the above-mentioned laminated sheet.

[0155] Figure 1 and Figure 2 1 is a cross-sectional view showing one embodiment of a sheet for optical semiconductor element sealing having an adhesive layer of the present invention. Figure 1 and Figure 2 As shown, the optical semiconductor element sealing sheet 1 can be used to seal one or more optical semiconductor elements arranged on a substrate, and includes a base material portion 4 and a sealing resin layer 2 formed on the base material portion 4. The base material portion 4 is composed of a base film 41 and a functional layer 42 as a surface treatment layer, but may be composed of the base film 41 without the functional layer 42.

[0156] Figure 1 In the optical semiconductor element sealing sheet 1 shown, the sealing resin layer 2 is formed of a single layer of the present invention's adhesive layer 21. A release liner 3 is attached to one surface of the present invention's adhesive layer 21, and a base material 4 is attached to the other surface.

[0157] Figure 2 In the optical semiconductor element sealing sheet 1 shown, the sealing resin layer 2 is formed of a laminate of the adhesive layer 21 of the present invention and the non-diffusion functional layer 22. The non-diffusion functional layer 22 is directly laminated on the adhesive layer 21 of the present invention. A release liner 3 is adhered to the adhesive layer 21 of the present invention, and a base material 4 is adhered to the non-diffusion functional layer 22.

[0158] Figure 1 and Figure 2In the figure, the functional layer 42 is a layer not included in the above-mentioned sealing resin layer, and layers that can impart various functions to the above-mentioned optical semiconductor element sealing sheet can be listed. As the above-mentioned functional layer, for example, a layer comprising a surface treatment layer can be listed. By having such a structure, the optical semiconductor element sealing sheet laminated with a functional layer comprising a surface treatment layer has excellent light diffusion and excellent light extraction efficiency. As the above-mentioned surface treatment layer, an anti-glare treatment layer (anti-glare treatment layer), an anti-reflection treatment layer, a hard coating treatment layer, etc. can be listed. The above-mentioned functional layer can be laminated on the above-mentioned sealing resin layer in the above-mentioned optical semiconductor element sealing sheet, and can also be laminated on the above-mentioned substrate portion when the above-mentioned substrate portion is provided, preferably laminated on the above-mentioned substrate portion, and preferably laminated on the opposite side of the above-mentioned substrate portion to the side having the above-mentioned sealing resin layer.

[0159] The haze value (initial haze value) of the laminated sheet is not particularly limited, but is preferably 80% or more, more preferably 85% or more, further preferably 90% or more, and particularly preferably 95% or more, from the viewpoint of suppressing uneven brightness and making the appearance more excellent. It should be noted that the upper limit of the haze value is not particularly limited.

[0160] The total light transmittance of the laminated sheet is not particularly limited, but is preferably 40% or less, more preferably 30% or less, and further preferably 20% or less from the viewpoint of further improving the function of preventing reflection of metal wiring and the like and improving contrast. In addition, from the viewpoint of ensuring brightness, the total light transmittance is preferably 0.5% or more.

[0161] The haze value and total light transmittance can be measured by the methods specified in JIS K7136 and JIS K7361-1, respectively, and can be controlled by the lamination order, type, thickness, etc. of each layer constituting the laminated sheet, such as the sealing resin layer and the substrate.

[0162] The thickness of the adhesive layer of the present invention is preferably 5 to 100 μm, more preferably 10 to 80 μm, and further preferably 20 to 70 μm. When the thickness is 5 μm or more, the anti-reflection property and light diffusion function are more excellent. When the thickness is 100 μm or less, it is easier to ensure light transmittance. In addition, the adhesive layer of the present invention can be set to a thickness of 100 μm or less while having the functions of both the conventional coloring layer and the light diffusion functional layer.

[0163] The thickness of the non-diffusing functional layer is, for example, 5 to 480 μm, preferably 5 to 100 μm, more preferably 10 to 80 μm, and further preferably 20 to 70 μm. When the thickness is 5 μm or more, the sealing property of the optical semiconductor element becomes better. When the thickness is 480 μm or less, it is easier to ensure the brightness of the optical semiconductor element when it emits light.

[0164] The thickness of the sealing resin layer is, for example, 100 to 500 μm, preferably 120 to 400 μm, and more preferably 150 to 300 μm. When the thickness is 100 μm or more, the sealing property of the optical semiconductor element becomes better. When the thickness is 500 μm or less, the thickness of the optical semiconductor device becomes thinner.

[0165] The thickness of the laminated sheet (e.g., the optical semiconductor element sealing sheet) is not particularly limited, but is preferably 500 μm or less, more preferably 400 μm or less, and further preferably 300 μm or less. The adhesive layer of the present invention has both the functions of the conventional coloring layer and the light diffusion functional layer, and thus can be thinner than the conventional laminated sheet having both the coloring layer and the light diffusion functional layer. In addition, the thickness is, for example, 10 μm or more.

[0166] [Release liner]

[0167] The adhesive layer of the present invention and the sealing resin layer can be formed on the peeling treatment surface on the release liner. When the adhesive layer of the present invention and the sealing resin layer are formed on the substrate portion, for the release liner, the adhesive layer of the present invention and the sealing resin layer on the opposite side of the substrate layer become the side in contact with the release liner. When the substrate portion is not provided, the two sides of the adhesive layer of the present invention and the sealing resin layer can also be the side in contact with the release liner. The release liner is used as a protective material for the adhesive layer of the present invention and the laminated sheet and is peeled off when attached to an adherend. It should be noted that the release liner may not be provided.

[0168] Examples of the release liner include polyethylene terephthalate (PET) films, polyethylene films, polypropylene films, plastic films surface-coated with a release agent such as a fluorine-based release agent or a long-chain alkyl acrylate-based release agent, and paper.

[0169] The thickness of the release liner is, for example, 10 to 200 μm, preferably 15 to 150 μm, and more preferably 20 to 100 μm. When the thickness is 10 μm or more, the release liner is not easily broken by cutting during processing. When the thickness is 200 μm or less, it is easier to peel the release liner from the laminated sheet during use.

[0170] [Method for producing optical semiconductor element sealing sheet]

[0171] An embodiment of the method for producing the optical semiconductor element sealing sheet is described below. Figure 1The optical semiconductor element sealing sheet 1 shown is used to prepare the adhesive layer 21 of the present invention sandwiched between the release-treated surfaces of two release liners. One of the release liners attached to the adhesive layer 21 of the present invention is the release liner 3. Next, one of the release liners attached to the adhesive layer 21 of the present invention (the release liner that is not the release liner 3) is peeled off to expose the surface of the adhesive layer 21 of the present invention, and the exposed surface is attached to the substrate 4. In this way, a substrate 4 in which the adhesive layer 21 of the present invention and the release liner 3 are sequentially laminated can be prepared. Figure 1 The optical semiconductor element sealing sheet 1 is shown.

[0172] In addition, about Figure 2 The optical semiconductor element sealing sheet 1 shown is, for example, prepared by separately preparing the adhesive layer 21 of the present invention and the non-diffusion functional layer 22, each of which is sandwiched by the release-treated surfaces of two release liners. One release liner bonded to the adhesive layer 21 of the present invention is the release liner 3. Next, one of the release liners bonded to the non-diffusion functional layer 22 is peeled off to expose the surface of the non-diffusion functional layer 22, and the exposed surface is bonded to the substrate portion 4. Then, one of the release liners bonded to the adhesive layer 21 of the present invention (the release liner that is not the release liner 3) is peeled off, and the exposed surface of the adhesive layer 21 of the present invention is bonded to the surface of the non-diffusion functional layer 22 exposed by peeling off the release liner on the surface of the non-diffusion functional layer 22. It should be noted that the lamination of various layers can be performed using a known roller or laminator. In this way, a sheet in which the non-diffusion functional layer 22, the adhesive layer 21 of the present invention and the release liner 3 are sequentially laminated on the substrate portion 4 can be prepared. Figure 2 The optical semiconductor element sealing sheet 1 is shown.

[0173] [Optical semiconductor device]

[0174] The optical semiconductor device sealing sheet of the present invention can be used to manufacture an optical semiconductor device such as a display. The optical semiconductor device manufactured using the optical semiconductor device sealing sheet comprises: a substrate, an optical semiconductor device arranged on the substrate, and the optical semiconductor device sealing sheet or a cured product obtained by curing the sheet for sealing the optical semiconductor device. The cured product is a cured product obtained by curing the radiation-curable resin layer by irradiation with radiation when the optical semiconductor device sealing sheet comprises a radiation-curable resin layer.

[0175] Examples of the optical semiconductor element include light emitting diodes (LEDs) such as a blue light emitting diode, a green light emitting diode, a red light emitting diode, and an ultraviolet light emitting diode.

[0176] In the above-mentioned optical semiconductor device, the above-mentioned optical semiconductor element sealing sheet has excellent followability to convex and concave portions when the optical semiconductor element is used as a convex portion and the gaps between multiple optical semiconductor elements are used as concave portions, and has excellent followability and filling properties of the optical semiconductor element, so it is preferred to seal multiple optical semiconductor elements at one time.

[0177] The height of the optical semiconductor element on the substrate (the height from the substrate surface to the end of the optical semiconductor element on the front side) is preferably 500 μm or less. When the height is 500 μm or less, the sealing resin layer has better followability to the uneven shape.

[0178] Figure 3 Show use Figure 1 One embodiment of an optical semiconductor device of the optical semiconductor element sealing sheet 1 shown. Figure 3 The optical semiconductor device 10 shown includes: a substrate 5, a plurality of optical semiconductor elements 6 arranged on one surface of the substrate 5, a sealing resin layer 7 for sealing the optical semiconductor elements 6, and a base material portion 4 laminated on the sealing resin layer 7. The plurality of optical semiconductor elements 6 are sealed by the sealing resin layer 7 at one time. The sealing resin layer 7 is formed of a single layer of a diffusion function coloring layer 71. The diffusion function coloring layer 71 follows the concave-convex shape formed by the plurality of optical semiconductor elements 6 and is in close contact with the optical semiconductor elements 6 and the substrate 5, thereby burying the optical semiconductor elements 6. In addition, the diffusion function coloring layer 71 follows the concave-convex shape, so that the interface on the optical semiconductor element 6 side has a concave-convex shape, and the interface on the other side becomes flat.

[0179] Figure 4 Show use Figure 2 One embodiment of an optical semiconductor device of the optical semiconductor element sealing sheet 1 shown. Figure 4 The optical semiconductor device 10 shown includes: a substrate 5, a plurality of optical semiconductor elements 6 arranged on one surface of the substrate 5, a sealing resin layer 7 for sealing the optical semiconductor elements 6, and a base material portion 4 laminated on the sealing resin layer 7. The plurality of optical semiconductor elements 6 are sealed by the sealing resin layer 7 at one time. The sealing resin layer 7 is formed by laminating a diffusion function coloring layer 71 and a non-diffusion function layer 73. The diffusion function coloring layer 71 follows the concave-convex shape formed by the plurality of optical semiconductor elements 6 and is in close contact with the optical semiconductor elements 6 and the substrate 5, thereby burying the optical semiconductor elements 6. In addition, the diffusion function coloring layer 71 follows the concave-convex shape, so that the interface on the optical semiconductor element 6 side has a concave-convex shape, and the interface on the other side becomes flat.

[0180] The sealing resin layer 7 is formed by the sealing resin layer 2. Specifically, in the optical semiconductor element sealing sheet 1, when the sealing resin layer 2 does not have a radiation-curable resin layer, the sealing resin layer 2 becomes the sealing resin layer 7 in the optical semiconductor device 10. On the other hand, in the optical semiconductor element sealing sheet 1, when the sealing resin layer 2 has a radiation-curable resin layer, for example, when the adhesive layer 21 of the present invention is a radiation-curable resin layer, the diffusion functional coloring 71 is formed by curing the adhesive layer 21 of the present invention to become the sealing resin layer 7.

[0181] It should be noted that in Figure 4 In the optical semiconductor device 10 shown in FIG. 1 , the optical semiconductor element 6 is completely buried in the diffusion function color layer 71 and sealed, and is indirectly sealed by the non-diffusion function layer 72. That is, the optical semiconductor element 6 is sealed by the sealing resin layer 7 formed by the laminate of the diffusion function color layer 71 and the non-diffusion function layer 72. The above optical semiconductor device is not limited to this method. For example, Figure 5 As shown, the optical semiconductor element 6 may be completely buried in the diffusion function colored layer 71 and the non-diffusion function layer 72 to be sealed.

[0182] The optical semiconductor device may be a device in which each optical semiconductor device is laid out in a tile. That is, the optical semiconductor device may be a device in which a plurality of optical semiconductor devices are arranged in a tile shape in a planar direction.

[0183] The optical semiconductor device preferably has a self-luminous display device. In addition, the self-luminous display device can be combined with a display panel as required to form a display body as an image display device. The optical semiconductor element at this time is an LED element. As the self-luminous display device, LED displays, backlights, or organic electroluminescent (organic EL) display devices can be listed. The backlight is particularly preferably a whole-surface direct-down backlight. The backlight, for example, includes a stacked body having the substrate and a plurality of optical semiconductor elements arranged on the substrate as at least a part of the constituent members. For example, in the self-luminous display device, a metal wiring layer for transmitting a light control signal to each LED element is stacked on the substrate. Each LED element emitting each color light of red (R), green (G), and blue (B) is alternately arranged on the substrate with a metal wiring layer between them. The metal wiring layer is formed of a metal such as copper, which adjusts the light emission degree of each LED element to display each color.

[0184] The optical semiconductor element sealing sheet can be used in an optical semiconductor device that is bent for use, such as an optical semiconductor device having a bendable image display device (flexible display) (especially a foldable image display device (foldable display)). Specifically, it can be used in a foldable backlight and a foldable self-luminous display device.

[0185] The optical semiconductor element sealing sheet is excellent in the followability and embedding property of the optical semiconductor element, and therefore can be preferably used in both the case where the optical semiconductor device is a mini LED display device and the case where it is a micro LED display device.

[0186] [Method for manufacturing optical semiconductor device]

[0187] The optical semiconductor device can be produced, for example, by bonding the optical semiconductor element sealing sheet to a substrate on which an optical semiconductor element is arranged and sealing the optical semiconductor element with a sealing resin layer.

[0188] (Sealing process)

[0189] In the method for manufacturing an optical semiconductor device using the above-mentioned optical semiconductor element sealing sheet, there is a sealing step as follows: the above-mentioned optical semiconductor element sealing sheet is bonded to a substrate on which an optical semiconductor element is arranged, and the optical semiconductor element is sealed with a sealing resin layer. In the above-mentioned sealing step, specifically, first, the release liner is peeled off from the above-mentioned optical semiconductor element sealing sheet to expose the sealing resin layer. Then, in a laminate (optical component, etc.) having a substrate and an optical semiconductor element (preferably a plurality of optical semiconductor elements) arranged on the above-mentioned substrate, the substrate surface on which the optical semiconductor element is arranged is bonded to the sealing resin layer layer as the exposed surface of the above-mentioned optical semiconductor element sealing sheet, and when the above-mentioned laminate has a plurality of optical semiconductor elements, the plurality of optical semiconductor elements are further arranged in a manner that the above-mentioned sealing resin layer fills the gaps between the plurality of optical semiconductor elements, so that the plurality of optical semiconductor elements are sealed together. Specifically, from Figure 1 or Figure 2 The optical semiconductor element sealing sheet 1 shown is prepared by peeling off the release liner 3, and arranging the exposed adhesive layer 21 of the present invention in a manner opposite to the surface of the substrate 5 on which the optical semiconductor element 6 is arranged, and the optical semiconductor element sealing sheet 1 is adhered to the surface of the substrate 5 on which the optical semiconductor element 6 is arranged, so that the optical semiconductor element 6 is buried in the sealing resin layer 2.

[0190] The temperature during the above-mentioned lamination is, for example, in the range of room temperature to 110°C. In addition, decompression or pressurization may be performed during the above-mentioned lamination. By decompression and pressurization, the formation of gaps between the sealing resin layer and the substrate or the optical semiconductor element can be suppressed. In addition, in the above-mentioned sealing step, it is preferred to laminate the optical semiconductor element sealing sheet under reduced pressure and then pressurize it. The pressure during decompression is, for example, 1 to 100 Pa, and the decompression time is, for example, 5 to 600 seconds. In addition, the pressure during pressurization is, for example, 0.05 to 0.5 MPa, and the pressurization time is, for example, 5 to 600 seconds.

[0191] (Radiation irradiation process)

[0192] When the sealing resin layer has a radiation-curable resin layer, the manufacturing method may further include the following radiation irradiation step: irradiating a laminate having the substrate, the optical semiconductor element disposed on the substrate, and the optical semiconductor element sealing sheet for sealing the optical semiconductor element with radiation, so that the radiation-curable resin layer is cured to form a cured product layer. As the radiation, as described above, electron beams, ultraviolet rays, α rays, β rays, γ rays, X-rays, etc. may be cited. Among them, ultraviolet rays are preferred. The temperature during radiation irradiation is, for example, in the range of room temperature to 100°C, and the irradiation time is, for example, 1 minute to 1 hour.

[0193] (Cutting process)

[0194] The manufacturing method may further include the following cutting step: cutting a laminate comprising the substrate, the optical semiconductor element disposed on the substrate, and the optical semiconductor element sealing sheet for sealing the optical semiconductor element. The laminate may also be subjected to the radiation irradiation step. When the laminate comprises a cured product layer obtained by curing the radiation-curable resin layer by the radiation irradiation, the cured product layer of the optical semiconductor element sealing sheet and the side end of the substrate are cut and removed in the cutting step. Thus, the surface of the cured product layer that is fully cured and has a lower adhesiveness can be exposed on the side. The cutting may be performed by a known and commonly used method, for example, by using a cutting blade or by laser irradiation.

[0195] (Laying process)

[0196] The manufacturing method may further include a tiling step of arranging the plurality of optical semiconductor devices obtained in the cutting step in contact with each other in the plane direction. In the tiling step, the plurality of laminates obtained in the cutting step are arranged in contact with each other in the plane direction and tiling. In this way, a large display body can be manufactured.

[0197] By operating as described above, an optical semiconductor device can be manufactured. In the optical semiconductor element sealing sheet 1, when the sealing resin layer 2 does not have a radiation-curable resin layer, the sealing resin layer 2 becomes the sealing resin layer 7 in the optical semiconductor device 10. On the other hand, in the optical semiconductor element sealing sheet 1, when the sealing resin layer 2 has a radiation-curable resin layer, for example, when the adhesive layer 21 of the present invention is a radiation-curable resin layer, the diffusion function coloring layer 71 is formed by curing the adhesive layer 21 of the present invention, and becomes the sealing resin layer 7.

[0198] Example

[0199] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0200] Production Example 1

[0201] (Preparation of acrylic prepolymer solution A)

[0202] Into a separable flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet tube, 67 parts by mass of butyl acrylate (BA), 14 parts by mass of cyclohexyl acrylate (CHA), 19 parts by mass of 4-hydroxybutyl acrylate (4-HBA), 0.09 parts by mass of a photopolymerization initiator (trade name "omnirad184", manufactured by IGM Resins Italia Srl) and 0.09 parts by mass of a photopolymerization initiator (trade name "omnirad 651", manufactured by IGM Resins Italia Srl) were added as monomer components, and nitrogen was passed through and nitrogen substitution was performed for about 1 hour while stirring. Then, the temperature was 5 mW / cm 2 The mixture was polymerized by irradiation with ultraviolet rays and the reaction rate was adjusted to 5 to 15%, thereby obtaining an acrylic prepolymer solution A.

[0203] Production Example 2

[0204] (Preparation of Adhesive Composition A)

[0205] To the acrylic prepolymer solution A prepared in Production Example 1 (the total amount of the prepolymer was 100 parts by mass), 9 parts by mass of 2-hydroxyethyl acrylate (HEA), 8 parts by mass of 4-hydroxybutyl acrylate (4HBA), 0.02 parts by mass of dipentaerythritol hexaacrylate (trade name "KAYARAD DPHA", manufactured by Shin-Nakamura Chemical Co., Ltd.) as a multifunctional monomer, 0.35 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd., 3-glycidoxypropyltrimethoxysilane) and 0.3 parts by mass of a photopolymerization initiator (trade name "omnirad 651", manufactured by IGM Resins Italia Srl) were added to obtain an adhesive composition A.

[0206] Examples 1 to 12

[0207] Adhesive composition A and additives were mixed in the mass ratios shown in Table 1 or Table 2. The mixture (adhesive composition) was coated on the release-treated surface of a release liner (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation, a polyethylene terephthalate film with a single surface subjected to release treatment, thickness 38 μm) to form a resin composition layer, and the release-treated surface of a release liner (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) was also attached to the resin composition layer. Next, ultraviolet rays of the illuminance shown in Table 1 or Table 2 were irradiated using a black light until the accumulated light amount reached 2520 mJ / cm 2 , and polymerization is performed to produce the adhesive layers (thickness 50 μm) of Examples 1 to 12. It should be noted that 9256BLACK is a 20% dispersion of a black pigment (trade name "9256BLACK", manufactured by TOKUSHIKI CO., Ltd.). In addition, Tospearl 145 is a silicone resin with a trade name of "Tospearl 145" (manufactured by Momentive Performance Materials Japan, refractive index: 1.42, average particle size: 4.5 μm). In addition, Ti-PURE R-706 is a titanium dioxide pigment with a trade name of "Ti-PURE-PAINT COATINGS-DRY GRADES R-706" (manufactured by DUPONT).

[0208] A release liner (trade name "MRE38") was peeled off from the adhesive layer obtained above, and the exposed adhesive surface was adhered to the adhesive surface of a non-diffusing functional adhesive layer (thickness 150 μm, total light transmittance: 92.1%, haze value: 0.4%) that was not intended to perform the function of diffusing light, thereby preparing adhesive sheets of Examples 1 to 12.

[0209] Embodiments 13 to 15

[0210] Adhesive composition A and additives were mixed in the mass ratio of Table 2. The mixture (adhesive composition) was coated on the release-treated surface of a release liner (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation, a polyethylene terephthalate film with a single surface subjected to release treatment, thickness 38 μm) to form a resin composition layer, and the release-treated surface of a release liner (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) was also attached to the resin composition layer. Next, ultraviolet rays of the illuminance described in Table 2 were irradiated using a black light until the cumulative light amount reached 2520 mJ / cm 2, and polymerization was performed to prepare the adhesive layers (adhesive sheets) of Examples 13 to 15 (thickness 50 μm). It should be noted that BA is butyl acrylate. In addition, DPHA is dipentaerythritol hexaacrylate (trade name "KAYARAD DPHA", manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In addition, 4HBA is 4-hydroxybutyl acrylate.

[0211] Comparative Examples 1 to 4

[0212] Adhesive composition A and additives were mixed in the mass ratio of Table 2. The mixture (adhesive composition) was coated on the release-treated surface of a release liner (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation, a polyethylene terephthalate film with a single surface subjected to release treatment, thickness 38 μm) to form a resin composition layer, and the release-treated surface of a release liner (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) was also attached to the resin composition layer. Next, ultraviolet rays of the illuminance described in Table 2 were irradiated using a black light until the cumulative light amount reached 2520 mJ / cm 2 , thereby polymerizing to produce the adhesive layers (thickness 50 μm) of Comparative Examples 1 to 4.

[0213] <Evaluation>

[0214] The pressure-sensitive adhesive layers obtained in Examples and Comparative Examples were evaluated as follows.

[0215] (1) Total light transmittance

[0216] The release liner on one side was peeled off from each adhesive layer (sandwiched by two release liners) prepared in the examples and comparative examples, and the exposed surface of each adhesive layer was bonded to a glass plate (slide, model "S-9112", manufactured by Matsunami Glass Industries, Ltd.). Then, the release liner on the other side was peeled off to prepare a measurement sample having a layer structure of [glass plate / adhesive layer]. For the above-mentioned measurement sample, the total light transmittance was measured using a haze meter (device name "HM-150", manufactured by Murakami Color Technology Research Institute, Ltd.). The measurement was performed by incident measurement light from the adhesive layer side.

[0217] (2) Haze value

[0218] The total light transmittance and diffuse transmittance of the measurement sample prepared for measuring the total light transmittance were measured using a haze meter (device name "HM-150", manufactured by Murakami Color Research Laboratory Co., Ltd.). Then, the haze value of the measurement sample was calculated by the mathematical formula "diffuse transmittance / total light transmittance × 100" as the initial haze value. The measurement light was incident from the adhesive layer side for measurement.

[0219] (3) Reflection L * Determination

[0220] On the inner rolled surface of an aluminum foil (width 30 cm × length 50 m × thickness 12 μm) manufactured by Mitsubishi Aluminum Co., Ltd., a surface obtained by peeling off a release liner of the adhesive layer obtained in the embodiment and the comparative example was bonded using a manual roller in a manner that does not mix bubbles, thereby preparing a measurement sample. After bonding, it was placed at 25°C and shielded from light for 30 minutes. Then, the bonded sample was cut out to a size greater than 5.0 cm × 5.0 cm. Then, the measurement sample was placed on a flat surface with the release liner of the adhesive layer facing outward. Then, L was measured from the release liner side using a spectrophotometer (trade name "CM-26dG", manufactured by Konica Minolta, Inc.) * (SCI) and L * (SCE) measurement. It should be noted that the colorimeter was set so that the measurement area came to the center of the measurement sample, and the measurement was performed under the following conditions. In addition, before the measurement using the above-mentioned spectrophotometer, zero point calibration, white calibration, and GROSS calibration were performed according to the manufacturer's manual. It should be noted that when only the aluminum foil (inner roll surface) was measured, L * (SCI) is 95.88, L * (SCE) is 88.32. Therefore, the reflection L * (SCI) and Reflection L * (SCE) When both were 60 or less, the anti-reflection property was evaluated as "0", when one was higher than 60 and lower than 70 and the other was lower than 70 (cases other than 0 and ×), it was evaluated as "△", and when at least one was higher than 70, it was evaluated as "×".

[0221] <Measurement Conditions>

[0222] Measurement method: Color and gloss

[0223] Geometry: di: 8°, de: 8°

[0224] Regular reflected light processing: SCI+SCE

[0225] Observation light source: D65

[0226] Observation conditions: 10° field of view

[0227] Measuring diameter: MAV (8mm)

[0228] UV Condition: 100% Full

[0229] Automatic average measurement: 3 times

[0230] Zero point calibration steps: valid

[0231] (4) Light diffusion effect confirmation test

[0232] One release liner of each adhesive layer prepared in the examples and comparative examples was peeled off, and the glass plate (slide, model "S-9112", manufactured by Matsunami Glass Industries, Ltd., 76 mm × 52 mm × 1.0-1.2 mm) was bonded to the surface using a manual roller without mixing in bubbles. After bonding, it was placed at 25°C and shielded from light for 30 minutes. The size of the bonded adhesive layer was appropriately cut to the same size as the glass plate to prepare a measurement sample. An LED lamp (trade name "LK-3PG", manufactured by EK JAPAN CO., LTD.) was set at a height of 2.4 cm on the upper part of the screen. The glass plate side of the obtained measurement sample was made to fit closely with the LED lamp. A battery box (trade name "AP-180", manufactured by EK JAPAN CO., LTD.) was connected to the LED lamp to light the LED lamp, and the diameter of the circular image projected on the screen was measured. When only the glass plate was measured without an adhesive layer, the diameter of the light projected on the screen was 16 mm. When measuring through the adhesive layer, the case where the light diameter is 65 mm or more is judged to have a good light diffusion effect (brightness unevenness "○"), the case where the light diameter is higher than 60 mm and lower than 65 mm is judged to have a light diffusion effect (brightness unevenness "△"), and the case where the light diameter is less than 60 mm is judged to have no light diffusion effect (brightness unevenness "×").

[0233] (5) Compatibility

[0234] The case where both anti-reflection property and brightness unevenness were “○” was evaluated as “○”, the case where one of anti-reflection property and brightness unevenness was “△” and the other was “○” or “△” was evaluated as “△”, and the case where at least one of anti-reflection property and brightness unevenness was “×” was evaluated as “×”.

[0235] [Table 1]

[0236] (Table 1)

[0237]

[0238] [Table 2]

[0239] (Table 2)

[0240]

[0241] [Table 3]

[0242] (Table 3)

[0243] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Total light transmittance [%] 19.7 21.9 5.0 22.7 14.7 12.4 13.2 63.8 62.0 40.4 Haze value [%] 88.8 95.4 98.0 63.0 94.6 84.7 65.2 94.4 82.4 67.8 Light diffusion effect confirmation [mm] 85 100 98 70 100 75 70 120 100 75 Reflectance L*(SCI) 40.92 40.05 46.30 42.68 37.70 37.76 37.66 69.17 68.33 50.63 Reflection L*(SCE) 25.87 25.65 34.91 28.01 18.75 18.77 18.32 62.79 61.50 41.09 Anti-reflective ○ ○ ○ ○ ○ ○ ○ △ △ ○ Uneven brightness ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ Compatibility ○ ○ ○ ○ ○ ○ ○ △ △ ○

[0244] [Table 4]

[0245] (Table 4)

[0246] Embodiment 11 Example 12 Embodiment 13 Embodiment 14 Embodiment 15 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Total light transmittance [%] 38.4 18.5 24.5 32.9 45.2 19.2 91.9 17.2 92.1 Haze value [%] 75.8 61.0 98.0 98.2 98.2 9.9 93.7 53.5 0.4 Light diffusion effect confirmation [mm] 80 70 90 100 120 55 130 60 50 Reflectance L*(SCI) 50.87 38.59 42.44 46.53 53.94 40.04 93.77 37.88 93.69 Reflection L*(SCE) 41.20 23.07 28.93 35.04 45.12 23.84 88.21 21.84 88.21 Anti-reflective ○ ○ ○ ○ ○ ○ × ○ × Uneven brightness ○ ○ ○ ○ ○ × ○ × × Compatibility ○ ○ ○ ○ ○ × × × ×

[0247] Modifications of the disclosed invention are described below.

[0248] [Supplementary Note 1] An adhesive layer having a haze value of 61% or more and a total light transmittance of 69% or less.

[0249] [Supplementary Note 2] A laminated sheet comprising the adhesive layer according to Supplementary Note 1.

[0250] [Supplementary Note 3] The laminated sheet according to Supplementary Note 2, which has an anti-glare and / or anti-reflection layer on one surface.

[0251] [Supplementary Note 4] The laminated sheet according to Supplementary Note 2, wherein the thickness is 500 μm or less.

[0252] [Supplementary Note 5] An adhesive composition comprising a colorant and light diffusing fine particles, wherein the adhesive composition has a haze value of 61% or more and a total light transmittance of 69% or less when the adhesive layer is formed.

[0253] [Supplementary Note 6] An optical semiconductor device comprising: a substrate; an optical semiconductor element disposed on the substrate; and the laminate sheet or a cured product thereof according to any one of Supplementary Notes 2 to 4 for sealing the optical semiconductor element.

Claims

1. An adhesive layer for sealing an optical semiconductor element, wherein the haze value is 61% or more and the total light transmittance is 69% or less, The adhesive layer contains a colorant and light diffusing fine particles, The light diffusing fine particles are fine particles made of silicone resin and have a refractive index of 1.2 to 5. 2 . A laminate sheet for optical semiconductor element sealing, comprising the adhesive layer for optical semiconductor element sealing according to claim 1 . 3 . The laminated sheet for optical semiconductor element sealing according to claim 2 , comprising a layer having antiglare and / or antireflection properties on one surface. 4 . The laminated sheet for optical semiconductor element sealing according to claim 2 , which has a thickness of 500 μm or less.

5. An adhesive composition for sealing an optical semiconductor element, comprising a colorant and light diffusing fine particles, The light diffusing fine particles are fine particles composed of silicone resin and have a refractive index of 1.2 to 5. The haze value when forming the pressure-sensitive adhesive layer is 61% or more, and the total light transmittance is 69% or less. 6 . An optical semiconductor device comprising: a substrate; an optical semiconductor element disposed on the substrate; and the laminate sheet for optical semiconductor element sealing according to any one of claims 2 to 4 or a cured product thereof for sealing the optical semiconductor element.

Citation Information

Patent Citations

  • Sticking film for electronic display

    JP1999335639A

  • Colored adhesive sheet and display body

    JP2020164702A

  • Adhesive sheet, back-light unit and display device

    JP2021138825A

  • Adhesive sheet and Anti-glare sheet

    JP2020007511A

  • Optical multilayer product

    TW202147662A