A production process of high-strength and tough cast aluminum alloy material

By analyzing the temperature change characteristics and differences of the solid solution image, the solution treatment time of the casting is adjusted in real time, which solves the performance problems caused by improper solution time of the aluminum alloy material during the solution treatment, and achieves high strength, toughness and uniformity.

CN118600256BActive Publication Date: 2024-10-22LIAONING PROGRESSING CAST METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067531.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-22
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing aluminum alloy materials have problems such as too long or too short solution treatment time, which leads to excessive diffusion of alloy elements or incomplete dissolution of the strengthening phase, affecting the microstructure and performance of the castings.

Method used

By collecting solid solution images, the temperature change continuity and temperature difference characteristics of the pixels are obtained, the solid solution area of ​​the casting is divided, the solid solution adequacy coefficient is calculated, and the solid solution treatment time is adjusted in real time to avoid excessive diffusion or unevenness of alloy elements.

Benefits of technology

It achieves the improvement of high strength, toughness and performance of castings, avoids the performance degradation caused by too long or too short solid solution time, and ensures the homogenization and full dissolution of alloy elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600256B_ABST
    Figure CN118600256B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of metal materials, and specifically to a production process of high-strength and tough cast aluminum alloy materials. The process includes: weighing AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source respectively as spare; placing AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source in a preheating furnace for preheating; melting the material to obtain a melt, drying, ventilating, and standing the melt before casting to obtain a casting; subjecting the obtained casting to a solution treatment, and during the solution treatment, determining the end time of the solution treatment stage according to the temperature value difference between pixels and the similarity and temperature distribution characteristics between regions; after the solution treatment, quenching and aging the casting to obtain a high-strength and tough cast aluminum alloy; a shot blasting step to remove surface defects of the high-strength and tough cast aluminum alloy to complete production. The present application avoids the problem of casting performance being affected by the solution time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal materials, and in particular to a production process of a high-strength and toughness cast aluminum alloy material. Background Art

[0002] With the development and progress of social science and technology, people's requirements for industrial materials have also increased. High-strength and tough cast aluminum alloy materials are widely used in the automotive and aerospace fields due to their light weight and high strength. Compared with other industrial materials such as magnesium alloys or composite materials, aluminum alloys have the advantages of low density, strong corrosion resistance and low production cost. Adding silicon source, magnesium source and other alloys to aluminum alloys can improve the strength and toughness of aluminum alloys while ensuring the plasticity index of aluminum alloys, making the application range of aluminum alloys more extensive.

[0003] However, in the preparation process of improving the strength and toughness of aluminum alloys by existing technologies, it is necessary to strictly control the solid solution time of the casting. When the solid solution treatment time of the casting is too long, it may cause excessive diffusion of alloy elements at high temperature, affecting the microstructure and performance of the casting after quenching treatment; when the solid solution treatment time of the casting is too short, it may cause the strengthening phase to fail to be completely dissolved, resulting in poor solid solution effect of the casting, which will also affect the strength of the casting after aging treatment. Summary of the invention

[0004] In order to solve the technical problem of poor casting strength caused by solution time, the present application provides a production process of high-strength and toughness cast aluminum alloy material, and the technical solution adopted is as follows:

[0005] The present application proposes a production process for a high-strength and tough cast aluminum alloy material, which comprises the following steps:

[0006] The material preparation step is to use AlSi9Mg alloy as a master alloy, and weigh AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source according to percentage as standby, wherein the AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source include main elements and impurity elements;

[0007] A preheating step, placing the AlSi9Mg master alloy, the strontium source, the magnesium source, the silicon source, and the titanium source into a preheating furnace, and gradually heating the preheating furnace to a preheating temperature for preheating;

[0008] The melting and casting step is to place the preheated AlSi9Mg master alloy in a furnace to melt, then add the preheated strontium source, magnesium source, silicon source and titanium source, stir evenly after melting to obtain a melt, dry, ventilate and let the melt stand before casting to obtain a casting;

[0009] A heat treatment step, wherein the obtained casting is subjected to a solution treatment, and after the solution treatment, the casting is subjected to a quenching and aging treatment to obtain a high-strength and tough cast aluminum alloy;

[0010] The following steps are involved in the solution treatment phase:

[0011] Collect the solid solution image at each moment;

[0012] Any pixel in the solid solution image is recorded as the central pixel, and the first solid solution feature of the central pixel is obtained according to the temperature difference between the pixels around the central pixel and the difference between the temperature value of the pixel and the fitting value;

[0013] The solid solution image is divided into a number of solid solution regions by clustering according to the first solid solution feature;

[0014] The solid solution sufficient coefficient of the solid solution image is obtained according to the similarity between all solid solution regions and the temperature distribution characteristics of the solid solution regions;

[0015] Controlling the end of the solution treatment phase according to the solubility sufficiency factor;

[0016] The shot blasting step is to perform shot blasting on the high-strength and tough cast aluminum alloy to obtain the high-strength and tough cast aluminum alloy without surface defects.

[0017] In the above scheme, the present application obtains the first solid solution feature through the temperature change continuity feature and the temperature difference feature within the pixel neighborhood range, and divides the solid solution area of ​​the casting based on this, preventing the traditional connected area marking method from dividing the connected domain only according to the temperature boundary, lacking the analysis of the continuous temperature change of the casting and the neighborhood temperature difference, and providing accurate regional division for the subsequent analysis of the consistency of the solid solution rate and the uniformity of the solid solution temperature distribution; the solid solution sufficiency coefficient is obtained according to the consistency of the solid solution rate and the uniformity of the solid solution temperature distribution in the solid solution area, and the solid solution treatment time of the casting is adjusted in time according to the real-time solid solution treatment status of the casting, avoiding the problem that the solid solution time of the casting is too long or too short, resulting in excessive diffusion of alloy elements or uneven supersaturated solid solution, which affects the performance of the casting, and realizing a production process for high-strength and toughness cast aluminum alloy materials.

[0018] Preferably, the main elements include Si, Mg, Fe, Cu, Ti, Sr, C, and B; the impurity elements include Ca, P, Mn, Cr, Ni, Pb, Sn, Be, Zr, and Zn.

[0019] Preferably, the preheating temperature in the preheating step is 170°C-210°C.

[0020] Preferably, in the melting and casting step, the temperature in the furnace is 730° C.-750° C., and the static treatment time is 15 min-20 min.

[0021] Preferably, in the heat treatment step, the temperature of the solution treatment stage is 540°C-580°C, the temperature of the quenching treatment stage is 40°C-60°C, the temperature of the aging treatment stage is 170°C-180°C, and the aging treatment time is 7.5 hours-9.5 hours.

[0022] Preferably, the method of recording any pixel in the solid solution image as the central pixel and obtaining the first solid solution feature of the central pixel according to the temperature difference between pixels around the central pixel and the difference between the temperature value of the pixel and the fitting value is:

[0023] Each pixel in the solid solution image is constructed as the central pixel Pixel window size;

[0024] The temperature values ​​of all pixels in each pixel window are sorted in ascending order of the horizontal coordinates and the vertical coordinates of the pixels to form a sequence, which is recorded as a temperature sequence; and a fitting curve of the temperature sequence is obtained;

[0025] The temperature change continuity of each central pixel is obtained according to the difference between the temperature value of each pixel in the pixel window and the fitted temperature value;

[0026] The continuity of temperature change in the central pixel is negatively correlated with the difference between the temperature value of the pixel and the fitted temperature value;

[0027] The accumulated result of the absolute value of the temperature difference between all pixels in each pixel window is taken as the neighborhood temperature difference of the central pixel;

[0028] The first solid solution feature of the central pixel is obtained according to the temperature change continuity of the central pixel and the temperature difference of the neighborhood;

[0029] The first solid solution feature of the central pixel is positively correlated with the continuity of the temperature change of the central pixel, and the first solid solution feature of the central pixel is negatively correlated with the temperature difference of the neighborhood of the central pixel.

[0030] Preferably, the method for obtaining the continuity of temperature change of each central pixel according to the difference between the temperature value of each pixel in the pixel window and the fitted temperature value is:

[0031]

[0032] Represents the absolute value of the difference between the temperature value of the jth pixel in the pixel window of the i-th central pixel and the fitted temperature value, Indicates the continuity of temperature change of the i-th central pixel, Indicates the number of pixels contained in the pixel window. Indicates preset constant parameters.

[0033] Preferably, the method for obtaining the solid solution sufficient coefficient of the solid solution image according to the similarity between all solid solution regions and the temperature distribution characteristics of the solid solution regions is:

[0034] For each solid solution region, the cluster center is taken as the solid solution center, and the sequence of the first solid solution features of all pixels in the cluster in ascending order is taken as the solid solution feature sequence of the solid solution region;

[0035] For the solid solution image at each moment, the two-dimensional coordinates of the solid solution centers of all the solid solution areas in the solid solution image are combined into a set and recorded as the solid solution center distribution set;

[0036] The reciprocal of the accumulated similarity of the solid solution characteristic sequences of all solid solution regions is taken as the consistency of the solid solution rate of the solid solution image;

[0037] The temperature distribution uniformity of the solid solution image is obtained according to the temperature difference of each area of ​​the solid solution image and the distribution of the solid solution center;

[0038] The product of the temperature distribution uniformity of the solution image and the consistency of the solution rate of the solution image was normalized and used as the solution sufficiency coefficient.

[0039] Preferably, the method for obtaining the temperature distribution uniformity of the solid solution image according to the temperature difference of each area of ​​the solid solution image and the distribution of the solid solution center is:

[0040] Calculate the standard deviation of the temperature values ​​of all pixels in each solid solution area of ​​the solid solution image, record the standard deviation as the temperature standard deviation of the solid solution area, and calculate the two-dimensional information entropy of the solid solution center distribution set of the solid solution image; the expression of temperature distribution uniformity is:

[0041]

[0042] represents the two-dimensional information entropy of the solid solution center distribution set corresponding to the solid solution image at the zth moment, is the standard deviation of the temperature values ​​of all pixels in the kth solid solution region in the solid solution image at the zth moment, represents the temperature distribution uniformity of the solid solution image at the zth moment, K represents the number of solid solution areas, Indicates preset constant parameters.

[0043] Preferably, the method for determining the end time of the solution treatment stage according to the solid solution sufficient coefficient is:

[0044] A sufficient solid solution threshold is preset, and when the sufficient solid solution coefficient is less than the sufficient solid solution threshold, the solid solution treatment stage is continued;

[0045] When the solid solution sufficient coefficient is greater than or equal to the solid solution sufficient threshold, the solid solution treatment stage is ended.

[0046] The beneficial effects of this application are:

[0047] The present application obtains the first solid solution feature through the temperature change continuity feature and the temperature difference feature within the pixel neighborhood range, and divides the solid solution area of ​​the casting based on this, preventing the traditional connected area marking method from dividing the connected domain only according to the temperature boundary, lacking the analysis of the continuous temperature change of the casting and the neighborhood temperature difference, and providing accurate regional division for the subsequent analysis of the consistency of the solid solution rate and the uniformity of the solid solution temperature distribution; the solid solution sufficiency coefficient is obtained according to the consistency of the solid solution rate and the uniformity of the solid solution temperature distribution in the solid solution area, and the solid solution treatment time of the casting is adjusted in time according to the real-time solid solution treatment status of the casting, avoiding the problem that the solid solution time of the casting is too long or too short, resulting in excessive diffusion of alloy elements or uneven supersaturated solid solution, which affects the performance of the casting, and realizing a production process for high-strength and toughness cast aluminum alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0049] Figure 1 A production process flow chart of a high-strength and tough cast aluminum alloy material provided in one embodiment of the present application;

[0050] Figure 2 This is the control flow chart for the solution treatment stage;

[0051] Figure 3 Schematic diagram of clustering effect;

[0052] Figure 4 The present invention is a flow chart of the preparation process of high-strength and tough cast aluminum alloy;

[0053] Figure 5 Schematic diagram of tensile strength and yield strength test;

[0054] Figure 6 Schematic diagram of the elongation test. DETAILED DESCRIPTION

[0055] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of the production process of a high-strength and tough cast aluminum alloy material proposed in the present application, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0056] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.

[0057] A production process embodiment of a high-strength and tough cast aluminum alloy material:

[0058] The specific scheme of the production process of a high-strength and toughness cast aluminum alloy material provided by the present application is described in detail below with reference to the accompanying drawings.

[0059] See also Figure 1 , which shows a production process flow chart of a high-strength and tough cast aluminum alloy material provided by an embodiment of the present application, the process comprises the following steps:

[0060] In the material preparation step, AlSi9Mg alloy is used as a master alloy, and AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source are weighed according to their percentages for standby use.

[0061] Among them, the strontium source is Al10Sr alloy; the magnesium source is one or more of pure magnesium block and magnesium alloy block, the magnesium alloy block is an alloy block composed of magnesium and one or more elements of Si, Al, and Fe; the silicon source is a silicon alloy block, the silicon alloy block is an alloy block composed of silicon and one or more elements of Al, Cu, and Ti, such as high iron aluminum silicon alloy; the titanium source is Al5TiBC alloy.

[0062] Preferably, in one embodiment of the present application, the strontium source is Al10Sr alloy, the magnesium source is an alloy block composed of magnesium, Si and Al, the silicon source is an alloy block composed of silicon and Al, and the titanium source is Al5TiBC alloy. The mass fraction of each component is: Si: 8.6wt%, Mg: 0.6wt%, Fe: 0wt%, Cu: 0wt%, Ti: 0.25wt%, Sr: 0.02wt%, C: 0.005wt%, B: 0.005wt%, total amount of impurity elements: 0.2wt%, the rest are Al, and the impurity elements are Ca, Mn, Pb, Sn, Be, Zr, and Zn.

[0063] Preferably, in one embodiment of the present application, the strontium source is Al10Sr alloy, the magnesium source is an alloy block composed of magnesium, Si and Fe, the silicon source is an alloy block composed of silicon, Al and Cu, and the titanium source is Al5TiBC alloy. The mass fraction of each component is: Si: 9.0wt%, Mg: 0.5wt%, Fe: 0.1wt%, Cu: 0.1wt%, Ti: 0.15wt%, Sr: 0.01wt%, C: 0.02wt%, B: 0.02wt%, total amount of impurity elements: 0.1wt%, and the rest are Al, and the impurity elements are Ca, P, Mn, Cr, Ni, Zr, and Zn.

[0064] Preferably, in one embodiment of the present application, the strontium source is Al10Sr alloy, the magnesium source is an alloy block composed of magnesium, Si, Al, and Fe, the silicon source is an alloy block composed of silicon, Al, Cu, and Ti, and the titanium source is Al5TiBC alloy. The mass fraction of each component is: Si: 9.5wt%, Mg: 0.4wt%, Fe: 0.15wt%, Cu: 0.05wt%, Ti: 0.2wt%, Sr: 0.02wt%, C: 0.01wt%, B: 0.01wt%, total amount of impurity elements: 0.05wt%, and the rest are Al, wherein the impurity elements are Ca, P, Mn, Cr, Ni, Pb, Sn, Be, Zr, and Zn.

[0065] In the preheating step, the AlSi9Mg master alloy, strontium source, magnesium source, silicon source and titanium source are placed in a preheating furnace, and the preheating furnace is gradually heated to a preheating temperature for preheating to reduce deformation resistance during the forging process of the alloy.

[0066] Preferably, in one embodiment of the present application, the preheating temperature is 170°C.

[0067] Preferably, in one embodiment of the present application, the preheating temperature is 190°C.

[0068] Preferably, in one embodiment of the present application, the preheating temperature is 210°C.

[0069] The melting and casting step is to place the preheated AlSi9Mg master alloy in a furnace for melting, and then add the preheated strontium source, magnesium source, silicon source, and titanium source. After all the raw materials are melted, they are evenly mixed by permanent magnetic stirring to obtain a melt, which is kept warm and dried by passing nitrogen. After drying, the nitrogen is stopped and the melt is allowed to stand. Then, the melt is poured into a metal mold for casting to obtain a casting.

[0070] Preferably, in one embodiment of the present application, the temperature in the furnace is 730° C., and the static treatment time is 15 minutes.

[0071] Preferably, in one embodiment of the present application, the temperature in the furnace is 740° C., and the static treatment time is 17 minutes.

[0072] Preferably, in one embodiment of the present application, the temperature in the furnace is 750° C., and the static treatment time is 20 minutes.

[0073] The heat treatment step is to place the casting obtained above in a resistance furnace for solution treatment. After the solution treatment, the treated casting is taken out and placed in water for quenching. After the quenching is completed, the quenched casting is aged in a resistance furnace to obtain a high-strength and tough cast aluminum alloy.

[0074] Preferably, in one embodiment of the present application, the temperature of the solution treatment stage is 540°C, the temperature of the quenching treatment stage is 40°C, the temperature of the aging treatment stage is 170°C, and the aging treatment time is 9.5 hours.

[0075] Preferably, in one embodiment of the present application, the temperature of the solution treatment stage is 560°C, the temperature of the quenching treatment stage is 50°C, the temperature of the aging treatment stage is 175°C, and the aging treatment time is 8.5 hours.

[0076] Preferably, in one embodiment of the present application, the temperature of the solution treatment stage is 580°C, the temperature of the quenching treatment stage is 60°C, the temperature of the aging treatment stage is 180°C, and the aging treatment time is 7.5 hours.

[0077] In the solution treatment stage, if the treatment time is too long or too short, it will affect the performance of the high-strength and toughness cast aluminum alloy. Therefore, it is necessary to accurately determine the time of the solution treatment stage to improve the performance of the high-strength and toughness cast aluminum alloy.

[0078] In the solution treatment stage of the heat treatment step, a control flow chart of the solution treatment stage is provided, such as Figure 2 The specific contents are as follows:

[0079] S1, collect the solid solution image at each moment.

[0080] The infrared thermal imaging images of the cast aluminum alloy during the solid solution treatment process are obtained by an infrared thermal imager at a top-down angle. The infrared thermal imaging image acquisition interval is t, that is, an infrared thermal imaging image is collected at each moment. In order to prevent the acquired infrared thermal imaging images of the casting solid solution from being disturbed by external environmental noise and affecting subsequent analysis, the acquired infrared thermal imaging images of the casting solid solution are denoised by an image denoising algorithm. The denoised infrared thermal imaging images of the casting solid solution are called solid solution images.

[0081] It should be noted that, in this embodiment, the infrared thermal imaging image acquisition interval is 1s, and the implementer can also adjust the acquisition interval according to the calculation amount; the image denoising algorithm used in this embodiment is the wavelet transform algorithm, and the implementer can also use other image denoising algorithms, such as the Gaussian denoising algorithm.

[0082] At this point, the solid solution image at each moment has been acquired.

[0083] S2, record any pixel in the solid solution image as the central pixel, and obtain the first solid solution feature of the central pixel according to the temperature difference between the pixels around the central pixel and the difference between the temperature value of the pixel and the fitting value.

[0084] Solution treatment of castings is a metal heat treatment process, which heats the alloy to a high-temperature single-phase region and maintains a constant temperature, so that the excess phase is fully dissolved into the solid solution and then rapidly cooled to obtain a supersaturated solid solution. The more appropriate the solution time of the casting is and the more complete the solution treatment is, the more uniform the temperature distribution in the solution image will be due to the homogenization of the alloy composition, and the more blurred the temperature difference caused by component segregation or second-phase ions will be; at the same time, the less obvious the inconsistency of the solution rate caused by the uneven microstructure or supersaturated solid solution will be, and the more significant the continuity of temperature change will be.

[0085] This embodiment takes the solid solution image at any moment as an example for subsequent analysis, and constructs a The pixel window of size is denoted as the center pixel. is the side length of the pixel window, which is 7. The implementer can select the value according to the demand, and the value is an odd number. The temperature values ​​of all pixels in each pixel window are sorted in ascending order of the horizontal coordinate and the vertical coordinate to form a sequence. The composed sequence is recorded as the temperature sequence of the pixel window. The least squares method is used to obtain the fitting curve of the temperature sequence of each pixel window. Since the least squares method is a well-known technology, the specific acquisition process will not be described in detail.

[0086] It should be noted that, in this embodiment, the least squares method is used to obtain the fitting curve of the temperature sequence of each pixel window. The implementer can use other methods of fitting the sequence to a curve to obtain the fitting curve, for example, the maximum likelihood estimation method.

[0087] When the solution treatment of the casting is more complete, the difference between the temperatures of adjacent pixels in the pixel window is smaller, and the temperature changes of adjacent pixels are more similar, and the difference between the fitted curve and the true curve is smaller.

[0088] The stronger the continuity of temperature change within the pixel neighborhood, the easier it is to predict the change of casting solution temperature at the corresponding position within the pixel neighborhood.

[0089] The temperature change continuity of each central pixel is obtained based on the difference between the temperature value of each pixel in the pixel window and the fitted temperature value.

[0090] The continuity of temperature change in the central pixel is negatively correlated with the difference between the temperature value of the pixel and the fitted temperature value.

[0091] It should be noted that negative correlation means that when one variable increases, the other variable decreases accordingly, and the two variables change in opposite directions. When one variable changes from large to small or from small to large, the other variable also changes from small to large or from large to small; it is determined by actual application and this application does not impose any special restrictions.

[0092] Preferably, in one embodiment of the present application, for each pixel window, the absolute value of the difference between the temperature value of each pixel and the fitted temperature value is calculated. , add up all the absolute values ​​of the differences and take the reciprocal to obtain the temperature change continuity of the central pixel , Represents the absolute value of the difference between the temperature value of the jth pixel in the pixel window of the i-th central pixel and the fitted temperature value, Indicates the continuity of temperature change of the i-th central pixel, Indicates the number of pixels contained in the pixel window. It is a constant parameter and has no practical meaning. Its function is to prevent the denominator from being 0. In this embodiment, it is set to 1.

[0093] Preferably, in one embodiment of the present application, for each pixel window, the absolute value of the difference between the temperature value of each pixel and the fitted temperature value is calculated. After accumulating the absolute values ​​of all differences, the temperature change continuity of the central pixel is obtained through the function , Represents an exponential function with the natural constant e as base.

[0094] The more fully the casting is solution treated, the stronger the continuity of the temperature change in the pixel neighborhood is, and the easier it is to predict the change in the casting solution temperature at the corresponding position in the pixel neighborhood. That is, the smaller the cumulative difference between the temperature values ​​of all pixels in the pixel neighborhood and the curve fitting temperature value is.

[0095] The accumulated result of the absolute value of the temperature difference between all pixels in each pixel window is taken as the neighborhood temperature difference of the central pixel; when the solid solution treatment of the casting is more complete, the solid solution temperature of the supersaturated solid solution is more uniform, and the temperature difference within the pixel neighborhood is smaller, that is, the accumulated result of the absolute value of the temperature difference between all pixels in the pixel window is smaller, and the neighborhood temperature difference is smaller.

[0096] The first solid solution feature of the central pixel is obtained according to the temperature change continuity of the central pixel and the temperature difference of the neighborhood;

[0097] The first solid solution feature of the central pixel is positively correlated with the continuity of the temperature change of the central pixel, and the first solid solution feature of the central pixel is negatively correlated with the temperature difference of the neighborhood of the central pixel.

[0098] It should be noted that negative correlation means that when one variable increases, the other variable decreases accordingly, and the two variables change in opposite directions. When one variable changes from large to small or from small to large, the other variable also changes from small to large or from large to small; it is determined by actual application and this application does not impose any special restrictions.

[0099] Preferably, in one embodiment of the present application, the ratio of the temperature change continuity of the central pixel to the temperature difference of the neighboring area is used as the first solid solution characteristic of the central pixel. . represents the neighborhood temperature difference of the i-th central pixel, Represents the first solid solution feature of the i-th central pixel.

[0100] Preferably, in one embodiment of the present application, the temperature change continuity of the central pixel is taken as the true number of the logarithmic function, the temperature difference of the neighborhood of the central pixel is taken as the base of the logarithmic function, and the logarithmic function is calculated to obtain the first solid solution characteristic .

[0101] Take each pixel as the central pixel and obtain the first solid solution feature of each pixel. , then only the pixels within the pixel window are used for calculation.

[0102] When the solution treatment of the casting is more complete, the solution rate of the supersaturated solid solution is more consistent, the difference in the solution temperature of the casting is smaller, the continuity of the temperature change is stronger, the difference in the neighborhood temperature is smaller, and the first solution feature of the pixel is obtained.

[0103] At this point, the first solid solution feature of each pixel is obtained.

[0104] S3, dividing the solid solution image into a plurality of solid solution regions by clustering according to the first solid solution feature.

[0105] The solid solution image at any moment and the first solid solution features of all pixels are used as input, and the K-mediods clustering algorithm is used to obtain all clusters and cluster centers in the solid solution image. In this embodiment, the number of clusters is set to 9, and the absolute value of the difference between the first solid solution features of two pixels is used as the metric distance between the two pixels. The K-mediods clustering algorithm is a well-known technology, and the specific acquisition process will not be described in detail. The clustering diagram is shown in FIG. Figure 3 shown.

[0106] It should be noted that the K-mediods clustering algorithm used in this embodiment is used to obtain all cluster clusters and their cluster centers in the solid solution image. Therefore, as long as the clustering algorithm can classify the solid solution image and obtain the cluster center, it can be implemented. The implementer can use other clustering algorithms, such as K-means clustering.

[0107] The beneficial effects of obtaining clusters in the solid solution image through a clustering algorithm and using the difference in the first solid solution feature as a distance metric are: avoiding the problem of inaccurate judgment of the subsequent solid solution treatment duration of the casting due to the lack of analysis of the continuity of the solid solution features in the connected domain, which is caused by the traditional connected domain labeling algorithm dividing the connected domain only according to the temperature boundary features in the solid solution image.

[0108] Each cluster in the solid solution image is recorded as a solid solution region, and the cluster center of each cluster is used as the solid solution center of each solid solution region. So far, all solid solution regions in the solid solution image at any time can be obtained according to the above method.

[0109] At this point, all the solid solution areas in the solid solution image at each moment are obtained.

[0110] S4, obtaining the solid solution sufficient coefficient of the solid solution image according to the similarity between all the solid solution regions and the temperature distribution characteristics of the solid solution regions.

[0111] For each solid solution region, a sequence consisting of the first solid solution features of all pixels therein in ascending order is taken as the solid solution feature sequence of the solid solution region.

[0112] For the solid solution image at each moment, the two-dimensional coordinates of the solid solution centers of all the solid solution areas in the solid solution image are grouped into a set and recorded as the solid solution center distribution set.

[0113] When the solution treatment effect of the casting reaches a fully saturated state at a certain moment, the temperature change in the solution zone should be more consistent, that is, the higher the continuity of all temperature changes corresponding to the solution zone and the similarity of the temperature difference in the neighboring areas, the greater the consistency of the solution rate in the solution zone.

[0114] The consistency of the dissolution rate of the solution image is obtained based on the similarity of the solution characteristic sequences of all solution regions.

[0115] Preferably, in one embodiment of the present application, for the solid solution characteristic sequences of any two solid solution regions, the JS divergence of the two solid solution characteristic sequences is calculated, the inverse of the JS divergence of the two solid solution characteristic sequences is taken as the similarity of the two solid solution characteristic sequences, and the similarities between all solid solution regions in the solid solution image are accumulated as the solid solution rate consistency of the solid solution image.

[0116] Preferably, in one embodiment of the present application, for the solid solution characteristic sequences of any two solid solution regions, their DTW distance is calculated, the inverse of the DTW distance is taken as the similarity between the two solid solution characteristic sequences, and the similarities between all solid solution regions in the solid solution image are accumulated as the solid solution rate consistency of the solid solution image.

[0117] When the solution treatment effect of the casting reaches a fully saturated state at a certain moment, the distribution of the solution centers of all the solution areas in the solution image becomes more uniform, and the temperature difference in all the solution areas becomes less severe. Based on this, the uniformity of the temperature distribution of the solution image is obtained.

[0118] The standard deviation of the temperature values ​​of all pixels in each solid solution area of ​​the solid solution image is calculated, and the standard deviation is recorded as the temperature standard deviation of the solid solution area. The two-dimensional information entropy of the solid solution center distribution set of the solid solution image is calculated.

[0119] The temperature distribution uniformity of the solution image is negatively correlated with the temperature standard deviation of all solution areas and the two-dimensional information entropy of the solution center distribution set.

[0120] Preferably, in one embodiment of the present application, the temperature standard deviation of all solid solution regions is accumulated and multiplied by the two-dimensional information entropy of the solid solution center distribution set, and the inverse of the product is used as the temperature distribution uniformity of the solid solution image. , represents the two-dimensional information entropy of the solid solution center distribution set corresponding to the solid solution image at the zth moment, is the standard deviation of the temperature values ​​of all pixels in the kth solid solution region in the solid solution image at the zth moment, It represents the uniformity of temperature distribution of the solid solution image at the zth moment, and K represents the number of solid solution areas.

[0121] Preferably, in one embodiment of the present application, , Represents an exponential function with the natural constant e as base.

[0122] The smaller the two-dimensional information entropy of the solid solution center distribution set corresponding to the solid solution image at the z moment, the smaller the standard deviation of the cumulative sequence of all pixel temperature values ​​in all solid solution areas in the solid solution image at the z moment, the greater the uniformity of the temperature distribution of the solid solution image corresponding to the z moment, and the more likely it is to reach full saturation.

[0123] The product of the temperature distribution uniformity of the solution image and the consistency of the solution rate of the solution image was normalized and used as the solution sufficiency coefficient.

[0124] When the dissolution rate of the supersaturated solid solution in the solid solution image is more consistent and the temperature distribution in the solid solution area is more uniform, the solid solution sufficiency coefficient of the casting is larger, indicating that the casting is more likely to have reached a saturated state.

[0125] At this point, the solid solution sufficient coefficient of the solid solution image is obtained.

[0126] S5, controlling the end of the solution treatment stage according to the solubility sufficient coefficient.

[0127] A sufficient solid solution threshold M is set. When the sufficient solid solution coefficient obtained in real time is less than the sufficient solid solution threshold M, it is considered that the solid solution treatment of the casting at the current moment has not reached a sufficient state and the solid solution treatment needs to be continued; when the sufficient solid solution coefficient of the casting obtained in real time is greater than or equal to the sufficient solid solution threshold M, it is considered that the solid solution treatment of the casting at the current moment has reached a sufficient state, the solid solution treatment of the casting can be stopped, and the casting can be taken out for subsequent quenching and aging treatment. The larger the sufficient solid solution threshold M is, the stricter the requirements for the solid solution treatment of the casting. In this embodiment, the sufficient solid solution threshold is 0.6, and the implementer can set the sufficient solid solution threshold according to the required aluminum alloy strength.

[0128] The shot blasting step is to perform shot blasting on the surface of the high-strength and tough cast aluminum alloy obtained in the above process, in order to remove defects on the surface of the cast aluminum alloy and improve the fatigue strength of the workpiece.

[0129] The high-strength and toughness cast aluminum alloy is prepared by the above steps, and the preparation process flow chart is as follows: Figure 4 As shown, Figure 4 In the figure, the white background process is the general processing process; the gray background process is the improved process in this application.

[0130] The cast aluminum alloy prepared as above was subjected to relevant performance tests, and the preparation method selected was the first embodiment. The test results are as follows:

[0131]

[0132] The schematic diagram of the casting aluminum alloy performance test results obtained for different embodiments is as follows Figure 5 , Figure 6 As shown, Figure 5 Schematic diagram of tensile strength and yield strength tests for multiple embodiments, Figure 6 Schematic diagram of elongation test for multiple embodiments.

[0133] It should be noted that the above-described embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

[0134] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

Claims

1. A production process for high-strength and tough cast aluminum alloy material, characterized in that: The process includes the following steps: The material preparation step is to use AlSi9Mg alloy as a master alloy, and weigh AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source according to percentage as standby, wherein the AlSi9Mg master alloy, strontium source, magnesium source, silicon source, and titanium source include main elements and impurity elements; A preheating step, placing the AlSi9Mg master alloy, the strontium source, the magnesium source, the silicon source, and the titanium source into a preheating furnace, and gradually heating the preheating furnace to a preheating temperature for preheating; The melting and casting step is to place the preheated AlSi9Mg master alloy in a furnace to melt, then add the preheated strontium source, magnesium source, silicon source and titanium source, stir evenly after melting to obtain a melt, dry, ventilate and let the melt stand before casting to obtain a casting; A heat treatment step, wherein the obtained casting is subjected to a solution treatment, and after the solution treatment, the casting is subjected to a quenching and aging treatment to obtain a high-strength and tough cast aluminum alloy; The following steps are involved in the solution treatment phase: Collect the solid solution image at each moment; Any pixel in the solid solution image is recorded as the central pixel, and the first solid solution feature of the central pixel is obtained according to the temperature difference between the pixels around the central pixel and the difference between the temperature value of the pixel and the fitting value; The solid solution image is divided into a number of solid solution regions by clustering according to the first solid solution feature; The solid solution sufficient coefficient of the solid solution image is obtained according to the similarity between all solid solution regions and the temperature distribution characteristics of the solid solution regions; Controlling the end of the solution treatment phase according to the solubility sufficiency factor; A shot blasting step is to perform shot blasting on the high-strength and tough cast aluminum alloy to obtain a high-strength and tough cast aluminum alloy without surface defects; The method of recording any pixel in the solid solution image as the central pixel and obtaining the first solid solution feature of the central pixel according to the temperature difference between the pixels around the central pixel and the difference between the temperature value of the pixel and the fitting value is: Each pixel in the solid solution image is constructed as the central pixel The pixel window size is is the side length of the pixel window, , take an odd number; The temperature values ​​of all pixels in each pixel window are sorted in ascending order of the horizontal coordinates and the vertical coordinates of the pixels to form a sequence, which is recorded as a temperature sequence; and a fitting curve of the temperature sequence is obtained; The temperature change continuity of each central pixel is obtained according to the difference between the temperature value of each pixel in the pixel window and the fitted temperature value; The continuity of temperature change in the central pixel is negatively correlated with the difference between the temperature value of the pixel and the fitted temperature value; The accumulated result of the absolute value of the temperature difference between all pixels in each pixel window is taken as the neighborhood temperature difference of the central pixel; The first solid solution feature of the central pixel is obtained according to the temperature change continuity of the central pixel and the temperature difference of the neighborhood; The first solid solution feature of the central pixel is positively correlated with the continuity of the temperature change of the central pixel, and the first solid solution feature of the central pixel is negatively correlated with the temperature difference of the neighborhood of the central pixel. The method for obtaining the solid solution sufficient coefficient of the solid solution image according to the similarity between all solid solution regions and the temperature distribution characteristics of the solid solution regions is: For each solid solution region, the cluster center is taken as the solid solution center, and the sequence of the first solid solution features of all pixels in the cluster in ascending order is taken as the solid solution feature sequence of the solid solution region; For the solid solution image at each moment, the two-dimensional coordinates of the solid solution centers of all the solid solution areas in the solid solution image are combined into a set and recorded as the solid solution center distribution set; The reciprocal of the accumulated similarity of the solid solution characteristic sequences of all solid solution regions is taken as the consistency of the solid solution rate of the solid solution image; The temperature distribution uniformity of the solid solution image is obtained according to the temperature difference of each area of ​​the solid solution image and the distribution of the solid solution center; The product of the temperature distribution uniformity of the solution image and the consistency of the solution rate of the solution image was normalized and used as the solution sufficiency coefficient.

2. A production process for a high-strength and tough cast aluminum alloy material as claimed in claim 1, characterized in that: The main elements include Si, Mg, Fe, Cu, Ti, Sr, C, and B; the impurity elements include Ca, P, Mn, Cr, Ni, Pb, Sn, Be, Zr, and Zn.

3. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: The preheating temperature in the preheating step is 170°C-210°C.

4. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: In the melting and casting step, the temperature in the furnace is 730° C.-750° C., and the static treatment time is 15 min-20 min.

5. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: In the heat treatment step, the temperature of the solution treatment stage is 540°C-580°C, the temperature of the quenching treatment stage is 40°C-60°C, the temperature of the aging treatment stage is 170°C-180°C, and the aging treatment time is 7.5 hours-9.5 hours.

6. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: The method for obtaining the continuity of temperature change of each central pixel according to the difference between the temperature value of each pixel in the pixel window and the fitted temperature value is: Represents the absolute value of the difference between the temperature value of the jth pixel in the pixel window of the i-th central pixel and the fitted temperature value, Indicates the continuity of temperature change of the i-th central pixel, Indicates the number of pixels contained in the pixel window. Indicates preset constant parameters.

7. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: The method for obtaining the temperature distribution uniformity of the solid solution image according to the temperature difference of each area of ​​the solid solution image and the distribution of the solid solution center is: Calculate the standard deviation of the temperature values ​​of all pixels in each solid solution area of ​​the solid solution image, record the standard deviation as the temperature standard deviation of the solid solution area, and calculate the two-dimensional information entropy of the solid solution center distribution set of the solid solution image; the expression of temperature distribution uniformity is: represents the two-dimensional information entropy of the solid solution center distribution set corresponding to the solid solution image at the zth moment, is the standard deviation of the temperature values ​​of all pixels in the kth solid solution region in the solid solution image at the zth moment, represents the temperature distribution uniformity of the solid solution image at the zth moment, K represents the number of solid solution areas, Indicates preset constant parameters.

8. The production process of a high-strength and tough cast aluminum alloy material according to claim 1, characterized in that: The method for determining the end time of the solution treatment stage according to the solid solution sufficient coefficient is: A sufficient solid solution threshold is preset, and when the sufficient solid solution coefficient is less than the sufficient solid solution threshold, the solid solution treatment stage is continued; When the solid solution sufficient coefficient is greater than or equal to the solid solution sufficient threshold, the solid solution treatment stage is ended.