Preparation and application of polyethylene plastic modified by nanoparticles
Through the preparation method of nanoparticle modified polyethylene plastic, the solvent exchange method is used to self-assemble lignin nanospheres and introduce nitrogen and phosphorus elements, combined with ZnO hybridization, the problems of flammability and aging of polyethylene plastics are solved, and safer , pollution-free flame retardant and antibacterial effects have enhanced its application value.
Patent Information
- Application Number
- CN202411027868.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Polyethylene plastics are prone to aging, low strength and rigidity, and lack of flammability, especially in burning, which leads to frequent fire accidents, which limits their application.
Using nanoparticle modified polyethylene plastic preparation method, self-assemble lignin nanospheres through solvent exchange method, introduce nitrogen and phosphorus elements to enhance dispersion and compatibility, and hybridize with ZnO to form a dense carbon layer structure, and improve flame retardant Performance and antibacterial effect, combined with polyethylene plastic to improve its performance.
It has achieved good flame retardant properties, antibacterial properties and anti-aging properties of polyethylene plastics, which is safer and pollution-free than traditional halogen-containing flame retardants, enhancing its application value in special fields.
Smart Images

Figure CN118546454B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of plastics, and mainly relates to the preparation of polyethylene plastics, and in particular to a preparation method of nano-particle modified polyethylene plastics and application thereof. Background Art
[0002] Polyethylene plastics are widely used due to their good chemical stability, good toughness and easy processing, but most polyethylene plastics are non-biodegradable substances, which poses a great threat to the environment.
[0003] However, plastics have some disadvantages such as easy aging, low strength and rigidity, and flammability. In particular, plastics are flammable. Once a fire breaks out, it is difficult to extinguish. Serious fire accidents have repeatedly occurred. Due to these disadvantages, its application is limited in many aspects. Therefore, it should be flame-retardant and enhanced to improve the practical value of plastics. Summary of the invention
[0004] In view of the above problems, the present invention proposes a preparation method and application of nanoparticle-modified polyethylene plastic.
[0005] In a first aspect, the present invention provides a method for preparing a nanoparticle-modified polyethylene plastic, and the specific steps are as follows:
[0006] S1, take 2-20g of lignin powder in 80-300ml of tetrahydrofuran solution, stir at room temperature for 20-40min, and after it is fully dissolved, continuously drip 150-250ml of deionized water, continue to fully stir for 60-90min to self-assemble into balls, then put the mixture into a dialysis bag with a cutoff relative molecular mass of 1000 and put it into ultrapure water, dialyze at 35-50°C for 24-72h to remove the residual tetrahydrofuran in the mixed solution, and then collect the product for freeze-drying to obtain nano-spherical lignin; this step self-assembles lignin into nanospheres by solvent exchange method, the method is simple to operate and the synthesized lignin nanospheres are concentrated in size and have good uniformity. In addition, due to the particularity of their structure, the nanospheres will have a better specific surface area and better surface properties;
[0007] S2, take 5-10g of the lignin nanospheres obtained in step S1 and dissolve them in 150-300ml of 1mol / L NaOH solution, ultrasonically treat for 1-1.5h to completely dissolve them, then add 0.5-1.5g of formaldehyde solution and 2-4g of 3-aminopropyltriethoxysilane, stir at 50-90°C for 3-6h, after the reaction is complete, adjust the pH of the mixed solution to 2-4 with 0.05mol / L HCl solution, precipitate the precipitate, wash the precipitate with deionized water 3-5 times, then freeze-dry the product for 8-12h, dry to constant weight and grind into powder to obtain nitrogen-modified lignin nanospheres;
[0008] S3, 5-10g of the modified lignin nanospheres obtained in step S2 above were placed in a beaker, added to 50-150ml of dimethylformamide, and ultrasonically treated for 1-1.5h to completely dissolve them, then 0.1-0.3g of formaldehyde solution and 2-3g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide were added, and the pH of the mixed solution was adjusted to 4 with 0.05mol / L HCl solution, and the reaction was carried out for 4-6h at a reaction temperature of 60-80°C. After the reaction was completed, the mixed solution was placed in a rotary evaporator and heated at 80-90°C to complete the reaction. The dimethylformamide is removed, and the product is then placed in freeze drying. After drying, functionalized lignin nanospheres can be obtained. This step enhances the dispersibility and compatibility of lignin in the polyethylene matrix by cleverly introducing nitrogen and phosphorus into the benzene ring of lignin. In addition, nitrogen and phosphorus, as halogen-free flame retardant elements, synergistically act with the carbon in lignin to promote the formation of a dense and continuous carbon layer structure, thereby giving the lignin nanospheres good flame retardant properties. Compared with the previous technology of adding halogen-containing flame retardants to produce HCl, HBr and other gases to isolate the air for flame retardancy, this step is safer and pollution-free.
[0009] S4, take 11-20g of Zn(NO3)2·6H2O and 3-10g of the functionalized lignin nanospheres obtained in the above step S3, dissolve them in 110ml of cyclohexamethylenetetramine solution with a mass concentration of 0.005-0.01g / ml, stir at 110-130℃ for 2-5h, then cool to room temperature, and then put it into a high-speed rotating centrifuge to obtain a precipitate, and freeze-dry it to obtain a ZnO hybrid lignin nanosphere material; this step effectively combines nano ZnO with functionalized lignin by a hydrothermal method. On the one hand, ZnO is a non-toxic and harmless material to the human body and the environment, and has a certain antibacterial effect. This step hybridizes ZnO and lignin nanospheres, and the synergistic effect between the two can effectively control the sustained release of zinc ions, so that the material has a longer-term antibacterial effect. At the same time, the effective combination of the two also gives the hybrid material a good synergistic ultraviolet light / line absorption ability, reducing the optical aging of ultraviolet light / line to it;
[0010] S5, take 5-10g of the ZnO hybrid lignin nanosphere material in the above step S4, stir it in 30-150ml of isopropanol solution for 10-30min, then use ultrasonic oscillation for 20-30min, add it to 40-100g of polyethylene, set the temperature to 30-50°C, stir at high speed for 1-2h, and after the isopropanol solution is fully evaporated, ensure that the nanoparticles are evenly dispersed in the polyethylene plastic, and obtain the preliminary modified polyethylene plastic; this step efficiently combines the ZnO hybrid lignin nanosphere material with the polyethylene plastic, and through the functionalization of the lignin nanosphere, it gives it excellent flame retardant properties, antibacterial properties and anti-aging ability, combines the biomass material with polyethylene, optimizes the polyethylene plastic at the lowest cost, and enhances its performance;
[0011] S6. Put the preliminarily modified polyethylene plastic obtained in the above step S5 into an open mixer, set the mixing temperature to 95-110°C, and the mixing time to 5-20min. After the mixing is completed, a blank is obtained. Then the blank is placed in a polyester film mold and pressed tightly, and then placed in a flat vulcanizer. The temperature is set to 110°C, and the pressure is increased by 5MPa every 10min. When the pressure reaches 20MPa, the temperature is adjusted to 175°C for cross-linking for 15-30min. After the cross-linking is completed, it is cooled to room temperature to obtain the nanoparticle-modified polyethylene plastic.
[0012] Preferably, the amount of deionized water used in step S1 is 175 ml.
[0013] Preferably, the amount of 3-aminopropyltriethoxysilane added in step S2 is 2.6 g.
[0014] Preferably, the temperature in step S2 is set to 70°C.
[0015] Preferably, in step S3, the amount of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide added is 2.5 g.
[0016] Preferably: the reaction temperature in step S3 is set to 88°C.
[0017] Preferably, the amount of Zn(NO3)2·6H2O added in step S4 is 12 g.
[0018] Preferably, the concentration of the hexamethylenetetramine solution in step S4 is 0.005 g / ml.
[0019] Preferably, the cross-linking time in step S6 is set to 18 minutes.
[0020] In a second aspect, the present invention provides a nanoparticle-modified polyethylene plastic obtained by the preparation method described above, which is used as a special material with requirements for fireproof and antibacterial properties.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. In the process of modifying polyethylene plastics of the present invention, functionalized biomass material lignin is used as the main additive. By efficiently combining the modified lignin nanospheres with polyethylene plastics, efficient synergistic effects are stimulated at a relatively low cost, thereby compensating for the performance deficiencies of polyethylene plastics.
[0023] 2. The present invention adopts a solvent exchange method to self-assemble lignin into nanospheres. The method is simple to operate and the synthesized lignin nanospheres are concentrated in size. The nanosphere structure has a better specific surface area and better surface properties, and is easier to functionalize and modify.
[0024] 3. The present invention enhances the dispersibility and compatibility of lignin in the polyethylene matrix by ingeniously introducing nitrogen and phosphorus into the benzene ring of lignin. The synergistic effect of nitrogen and phosphorus as halogen-free flame retardant elements and carbon in lignin can promote the formation of a dense and continuous carbon layer structure after combustion. After the polyethylene plastic is modified by the halogen-containing flame retardant, the polyethylene plastic can be endowed with good flame retardant properties. Compared with the previous technology of adding halogen-containing flame retardants to produce HCl, HBr and other gases to isolate the air for flame retardancy, this step is safer and pollution-free.
[0025] 4. In this step, ZnO and lignin nanospheres are hybridized. The synergistic effect between the two can effectively control the sustained release of zinc ions, so that the material has a longer-term antibacterial effect. At the same time, the effective combination of the two can also give it a good synergistic ultraviolet light / ray absorption ability, reduce the optical aging of ultraviolet light / ray, so as to improve the antibacterial performance and anti-aging ability of polyethylene plastics, and further enhance the wide application of polyethylene plastics in special fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0027] Figure 1 This is a scan of the nano-spherical lignin prepared in Example 1 of the present invention.
[0028] Figure 2 This is a scan of the lignin in Comparative Example 1 prepared in the present invention.
[0029] Figure 3 The antibacterial rates of Example 1 and Comparative Example 1 prepared in the present invention.
[0030] Figure 4 The scanning electron microscope image (left) and EDS energy spectrum (right) of the ZnO hybrid lignin nanosphere material prepared in Example 1 of the present invention.
[0031] Figure 5 UV-visible diffuse reflectance spectra of Example 3 and Comparative Example 5 prepared in the present invention. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the content of the present invention and are not used to limit the present invention.
[0033] Embodiment 1:
[0034] S1. Take 8g of lignin powder and put it into 120ml of tetrahydrofuran solution, stir at room temperature for 30min, and then drip 150ml of deionized water continuously after it is fully dissolved, and continue to stir for 60min to self-assemble into balls. Then put the mixture into a dialysis bag with a relative molecular mass cutoff of 1000 and put it into ultrapure water, and dialyze it at 35°C for 24h to remove the residual tetrahydrofuran in the mixed solution, and then collect the product for freeze-drying to obtain nano-spherical lignin;
[0035] S2, take 5g of the lignin nanospheres obtained in step S1 and dissolve them in 180ml of 1mol / L NaOH solution, perform ultrasonic treatment for 1.5h to completely dissolve them, then add 1.0g of formaldehyde solution and 2.6g of 3-aminopropyltriethoxysilane, stir at 70°C for 4h, after the reaction is complete, adjust the pH of the mixed solution to 3 with 0.05mol / L HCl solution, precipitate the precipitate, wash the precipitate with deionized water 5 times, then freeze-dry the product for 12h, dry to constant weight and grind into powder to obtain nitrogen-modified lignin nanospheres;
[0036] S3, 8g of the modified lignin nanospheres obtained in step S2 above were placed in a beaker, added to 80ml of dimethylformamide, and subjected to ultrasonic treatment for 1h to completely dissolve them, followed by adding 0.2g of formaldehyde solution and 2.5g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, adjusting the pH of the mixed solution to 4 with 0.05mol / L HCl solution, and reacting for 6h at a reaction temperature of 60°C. After the reaction was completed, the mixed solution was placed in a rotary evaporator to remove dimethylformamide at 88°C, and then the product was placed in freeze drying to obtain functionalized lignin nanospheres after drying;
[0037] S4, taking 12g of Zn(NO3)2·6H2O and 8g of the functionalized lignin nanospheres obtained in the above step S3, dissolving them in 110ml of a 0.005g / ml hexamethylenetetramine solution, stirring at 115°C for 2h, then cooling to room temperature, and then placing the precipitate in a high-speed rotating centrifuge to obtain a precipitate, and freeze-drying the precipitate to obtain a ZnO hybrid lignin nanosphere material;
[0038] S5, taking 10g of the ZnO hybrid lignin nanosphere material in the above step S4, stirring it in 80ml of isopropanol solution for 25min, then oscillating it with ultrasound for 20min, adding it to 100g of polyethylene, setting the temperature to 40°C, stirring it at high speed for 2h, and after the isopropanol solution is fully evaporated, ensuring that the nanoparticles are evenly dispersed in the polyethylene plastic, a preliminary modified polyethylene plastic can be obtained;
[0039] S6. Put the preliminarily modified polyethylene plastic obtained in the above step S5 into an open mixer, set the mixing temperature to 95°C, and the mixing time to 10 minutes. After the mixing is completed, a blank is obtained. Then the blank is placed in a polyester film mold and pressed tightly, and then placed in a flat vulcanizer. The temperature is set to 110°C, and the pressure is increased by 5MPa every 10 minutes. When the pressure reaches 20MPa, the temperature is adjusted to 175°C for cross-linking for 18 minutes. After the cross-linking is completed, it is cooled to room temperature to obtain the nanoparticle-modified polyethylene plastic.
[0040] Comparative Example 1: Except that deionized water is not added in step S1, the remaining steps are the same as those in Example 1.
[0041] Example 1 A nano-spherical lignin was synthesized by self-assembly technology, such as Figure 1 As shown, the overall average size is about 310nm and the spherical shape is obvious, while the comparative example 1 is only lignin powder. Figure 2Scanning electron microscopy shows that lignin presents an amorphous structure with a size of about 1.5 μm. In addition, the present invention evaluates the antibacterial effect of lignin nanomaterial modified polyethylene plastic through a contact antibacterial test. 10 μl of bacterial suspension is pipetted into a culture dish containing 25 mg of modified polyethylene plastic material, and a control group is set for testing. After incubation at 25°C for 6 hours, 1 ml of sterile PBS is added to each well to resuspend the surviving bacteria. The treated bacterial suspension forms colonies, and then the experimental data is analyzed to obtain the antibacterial rate. Figure 3 As shown, the antibacterial rates of Example 1 against Staphylococcus aureus and Escherichia coli can reach more than 90%, while the antibacterial rates of Comparative Example 1 against Staphylococcus aureus and Escherichia coli are 53% and 48%, respectively. The results of Comparative Example 1 show that the antibacterial rate of the modified polyethylene plastic with only lignin powder added is much lower than that of the polyethylene plastic modified with spherical lignin in Example 1. This is because the complex of lignin powder and zinc oxide has a certain antibacterial effect, and the nano-spherical lignin proposed in the present invention has a larger specific surface area and excellent adsorption due to its nano-scale size and special spherical morphology, exposing more active sites, increasing the contact process, and effectively solving the agglomeration problem of ZnO after hybridization in step S4. Figure 4 The scanning electron microscope image (left) shows that the surface of the lignin nanospheres is rough but the morphology has not changed significantly after ZnO hybridization. At the same time, the EDS energy spectrum (right) also shows that the Zn element is evenly dispersed without obvious aggregation or agglomeration, indicating that the ZnO hybrid on the lignin nanospheres is evenly dispersed, which strengthens the synergistic effect between the two, effectively controls the sustained release of zinc ions, and the antibacterial effect can be controlled and prolonged, making the material have a better antibacterial effect.
[0042] Embodiment 2:
[0043] S1. Take 8g of lignin powder and put it into 110ml of tetrahydrofuran solution, stir at room temperature for 30min, and then drip 150ml of deionized water continuously after it is fully dissolved, and continue to stir for 60min to self-assemble into balls. Then put the mixture into a dialysis bag with a relative molecular mass of 1000 and put it into ultrapure water, and dialyze it at 35°C for 24h to remove the residual tetrahydrofuran in the mixed solution, and then collect the product for freeze-drying to obtain nano-spherical lignin;
[0044] S2, take 5g of the lignin nanospheres obtained in step S1 and dissolve them in 180ml of 1mol / L NaOH solution, ultrasonically treat for 2h to completely dissolve them, then add 1.0g of formaldehyde solution and 2.6g of 3-aminopropyltriethoxysilane, stir at 70°C for 5h, after the reaction is complete, adjust the pH of the mixed solution to 3 with 0.05mol / L HCl solution, precipitate the precipitate, wash the precipitate with deionized water 5 times, then freeze-dry the product for 12h, dry to constant weight and grind into powder to obtain nitrogen-modified lignin nanospheres;
[0045] S3, 8g of the modified lignin nanospheres obtained in step S2 above were placed in a beaker, added to 80ml of dimethylformamide, and subjected to ultrasonic treatment for 1.5h to completely dissolve them, followed by adding 0.2g of formaldehyde solution and 2.5g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, adjusting the pH of the mixed solution to 4 with 0.05mol / L HCl solution, and reacting for 6.5h at a reaction temperature of 60°C. After the reaction was completed, the mixed solution was placed in a rotary evaporator to remove dimethylformamide at 88°C, and the product was then placed in freeze drying to obtain functionalized lignin nanospheres after drying;
[0046] S4, taking 12g of Zn(NO3)2·6H2O and 8g of the functionalized lignin nanospheres obtained in the above step S3, dissolving them in 110ml of a 0.005g / ml hexamethylenetetramine solution, stirring at 110°C for 2h, then cooling to room temperature, and then placing the precipitate in a high-speed rotating centrifuge to obtain a precipitate, and freeze-drying the precipitate to obtain a ZnO hybrid lignin nanosphere material;
[0047] S5, taking 10g of the ZnO hybrid lignin nanosphere material in the above step S4, stirring it in 80ml of isopropanol solution for 25min, then oscillating it with ultrasound for 20min, adding it to 100g of polyethylene, setting the temperature to 40°C, stirring it at high speed for 2h, and after the isopropanol solution is fully evaporated, ensuring that the nanoparticles are evenly dispersed in the polyethylene plastic, a preliminary modified polyethylene plastic can be obtained;
[0048] S6. Put the preliminarily modified polyethylene plastic obtained in the above step S5 into an open mixer, set the mixing temperature to 95°C, and the mixing time to 10 minutes. After the mixing is completed, a blank is obtained. Then the blank is placed in a polyester film mold and pressed tightly, and then placed in a flat vulcanizer. The temperature is set to 110°C, and the pressure is increased by 5MPa every 10 minutes. When the pressure reaches 20MPa, the temperature is adjusted to 175°C for cross-linking for 18 minutes. After the cross-linking is completed, it is cooled to room temperature to obtain the nanoparticle-modified polyethylene plastic.
[0049] Comparative Example 2: Except that 3-aminopropyltriethoxysilane is not added in step S2, the remaining steps are the same as those in Example 2.
[0050] Comparative Example 3: Except that 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is not added in step S3, the remaining steps are the same as those in Example 2.
[0051] Comparative Example 4: Except that 3-aminopropyltriethoxysilane in step S2 and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in step S3 were not added, the remaining steps were the same as those in Example 2.
[0052] In Example 2, nitrogen and phosphorus are cleverly introduced into the benzene ring of lignin, which can give polyethylene plastic good flame retardant properties. The present invention makes samples of Example 2, Comparative Example 2, Comparative Example 3 and Comparative Example 4, and conducts comparative tests on flame retardant properties, wherein the limiting oxygen index is tested in the limiting oxygen index tester YZS-10A with reference to the GB / T2406.2-2009 standard. The results are shown in Table 1, and the enhancement effect of Example 2 is the most significant, followed by Comparative Example 3 and Comparative Example 2, and the flame retardant effect of Comparative Example 4 is the worst, wherein the modified polyethylene plastic of Example 2 will basically extinguish immediately after leaving the flame, and cannot spontaneously combust, which indicates that nitrogen and phosphorus as halogen-free flame retardant elements will produce effective synergistic effects with carbon in lignin, and this synergistic effect can promote the formation of a dense and continuous carbon layer structure after the polyethylene plastic is burned, thereby enhancing the flame retardant effect, and compared with the previous technology of adding halogen-containing flame retardants to produce HCl, HBr and other gases to isolate the air for flame retardancy, this step is safer and pollution-free.
[0053] Table 1
[0054] Softening temperature(℃) Oxygen demand index Combustion state Limiting oxygen index Example 2 178±10 63.2±2.2% Self-extinguishing 26.8±3.6% Comparative Example 2 150±5 45.6±3.2% Gradually extinguishes after burning 17.5±2.0% Comparative Example 3 145±10 44.5±0.6% Gradually extinguishes after burning 19.2±3.1% Comparative Example 4 115±6 25.8±3.8% Ongoing 10.1±5.1%
[0055] Embodiment 3:
[0056] S1. Take 8g of lignin powder and put it into 120ml of tetrahydrofuran solution, stir at room temperature for 30min, and then drip 150ml of deionized water continuously after it is fully dissolved, and continue to stir for 60min to self-assemble into balls. Then put the mixture into a dialysis bag with a relative molecular mass cutoff of 1000 and put it into ultrapure water, and dialyze it at 35°C for 24h to remove the residual tetrahydrofuran in the mixed solution, and then collect the product for freeze-drying to obtain nano-spherical lignin;
[0057] S2, take 5g of the lignin nanospheres obtained in step S1 and dissolve them in 180ml of 1mol / L NaOH solution, perform ultrasonic treatment for 1.5h to completely dissolve them, then add 1.0g of formaldehyde solution and 2.6g of 3-aminopropyltriethoxysilane, stir at 70°C for 4h, after the reaction is complete, adjust the pH of the mixed solution to 3 with 0.05mol / L HCl solution, precipitate the precipitate, wash the precipitate with deionized water 5 times, then freeze-dry the product for 12h, dry to constant weight and grind into powder to obtain nitrogen-modified lignin nanospheres;
[0058] S3, 8g of the modified lignin nanospheres obtained in step S2 above were placed in a beaker, added to 80ml of dimethylformamide, and subjected to ultrasonic treatment for 1h to completely dissolve them, followed by adding 0.2g of formaldehyde solution and 2.5g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, adjusting the pH of the mixed solution to 4 with 0.05mol / L HCl solution, and reacting for 6h at a reaction temperature of 60°C. After the reaction was completed, the mixed solution was placed in a rotary evaporator to remove dimethylformamide at 88°C, and then the product was placed in freeze drying to obtain functionalized lignin nanospheres after drying;
[0059] S4, taking 12g of Zn(NO3)2·6H2O and 8g of the functionalized lignin nanospheres obtained in the above step S3, dissolving them in 110ml of a 0.005g / ml hexamethylenetetramine solution, stirring at 105°C for 2h, then cooling to room temperature, and then placing the precipitate in a high-speed rotating centrifuge to obtain a precipitate, and freeze-drying the precipitate to obtain a ZnO hybrid lignin nanosphere material;
[0060] S5, taking 10g of the ZnO hybrid lignin nanosphere material in the above step S4, stirring it in 80ml of isopropanol solution for 25min, then oscillating it with ultrasound for 30min, adding it to 90g of polyethylene, setting the temperature to 40°C, stirring it at high speed for 2h, and after the isopropanol solution is fully evaporated, ensuring that the nanoparticles are evenly dispersed in the polyethylene plastic, a preliminary modified polyethylene plastic can be obtained;
[0061] S6. Put the preliminarily modified polyethylene plastic obtained in the above step S5 into an open mixer, set the mixing temperature to 90°C, and the mixing time to 10 minutes. After the mixing is completed, a blank is obtained. Then the blank is placed in a polyester film mold and pressed tightly, and then placed in a flat vulcanizer. The temperature is set to 110°C, and the pressure is increased by 5MPa every 10 minutes. When the pressure reaches 20MPa, the temperature is adjusted to 175°C for cross-linking for 18 minutes. After the cross-linking is completed, it is cooled to room temperature to obtain the nanoparticle-modified polyethylene plastic.
[0062] Comparative Example 5: Except that Zn(NO3)2·6H2O is not added in step S4, the remaining steps are the same as those in Example 3.
[0063] The present invention uses a comprehensive thermal analyzer to test the oxidation induction time of Example 3 and Comparative Example 5 to evaluate the anti-aging performance test. The test steps are: 6 mg of the tested material is heated to 150° C. in a nitrogen environment, the heating rate is set to 10° C. / min, and then maintained for 10 minutes, and then the nitrogen is switched to oxygen, and 150° C. is continued to be maintained until the sample is completely oxidized. The results show that the oxidation induction time of Example 3 is 6.1 minutes, while the oxidation induction time of Comparative Example 5 is only 3.0 minutes, indicating that the ZnO hybrid lignin nanosphere material has certain antioxidant properties. This is because lignin contains a large amount of phenolic hydroxyl groups and has a strong ability to capture free radicals. In addition, the present invention uses ultraviolet-visible diffuse reflectance spectroscopy to characterize the optical properties of Example 3 and Comparative Example 5, such as Figure 5 As shown, Example 3 has the effect of synergistically enhancing ultraviolet light / ray absorption. This is because when ZnO is irradiated under ultraviolet light, the photoelectrons in ZnO can be transferred to the lignin molecules under the retraction of the unsaturated bonds in lignin. The synergistic effect between the two can give it a good synergistic ultraviolet light / ray absorption ability, reduce the optical aging of ultraviolet light / ray to it, thereby improving the optical anti-aging ability of polyethylene plastics and further enhancing the wide application of polyethylene plastics in special fields.
[0064] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing nanoparticle-modified polyethylene plastic, characterized in that: The specific synthesis steps are as follows: S1. Take 2-20g of lignin powder and put it into 80-300ml of tetrahydrofuran solution, stir it at room temperature for 20-40min, and after it is fully dissolved, continuously drip 150-250ml of deionized water, continue to stir for 60-90min to self-assemble into balls, then put the mixture into a dialysis bag with a cutoff relative molecular mass of 1000 and put it into ultrapure water, dialyze it at 35-50℃ for 24-72h to remove the residual tetrahydrofuran in the mixed solution, and then collect the product for freeze-drying to obtain nano-spherical lignin; S2, take 5-10g of the lignin nanospheres obtained in step S1 and dissolve them in 150-300ml of 1mol / L NaOH solution, ultrasonically treat for 1-1.5h to completely dissolve them, then add 0.5-1.5g of formaldehyde solution and 2-4g of 3-aminopropyltriethoxysilane, stir at 50-90°C for 3-6h, after the reaction is complete, adjust the pH of the mixed solution to 2-4 with 0.05mol / L HCl solution, precipitate the precipitate, wash the precipitate with deionized water 3-5 times, then freeze-dry the product for 8-12h, dry to constant weight and grind into powder to obtain nitrogen-modified lignin nanospheres; S3, 5-10g of the nitrogen-modified lignin nanospheres obtained in the above step S2 are placed in a beaker, added to 50-150ml of dimethylformamide, and ultrasonically treated for 1-1.5h to completely dissolve them, followed by adding 0.1-0.3g of formaldehyde solution and 2-3g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and adjusting the pH of the mixed solution to 4 with 0.05mol / L HCl solution, and reacting for 4-6h at a reaction temperature of 60-80°C. After the reaction is completed, the mixed solution is placed in a rotary evaporator to remove dimethylformamide at 80-90°C, and then the product is placed in freeze drying, and the functionalized lignin nanospheres can be obtained after drying; S4, taking 11-20g of Zn(NO3)2·6H2O and 3-10g of the functionalized lignin nanospheres obtained in the above step S3, dissolving them in 110ml of a cyclohexamethylenetetramine solution with a mass concentration of 0.005-0.01g / ml, stirring at 110-130°C for 2-5h, then cooling to room temperature, and then placing the precipitate in a high-speed rotating centrifuge to obtain a precipitate, and freeze-drying the precipitate to obtain a ZnO hybrid lignin nanosphere material; S5, take 5-10g of the ZnO hybrid lignin nanosphere material in the above step S4, stir it in 30-150ml of isopropanol solution for 10-30min, then oscillate it with ultrasound for 20-30min, add it to 40-100g of polyethylene, set the temperature to 30-50°C, stir it at high speed for 1-2h, and after the isopropanol solution is fully evaporated, ensure that the nanoparticles are evenly dispersed in the polyethylene plastic, and obtain the preliminary modified polyethylene plastic; S6. Put the preliminarily modified polyethylene plastic obtained in the above step S5 into an open mixer, set the mixing temperature to 95-110°C, and the mixing time to 5-20min. After the mixing is completed, a blank is obtained. Then the blank is placed in a polyester film mold and pressed tightly, and then placed in a flat vulcanizer. The temperature is set to 110°C, and the pressure is increased by 5MPa every 10min. When the pressure reaches 20MPa, the temperature is adjusted to 175°C for cross-linking for 15-30min. After the cross-linking is completed, it is cooled to room temperature to obtain the nanoparticle-modified polyethylene plastic.
2. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 1, characterized in that: The amount of deionized water used in step S1 is 175 ml.
3. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 1 or 2, characterized in that: The amount of 3-aminopropyltriethoxysilane added in step S2 is 2.6 g.
4. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 2, characterized in that: In step S2, the temperature is set to 70°C.
5. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 4, characterized in that: The amount of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide added in step S3 is 2.5 g.
6. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 5, characterized in that: The amount of Zn(NO3)2·6H2O added in step S4 is 12 g.
7. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 6, characterized in that: The concentration of the hexamethylenetetramine solution in step S4 is 0.005 g / ml.
8. The method for preparing a nanoparticle-modified polyethylene plastic according to claim 6 or 7, characterized in that: The cross-linking time in step S6 is set to 18 minutes.
9. A nanoparticle-modified polyethylene plastic obtained by the preparation method according to any one of claims 1 to 8, used as a material with requirements for fireproof and antibacterial properties.