Production method of low yield ratio, easy-to-weld, high-strength and tough bridge steel
A controlled production method for bridge steel plates with reduced high-cost alloy content achieves low yield strength ratio, easy welding, and high strength and toughness, addressing the limitations of existing technologies.
Patent Information
- Application Number
- CN202411103094.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing bridge steel plates face challenges in achieving a balance between mechanical properties such as low yield strength ratio, easy welding, high strength, and toughness, while also dealing with poor welding performance and high production costs due to excessive alloy content of metals like Ni, Mo, and Cr.
A production method involving specific chemical compositions and controlled processes, including smelting, heating, rolling, and cooling, reduces the content of high-cost alloys and ensures mechanical properties through controlled precipitation and phase transformation, resulting in a steel plate with low yield strength ratio, easy welding, and high strength and toughness.
The method produces steel plates with improved mechanical properties and weldability, reducing production complexity and cost, making them suitable for bridge engineering applications.
Smart Images

Figure CN118621117B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel alloy materials and relates to a production method of a low-yield ratio, easy-to-weld, high-strength and toughness bridge steel. Background Art
[0002] With the rapid development of expressways and high-speed railways, the steel bridge manufacturing industry has developed rapidly. While meeting the functionality, steel bridges are developing in the direction of multi-function, multi-lane, heavy-load, and large span. Structural steel for bridges is mainly used in key projects such as the construction of railways, highways, cross-sea and cross-river bridges. Due to the particularity of its use environment, it has strict requirements on comprehensive performance, such as low yield strength ratio, good weldability, and high toughness.
[0003] In the existing manufacturing of bridge steel plates, in order to improve the mechanical properties (toughness, strength, yield strength ratio, etc.), the chemical composition system usually adopts high alloy content of precious metals such as Ni, Mo, Cr, etc., but it will lead to defects such as poor welding performance, affecting the application effect of steel plates in bridge engineering, and also increase the difficulty of production, such as having to rely on post-rolling heat treatment, and long production cycle. In addition, with the excessive addition of alloy content, the production cost of steel is also greatly increased. Summary of the invention
[0004] In order to solve the problem that existing bridge steel plates cannot take into account both mechanical properties, the purpose of the present invention is to provide a steel production method, and the resulting steel plates have the advantages of low yield strength ratio, easy welding, high strength and toughness, and are suitable for bridge engineering.
[0005] To achieve the above-mentioned purpose, an embodiment of the present invention provides a method for producing steel. The production method comprises the following steps:
[0006] A steel billet is obtained by smelting and casting molten steel, wherein the chemical composition of the steel billet comprises, by mass percentage, C: 0.08-0.14%, Si: 0.11-0.18%, Mn: 1.31-1.47%, Nb: 0.011-0.032%, Ti: 0.009-0.017%, Al: 0.026-0.046%, Cr≤0.13%, Ni≤0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities;
[0007] The billet is heated in a heating furnace to a temperature above T1+10℃ and below T2, where T1 is T NbC , T NbN and T TiC The maximum value of T2 is T1+50℃, T TiN -150℃ maximum value; where T NbC , T NbN , TTiC and T TiN are the complete solution temperatures of NbC, NbN, TiC and TiN respectively;
[0008] After leaving the heating furnace, the billet is first rolled at a rolling temperature of T3 or above and below T3+40℃ to 4~6.8 times the thickness of the finished product to obtain the first intermediate plate; then rolled at a rolling temperature of T4-50℃ or above and below T4+20℃ to 1.8~3.2 times the thickness of the finished product to obtain the second intermediate plate; finally, rolled at a rolling temperature of T5-55℃ or above and below T5 to the thickness of the finished product;
[0009] The rolled steel plate is air-cooled to a temperature above T6-50°C and below T6+20°C at a cooling rate of 1-10°C / s, then water-cooled to a temperature above T7-30°C and below T7+130°C at a cooling rate of 5-30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate;
[0010] Among them, T3≥T4≥T5≥T6≥T7, T7=539-423[C]-17.7[Ni]-12.1[Cr]-11[Si]-30.4[Mn], T3=887+464[C]+6445[Nb]-644 +890[Ti]+363[Al]-357[Si], T6=830-270[C]-90[Mn]-37[Ni]-70[Cr], T5=910-310[C]-80[Mn]-15[Cr], T4=910-203 -15.2[Ni]+44.7[Si], [C], [Nb], [Ti], [Al], [Si], [Ni], [Mn], and [Cr] are the mass percentages of C, Nb, Ti, Al, Si, Ni, Mn, and Cr in the steel billet respectively.
[0011] Preferably, the chemical composition of the steel billet includes, by mass percentage: P: 0.0101-0.0151%, S: 0.0020-0.0080%, N: 0.0025-0.0045%.
[0012] Preferably, the carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.318~0.380.
[0013] Preferably, the chemical composition of the steel billet includes, by mass percentage, C: 0.11-0.14%, Si: 0.11-0.18%, Mn: 1.31-1.39%, Nb: 0.011-0.019%, Ti: 0.009-0.017%, Al: 0.026-0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
[0014] Preferably, the chemical composition of the steel billet includes, by mass percentage, C: 0.10~0.13%, Si: 0.11~0.18%, Mn: 1.34~1.42%, Nb: 0.014~0.022%, Ti: 0.009~0.017%, Al: 0.026~0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
[0015] Preferably, the chemical composition of the steel billet includes, by mass percentage, C: 0.09~0.12%, Si: 0.11~0.18%, Mn: 1.37~1.45%, Nb: 0.024~0.032%, Ti: 0.009~0.017%, Al: 0.026~0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
[0016] Preferably, the chemical composition of the steel billet includes, by mass percentage, C: 0.08~0.11%, Si: 0.11~0.18%, Mn: 1.39~1.47%, Ni: 0.07~0.13%, Nb: 0.021~0.029%, Ti: 0.009~0.017%, Al: 0.026~0.046%, Cr: 0.07~0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
[0017] Preferably, the residence time of the steel billet at a temperature above T1+10°C and below T2 is 0.07-0.13 min / mm, and the total residence time in the heating furnace is 1.15-1.35 min / mm.
[0018] Preferably, the steel billet adopts a five-stage process including a heat recovery section, a preheating section, a first heating section, a second heating section and a soaking section in the heating furnace, the temperature of the second heating section is above T1+10°C and below T2, the temperature of the soaking section is lower than the temperature of the second heating section, and the temperature of the soaking section is 20-40°C lower than the temperature of the second heating section;
[0019] Alternatively, the steel billet adopts a three-stage process including a preheating section, a heating section and a soaking section in the heating furnace. The temperature of the heating section is above T1+10°C and below T2, the temperature of the soaking section is lower than the temperature of the heating section, and the temperature of the soaking section is 20~40°C lower than the temperature of the heating section.
[0020] Preferably, in the five-stage process, the temperature of the first stage is 1120±15°C;
[0021] Among them, through lg([Nb]×[N])=3.70-10800 / (T NbN +273.15), lg([Nb]×[C])=2.26-6770 / (T NbC +273.15), lg([Ti]×[C])=5.33-10475 / (T TiC +273.15), lg([Ti]×[N])=0.32-8000 / (T TiN +273.15) respectively to calculate T NbC , T NbN , T TiC and T TiN , [Nb], [N]), [C], and [Ti] are the mass percentages of Nb, N, C, and Ti in the steel billet, respectively.
[0022] Preferably, the second intermediate plate is rolled to a finished thickness at a rolling temperature of above T5-55°C and below T5-15°C;
[0023] The rolled steel plate is air-cooled to a temperature between T6-50°C and T6-30°C at a cooling rate of 1-10°C / s, and then water-cooled to a temperature between T7+90°C and T7+130°C at a cooling rate of 8-30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate; alternatively, the rolled steel plate is air-cooled to a temperature between T6-30°C and T6-10°C at a cooling rate of 1-10°C / s, and then water-cooled to a temperature between T7+50°C and T7+90°C at a cooling rate of 8-30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0024] Preferably, the second intermediate plate is rolled to a finished thickness at a rolling temperature of above T5-40°C and below T5;
[0025] The rolled steel plate is air-cooled to above T6-10°C and below T6+10°C at a cooling rate of 1~10°C / s, and then water-cooled to above T7+10°C and below T7+50°C at a cooling rate of 8~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate; alternatively, the rolled steel plate is air-cooled to above T6 and below T6+20°C at a cooling rate of 1~10°C / s, and then water-cooled to above T7-30°C and below T7+10°C at a cooling rate of 8~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0026] Preferably, when rolling to obtain the first intermediate plate, the starting rolling temperature is above T3+20°C and below T3+40°C, and the finishing rolling temperature is above T3 and below T3+20°C;
[0027] When rolling to obtain the second intermediate plate, the starting rolling temperature is above T4 and below T4+20°C, and the finishing rolling temperature is above T4-50°C and below T4-30°C;
[0028] When the second intermediate plate is rolled to the finished thickness, the starting rolling temperature is above T5-30°C and below T5-15°C, and the final rolling temperature is above T5-55°C and below T5-40°C, or the starting rolling temperature is above T5-15°C and below T5, and the final rolling temperature is above T5-40°C and below T5-25°C.
[0029] Compared with the prior art, the beneficial effect of one embodiment is that compared with the existing high-content components of Ni, Mo, and Cr, the content of these alloys is greatly reduced. Through the design of chemical composition and the specific process control of heating, rolling, and cooling, the defects of poor welding performance caused by high alloy content are eliminated while still ensuring mechanical properties, such as toughness, strength, and yield strength ratio (that is, the mechanical properties brought by these elements are not reduced due to the reduction of the content of these elements), so that under the conditions of low alloy content, low production difficulty, and short production process, the steel plate can be comprehensively improved in terms of low yield strength ratio, easy welding, high strength and toughness, and good plate shape, and the resulting steel plate is suitable for bridge engineering. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a flowchart of the steel production method of the present invention;
[0031] Figure 2 is a metallographic structure diagram of a steel plate according to Embodiment 1 of the present invention;
[0032] Figure 3 is a metallographic structure diagram of a steel plate according to Embodiment 2 of the present invention;
[0033] Figure 4 is a metallographic structure diagram of a steel plate according to Embodiment 3 of the present invention;
[0034] Figure 5 This is a metallographic structure diagram of a steel plate according to Example 4 of the present invention. DETAILED DESCRIPTION
[0035] An embodiment of the present invention provides a method for producing steel, which is improved in terms of chemical composition and preparation process. Compared with the prior art, a finished steel plate with low yield ratio, easy welding and high strength and toughness can be prepared with low alloy content, low production difficulty and short production cycle.
[0036] In terms of chemical composition, the chemical composition of the steel according to one embodiment of the present invention includes, by mass percentage, C: 0.08~0.14%, Si: 0.11~0.18%, Mn: 1.31~1.47%, Nb: 0.011~0.032%, Ti: 0.009~0.017%, Al: 0.026~0.046%, Cr≤0.13%, Ni≤0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest are iron and unavoidable impurities.
[0037] The role and control of each chemical component are described in detail below.
[0038] C: Carbon is the most economical strengthening element in steel, with significant solid solution strengthening effect, which can effectively reduce the yield strength ratio. At the same time, it forms carbides with Nb, Ti, Cr, Mo, etc., which play a precipitation strengthening role. When the carbon content is lower than 0.08%, the effect of improving strength and reducing the yield strength ratio is not obvious. When the carbon content is higher than 0.14%, the toughness and welding performance will deteriorate. In some embodiments, the C content is preferably 0.11-0.14%, 0.10-0.13%, 0.09-0.12% or 0.08-0.11%.
[0039] Si: Silicon has a solid solution strengthening effect in steel. When the Si content is lower than 0.11%, the solid solution strengthening effect is not obvious. When the Si content exceeds 0.18%, Fe2SiO4 is easily generated on the surface of the continuous casting billet, which is difficult to remove during descaling and is not conducive to the surface quality of the steel plate.
[0040] Mn: Manganese plays a role in solid solution strengthening in steel and is the most economical strengthening element besides carbon. When the Mn content is lower than 1.31%, the solid solution strengthening effect is not obvious; when the Mn content exceeds 1.47%, it is easy to form segregation in the center of the slab, reducing the low temperature toughness of the steel plate and being unfavorable to the welding performance. In some embodiments, the Mn content is preferably 1.31-1.39%, 1.34-1.42%, 1.37-1.45% or 1.39-1.47%.
[0041] Nb: Niobium is an important grain-refining element in steel. When the Nb content exceeds 0.011%, carbonitride precipitates of niobium are formed during rolling to refine the recrystallized grains. During cooling, niobium can continue to precipitate in the form of carbonitrides, which refines the microstructure after phase transformation and improves strength and toughness. However, when Nb is greater than 0.032%, the alloy cost will increase, and precipitation strengthening will be unfavorable to the yield strength ratio. In some embodiments, the Nb content is preferably 0.011-0.019%, 0.014-0.022%, 0.024-0.032%, or 0.021-0.029%.
[0042] Ti: Titanium is a nitrogen-fixing element in steel. It can form dispersed titanium nitride particles, which inhibit the coarsening of austenite grains during billet heating and rolling. However, when the Ti content is less than 0.009%, Ti cannot fully play its role. When the Ti content is greater than 0.017%, titanium carbonitride precipitation is easily formed in the core of the ingot, affecting the low-temperature toughness of the core of the steel plate.
[0043] Al: Aluminum is a deoxidizing element in steel. When the content is lower than 0.026%, Al cannot effectively achieve its deoxidation effect. When the content is higher than 0.046%, the Al2O3 inclusions in the steel increase, affecting the low-temperature toughness of the steel.
[0044] P, S, N: impurity elements; however, S can also form MnS inclusions with Mn, reducing the low temperature toughness of steel. In some embodiments, the P content is preferably 0.0101-0.0151%, the N content is preferably 0.0025-0.0045%, and the S content is preferably 0.0020-0.0080%.
[0045] Ni: Nickel plays a role of solid solution strengthening in steel and is beneficial to low temperature toughness. Therefore, in the present invention, the Ni element can be selectively not added or a certain amount of Ni element can be added. For example, when the Ni content is 0.07-0.13%, the low temperature toughness can be greatly improved.
[0046] Cr: Chromium plays a role in solid solution strengthening in steel and can delay pearlite transformation. Therefore, in the present invention, Cr element can be selectively not added or a certain amount of Cr element can be added. For example, when the Cr content is above 0.07%, the low temperature toughness can be greatly improved. At the same time, if the Cr content exceeds 0.13%, it is not conducive to welding performance. Therefore, in one embodiment, the Cr content is preferably 0.07-0.13%.
[0047] Furthermore, in terms of chemical composition, the carbon equivalent CEV of the steel satisfies 0.328~0.371.
[0048] Among them, carbon equivalent CEV=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15, where [C], [Mn], [Cr], [Mo], [V], [Cu], and [Ni] represent the mass percentages of elements such as C, Mn, Cr, Mo, V, Cu, and Ni in steel. For example, when the mass percentage of C in steel is 0.09%, the mass percentage of C is 0.09. Substitute this value into the CEV formula.
[0049] In addition, in the present application, the content of each element in the steel can be determined by sampling the steel in a solid form such as a steel billet or a steel plate product and measuring it.
[0050] In a preferred embodiment, the chemical composition of the steel includes, by mass percentage, C: 0.11-0.14%, Si: 0.11-0.18%, Mn: 1.31-1.39%, Nb: 0.011-0.019%, Ti: 0.009-0.017%, Al: 0.026-0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest are iron and unavoidable impurities; and the carbon equivalent CEV satisfies 0.328-0.371.
[0051] In a preferred embodiment, the chemical composition of the steel includes, by mass percentage: C: 0.10~0.13%, Si: 0.11~0.18%, Mn: 1.34~1.42%, Nb: 0.014~0.022%, Ti: 0.009~0.017%, Al: 0.026~0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest are iron and unavoidable impurities; the carbon equivalent CEV satisfies 0.323~0.366.
[0052] In a preferred embodiment, the chemical composition of the steel includes, by mass percentage: C: 0.09~0.12%, Si: 0.11~0.18%, Mn: 1.37~1.45%, Nb: 0.024~0.032%, Ti: 0.009~0.017%, Al: 0.026~0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest are iron and unavoidable impurities; the carbon equivalent CEV satisfies 0.318~0.361.
[0053] In a preferred embodiment, the chemical composition of the steel includes, by mass percentage, C: 0.08-0.11%, Si: 0.11-0.18%, Mn: 1.39-1.47%, Ni: 0.07-0.13%, Nb: 0.021-0.029%, Ti: 0.009-0.017%, Al: 0.026-0.046%, Cr: 0.07-0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest are iron and unavoidable impurities; the carbon equivalent CEV satisfies 0.333-0.380.
[0054] Furthermore, in terms of production process, a production method according to one embodiment of the present invention includes the following steps.
[0055] Step 1, Steel Casting Step
[0056] That is, a steel billet is obtained by smelting molten steel and casting, and the chemical composition of the steel billet is as described above.
[0057] The specific molten steel smelting technology and casting technology can be implemented by using the technology disclosed in the art. For example, KR desulfurization, converter smelting, RH refining, LF refining, and continuous casting can be used to prepare a steel billet with the chemical composition described above.
[0058] Step 2, heating step
[0059] That is, the billet is heated in the heating furnace to a maximum temperature of T1+10°C or higher and T2 or lower. In other words, the billet is heated in the heating furnace to a temperature of T1+10°C or higher and T2 or lower. Usually, the set temperature of the heating furnace is considered to be the temperature reached by the billet in the heating furnace, and it is not necessary to directly contact / measure the billet with a temperature measuring element to determine the temperature of the billet.
[0060] T1 is T NbC , T NbN and T TiC The maximum value in .
[0061] Among them, T NbC , T NbN , T TiC and T TiN They are the complete solution temperatures of NbC, NbN, TiC and TiN respectively.
[0062] In an optional embodiment, the method can be performed by lg([Nb]×[N])=3.70-10800 / (T NbN +273.15), lg([Nb]×[C])=2.26-6770 / (T NbC +273.15), lg([Ti]×[C])=5.33-10475 / (T TiC +273.15), lg([Ti]×[N])=0.32-8000 / (T TiN +273.15) respectively to calculate T NbC , T NbN , T TiC and T TiN , [Nb], [N]), [C], and [Ti] are the mass percentages of Nb, N, C, and Ti in the steel billet, respectively.
[0063] Of course, in a variation, T NbC , T NbN , T TiC and T TiN It can also be obtained by using methods known in the art, such as industry experience values.
[0064] T2 is T1+50℃, T TiN Maximum value at -150℃.
[0065] In this way, by controlling the temperature in the heating furnace above T1+10°C and below T2, it can be ensured that the Nb precipitates in the steel are completely dissolved, the Ti carbides are completely dissolved, and the Ti nitrides are retained, thereby preventing the abnormal growth of austenite grains, and ultimately ensuring the comprehensive performance of the finished steel plate.
[0066] Step 3, controlled rolling step
[0067] After leaving the heating furnace, the steel billet is first rolled at a rolling temperature above T3 and below T3+40℃ to 4~6.8 times the thickness of the finished product to obtain the first intermediate plate; then rolled at a rolling temperature above T4-50℃ and below T4+20℃ to 1.8~3.2 times the thickness of the finished product to obtain the second intermediate plate; finally, rolled at a rolling temperature above T5-55℃ and below T5 to the thickness of the finished product.
[0068] That is to say, one embodiment of the present invention controls the temperature of the steel billet during rolling to 4 to 6.8 times the thickness of the finished product, the temperature during rolling from 4 to 6.8 times the thickness of the finished product to 1.8 to 3.2 times the thickness of the finished product, and the temperature during rolling from 1.8 to 3.2 times the thickness of the finished product to completion of rolling. In this way, on the one hand, sufficient recrystallization and refinement of the recrystallized grains can be ensured, and on the other hand, the recrystallized equiaxed grains can be deformed and flattened. On the other hand, rolling deformation can be used to induce ferrite phase transformation, and ferrite phase transformation occurs on the deformation band or in the grain boundary to obtain fine ferrite grains, thereby ensuring the yield strength and good toughness of the steel plate.
[0069] Among them, T3 ≥ T4 ≥ T5, T5 = 910-310 [C] -80 [Mn] -15 [Cr], T4 = 910-203 -15.2[Ni]+44.7[Si], T3=887+464[C]+6445[Nb]-644 +890[Ti]+363[Al]-357[Si], [C], [Nb], [Ti], [Al], [Si], [Ni] are the mass percentages of C, Nb, Ti, Al, Si, and Ni in the steel billet respectively.
[0070] Step 4, controlled cooling step
[0071] The rolled steel plate is air-cooled to above T6-50°C and below T6+20°C at a cooling rate of 1~10°C / s, then water-cooled to above T7-30°C and below T7+130°C at a cooling rate of 5~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0072] That is to say, in one embodiment of the present invention, the hot-rolled steel plate is divided into three stages with different cooling rates and cooling methods during cooling. Thus, in the first cooling stage, ferrite phase transformation occurs, and the presence of ferrite ensures the low yield strength of the steel plate; and in the second stage, the carbon-rich supercooled austenite phase in the steel plate is rapidly cooled to transform it into acicular ferrite / bainite structure, and the acicular ferrite / bainite phase transformation is complete through the control of the final cooling temperature; in addition, the control of the cooling rate can well avoid the generation of martensite phase or pearlite phase; furthermore, the above temperature control can also improve the shape of the finished steel plate. Combining the above aspects, the steel plate finally ensures higher tensile strength, lower yield strength ratio, excellent low-temperature toughness, excellent shape and good welding performance.
[0073] Among them, T5≥T6≥T7, T7=539-423[C]-17.7[Ni]-12.1[Cr]-11[Si]-30.4[Mn], T6=830-270[C]-90[Mn]-37[Ni]-70[Cr], [C], [Si], [Ni], [Mn], [Cr] are the mass percentages of C, Si, Ni, Mn, and Cr in the steel billet respectively.
[0074] Thus, the metallographic structure of the finished steel plate prepared in one embodiment of the present invention is a complex structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite. Here, the metallographic structure of the steel can be obtained by conducting a structure test using the GB / T 15125-2009 "Specimens and Test Methods for Metallographic Examination of Metallic Materials" standard.
[0075] The thickness of the finished steel plate is 6-64mm, the yield strength of the steel plate is ≥360MPa, the tensile strength is ≥510MPa, the elongation is ≥25%, and the yield strength ratio is ≤0.75. Here, the mechanical properties test can be carried out in accordance with GB / T 228.1-2021 "Tensile test of metallic materials Part 1: Room temperature test method".
[0076] The impact energy of the finished steel plate at -20℃ KV2≥260J, and the impact energy of the finished steel plate at -40℃ KV2≥240J. Here, the low temperature toughness test can be carried out according to GB / T229-2007 "Metallic Materials Charpy Pendulum Impact Test Method".
[0077] The unevenness of the finished steel plate is ≤1mm / m. Here, the unit mm / m refers to mm per unit length of the steel plate, and the unit length is calculated in m.
[0078] In addition, the weldability of the finished steel plate is excellent.
[0079] Further preferably, in step 2, the residence time of the steel billet in the heating furnace at a temperature above T1+10°C and below T2 is 0.07-0.13 min / mm, and the total residence time in the heating furnace is 1.15-1.35 min / mm.
[0080] Here, the unit min / mm refers to the unit thickness of each steel billet per minute, and the unit thickness is calculated in mm.
[0081] More specifically, in an optional embodiment, the steel billet may adopt a five-stage process in the heating furnace, including a heat recovery stage, a preheating stage, a first heating stage, a second heating stage and a soaking stage.
[0082] In this five-stage process, the temperature of the second heating stage limits the maximum temperature of the steel billet, that is, the temperature of the second heating stage is set to be above T1+10℃ and below T2, and the residence time of the steel billet in the second heating stage is 0.07~0.13min / mm.
[0083] In the five-stage process, the temperature of the first stage is 1120±15°C.
[0084] Furthermore, in the five-stage process, preferably, the temperature of the soaking stage is lower than that of the second heating stage, and the temperature of the soaking stage is 20-40° C. lower than that of the second heating stage. This arrangement can further improve the toughness of the finished steel plate.
[0085] In an optional variation, the steel billet is heated in the heating furnace using a three-stage process comprising a preheating stage, a heating stage and a soaking stage.
[0086] Among them, in this three-stage process, the temperature of the heating section limits the maximum temperature of the steel billet, that is, the temperature of the heating section is set to be above T1+10°C and below T2, and the residence time of the steel billet in the heating section is 0.07~0.13min / mm.
[0087] Furthermore, in the three-stage process, preferably, the temperature of the soaking section is lower than that of the heating section, and the temperature of the soaking section is 20-40° C. lower than that of the heating section. This arrangement can further improve the toughness of the finished steel plate.
[0088] In step 3, during the rolling of the steel billet into the first intermediate plate, the reduction in each pass is ≥20mm; during the rolling of the first intermediate plate into the second intermediate plate, the reduction in each pass is ≥12mm; during the rolling of the second intermediate plate into the finished product thickness, the reduction in each pass is ≥4mm.
[0089] Preferably, during rolling the steel billet into the first intermediate plate, the start rolling temperature is higher than T3+20°C and lower than T3+40°C, and the finish rolling temperature is higher than T3 and lower than T3+20°C.
[0090] Preferably, during rolling the first intermediate plate into the second intermediate plate, the start rolling temperature is greater than T4 and less than T4+20°C, and the finish rolling temperature is greater than T4-50°C and less than T4-30°C.
[0091] Furthermore, in step 3, the second intermediate plate is rolled to a finished thickness at a rolling temperature of T5-55°C or higher and T5-15°C or lower. For example, in some embodiments, the start rolling temperature is T5-30°C or higher and T5-15°C or lower, and the final rolling temperature is T5-55°C or higher and T5-40°C or lower.
[0092] Alternatively, the second intermediate plate is rolled to a finished thickness at a rolling temperature of T5-40°C or higher and T5 or lower. For example, in some embodiments, the start rolling temperature is T5-15°C or higher and T5 or lower, and the final rolling temperature is T5-40°C or higher and T5-25°C or lower.
[0093] Further, when the second intermediate plate is rolled to the finished thickness at a starting rolling temperature of T5-30°C or higher and T5-15°C or lower and a finishing rolling temperature of T5-55°C or higher and T5-40°C or lower, in step 4:
[0094] In some preferred embodiments, the rolled steel plate is air-cooled to above T6-50°C and below T6-30°C at a cooling rate of 1-10°C / s, and then water-cooled to above T7+90°C and below T7+130°C at a cooling rate of 8-30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate. In this way, the obtained structure is a complex phase structure of deformation-induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation-induced ferrite in the metallographic sampling surface accounts for approximately 35% to 45%, and the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 10% to 20%. The proportion is approximately 35%~45%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 10%~20%, and the area of bainite in the metallographic sampling surface accounts for approximately 0%~10%; the thickness of the finished steel plate is 6~64mm, the yield strength is ≥360MPa, the tensile strength is ≥510MPa, the elongation is ≥30%, the yield strength ratio is ≤0.75, the impact energy KV2 at 0℃ is ≥280J, the impact energy KV2 at -20℃ is ≥260J, the impact energy KV2 at -40℃ is ≥250J, the unevenness of the steel plate is ≤1mm / m, and the welding performance is excellent;
[0095] In some variant implementation modes, the rolled steel plate is air-cooled to a temperature between T6-30°C and T6-10°C at a cooling rate of 1-10°C / s, and then water-cooled to a temperature between T7+50°C and T7+90°C at a cooling rate of 8-30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate. In this way, the obtained structure is a complex phase structure of deformation-induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation-induced ferrite in the metallographic sampling surface accounts for approximately 35% to 45%, and the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 10% to 20%. The ratio is approximately 10%~30%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 15%~25%, and the area of bainite in the metallographic sampling surface accounts for approximately 10%~30%; the thickness of the finished steel plate is 6~64mm, the yield strength is ≥390MPa, the tensile strength is ≥530MPa, the elongation is ≥28%, the yield strength ratio is ≤0.75, the impact energy KV2 at 0℃ is ≥280J, the impact energy KV2 at -20℃ is ≥260J, the impact energy KV2 at -40℃ is ≥250J, the steel plate unevenness is ≤1mm / m, and the welding performance is excellent.
[0096] Further, when the second intermediate plate is rolled to the finished thickness at a starting rolling temperature of T5-15°C or higher and T5 or lower and a finishing rolling temperature of T5-40°C or higher and T5-25°C or lower, in step 4:
[0097] In some preferred embodiments, the rolled steel plate is air-cooled to above T6-10°C and below T6+10°C at a cooling rate of 1~10°C / s, and then water-cooled to above T7+10°C and below T7+50°C at a cooling rate of 8~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate. In this way, the obtained structure is a complex phase structure of deformation-induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation-induced ferrite in the metallographic sampling surface accounts for approximately 10%~25%, and the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 10%~25%. Approximately 10%~25%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 20%~30%, and the area of bainite in the metallographic sampling surface accounts for approximately 30%~50%; the thickness of the finished steel plate is 6~64mm, the yield strength is ≥440MPa, the tensile strength is ≥585MPa, the elongation is ≥26%, the yield strength ratio is ≤0.75, the impact energy KV2 at -20℃ is ≥270J, the impact energy KV2 at -40℃ is ≥250J, the impact energy KV2 at -60℃ is ≥200J, the unevenness of the steel plate is ≤1mm / m, and the welding performance is excellent;
[0098] In some variant implementation modes, the rolled steel plate is air-cooled to above T6°C and below T6+20°C at a cooling rate of 1~10°C / s, and then water-cooled to above T7-30°C and below T7+10°C at a cooling rate of 8~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate. In this way, the obtained structure is a complex phase structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation induced ferrite in the metallographic sampling surface accounts for approximately 5%~10%, and the area of polygonal ferrite in the metallographic sampling surface accounts for a large The area of acicular ferrite in the metallographic sampling surface accounts for about 5%~10%, and the area of bainite in the metallographic sampling surface accounts for about 70%~85%; the thickness of the finished steel plate is 6~64mm, the yield strength is ≥500MPa, the tensile strength is ≥670MPa, the elongation is ≥25%, the yield strength ratio is ≤0.75, the impact energy KV2 at -20℃ is ≥260J, the impact energy KV2 at -40℃ is ≥240J, the impact energy KV2 at -60℃ is ≥200J, the steel plate unevenness is ≤1mm / m, and the welding performance is excellent.
[0099] In summary, the beneficial effects of the present invention are:
[0100] Compared with the existing high-content components of Ni, Mo, and Cr, the content of these alloys is greatly reduced. Through the design of chemical composition and the specific process control of heating, rolling, and cooling, while eliminating the defects of poor welding performance caused by high alloy content, the mechanical properties, such as toughness, strength, and yield strength ratio, are still guaranteed (that is, the mechanical properties brought by these elements are not reduced due to the reduction of the content of these elements). This allows the steel plate to be comprehensively improved in terms of low yield strength ratio, easy welding, high strength and toughness, and good plate shape under the conditions of low alloy content, low production difficulty, and short production process. The resulting steel plate is suitable for bridge engineering.
[0101] Some specific embodiments are introduced below to supplement the beneficial effects of the present invention.
[0102] Example 1
[0103] A continuous casting billet is prepared by steelmaking and continuous casting. The chemical composition of the continuous casting billet includes, by mass percentage, C: 0.13%, Si: 0.14%, Mn: 1.33%, P: 0.0131%, S: 0.0040%, Nb: 0.014%, Ti: 0.014%, Al: 0.036%, N: 0.0035%, CEV=0.352, and the rest is Fe and unavoidable impurities.
[0104] A three-stage process is adopted, with the temperature of the preheating section ≤1000℃, the temperature of the heating section 1198℃, the residence time in the heating section 0.07~0.13min / mm, the temperature of the soaking section 1168℃, and the total time in the heating furnace is 1.15~1.35min / mm.
[0105] After leaving the heating furnace, the steel billet is first rolled to 156mm at an initial rolling temperature of 967±10℃ and a final rolling temperature of 947±10℃ to obtain the first intermediate plate; then rolled to 72mm at an initial rolling temperature of 853±10℃ and a final rolling temperature of 803±10℃ to obtain the second intermediate plate; finally, rolled to 24mm at an initial rolling temperature of 731~746℃ and a final rolling temperature of 706~721℃ to obtain a hot-rolled steel plate.
[0106] The hot rolled steel plate is air cooled to 635±10°C at a cooling rate of 1~10°C / s, then water cooled to 552±20°C at a cooling rate of 5~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0107] Sampling and testing of finished steel plates revealed:
[0108] (1) Metallographic structure Figure 2 As shown, it is a complex phase structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation induced ferrite in the metallographic sampling surface accounts for approximately 40%, the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 40%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 15%, and the area of bainite in the metallographic sampling surface accounts for approximately 5%.
[0109] (2) Yield strength 365 MPa, tensile strength 521 MPa, yield strength ratio 0.70, elongation 41%;
[0110] (3) The impact energy KV2 at 0℃ is 320J, 331J, 326J; the impact energy KV2 at -20℃ is 295J, 298J, 290J; the impact energy KV2 at -40℃ is 260J, 255J, 262J;
[0111] (4) Roughness ≤ 1mm / m, and excellent welding performance.
[0112] Example 2
[0113] A continuous casting billet is prepared by steelmaking and continuous casting. The chemical composition of the continuous casting billet includes, by mass percentage, C: 0.11%, Si: 0.14%, Mn: 1.38%, P: 0.0128%, S: 0.0056%, Nb: 0.018%, Ti: 0.0013%, Al: 0.034%, N: 0.0031%, CEV=0.340, and the rest is Fe and unavoidable impurities.
[0114] A five-stage process is adopted, with the temperature of the heat recovery section ≤900℃, the temperature of the preheating section ≤1000℃, the temperature of the first heating section 1120℃, the temperature of the second heating section 1188℃, the residence time in the second heating section 0.07~0.13min / mm, the temperature of the soaking section 1158℃, and the total time in the heating furnace is 1.15~1.35min / mm.
[0115] After leaving the heating furnace, the steel billet is first rolled to 160mm at an initial rolling temperature of 972±10℃ and a final rolling temperature of 952±10℃ to obtain the first intermediate plate; then rolled to 84mm at an initial rolling temperature of 859±10℃ and a final rolling temperature of 809±10℃ to obtain the second intermediate plate; finally, rolled to 28mm at an initial rolling temperature of 733~748℃ and a final rolling temperature of 708~723℃ to obtain a hot-rolled steel plate.
[0116] The hot rolled steel plate is air cooled to 656±10°C at a cooling rate of 1~10°C / s, then water cooled to 519±20°C at a cooling rate of 5~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0117] Sampling and testing of finished steel plates revealed:
[0118] (1) Metallographic structure Figure 3 As shown, it is a complex phase structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite, wherein the area of deformation induced ferrite in the metallographic sampling surface accounts for approximately 40%, the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 20%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 20%, and the area of bainite in the metallographic sampling surface accounts for approximately 20%.
[0119] (2) Yield strength 410 MPa, tensile strength 570 MPa, yield strength ratio 0.72, elongation 39%;
[0120] (3) The impact energy KV2 at 0℃ is 292J, 288J, 295J; the impact energy KV2 at -20℃ is 272J, 269J, 273J; the impact energy KV2 at -40℃ is 271J, 259J, 263J;
[0121] (4) Roughness ≤ 1mm / m, and excellent welding performance.
[0122] Example 3
[0123] A continuous casting billet is prepared by steelmaking and continuous casting. The chemical composition of the continuous casting billet includes, by mass percentage, C: 0.10%, Si: 0.13%, Mn: 1.41%, P: 0.0132%, S: 0.0053%, Nb: 0.028%, Ti: 0.0015%, Al: 0.031%, N: 0.0031%, CEV=0.335, and the rest is Fe and unavoidable impurities.
[0124] A three-stage process is adopted, with the temperature of the preheating section ≤1000℃, the temperature of the heating section 1220℃, the residence time in the heating section 0.07~0.13min / mm, the temperature of the soaking section 1190℃, and the total time in the heating furnace is 1.15~1.35min / mm.
[0125] After leaving the heating furnace, the steel billet is first rolled to 180mm at an initial rolling temperature of 1014±10℃ and a final rolling temperature of 994±10℃ to obtain the first intermediate plate; then rolled to 80mm at an initial rolling temperature of 862±10℃ and a final rolling temperature of 812±10℃ to obtain the second intermediate plate; finally, rolled to 36mm at an initial rolling temperature of 748~763℃ and a final rolling temperature of 723~738℃ to obtain a hot-rolled steel plate.
[0126] The hot rolled steel plate is air cooled to 676±10°C at a cooling rate of 1~10°C / s, then water cooled to 482±20°C at a cooling rate of 5~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0127] Sampling and testing of finished steel plates revealed:
[0128] (1) Metallographic structure Figure 4 As shown, it is a complex phase structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite, among which, the area of deformation induced ferrite in the metallographic sampling surface accounts for approximately 18%, the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 16%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 26%, and the area of bainite in the metallographic sampling surface accounts for approximately 40%.
[0129] (2) Yield strength 460MPa, tensile strength 630MPa, yield strength ratio 0.73, elongation 32%;
[0130] (3) The impact energy KV2 at -20℃ is 289J, 291J, 286J; the impact energy KV2 at -40℃ is 269J, 272J, 277J; the impact energy KV2 at -60℃ is 232J, 245J, 233J;
[0131] (4) Roughness ≤ 1mm / m, and excellent welding performance.
[0132] Example 4
[0133] A continuous casting billet is prepared by steelmaking and continuous casting. The chemical composition of the continuous casting billet includes, by mass percentage, the following: C: 0.10%, Si: 0.15%, Mn: 1.43%, P: 0.0120%, S: 0.0030%, Cr: 0.12%, Ni: 0.12%, Nb: 0.025%, Ti: 0.015%, Al: 0.033%, N: 0.0032%, CEV=0.370, and the rest is Fe and unavoidable impurities.
[0134] A five-stage process is adopted, with the temperature of the heat recovery section ≤900℃, the temperature of the preheating section ≤1000℃, the temperature of the first heating section 1120℃, the temperature of the second heating section 1215℃, the residence time in the second heating section 0.07~0.13min / mm, the temperature of the soaking section 1185℃, and the total time in the heating furnace is 1.15~1.35min / mm.
[0135] After leaving the heating furnace, the steel billet is first rolled to 200mm at an initial rolling temperature of 995±10℃ and a final rolling temperature of 975±10℃ to obtain the first intermediate plate; then rolled to 100mm at an initial rolling temperature of 861±10℃ and a final rolling temperature of 811±10℃ to obtain the second intermediate plate; finally, rolled to 50mm at an initial rolling temperature of 745~760℃ and a final rolling temperature of 720~735℃ to obtain a hot-rolled steel plate.
[0136] The hot rolled steel plate is air cooled to 672±10°C at a cooling rate of 1~10°C / s, then water cooled to 538±20°C at a cooling rate of 5~30°C / s, and then naturally cooled to room temperature to obtain a finished steel plate.
[0137] Sampling and testing of finished steel plates revealed:
[0138] (1) Metallographic structure Figure 5 As shown, it is a complex phase structure of deformation induced ferrite + polygonal ferrite + acicular ferrite + bainite, among which, the area of deformation induced ferrite in the metallographic sampling surface accounts for approximately 7%, the area of polygonal ferrite in the metallographic sampling surface accounts for approximately 8%, the area of acicular ferrite in the metallographic sampling surface accounts for approximately 9%, and the area of bainite in the metallographic sampling surface accounts for approximately 76%.
[0139] (2) Yield strength 520MPa, tensile strength 695MPa, yield strength ratio 0.75, elongation 30%;
[0140] (3) The impact energy KV2 at -20℃ is 278J, 284J, 285J; the impact energy KV2 at -40℃ is 262J, 258J, 265J; the impact energy KV2 at -60℃ is 244J, 250J, 239J;
[0141] (4) Roughness ≤ 1mm / m, and excellent welding performance.
Claims
1. A method for producing steel, It is characterized in that Includes steps: A steel billet is obtained by smelting and casting molten steel, wherein the chemical composition of the steel billet comprises, by mass percentage, C: 0.08-0.14%, Si: 0.11-0.18%, Mn: 1.31-1.47%, Nb: 0.011-0.032%, Ti: 0.009-0.017%, Al: 0.026-0.046%, Cr≤0.13%, Ni≤0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities; The billet is heated in a heating furnace to T 1 +10℃ or above, T 2 Below, T 1 The value is T NbC 、T NbN and T TiC The maximum value in T 2 The value is T 1 +50℃、T TiN -150℃ maximum value; where T NbC 、T NbN 、T TiC and T TiN are the complete solution temperatures of NbC, NbN, TiC and TiN respectively; After leaving the heating furnace, the billet is first heated to the rolling temperature T 3 Above, T 3 The first intermediate plate is obtained by rolling at a temperature below +40℃ to 4~6.8 times the thickness of the finished product; 4 -50℃ or above, T 4 The second intermediate plate is obtained by rolling at a temperature below +20℃ to 1.8~3.2 times the thickness of the finished product; finally, the rolling temperature is T 5 -55℃ or above, T 5 The following is rolled to the finished thickness; The rolled steel plate is air-cooled to T at a cooling rate of 1-10°C / s. 6 -50℃ or above, T 6 +20℃ or below, then water cool to T at a cooling rate of 5~30℃ / s 7 -30℃ or above, T 7 +130℃ or below, then naturally cool to room temperature to obtain the finished steel plate; Among them, T 3 ≥T 4 ≥T 5 ≥T 6 ≥T 7 , T 7 =539-423[C]-17.7[Ni]-12.1[Cr]-11[Si]-30.4[Mn], T 3 =887+464[C]+6445[Nb]-644 +890[Ti]+363[Al]-357[Si],T 6 =830-270[C]-90[Mn]-37[Ni]-70[Cr], T 5 =910-310[C]-80[Mn]-15[Cr],T 4 =910-203 -15.2[Ni]+44.7[Si], [C], [Nb], [Ti], [Al], [Si], [Ni], [Mn], and [Cr] are the mass percentages of C, Nb, Ti, Al, Si, Ni, Mn, and Cr in the steel billet respectively.
2. The method for producing steel according to claim 1, It is characterized in that The chemical composition of the steel billet includes, by mass percentage, P: 0.0101-0.0151%, S: 0.0020-0.0080%, and N: 0.0025-0.0045%.
3. The method for producing steel according to claim 1, It is characterized in that The carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.318~0.
380.
4. The method for producing steel according to claim 3, It is characterized in that The chemical composition of the steel billet includes, by mass percentage, C: 0.11-0.14%, Si: 0.11-0.18%, Mn: 1.31-1.39%, Nb: 0.011-0.019%, Ti: 0.009-0.017%, Al: 0.026-0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
5. The method for producing steel according to claim 4, It is characterized in that The carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.328~0.
371.
6. The method for producing steel according to claim 3, It is characterized in that The chemical composition of the steel billet includes, by mass percentage, C: 0.10-0.13%, Si: 0.11-0.18%, Mn: 1.34-1.42%, Nb: 0.014-0.022%, Ti: 0.009-0.017%, Al: 0.026-0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
7. The method for producing steel according to claim 6, It is characterized in that The carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.323~0.
366.
8. The method for producing steel according to claim 3, It is characterized in that The chemical composition of the steel billet includes, by mass percentage, C: 0.09-0.12%, Si: 0.11-0.18%, Mn: 1.37-1.45%, Nb: 0.024-0.032%, Ti: 0.009-0.017%, Al: 0.026-0.046%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
9. The method for producing steel according to claim 8, It is characterized in that The carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.318~0.
361.
10. The method for producing steel according to claim 3, It is characterized in that The chemical composition of the steel billet includes, by mass percentage, C: 0.08-0.11%, Si: 0.11-0.18%, Mn: 1.39-1.47%, Ni: 0.07-0.13%, Nb: 0.021-0.029%, Ti: 0.009-0.017%, Al: 0.026-0.046%, Cr: 0.07-0.13%, P≤0.0151%, S≤0.0080%, N≤0.0045%, and the rest is iron and unavoidable impurities.
11. The method for producing steel according to claim 10, It is characterized in that The carbon equivalent CEV of the chemical composition of the steel billet satisfies 0.333~0.
380.
12. The method for producing steel according to claim 1, It is characterized in that Billet in T 1 +10℃ or above, T 2 The residence time at the following temperature is 0.07~0.13min / mm, and the total time in the heating furnace is 1.15~1.35min / mm.
13. The method for producing steel according to claim 1, It is characterized in that The billet is heated in a five-stage process in the heating furnace, including a heat recovery section, a preheating section, a first heating section, a second heating section, and a soaking section. The temperature of the second heating section is T 1 +10℃ or above, T 2 Below, the temperature of the soaking section is lower than that of the second heating section, and the temperature of the soaking section is 20~40℃ lower than that of the second heating section; Alternatively, the steel billet is heated in a heating furnace using a three-stage process including a preheating section, a heating section, and a soaking section, wherein the temperature of the heating section is T 1 +10℃ or above, T 2 Below, the temperature of the soaking section is lower than the temperature of the heating section, and the temperature of the soaking section is 20~40℃ lower than the temperature of the heating section.
14. The method for producing steel according to claim 13, It is characterized in that In the five-stage process, the temperature of the first stage is 1120±15℃; Among them, through lg([Nb]×[N])=3.70-10800 / (T NbN +273.15), lg([Nb]×[C])=2.26-6770 / (T NbC +273.15), lg([Ti]×[C])=5.33-10475 / (T TiC +273.15), lg([Ti]×[N])=0.32-8000 / (T TiN +273.15) respectively to calculate T NbC 、T NbN 、T TiC and T TiN , [Nb], [N]), [C], and [Ti] are the mass percentages of Nb, N, C, and Ti in the steel billet, respectively.
15. The method for producing steel according to claim 1, It is characterized in that The second intermediate plate is rolled at a temperature of T 5 -55℃ or above, T 5 Rolling to finished product thickness below -15℃; The rolled steel plate is air-cooled to T at a cooling rate of 1-10°C / s. 6 -50℃ or above, T 6 Below -30℃, then water cool to T at a cooling rate of 8~30℃ / s 7 +90℃ or above, T 7 +130℃ or less, and then naturally cool to room temperature to obtain a finished steel plate; or, air cool the rolled steel plate at a cooling rate of 1-10℃ / s to T 6 -30℃ or above, T 6 Below -10℃, then water cool to T at a cooling rate of 8~30℃ / s 7 +50℃ or above, T 7 +90℃ or below, and then naturally cool to room temperature to obtain the finished steel plate.
16. The method for producing steel according to claim 1, It is characterized in that The second intermediate plate is rolled at a temperature of T 5 -40℃ or above, T 5 The following is rolled to the finished thickness; The rolled steel plate is air-cooled to T at a cooling rate of 1-10°C / s. 6 -10℃ or above, T 6 +10℃ or below, then water cool to T at a cooling rate of 8~30℃ / s 7 +10℃ or above, T 7 +50℃ or less, and then naturally cool to room temperature to obtain a finished steel plate; or, air cool the rolled steel plate at a cooling rate of 1-10℃ / s to T 6 Above, T 6 +20℃ or below, then water cool to T at a cooling rate of 8~30℃ / s 7 -30℃ or above, T 7 +10℃ or less, and then naturally cool to room temperature to obtain the finished steel plate.
17. The method for producing steel according to claim 1, It is characterized in that When the first intermediate plate is rolled, the rolling temperature is T 3 +20℃ or above, T 3 +40℃ or below, the final rolling temperature is T 3 Above, T 3 +20℃ or below; When the second intermediate plate is rolled, the rolling temperature is T 4 Above, T 4 +20℃ or below, the final rolling temperature is T 4 -50℃ or above, T 4 -30℃ or less; When the second intermediate plate is rolled to the finished product thickness, the rolling temperature is T 5 -30℃ or above, T 5 Below -15℃, the final rolling temperature is T 5 -55℃ or above, T 5 -40℃ or below, or the rolling temperature is T 5 -15℃ or above, T 5 Below, the final rolling temperature is T 5 -40℃ or above, T 5 -25℃ or below.
Citation Information
Patent Citations
Steel plate for high-strength high-toughness low-yield easily-welding structure and method for manufacturing same
CN101619423A
Low-yield-ratio weather-proof structural steel with yield strength greater than or equal to 690MPa for bridge and production method thereof
CN108531808A
Thin-specification low-yield-ratio high-strength bridge steel and production method thereof
CN111979481A
Low-yield-ratio high-toughness TMCP type bridge steel plate and production method thereof
CN112322995A
Large-thickness subsea pipeline steel plate and production method thereof
CN118241125A