A non-aqueous electrolyte, sodium ion secondary battery and preparation method thereof
The non-aqueous electrolyte with specific additives forms stable films on electrodes, addressing discharge capacity and resistance issues in sodium ion secondary batteries, enhancing high-temperature performance and maintaining low-temperature output.
Patent Information
- Application Number
- CN202410468205.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-04-18
AI Technical Summary
Sodium ion secondary batteries face challenges in maintaining discharge capacity and inhibiting the increase in DC internal resistance in high temperature environments, while also ensuring excellent low-temperature output performance.
A non-aqueous electrolyte comprising a sodium salt, a non-aqueous solvent, and specific additives such as a first additive (e.g., sodium 1,1-dimethyl-3,4-disulfomethylpyrrolidinium betaine), a second additive (cyclic sulfur-containing ester compound), and a third additive (sodium salt additives) to form stable SEI and CEI films on the electrodes, enhancing thermal and chemical stability.
The electrolyte improves high-temperature cycle capacity retention and reduces DC internal resistance, while maintaining excellent low-temperature output performance by forming stable films that suppress side reactions and elution of components.
Smart Images

Figure CN118522954B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a non-aqueous electrolyte, a sodium ion secondary battery and a preparation method thereof. Background Art
[0002] Sodium ion secondary batteries have attracted much attention due to their advantages such as low cost, excellent low temperature performance, good safety and moderate energy density. Patent document CN106920988A discloses a sodium ion secondary battery involving a non-aqueous electrolyte (hereinafter referred to as "sodium ion secondary battery"), and the disclosed sodium ion secondary battery includes a positive electrode, a negative electrode and a non-aqueous electrolyte. The negative electrode is made of a negative electrode material that can absorb and release sodium. The non-aqueous electrolyte is composed of an organic solvent and a solute. The non-aqueous solvent contains fluorocarbons, cyclic sulfates and cyclic sulfonates. Sodium ion secondary batteries can be used not only in warm areas, but also in cold and hot areas. Therefore, sodium ion secondary batteries need to suppress the decrease in discharge capacity and the increase in DC internal resistance after long-term charging and discharging in a high temperature environment, and the low-temperature output performance should also be excellent. Summary of the invention
[0003] In view of the above situation, the present invention provides a non-aqueous electrolyte for sodium ion secondary batteries and a method for manufacturing sodium ion secondary batteries. The non-aqueous electrolyte can improve the high temperature cycle capacity retention rate of sodium ion secondary batteries, inhibit the increase of DC internal resistance, and also has excellent low temperature output performance.
[0004] The technical solution adopted by the present invention is as follows:
[0005] A non-aqueous electrolyte, comprising a sodium salt, a non-aqueous solvent and an additive, wherein the additive comprises a first additive, a second additive and a third additive, wherein: the first additive is as shown in formula (I), the second additive is a cyclic sulfur-containing ester compound (Formula II), and the third additive is a sodium salt additive (Formula III);
[0006]
[0007] Where:
[0008] R1 and R2 are each independently selected from a hydrogen atom, an alkyl group having 1 to 6 carbon atoms or a substituted alkyl group (at least one hydrogen atom in the alkyl group may be substituted by a halogen atom), an alkenyl group having 2 to 6 carbon atoms or a substituted alkenyl group (at least one hydrogen atom in the alkenyl group may be substituted by a halogen atom), an alkynyl group having 2 to 6 carbon atoms, a benzyl group or an aryl group.
[0009] The first additive of the present invention is shown in formula (I), and its function is to suppress the reduction of the cyclic discharge capacity, the increase of the DC internal resistance and the reduction of the output performance at low temperature of the sodium ion secondary battery in a high temperature environment. Its mechanism of action is as follows: when a sodium ion secondary battery is prepared using a non-aqueous electrolyte to which the first additive (I) of the present invention is added, an SEI film is formed on the negative electrode surface of the sodium ion secondary battery during the preparation process (such as the formation process described later). This component moves to the vicinity of the positive electrode surface during the manufacturing process and adheres to the positive electrode surface to form a CEI film. This improves the stability of the sodium ion secondary battery in a high temperature environment. For example, the dissolution of metal elements in the positive electrode active material is suppressed. Therefore, when the sodium ion secondary battery is operated in a high temperature environment, the increase of the DC internal resistance of the sodium ion secondary battery is suppressed.
[0010] As described above, the stability of the sodium ion secondary battery using the first additive (I) is excellent even in a high temperature environment. That is to say, even if the sodium ion secondary battery is stored in a high temperature environment, the battery side reaction is difficult to proceed. The battery reaction is manifested as the reaction of sodium ion deintercalation and insertion of positive and negative electrodes. Side reactions include the reduction decomposition reaction of the negative electrode to the electrolyte, the oxidation decomposition reaction of the positive electrode to the electrolyte, the elution of metal elements in the positive electrode active material, etc. Therefore, the decomposition reaction of the non-aqueous electrolyte is suppressed. Therefore, even if the sodium ion secondary battery is operated in a high temperature environment, the discharge capacity of the sodium ion secondary battery is difficult to reduce.
[0011] In addition, the first additive (I) has a multivalent anion in the molecular skeleton of the coating component formed on the positive and negative electrodes, which will form a multivalent salt with the salt in the electrolyte, thereby improving thermal stability and suppressing the increase in impedance.
[0012] Based on the above reasons, when the first additive (I) of the present invention is added to a non-aqueous electrolyte for use, when the sodium ion secondary battery is operated in a high temperature environment, the reduction in discharge capacity, the increase in DC internal resistance and the reduction in low-temperature output performance can be suppressed.
[0013] In the present invention, the amount of the first additive (I) added is 0.01% to 5.0%, preferably 0.1% to 3.0%, and particularly preferably 0.3% to 1.0%, based on the total mass of the non-aqueous electrolyte.
[0014] Relative to the total mass of the non-aqueous electrolyte, the upper limit of the content of the first additive (I) is preferably 5.0 mass % or less, more preferably 3.0 mass % or less, and particularly preferably 1.0 mass % or less. It was found through experiments that when the upper limit of the content of the first additive (I) is within the above range, the sodium ion secondary battery can work, and the SEI film will not damage the conductivity of the sodium ions. In addition, as the SEI film contains a sulfonic acid structure, the characteristics of the sodium ion secondary battery are improved.
[0015] Relative to the total mass of the non-aqueous electrolyte, the lower limit of the content of the first additive (I) is preferably 0.01% by mass or higher, more preferably 0.05% by mass or higher, more preferably 0.10% by mass or higher, particularly preferably 0.20% by mass or higher, more preferably 0.30% by mass or higher. If the lower limit of the content of the first additive (I) is within the above range, the SEI / CEI film contains a sufficient amount of the structure from the first additive (I). Therefore, it is easy to form a thermally and chemically stable inorganic salt or polymer structure. Therefore, at high temperatures, it is not easy to cause elution of SEI / CEI film components and SEI / CEI film deterioration, etc., which damage the durability of the SEI / CEI film. As a result, the durability of the SEI / CEI film and the high temperature characteristics of the sodium ion secondary battery are improved.
[0016] Preferably, the first additive (I) is selected from sodium 1,1-dimethyl-3,4-disulfomethylpyrrolidinium betaine shown in formula (I-1) and sodium 1-dimethyl-1-allyl-3,4-disulfomethylpyrrolidinium betaine shown in formula (I-2). Under the above selection, when the sodium ion secondary battery is operated in a high temperature environment, the reduction of discharge capacity, the increase of DC internal resistance and the reduction of low temperature output performance can be better suppressed.
[0017]
[0018] The second additive of the present invention is a cyclic sulfur-containing ester compound (II).
[0019]
[0020] In Formula II:
[0021] R3 is selected from an oxygen atom, an alkylene group having 1 to 6 carbon atoms, and a vinylene group;
[0022] R4 is selected from an alkylene group having 1 to 6 carbon atoms, a group represented by formula ii-1 or a group represented by formula ii-2; wherein: "*" represents the binding position, R 41 is an oxygen atom, an alkyl group having 1 to 6 carbon atoms, or an oxymethylene group, R 42 It is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.
[0023] Since the non-aqueous electrolyte of the present invention contains a cyclic sulfur-containing ester compound (II) in addition to the first additive (I), the decrease in discharge capacity and the increase in DC internal resistance at 45°C can be better suppressed even when operating in a high temperature environment. Its mechanism of action is: when a sodium ion secondary battery is produced using the non-aqueous electrolyte disclosed in the present invention, during its production process (such as the formation process described later), the reaction product includes the product of the reaction of the cyclic sulfur-containing ester compound (II) with a compound produced by the electrolyte (for example, NaF). This further improves the stability of the sodium ion secondary battery in a high temperature environment. Therefore, even if the sodium ion secondary battery is circulated in a high temperature environment, the increase in the DC internal resistance of the sodium secondary battery at 45°C will be better suppressed. In addition, the decomposition reaction of the non-aqueous electrolyte is further suppressed. Therefore, even if the sodium ion secondary battery is circulated in a high temperature environment, the decrease in the discharge capacity of the sodium ion secondary battery is suppressed.
[0024] In the present invention, the amount of the cyclic sulfur-containing ester compound (II) added is 0.01% to 5.0%, preferably 0.1% to 3.0%, and particularly preferably 1.0% to 2.0%, based on the total mass of the non-aqueous electrolyte.
[0025] Relative to the total mass of the non-aqueous electrolyte, the upper limit of the content of the cyclic sulfur-containing ester compound (II) is preferably 5.0 mass % or less of the total amount of the non-aqueous electrolyte, more preferably 3.0 mass % or less, and particularly preferably 2.0 mass % or less. When the upper limit of the content of the cyclic sulfur-containing ester compound (II) is within the above range, the sodium ion secondary battery can operate without the SEI membrane, etc. damaging the conductivity of the sodium ions. In addition, as the SEI membrane, etc. contain a cyclic sulfur-containing ester structure, the battery characteristics of the sodium ion secondary battery are improved.
[0026] Relative to the total mass of the non-aqueous electrolyte, the lower limit of the content of the cyclic sulfur-containing ester compound (II) is preferably 0.01% by mass or more of the total amount of the non-aqueous electrolyte, more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more. If the lower limit of the content of the cyclic sulfur-containing ester compound (II) is within the above range, the SEI film and the like contain a sufficient amount of cyclic sulfur-containing ester structure. Therefore, it is easy to form a thermally and chemically stable inorganic salt or polymer structure. Therefore, at high temperatures, the elution of components such as the SEI film and the deterioration of the SEI film are difficult to occur, which improves the durability of the SEI film and the high temperature durability of the sodium ion secondary battery.
[0027] When the cyclic sulfur-containing ester compound (II) is selected from the following compounds, it will have a better effect:
[0028] In the cyclic sulfur-containing ester compound (II), R3 is preferably an oxygen atom: this easily forms a thermally and chemically stable inorganic salt structure. Therefore, at high temperatures, the elution of components such as the SEI film and the deterioration of the SEI film are unlikely to occur, improving the durability of the SEI film and the high-temperature durability of the sodium-ion secondary battery.
[0029] In the cyclic sulfur-containing ester compound (II), R4 is preferably a group represented by formula ii-1 or a group represented by formula ii-2. In formula ii-1, R 41 It is preferably an alkyl group having 1 to 3 carbon atoms, or an oxymethylene group, and is particularly preferably an oxymethylene group. In formula ii-2, R 42 An alkyl group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms is preferred, and a propyl group is particularly preferred.
[0030] Particularly preferably, the cyclic sulfur-containing ester compound (II) is selected from any one or more of the compounds represented by formulae II-1 to II-7.
[0031]
[0032] The third additive of the present invention is a sodium salt additive (III).
[0033] The sodium salt additive (III) is selected from any one or more of acesulfame sodium trifluoride boron compound (III-1), sodium difluorooxalate borate (NaDFOB, III-2), sodium difluorophosphate (NaDFP, III-3), sodium difluorobis(oxalate) phosphate (NaPF2((C2O4)2, III-4), sodium tetrafluorooxalate phosphate (NaPF4(C2O4), III-5) and sodium bis(fluorosulfonyl)imide (NaFSI, III-6).
[0034]
[0035] Since the non-aqueous electrolyte of the present invention contains other sodium salt additives (III) in addition to the first additive (I), the decrease in discharge capacity, the increase in DC internal resistance at 45°C and the decrease in output performance at -20°C can be better suppressed even in charge and discharge cycles under high temperature environments. It is speculated that this effect is based on the following reasons: Since the non-aqueous electrolyte contains a sodium salt additive in addition to the first additive (I), the SEI film, etc. can include a combination from the sodium salt additive, as well as the above-mentioned reaction products, etc. inside it. Therefore, it is easy to form a thermally and chemically stable inorganic salt or polymer structure. Therefore, at high temperatures, it is difficult for components such as membranes that damage the durability of SEI / CEI membranes, etc. to be eluted and the membranes to deteriorate. Therefore, even in charge and discharge cycles under high temperature environments, the decrease in discharge capacity, the increase in DC internal resistance at 45°C and the decrease in output performance at -20°C are better suppressed.
[0036] In the present invention, the amount of the sodium salt additive (III) added is 0.001% to 5.0%, preferably 0.01% to 3.0%, and particularly preferably 0.1% to 2.0%, based on the total mass of the non-aqueous electrolyte.
[0037] When the non-aqueous electrolyte contains a sodium salt additive (III), the upper limit of the content of compound (III) is preferably less than 5% by mass, more preferably less than 3% by mass, and more preferably less than 2% by mass relative to the total amount of the non-aqueous electrolyte. If the upper limit of the content of compound (III) is within the above range, the solubility of the sodium salt additive in the non-aqueous solvent can be guaranteed. The lower limit of the content of compound (III) is preferably 0.001% by mass or higher, more preferably 0.01% by mass or higher, more preferably 0.1% by mass or higher relative to the total amount of the non-aqueous electrolyte. If the lower limit of the content of compound (III) is within the above range, the DC internal resistance of the sodium ion secondary battery can be further reduced.
[0038] The non-aqueous electrolyte of the present invention may contain other additives in addition to the aforementioned first additive, second additive, and third additive. There is no particular limitation on other additives, and any known additives may be used, such as the additives described in paragraphs 0048-0079 of CN106920988A.
[0039] The non-aqueous solvent of the present invention can be selected from various known non-aqueous solvents such as organic solvents. The non-aqueous solvent can be selected from one or more than two.
[0040] The non-aqueous solvent described in the present invention can be selected from any one or more of cyclic carbonates, fluorinated cyclic carbonates, chain carbonates, fluorinated chain carbonates, aliphatic carboxylates, fluorinated aliphatic carboxylates, γ-lactones, fluorinated γ-lactones, cyclic ethers, fluorinated cyclic ethers, chain ethers, fluorinated chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, diethyl sulfoxide, dimethyl sulfoxide, etc.
[0041] Some choices of non-aqueous solvents are shown below:
[0042] The cyclic carbonates are selected from any one or both of ethylene carbonate (EC) and propylene carbonate (PC).
[0043] The fluorine-containing cyclic carbonates are, for example, fluoroethylene carbonate (FEC).
[0044] The chain carbonate is selected from any one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), dipropyl carbonate (DPC) and the like.
[0045] The aliphatic carboxylic acid esters are selected from any one or more of methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, ethyl trimethylbutyrate, etc.
[0046] The γ-lactones can be selected from any one or more of γ-butyrolactone, γ-valerolactone, etc.
[0047] The cyclic ethers are selected from any one or more of tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxane, 4-methyl-1,3-dioxane, 1,4-dioxane and the like.
[0048] The chain ethers are selected from any one or more of 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, 1,2-dibutoxyethane, etc.
[0049] The nitrile is selected from any one or more of acetonitrile, propionitrile, capronitrile, methoxyacetonitrile, 3-methoxypropionitrile and the like.
[0050] The amides can be selected from N,N-dimethylformamide and the like.
[0051] The lactam is selected from any one or more of N-methylpyrrolidone, N-methyloxazolidinone, N,N-dimethylimidazolidinone and the like.
[0052] As the preferred technical solution:
[0053] The non-aqueous solvent includes cyclic carbonate, which is propylene carbonate (PC) and / or ethylene carbonate (EC); the volume percentage of the cyclic carbonate in the non-aqueous solvent is 35% to 65%, and more preferably 40% to 60%.
[0054] The non-aqueous solvent includes chain carbonate, which is one or more of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC); the volume percentage of the chain carbonate in the non-aqueous solvent is 40% to 60%.
[0055] When the non-aqueous solvent includes cyclic carbonate and chain carbonate, the volume ratio of the cyclic carbonate to the chain carbonate is preferably 2:3 to 3:2.
[0056] The non-aqueous solvent of the present invention may also contain carboxylate. When the non-aqueous solvent is carbonate and carboxylate, the volume ratio of carbonate and carboxylate is preferably 3:7 to 7:3. The carboxylate is preferably one or more of methyl formate (FA), ethyl acetate (EA) and methyl butyrate (BA); more preferably ethyl acetate (EA).
[0057] The non-aqueous electrolyte of the present invention uses sodium salt as electrolyte salt.
[0058] The sodium salt of the present invention comprises at least one fluorine-containing sodium salt.
[0059] The fluorine-containing sodium salt is selected from inorganic acid anion salts or organic acid anion salts and the like.
[0060] The inorganic acid anion salt is selected from any one or more of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium hexafluoroarsenate (NaAsF6), sodium hexafluorotantalate (NaTaF6), etc.
[0061] The organic acid anion salt is selected from any one or more of sodium trifluoromethanesulfonate (NaCF3SO3), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium bis(pentafluoroethanesulfonyl)imide (Na(C2F5SO2)2N), etc.
[0062] Among them, sodium hexafluorophosphate (NaPF6) is particularly preferred as the fluorine-containing sodium salt.
[0063] The sodium salt described in the present invention may also include a fluorine-free sodium salt, and the fluorine-free sodium salt is selected from any one of sodium perchlorate (NaClO4), sodium tetrachloroaluminate (NaAlCl4), etc.
[0064] When the electrolyte contains a fluorine-containing sodium salt and a fluorine-free sodium salt, the content ratio of the fluorine-containing sodium salt is preferably 50 mass % to 100 mass %, particularly preferably 80 mass % to 100 mass % based on the total amount of the electrolyte.
[0065] The amount of sodium salt added according to the present invention, calculated on the basis of non-aqueous electrolyte, is such that the concentration of the sodium salt in the non-aqueous electrolyte is 0.1 mol / L to 3 mol / L, preferably 0.5 mol / L to 2 mol / L, and particularly preferably sodium hexafluorophosphate (NaPF6) is selected, and the concentration of sodium hexafluorophosphate (NaPF6) in the non-aqueous electrolyte is 0.5 mol / L to 2 mol / L.
[0066] The non-aqueous electrolyte of the present invention may contain other components as required, such as acid anhydride, isocyanate compound, TMSP, TMSB, etc., in addition to the sodium salt, non-aqueous solvent and additives.
[0067] The present invention also provides a method for preparing the aforementioned non-aqueous electrolyte, which is not particularly limited and can be prepared by conventional electrolyte preparation methods in the art. For example, the aforementioned sodium salt and the aforementioned additive are added to the aforementioned non-aqueous solvent and then mixed evenly.
[0068] The present invention provides an application of the non-aqueous electrolyte in a sodium ion secondary battery.
[0069] A sodium ion secondary battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; the positive electrode sheet comprises a positive electrode current collector and a positive electrode membrane containing a positive electrode active material disposed on the positive electrode current collector; the negative electrode sheet comprises a negative electrode current collector and a negative electrode membrane containing a negative electrode active material disposed on the negative electrode current collector; the separator is disposed between the positive electrode sheet and the negative electrode sheet; the electrolyte adopts the aforementioned non-aqueous electrolyte.
[0070] The positive electrode active material includes a material that can release and accept sodium ions; preferably, a sodium transition metal composite oxide; further preferably, one or more of a sodium transition metal oxide, a compound obtained by adding other transition metals or non-transition metals to a sodium transition metal oxide, further preferably, one or more of a sodium cobalt oxide, a sodium manganese oxide, a sodium-based multinary transition metal compound, a transition metal sodium phosphate salt, and a transition metal sodium fluorophosphate salt; further preferably, Na X CoO2、Na X MnO2、NaNi 0.33 Fe 0.33 Mn 0.33 02. One or more of Na4Fe3(PO4)2(P2O7), NaVPO4;
[0071] The negative electrode active material includes a material that can accept and release sodium ions; preferably, it is one or more of soft carbon, hard carbon, acetylene black, sodium titanate and a metal that can form an alloy with sodium.
[0072] The third aspect of the present invention is to provide a method for preparing a sodium ion secondary battery, which comprises the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, with the separator being located between the positive electrode sheet and the negative electrode sheet to play an isolating role, then stacking to obtain a bare battery cell, placing the bare battery cell in an outer package, injecting the non-aqueous electrolyte, encapsulating, and forming to obtain a sodium ion secondary battery.
[0073] The beneficial effects of the present invention are as follows:
[0074] The present invention provides an additive for a sodium ion secondary battery containing sodium 1,1-dialkyl-3,4-disulfonmethylpyrrolidinium betaine, a non-aqueous electrolyte for a sodium ion secondary battery, a method for manufacturing a sodium ion secondary battery, and a sodium ion secondary battery. The above technical scheme can improve the high-temperature cycle capacity retention rate of the sodium ion secondary battery, inhibit the increase of the DC internal resistance, and has excellent low-temperature output performance.
[0075] The present invention is further described below in conjunction with specific implementation modes. DETAILED DESCRIPTION
[0076] In this specification, the numerical range represented by "~" refers to the range with the numerical values described before and after "~" as the lower limit and upper limit. The reagents and raw materials used in the present invention are commercially available unless otherwise specified. The synthesis method of sodium 1,1-dimethyl-3,4-disulfomethylpyrrolidinoammonium betaine of formula (I-1) and sodium 1-dimethyl-1-allyl-3,4-disulfomethylpyrrolidinoammonium betaine of formula (I-2) refers to the method disclosed in EP0163319 A2. The following describes the preparation implementation methods of the sodium ion secondary battery additive, the non-aqueous electrolyte for sodium ion secondary battery, and the sodium ion secondary battery of the present invention.
[0077] Example 1
[0078] Preparation of non-aqueous electrolyte:
[0079] Fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are mixed at a volume ratio of FEC:EC:PC:DMC:EMC=1:5:25:35:35 to obtain a mixed solvent as a non-aqueous solvent. NaPF6 as an electrolyte is dissolved in the obtained mixed solvent to a concentration of 1 mol / L in the electrolyte, and the obtained electrolyte is referred to as a "basic electrolyte".
[0080] As additives, sodium 1,1-dimethyl-3,4-disulfonmethylpyrrolidinium betaine (I-1): 0.3 mass%, cyclic thioester compound (II-1): 1.0 mass%, (II-7): 1.0 mass%, and sodium salt additive (III-1): 0.2 mass% were added to the basic electrolyte to obtain a non-aqueous electrolyte. The composition and content of the additives are shown in Table 1.
[0081] Preparation of positive electrode:
[0082] NaNi 0.33 Fe 0.33 Mn 0.3302 (90% by mass) as a positive electrode active material, carbon black SP (5% by mass) as a conductive aid, and polyvinylidene fluoride (PVDF) (5% by mass) as a binder, the mixture of the above composition is dispersed in an N-methylpyrrolidone solvent to obtain a positive electrode mixture slurry. A 20 μm thick aluminum foil is prepared as a positive electrode current collector, and the obtained positive electrode mixture slurry is applied to the aluminum foil, and after drying, it is rolled with a press to obtain a sheet positive electrode. The positive electrode consists of a positive electrode current collector and a positive electrode active material layer.
[0083] Preparation of negative electrode:
[0084] 96% by mass of hard carbon is used as the negative electrode active material, 1% by mass of carbon black is used as the conductive aid, 1% by mass of sodium carboxymethyl cellulose dispersed in pure water is used as the thickener, and 2% by mass of styrene-butadiene rubber dispersed in pure water is used as the binder. The negative electrode mixture slurry is obtained after mixing. Aluminum foil with a thickness of 20 μm is used as the negative electrode current collector. The obtained slurry is applied to the aluminum foil, and after drying, it is rolled with a press to obtain a sheet-like negative electrode. The negative electrode consists of a negative electrode current collector and a negative electrode active material layer.
[0085] Diaphragm:
[0086] A porous polyethylene film is selected as the diaphragm.
[0087] A soft-pack sodium-ion secondary battery with a capacity of 1Ah is prepared by using the positive and negative electrodes, separator and electrolyte.
[0088] Formation steps:
[0089] The sodium ion secondary battery was charged at 25°C within a voltage range of 1.5V to 3.5V and then left for 50 hours. Next, the battery was charged at 25°C within a voltage range of 3.5V to 4.0V and left for 50 hours. Next, the battery was charged to 4.0V at 25°C and then discharged to 1.5V.
[0090] Initial charge and discharge treatment:
[0091] The formed battery was subjected to the following initial charge and discharge treatment in a temperature environment of 25°C.
[0092] Keep it at 25℃ for 12 hours. Then, charge the formed battery with constant current and constant voltage (0.2C, CC-CV) at a charging rate of 0.2C to 4.0V (charged 100%), then let it stand for 30 minutes, and discharge it with a constant current (0.2C, CC) at a discharge rate of 0.2C to 1.5V. Perform 3 cycles to stabilize the battery. After that, charge it with constant current and constant voltage (0.5C, CC-CV) to 4.0V, then let it stand for 30 minutes, and then discharge it with 1C constant current (1C, CC) to 1.5V.
[0093] Example 2
[0094] A sodium ion secondary battery was prepared in the same manner as in Example 1, except that 0.5 mass % of the compound of formula I-1 was added as additive I to prepare the nonaqueous electrolyte (see Table 1 below).
[0095] Example 3
[0096] A sodium ion secondary battery was prepared in the same manner as in Example 1, except that 1.0 mass % of the compound of formula I-1 was added as additive I to prepare the nonaqueous electrolyte (see Table 1 below).
[0097] Example 4
[0098] A sodium ion secondary battery was prepared in the same manner as in Example 1, except that in the preparation of the nonaqueous electrolyte, 0.5 mass % of the compound of formula I-2 was added instead of the compound of formula I-1 as additive I to prepare the nonaqueous electrolyte (see Table 1 below).
[0099] Example 5
[0100] A sodium ion secondary battery was prepared in the same manner as in Example 1, except that in the preparation of the non-aqueous electrolyte, an additive composition consisting of 0.5 mass % of sodium 1,1-dimethyl-3,4-disulfonmethylpyrrolidinium betaine (I-1), 1.0 mass % of a cyclic thioester compound (II-4), 1.0 mass % of (II-7), and 0.3 mass % of a sodium salt additive (III-2) was added to the basic electrolyte to obtain a non-aqueous electrolyte (see Table 1 below).
[0101] Example 6
[0102] A sodium ion secondary battery was prepared in the same manner as in Example 5, except that in the preparation of the non-aqueous electrolyte, the sodium salt additive (III-3) compound was selected instead of (III-2) and added to the basic electrolyte, thereby obtaining a non-aqueous electrolyte (see Table 1 below).
[0103] Example 7
[0104] A sodium ion secondary battery was prepared in the same manner as in Example 5, except that in the preparation of the non-aqueous electrolyte, the sodium salt additive (III-4) was selected instead of (III-2) and added to the basic electrolyte, thereby obtaining a non-aqueous electrolyte (see Table 1 below).
[0105] Example 8
[0106] A sodium ion secondary battery was prepared in the same manner as in Example 5, except that in the preparation of the non-aqueous electrolyte, sodium salt additives (III-2) 0.5 mass % and (III-6) 1.0 mass % were selected instead of (III-2) and added to the basic electrolyte, thereby obtaining a non-aqueous electrolyte (see Table 1 below).
[0107] Comparative Example 1
[0108] A sodium ion secondary battery was prepared in the same manner as in Example 2, except that additive I represented by the compound of formula I-1 was not added during the preparation of the nonaqueous electrolyte to prepare the nonaqueous electrolyte (see Table 1 below).
[0109] Comparative Example 2
[0110] A sodium ion secondary battery was prepared in the same manner as in Example 2, except that additive II represented by compounds of formula II-1 and II-7 was not added to prepare the nonaqueous electrolyte (see Table 1 below).
[0111] Comparative Example 3
[0112] A sodium ion secondary battery was prepared in the same manner as in Example 2, except that in the preparation of the non-aqueous electrolyte, additive III represented by the compound of formula III-1 was not added to prepare the non-aqueous electrolyte (see Table 1 below).
[0113] Comparative Example 4
[0114] A sodium ion secondary battery was prepared in the same manner as in Example 2, except that in the preparation of the nonaqueous electrolyte, the content of the additive I represented by the compound of formula I-1 was increased to 5.0 mass %, thereby preparing a nonaqueous electrolyte (see Table 1 below).
[0115] Table 1 Non-aqueous electrolytes with different additives
[0116]
[0117]
[0118] In Table 1, the amount of additives added is the percentage of the total mass of the non-aqueous electrolyte.
[0119] Performance Test:
[0120] The sodium ion secondary batteries prepared in the above examples were tested for performance according to the following methods, and the results are shown in Table 2:
[0121] DC internal resistance evaluation:
[0122] After the sodium ion secondary batteries prepared in Examples 1 to 8 and the sodium ion secondary batteries prepared in Comparative Examples 1 to 4 were charged to 4.0 V at a rate of 0.33 C under constant current / constant voltage conditions at 25° C., each sodium ion secondary battery was discharged to a discharge depth of 50% to adjust the state of charge to 50%, and then discharged at a rate of 2.5 C for 10 seconds to measure the DC internal resistance.
[0123] High temperature cycle characteristics evaluation:
[0124] The sodium ion secondary batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were charged to 4.0 V at a rate of 1C under constant current / constant voltage conditions at 45°C, and then discharged to 1.5 V at a rate of 1C under constant current conditions, which was defined as one cycle. After 100 charge and discharge cycles, the capacity retention rate (%) and the DC internal resistance increase rate (%) were measured.
[0125] The capacity retention rate (%) was calculated according to the following equation 1, and the DC internal resistance increase rate (%) was calculated according to the following equation 2. The measurement results are listed in Table 2 below.
[0126] [Equation 1]
[0127] Capacity retention rate (%) = (discharge capacity after 100 cycles / discharge capacity after 1 cycle) × 100
[0128] [Equation 2]
[0129] DC internal resistance increase rate (%) = {(DC internal resistance after 100 cycles - DC internal resistance after 1 cycle) / DC internal resistance after 1 cycle} × 100
[0130] Low temperature discharge test:
[0131] Low temperature discharge test: At 25℃, charge and discharge the secondary battery once at a voltage range of 1.5~4.0V and 0.33C, and record the battery discharge capacity as C0; place the battery in a -20℃ oven for 12h, charge and discharge the secondary battery once at a voltage range of 1.5~4.0V and 0.33C / 0.33C, and record the discharge capacity as C1, and calculate the low temperature charge and discharge performance.
[0132] Low temperature discharge performance (%) = (C1 / C0)*100.
[0133] Table 2
[0134]
[0135]
[0136] Referring to Table 2, we can see that:
[0137] 1. The capacity retention rate of the sodium ion secondary batteries of Examples 1 to 8 of the present invention after 100 cycles is about 98% or more, and the increase rate (%) of the DC internal resistance is about 10.2% or less.
[0138] On the contrary, for the sodium ion secondary battery of Comparative Example 1 in which the non-aqueous electrolyte does not contain the compound of Formula I, the secondary battery of Comparative Example 2 in which the non-aqueous electrolyte does not contain the compound of Formula II, and the secondary battery of Comparative Example 3 in which the non-aqueous electrolyte does not contain the compound of Formula III, it can be seen that compared with the secondary batteries of Examples 1 to 8, the capacity retention rate (%) and the DC internal resistance increase rate (%) after 100 cycles are significantly worse.
[0139] In addition, by comparing Example 2 and Comparative Example 4, in Comparative Example 4, in which the non-aqueous electrolyte contains 5% by mass of the compound of Formula I-1, the capacity retention rate (%) and the DC internal resistance increase rate (%) after 100 cycles are significantly deteriorated, which indicates that an increase in the content of the compound of Formula I-1 will deteriorate the performance of the battery. Preferably, the addition amount of the compound of Formula I-1 is preferably within 1% by mass.
[0140] 2. On the other hand, the sodium ion secondary batteries of Examples 1 to 8 of the present invention have significantly higher discharge capacities than those of Comparative Examples 1 to 3 under -20°C charge and discharge conditions. The reason for this is that the additives of the non-aqueous electrolyte of the present invention include the first additive (I), the cyclic sulfur-containing ester compound (II) and the sodium salt compound (III), and the combination of the three can improve the interface transport resistance of SEI / CEI and improve the high-temperature stability of the interface film. Therefore, the non-aqueous electrolyte can maintain a stable solid electrolyte interface film under high-temperature cycle conditions, thereby improving the high-temperature cycle performance of the sodium ion battery, and at the same time, it can also improve the low-temperature discharge performance of the sodium ion battery.
Claims
1. A non-aqueous electrolyte, comprising a sodium salt, a non-aqueous solvent and an additive, wherein the additive comprises a first additive, a second additive and a third additive, wherein: The first additive is as shown in formula (I), the second additive is a cyclic sulfur-containing ester compound, and the third additive is a sodium salt additive; Where: R1 and R2 are each independently selected from a hydrogen atom, an alkyl group or a substituted alkyl group having 1 to 6 carbon atoms (at least one hydrogen atom in the alkyl group may be substituted by a halogen atom), an alkenyl group or a substituted alkenyl group having 2 to 6 carbon atoms (at least one hydrogen atom in the alkenyl group may be substituted by a halogen atom), an alkynyl group having 2 to 6 carbon atoms, a benzyl group or an aryl group; The first additive has a content of 0.01% to 5.0% based on the total mass of the non-aqueous electrolyte; The amount of the cyclic sulfur-containing ester compound added is 0.01% to 5.0% based on the total mass of the non-aqueous electrolyte; The amount of the sodium salt additive added is 0.001% to 5.0% based on the total mass of the non-aqueous electrolyte; The non-aqueous electrolyte is applied to sodium ion batteries.
2. A non-aqueous electrolyte according to claim 1, characterized in that: The first additive is selected from sodium 1,1-dimethyl-3,4-disulfomethylpyrrolidinium betaine represented by formula (I-1) or sodium 1-dimethyl-1-allyl-3,4-disulfomethylpyrrolidinium betaine represented by formula (I-2); 3. A non-aqueous electrolyte according to claim 1, characterized in that: The cyclic sulfur-containing ester compound is shown in formula (II): In Formula II: R3 is selected from an oxygen atom, an alkylene group having 1 to 6 carbon atoms, and a vinylene group; R4 is selected from an alkylene group having 1 to 6 carbon atoms, a group represented by formula ii-1 or a group represented by formula ii-2; wherein: "*" represents the binding position, R 41 is an oxygen atom, an alkyl group having 1 to 6 carbon atoms, or an oxymethylene group, R 42 It is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.
4. A non-aqueous electrolyte according to claim 1, characterized in that: The cyclic sulfur-containing ester compound is selected from any one or more of the compounds represented by formula II-1 to II-7:
5. A non-aqueous electrolyte according to claim 1, characterized in that: The sodium salt additive is selected from any one or more of acesulfame sodium borotrifluoride compound, difluoro sodium oxalate borate, sodium difluorophosphate, difluoro sodium bisoxalate phosphate, tetrafluoro sodium oxalate phosphate and sodium bis(fluorosulfonyl)imide.
6. A non-aqueous electrolyte according to claim 1, characterized in that: The sodium salt includes at least one fluorine-containing sodium salt, and the fluorine-containing sodium salt is selected from inorganic acid anion salts or organic acid anion salts; the non-aqueous solvent is selected from any one or more of cyclic carbonates, chain carbonates, aliphatic carboxylates, γ-lactones, cyclic ethers, chain ethers, nitriles, amides, lactams, sulfolane, and phosphates.
7. Use of the non-aqueous electrolyte according to any one of claims 1 to 6 in a sodium ion secondary battery, characterized in that: The sodium ion secondary battery comprises a positive electrode sheet, a negative electrode sheet, a separator, and a non-aqueous electrolyte. The positive electrode sheet comprises a positive electrode collector and a positive electrode membrane containing a positive electrode active material disposed on the positive electrode collector; the negative electrode sheet comprises a negative electrode collector and a negative electrode membrane containing a negative electrode active material disposed on the negative electrode collector; and the separator is disposed between the positive electrode sheet and the negative electrode sheet.
Citation Information
Patent Citations
Electrolyte of sodium ion battery, and preparation method and application of electrolyte
CN106920988A
3-Sulfinatomethyl and 3-sulfonatomethyl-4-sulfomethyl-pyrrolidinium betain and their salts, and process for their preparation
EP0163319A2
Electrolyte and battery containing electrolyte
CN109904521A
High-temperature electrolyte additive, battery electrolyte and sodium ion battery
CN114243113A
Sodium ion secondary battery
CN116247282A