A composite coagulant for oil well cement and preparation method thereof
By using a composite coagulant of acrylamide, dimethylaminoethyl methacrylate copolymer and inorganic salt accelerator, the problem of ultra-retarded setting of oil well cement at the top of the sealing section was solved, and the cementing cement was achieved. Rapid condensation and early compressive strength improvement make it suitable for cementing conditions in deep reservoirs.
Patent Information
- Application Number
- CN202410215425.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-02-27
AI Technical Summary
Oil well cement has a super-retarded setting phenomenon at the top of the sealing section, which results in a long setting time and cannot meet the high temperature and long sealing section requirements of deep oil reservoir cementing.
A composite coagulant composed of a copolymer of acrylamide and dimethylaminoethyl methacrylate is used as the wall material and an inorganic salt coagulant. The microcapsule coagulant is prepared by ultrasonic dispersion and spray drying to promote The cement solidifies quickly at the top of the sealing section.
It effectively shortens the setting time of cementing cement, improves early compressive strength, solves the problem of super-retarded setting, and is suitable for the cementing needs of deep reservoirs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil well cement admixtures, and in particular to a composite coagulant for oil well cement and a preparation method thereof. Background Art
[0002] At present, oil and gas exploration has entered the "low and deep" deep oil reservoirs. The problems faced by cementing in deep oil reservoirs are deep burial, high well temperature, long sealing section, low pressure coefficient, etc., which puts higher requirements on the performance of cementing cement. The extension of the sealing section makes it span multiple temperature ranges, and the cementing cement has different setting times at the top and bottom due to different temperatures. Therefore, retarders are often added to delay the setting time of cement. Due to the addition of retarders, the setting time of cementing cement at the top of the sealing section is too long, which is the super-retarded setting phenomenon.
[0003] It is necessary to develop a coagulant to make cement solidify quickly at the top of the sealing section to solve the problem of ultra-slow setting of cementing cement at the top of the sealing section. Summary of the invention
[0004] The invention provides a composite coagulant for oil well cement and a preparation method thereof, which solves the problem of ultra-slow setting of cement at the top of the sealing section in the prior art.
[0005] The technical solution of the present invention is as follows:
[0006] The invention provides a composite coagulant for oil well cement, which is composed of a wall material and a capsule material. The wall material comprises a copolymer of acrylamide and dimethylaminoethyl methacrylate, and the capsule material is an inorganic salt coagulant.
[0007] In the present invention, a copolymer of acrylamide and dimethylaminoethyl methacrylate is used as the wall material, and the amide groups, amino groups and ester groups on the surface can be adsorbed on the cementing cement to promote cement hydration, and cooperate with the inorganic salt coagulant in the capsule material to make the cementing cement quickly coagulate at the top of the sealing section, thereby solving the problem of ultra-slow coagulation of the cementing cement at the top of the sealing section. The prepared composite coagulant is added to the cementing cement to improve the early compressive strength of the cementing cement.
[0008] As a further technical solution, the mass ratio of the wall material to the capsule material is 2-3:1.
[0009] In the present invention, when the mass ratio of the wall material to the capsule material is 2-3:1, the obtained coagulant can further promote and shorten the setting time of the cementing cement.
[0010] As a further technical solution, the viscosity average molecular weight of the copolymer of acrylamide and dimethylaminoethyl methacrylate is 50,000 to 200,000.
[0011] As a further technical solution, the preparation method of the copolymer of acrylamide and dimethylaminoethyl methacrylate comprises the following steps:
[0012] In the solution, acrylamide and dimethylaminoethyl methacrylate undergo polymerization reaction under the action of an initiator to obtain a copolymer of acrylamide and dimethylaminoethyl methacrylate.
[0013] As a further technical solution, the molar ratio of acrylamide to dimethylaminoethyl methacrylate is 5-10:1.
[0014] The solution is an aqueous solution;
[0015] The initiator is potassium persulfate or ammonium persulfate.
[0016] As a further technical solution, the inorganic salt coagulant includes one or more of sodium silicate, calcium formate, sodium sulfate, calcium chloride, sodium carbonate, and calcium oxalate.
[0017] As a further technical solution, the inorganic salt coagulant is a mixture of sodium silicate and calcium oxalate in a mass ratio of 3 to 8:2.
[0018] As a further technical solution, the mass ratio of the sodium silicate to calcium formate is 5:2.
[0019] In the present invention, an inorganic salt coagulant composed of sodium silicate and calcium oxalate in a specific mass ratio is used, which further improves the accelerating effect of the composite coagulant on cementing cement.
[0020] The invention also proposes a method for preparing the composite coagulant for oil well cement, comprising the following steps: dissolving a copolymer of acrylamide and dimethylaminoethyl methacrylate in ethanol, adding an inorganic salt coagulant, uniformly dispersing by ultrasonication, and spray drying to obtain the composite coagulant.
[0021] In the present invention, a microcapsule-type composite coagulant is prepared by a spray drying method, and the inorganic salt coagulant is better coated in the wall material, thereby further improving the accelerating effect of the coagulant on cementing cement.
[0022] As a further technical solution, the power of the ultrasonic dispersion is 200W~300W, and the time is 30~50min.
[0023] In the present invention, when the microcapsule composite coagulant is prepared by the spray drying method, the inorganic salt coagulant is dispersed more evenly in the wall material solution through ultrasonic dispersion. When the power of the ultrasonic dispersion is 200W-300W and the time is 30-50min, the dispersion uniformity of the coagulant is further improved, thereby further improving the accelerating effect of the coagulant on cementing cement.
[0024] The working principle and beneficial effects of the present invention are:
[0025] 1. In the present invention, a copolymer of acrylamide and dimethylaminoethyl methacrylate is used as a wall material, an inorganic salt coagulant is used as a capsule material, and the inorganic salt coagulant is coated in the copolymer of acrylamide and dimethylaminoethyl methacrylate. The present invention is stable during the high-speed slurry preparation process of cementing cement, and can effectively shorten the thickening time of cementing cement, thereby solving the problem of ultra-slow setting of cementing cement at the top of the sealing section. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In the following embodiments,
[0028] The viscosity average molecular weight of the copolymer of acrylamide and dimethylaminoethyl methacrylate was determined according to GB / T 12005.10-1992 "Polyacrylamide Molecular Weight Determination Viscosity Method";
[0029] The cement slurry was prepared according to the method specified in Chapter 5 of GB / T 19139-2012 "Test Methods for Oil Well Cement" with a density of 1.88 g / cm 3 ;
[0030] According to the scheme of 3660m well depth specified in Chapter 7 of GB / T 19139-2012 "Test Methods for Oil Well Cement", the temperature is increased gradually for 90 minutes and the curing pressure is 20700kPa±3400kPa. After curing, the compressive strength of cementing cement is tested;
[0031] The thickening time of cementing cement at 80MPa and 95℃ was tested according to the method specified in Chapter 9 of GB / T 19139-2012 "Test Methods for Oil Well Cement".
[0032] Example 1
[0033] Preparation of wall materials:
[0034] 35.54 g of acrylamide and 15.72 g of dimethylaminoethyl methacrylate were added to a reaction bottle, and 400 g of deionized water was added. After stirring until completely dissolved, nitrogen was passed through to deoxygenate for 30 minutes, and then the temperature was raised to 40°C and 1.14 g of ammonium persulfate was added. After the reaction was kept warm for 10 hours, the obtained product was granulated, dried, and crushed to obtain a copolymer of acrylamide and dimethylaminoethyl methacrylate. The viscosity average molecular weight was measured by viscosity method to be 51,000.
[0035] The obtained copolymer of acrylamide and dimethylaminoethyl methacrylate was measured by infrared spectroscopy, and it was found that -1 The vibration absorption peak of the carbonyl group in dimethylaminoethyl methacrylate appeared at 1650cm -1 (I band) and 1550 cm -1 The vibration absorption peak of the amide group in acrylamide appeared at (Band II), from which it can be determined that the product is a copolymer of acrylamide and dimethylaminoethyl methacrylate.
[0036] Preparation of composite coagulant:
[0037] 7 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 7 g of sodium silicate was added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0038] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0039] Table 1 Effect of the composite coagulant of Example 1 on the thickening time and compressive strength of cement
[0040]
[0041] Example 2
[0042] Preparation of wall materials:
[0043] 35.54 g of acrylamide and 7.86 g of dimethylaminoethyl methacrylate were added to a reaction bottle, and 400 g of deionized water was added. After stirring until completely dissolved, nitrogen was passed through to deoxygenate for 30 minutes, and then the temperature was raised to 40°C and 1.14 g of ammonium persulfate was added. After the reaction was kept warm for 10 hours, the obtained product was granulated, dried, and crushed to obtain a copolymer of acrylamide and dimethylaminoethyl methacrylate. The viscosity average molecular weight was measured by viscosity method to be 86,000.
[0044] Preparation of composite coagulant:
[0045] 7 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 7 g of sodium silicate was added, and ultrasonic dispersion was performed at a power of 300 W for 30 minutes. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0046] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0047] Table 2 Effect of the composite coagulant of Example 2 on the thickening time and compressive strength of cement
[0048]
[0049] Example 3
[0050] Preparation of wall material: The method is the same as Example 1.
[0051] Preparation of composite coagulant:
[0052] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 7 g of sodium silicate was added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0053] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0054] Table 3 Effect of the composite coagulant of Example 3 on the thickening time and compressive strength of cement
[0055]
[0056] Example 4
[0057] Preparation of wall material: The method is the same as Example 1.
[0058] Preparation of composite coagulant:
[0059] 21 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 7 g of sodium silicate was added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0060] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0061] Table 4 Effect of the composite coagulant of Example 4 on the thickening time and compressive strength of cement
[0062]
[0063] Example 5
[0064] Preparation of wall material: The method is the same as Example 1.
[0065] Preparation of composite coagulant:
[0066] 28g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200mL of anhydrous ethanol, 7g of sodium silicate was added, and ultrasonic dispersion was performed at a power of 200W for 50min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0067] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0068] Table 5 Effect of the composite accelerator of Example 5 on the thickening time and compressive strength of cement
[0069]
[0070] Example 6
[0071] Preparation of wall material: The method is the same as Example 1.
[0072] Preparation of composite coagulant:
[0073] 21 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 7 g of calcium oxalate was added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0074] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0075] Table 6 Effect of the composite accelerator of Example 6 on the thickening time and compressive strength of cement
[0076]
[0077] Example 7
[0078] Preparation of wall material: The method is the same as Example 1.
[0079] Preparation of composite coagulant:
[0080] 21g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200mL of anhydrous ethanol, 5g of sodium silicate and 2g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200W for 50min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0081] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0082] Table 7 Effect of the composite accelerator of Example 7 on the thickening time and compressive strength of cement
[0083]
[0084] Example 8
[0085] Preparation of wall material: The method is the same as Example 1.
[0086] Preparation of composite coagulant:
[0087] 21 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 4.2 g of sodium silicate and 2.8 g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0088] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0089] Table 8 Effect of the composite accelerator of Example 8 on the thickening time and compressive strength of cement
[0090]
[0091] Example 9
[0092] Preparation of wall material: The method is the same as Example 1.
[0093] Preparation of composite coagulant:
[0094] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 5.6 g of sodium silicate and 1.4 g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0095] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0096] Table 9 Effect of the composite accelerator of Example 9 on the thickening time and compressive strength of cement
[0097]
[0098] Example 10
[0099] Preparation of wall material: The method is the same as Example 1.
[0100] Preparation of composite coagulant:
[0101] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 3.5 g of sodium silicate and 3.5 g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0102] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0103] Table 10 Effect of the composite coagulant of Example 10 on the thickening time and compressive strength of cement
[0104]
[0105] Embodiment 11
[0106] Preparation of wall material: The method is the same as Example 1.
[0107] Preparation of composite coagulant:
[0108] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 6 g of sodium silicate and 1 g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0109] The obtained composite coagulant was applied to cementing cement to test its effect on the thickening time and compressive strength of cementing cement. The test results are shown in the following table:
[0110] Table 11 Effect of the composite accelerator of Example 11 on the thickening time and compressive strength of cement
[0111]
[0112] Example 12
[0113] Preparation of wall material: The method is the same as Example 1.
[0114] Preparation of composite coagulant:
[0115] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 5 g of sodium silicate and 2 g of calcium formate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0116] Table 12 Effect of the composite accelerator of Example 12 on the thickening time and compressive strength of cement
[0117]
[0118] Example 13
[0119] Preparation of wall material: The method is the same as Example 1.
[0120] Preparation of composite coagulant:
[0121] 14 g of a copolymer of acrylamide and dimethylaminoethyl methacrylate was dissolved in 200 mL of anhydrous ethanol, 5 g of sodium sulfate and 2 g of calcium oxalate were added, and ultrasonic dispersion was performed at a power of 200 W for 50 min. After uniform dispersion, the mixture was spray-dried to obtain a composite coagulant.
[0122] Table 13 Effect of the composite accelerator of Example 13 on the thickening time and compressive strength of cement
[0123]
[0124] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite accelerator for oil well cement, It is characterized in that It is composed of a wall material and a capsule material, wherein the wall material comprises a copolymer of acrylamide and dimethylaminoethyl methacrylate, and the capsule material is an inorganic salt coagulant; The mass ratio of the wall material to the capsule material is 2-3:1; The molar ratio of acrylamide to dimethylaminoethyl methacrylate is 5-10:
1.
2. A composite coagulant for oil well cement according to claim 1, It is characterized in that The viscosity average molecular weight of the copolymer of acrylamide and dimethylaminoethyl methacrylate is 50,000 to 200,000.
3. A composite accelerator for oil well cement according to claim 1, It is characterized in that The preparation method of the copolymer of acrylamide and dimethylaminoethyl methacrylate comprises the following steps: In the solution, acrylamide and dimethylaminoethyl methacrylate undergo polymerization reaction under the action of an initiator to obtain a copolymer of acrylamide and dimethylaminoethyl methacrylate.
4. A composite accelerator for oil well cement according to claim 3, It is characterized in that The solution is an aqueous solution; The initiator is potassium persulfate or ammonium persulfate.
5. The composite coagulant for oil well cement according to claim 1, It is characterized in that The inorganic salt coagulant includes one or more of sodium silicate, calcium formate, sodium sulfate, calcium chloride, sodium carbonate, and calcium oxalate.
6. A composite coagulant for oil well cement according to claim 5, It is characterized in that The inorganic salt coagulant is a mixture of sodium silicate and calcium oxalate in a mass ratio of 3 to 8:
2.
7. A composite accelerator for oil well cement according to claim 6, It is characterized in that The mass ratio of the sodium silicate to calcium formate is 5:
2.
8. A method for preparing a composite coagulant for oil well cement according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: dissolving a copolymer of acrylamide and dimethylaminoethyl methacrylate in ethanol, adding an inorganic salt coagulant, uniformly dispersing by ultrasonication, and spray drying to obtain a composite coagulant.
9. The method for preparing a composite coagulant for oil well cement according to claim 8, It is characterized in that The power of the ultrasonic dispersion is 200W-300W, and the time is 30-50min.
Citation Information
Patent Citations
Oil-well cement temperature-sensitive slow-release coagulation accelerator
CN106916577A