A preparation method of dolomite-based composite mineral admixture and the admixture prepared therefrom
By calcining dolomite powder and low-melting glass powder to form a shell-core structure and mixing it with high-aluminum active blends, dolomite-based composite mineral blends are prepared, which solves the problem of insufficient hydration activity of dolomite powder and improves the The durability and crack resistance of concrete are suitable for large-volume and long-design age projects.
Patent Information
- Application Number
- CN202411119030.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
When using dolomite as concrete blend, the reduction of hydration products leads to deterioration of pore structure, increasing shrinkage, reduced durability such as anti-seepage and freezing, and lacks methods to efficiently utilize the mineral components of dolomite itself.
By mixing natural dolomite powder with low-melting glass powder and calcining at 650~750°C, the shell-core structure semi-calcined dolomite powder is formed and mixed with high-aluminum active blends to prepare dolomite matrix composite mineral dolomite compound dolomite powder is prepared The composite material uses the early rapid hydration of glass powder and the hydration reaction of lightly calcined magnesium oxide to regulate the hydration products and improve the activity and durability of concrete.
It effectively compensates for the insufficient early activity of dolomite powder, improves the long-term strength and crack resistance of concrete, reduces the amount of gelled materials, and is suitable for large-volume and long-term concrete projects with significant economic and technical effects.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building material concrete admixtures, and in particular to a preparation method of a dolomite-based composite mineral admixture and the prepared admixture. Background Art
[0002] As major water conservancy, hydropower, highway and railway projects are being built in western my country, conventional mineral admixtures such as fly ash, slag powder and silica fume are scarce. The use of natural materials to prepare mineral admixtures can achieve better technical, economic, quality and safety benefits. Limestone powder has a long history of application in the fields of hydropower and railways, and has formed national and industry standards such as GB / T 35164 "Limestone powder used in cement, mortar and concrete", DL / T 5304 "Technical specification for limestone powder added to hydraulic concrete", JGJ / T 318 "Technical specification for the application of limestone powder in concrete", and TB 3275 "Railway concrete". The main mineral component of dolomite is dolomite, which is a complex salt composed of calcium carbonate and magnesium carbonate. Dolomite and calcite, the main mineral in limestone powder, belong to the same trigonal system, and the main elements are the same main group. The basic physical and chemical properties they exhibit are similar, but relevant standards in the application field of mineral admixtures have not yet been formed. CN112694301A discloses a long-term shrinkage-reducing dolomite powder self-compacting concrete and a preparation method thereof, which achieves a reduction in the shrinkage rate of the self-compacting concrete from 0 to 70 days by compounding dolomite powder with a specific fineness, particle shape, specific surface area and dosage with fly ash, and by designing the mix ratio, but the technical effect is mainly achieved by the mix ratio design. CN106747090A discloses a modified dolomite powder-based mineral admixture and a preparation method thereof, which achieves an improvement in the mechanical properties, durability and deformation properties of the concrete by compounding 50 to 60% dolomite powder, 15 to 20% mineral powder, 15 to 20% fly ash and 5 to 10% bentonite in a certain proportion, but the proportion of dolomite powder is relatively low, and the beneficial effects of using dolomite powder are not described. CN114988738A discloses a modified dolomite powder, a preparation method thereof and concrete, which promotes the dissolution and chemical reaction of dolomite powder by adding a catalytic agent, dihydrogen phosphate and sulfate capillary filler, thereby improving its activity and water retention, but the sulfate and phosphate introduced thereby may have a negative impact on the setting time and durability of concrete. CN108046621A discloses a preparation method of calcined dolomite powder, which can be used as the main raw material of magnesium phosphate cement and magnesium oxychloride cement after compounding a certain proportion of silicon-containing components with dolomite, calcining and grinding, but does not explain the technical effect for conventional silicate cement concrete. CN117585950A discloses a dolomite powder concrete and a preparation method thereof, which inhibits the agglomeration of dolomite powder and promotes cement hydration by using methyl vinyl ether-maleic anhydride copolymer and polyvinyl pyridine, and compounding zeolite powder and magnetite powder, thereby improving the mechanical properties of dolomite powder concrete. In summary, in the existing technology of using dolomite as a mineral admixture, the technical effect is mostly improved through grinding, compounding with other admixtures and chemical modification.A large number of studies have shown that when inert stone powders such as dolomite powder, limestone powder, and granite powder are used as concrete admixtures, the reduction of hydration products leads to deterioration of the pore structure, increased shrinkage, and reduced durability such as impermeability and frost resistance. Therefore, there are great limitations on their application in large-volume concrete or concrete with high environmental action levels.
[0003] Another important application of dolomite is to calcine concrete calcium-magnesium composite expansion agent. The relevant technology directly prepares a composite expansion agent containing both calcium oxide and magnesium oxide by calcining and decarbonizing dolomite at high temperature. CN117843273 discloses a partially calcined dolomite as a calcium-magnesium concrete expansion agent. Dolomite powder is calcined at 700~1000℃ to obtain a calcium-magnesium expansion agent mainly composed of 20~35% magnesium oxide and 0~45% calcium oxide, which is used to reduce the shrinkage of ultra-high performance concrete. CN110028262A discloses a preparation method and application of a composite magnesium oxide expansion agent. A mixture of dolomite and serpentine is calcined at 1050~1150℃, which mainly contains 25~30% magnesium oxide and 35~45% dicalcium silicate. CN 110066129A discloses a calcium-magnesium composite expansion agent and a preparation method thereof, which is prepared by calcining at 1000-1050°C with dolomite as the main raw material, free calcium oxide seed crystals and aluminum hydroxide as auxiliary raw materials, and the main components are 22-26% magnesium oxide, 34-40% calcium oxide and 12-20% calcium heptaaluminate. In the relevant preparation methods of calcium-magnesium composite expansion agents disclosed in CN 110066123A and CN 110066127A, the difference in decomposition temperature and material weight between magnesium carbonate and calcium carbonate is utilized, and the magnesium oxide and calcium carbonate are separated by calcining at 550-650°C and using a suspension reaction tower. In the above patents, the hydration activity and shrinkage compensation effect of magnesium oxide and calcium oxide are mainly affected by the calcination temperature, while the method of coating the particle surface with calcium heptaaluminate by calcination to achieve hydration process regulation has a high requirement for the calcination temperature.
[0004] In summary, how to make full use of the mineral composition and chemical composition characteristics of dolomite itself and achieve efficient utilization in the field of building materials is a technical problem that urgently needs to be solved in the current engineering community. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a method for preparing a dolomite-based composite mineral admixture and the admixture prepared thereby.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a dolomite-based composite mineral admixture comprises the following steps:
[0008] S1. Mechanically crush and grind natural dolomite to obtain a specific surface area of 450~600 m 2 / kg of dolomite powder;
[0009] S2, mixing dolomite powder and low-melting-point glass powder into raw material in a weight ratio of 95:5-85:15, calcining at 650-750°C for 0.5-2h, cooling naturally in air, and grinding to obtain semi-calcined dolomite powder with a shell-core structure and a glass phase covering the surface;
[0010] S3. Evenly mix the shell-core structure semi-calcined dolomite powder and the high-alumina active admixture in a ratio of 70:30 to 80:20 to obtain a finished dolomite-based composite mineral admixture.
[0011] Among them, the total content of calcium carbonate and magnesium carbonate in the above-mentioned dolomite is ≥90%, and the content of magnesium carbonate is ≥30%.
[0012] The low melting point glass powder is a mixture of one or more of phosphate and borate series, with a total content of calcium oxide and bismuth oxide ≥ 20%, a softening temperature ≤ 600 ° C, a crystallization temperature ≥ 750 ° C, and a maximum particle size ≤ 45 μm.
[0013] The semi-calcined dolomite powder with shell-core structure has a 45 μm sieve residue fineness of ≤5.0%, a magnesium oxide content of ≥15%, and a free calcium oxide content of ≤1.0%.
[0014] The above-mentioned high-alumina active admixture is a mixture of one or more of metakaolin, calcined bauxite, natural volcanic ash material, fly ash, and slag powder, and the alumina content is ≥20%.
[0015] A second aspect of the present invention provides a dolomite-based composite mineral admixture, which is prepared by the above-mentioned preparation method.
[0016] The beneficial effects of the present invention are:
[0017] 1) In the preparation of the semi-calcined dolomite powder with a core-shell structure, the present invention calcines dolomite at a low temperature of 650-750°C to obtain the semi-calcined dolomite powder whose main components are light-burned magnesium oxide and calcium carbonate. A small amount of low-melting point glass powder is introduced to coat the surfaces of the light-burned magnesium oxide and calcium carbonate during the low-temperature calcination stage. On the one hand, the early rapid hydration of the glass powder compensates for the problem of insufficient early activity of the inert dolomite powder. On the other hand, the early hydration reaction rate of the light-burned magnesium oxide is regulated, so that the semi-calcined dolomite powder has the function of effectively compensating for shrinkage during the rapid cooling stage of concrete.
[0018] 2) Compared with conventional technologies such as chemical modification to improve the activity of dolomite powder admixtures and compounding with other active admixtures with a high proportion, the active admixture in the present invention only accounts for 20% to 30%, and the activity is mainly generated through the synergistic hydration with the core-shell structure semi-calcined dolomite powder's own minerals and hydration products, rather than just reacting with cement hydration products. This improves the long-term strength contribution and effectively reduces the amount of cementitious materials in long-design age concrete.
[0019] 3) The present invention improves the application effect of dolomite powder as a concrete admixture, and has significant economic and technical effects for large-volume concrete projects with the need to prevent and control early temperature cracks, concrete projects with a long design age, and projects in remote areas that lack conventional mineral admixtures such as fly ash and slag powder. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0021] The raw materials used in the following embodiments and comparative examples of the present invention are as follows:
[0022] Dolomite is produced in Jiangyou, Sichuan. The total content of calcium carbonate and magnesium carbonate is 99.5%, and the content of magnesium carbonate is 45.3%. The main chemical composition is shown in Table 1.
[0023] Phosphate-based low-melting-point glass powder, produced in Lingshou, Hebei, 400 mesh, softening temperature 530 °C, crystallization temperature 755 °C, main chemical composition see Table 1.
[0024] Borate low melting point glass powder, produced in Lingshou, Hebei, 400 mesh, softening temperature 595 ℃, crystallization temperature 770 ℃, main chemical composition see Table 1.
[0025] Metakaolin is produced in Lianyungang, Jiangsu Province. The main chemical composition is shown in Table 1.
[0026] Fly ash, produced in Jintang, Sichuan, Class F, Grade I, main chemical composition is shown in Table 1.
[0027] Natural volcanic ash material, produced in Batang, Sichuan, the main chemical composition is shown in Table 1.
[0028] Slag powder, produced in Panzhihua, Sichuan, S95, main chemical composition is shown in Table 1.
[0029] Table 1 Chemical composition of each raw material (%)
[0030]
[0031] Example 1
[0032] This embodiment provides a method for preparing a dolomite-based composite mineral admixture, comprising the following steps:
[0033] S1. Mechanically crush and grind the dolomite to obtain a specific surface area of 453 m 2 / kg of dolomite powder;
[0034] S2, mixing dolomite powder and phosphate-based low-melting-point glass in a weight ratio of 95:5 into a raw material, calcining at 650°C for 0.5h, cooling naturally in air, and grinding to obtain semi-calcined dolomite powder with a shell-core structure and a surface-coated glass phase with a fineness (45 μm sieve residue) of 3.8%, a magnesium oxide content of 22.3%, and a free calcium oxide content of 0.3%;
[0035] S3. Evenly mix the semi-calcined dolomite powder with a shell-core structure and the metakaolin in a weight ratio of 80:20 to obtain a finished dolomite-based composite mineral admixture.
[0036] Example 2
[0037] This embodiment provides a method for preparing a dolomite-based composite mineral admixture, comprising the following steps:
[0038] S1. Mechanically crush and grind the dolomite to obtain a specific surface area of 550 m 2 / kg of dolomite powder;
[0039] S2, dolomite powder and phosphate-based low-melting-point glass powder were mixed into a raw material in a weight ratio of 85:15, calcined at 750°C for 2 hours, naturally cooled in air, and ground to obtain semi-calcined dolomite powder with a shell-core structure and a surface-coated glass phase with a fineness (45 μm sieve residue) of 2.5%, a magnesium oxide content of 24.2%, and a free calcium oxide content of 0.8%;
[0040] S3. Evenly mix the shell-core structure semi-calcined dolomite powder and the natural volcanic ash material in a weight ratio of 70:30 to obtain a finished dolomite-based composite mineral admixture.
[0041] Example 3
[0042] This embodiment provides a method for preparing a dolomite-based composite mineral admixture, comprising the following steps:
[0043] S1. Mechanically crush and grind the dolomite to obtain a specific surface area of 521 m 2 / kg of dolomite powder;
[0044] S2, dolomite powder and borate low-melting point glass were mixed into a raw material in a weight ratio of 95:5, calcined at 650°C for 0.5h, naturally cooled in air, and ground to obtain semi-calcined dolomite powder with a shell-core structure and a surface-coated glass phase with a fineness of 3.7% (45 μm sieve residue), a magnesium oxide content of 23.0%, and a free calcium oxide content of 0.4%;
[0045] S3. The semi-calcined dolomite powder with a shell-core structure is uniformly mixed with a high-alumina active admixture in a weight ratio of 80:20 to obtain a finished dolomite-based composite mineral admixture, wherein the high-alumina active admixture is a mixture of metakaolin and slag powder in a weight ratio of 1:1.
[0046] Example 4
[0047] This embodiment provides a method for preparing a dolomite-based composite mineral admixture, comprising the following steps:
[0048] S1. Mechanically crush and grind the dolomite to obtain a specific surface area of 585 m 2 / kg of dolomite powder;
[0049] S2, dolomite powder and borate low-melting point glass powder were mixed into a raw material in a weight ratio of 85:15, calcined at 750 ° C for 2 hours, naturally cooled in air, and ground to obtain semi-calcined dolomite powder with a shell-core structure and a surface-coated glass phase with a fineness (45 μm sieve residue) of 4.2%, a magnesium oxide content of 24.5%, and a free calcium oxide content of 0.9%;
[0050] S3. Evenly mix the shell-core structure semi-calcined dolomite powder and calcined bauxite in a weight ratio of 70:30 to obtain a finished dolomite-based composite mineral admixture.
[0051] Example 5
[0052] This embodiment provides a method for preparing a dolomite-based composite mineral admixture, comprising the following steps:
[0053] S1. Mechanically crush and grind the dolomite to obtain a specific surface area of 482 m 2 / kg of dolomite powder;
[0054] S2. After mixing dolomite powder and low-melting point glass powder in a weight ratio of 90:10 into a raw material, calcining at 700°C for 1 hour, cooling naturally in air, and grinding to obtain semi-calcined dolomite powder with a shell-core structure and a surface-coated glass phase with a fineness (45 μm sieve residue) of 3.5%, a magnesium oxide content of 23.1%, and a free calcium oxide content of 0.5%, wherein the low-melting point glass powder is a mixture of borate low-melting point glass powder and phosphate low-melting point glass powder in a weight ratio of 1:1;
[0055] S3. Evenly mix the semi-calcined dolomite powder with a shell-core structure and fly ash in a weight ratio of 75:25 to obtain a finished dolomite-based composite mineral admixture.
[0056] Comparative Example 1
[0057] The main difference between this comparative example and the embodiment is that no low melting point glass powder is added during calcination, and the specific surface area of 453 m 2 / kg of dolomite powder was calcined at 750℃ for 2h, cooled naturally in air, and ground to obtain semi-calcined dolomite powder with a fineness (45 μm sieve residue) of 1.8%, a magnesium oxide content of 28.5%, and a free calcium oxide content of 0.8%. The semi-calcined dolomite powder and metakaolin were evenly mixed in a weight ratio of 70:30 to obtain the finished product.
[0058] Comparative Example 2
[0059] The main difference between this comparative example and the embodiment is that no low melting point glass powder is added during calcination, and the specific surface area of 453 m 2 / kg dolomite powder was calcined at 750℃ for 2h, cooled naturally in air, and ground to obtain semi-calcined dolomite powder with a fineness (45 μm sieve residue) of 1.8%, a magnesium oxide content of 28.5%, and a free calcium oxide content of 0.8%. No high-alumina active admixture was added subsequently.
[0060] Comparative Example 3
[0061] The main difference between this comparative example and the embodiment is that: the specific surface area of 453 m 2 / kg of dolomite powder and metakaolin are compounded in a weight ratio of 70:30, and the dolomite powder is not processed in step S2.
[0062] Comparative Example 4
[0063] The main difference between this comparative example and the embodiment is that only the dolomite is ground to obtain a specific surface area of 453m 2 / kg of dolomite powder.
[0064] Product Testing
[0065] Pure cement was used as the blank group, and the dolomite-based composite mineral admixtures of each embodiment and comparative example were added to the cement as the experimental group. The cement used in this test is the benchmark cement, produced in Qufu, Shandong, and meets the requirements of Appendix A of GB 8076 "Concrete Admixtures". The weight ratio of cement to admixture in all the above experimental groups is 70:30. The activity index test method refers to Appendix A of JG / T 486 "Composite Admixtures for Concrete"; the limited expansion rate test method refers to Appendix A of GB / T23439 "Concrete Expansion Agents", and curing is carried out in 20 ℃ water.
[0066] The activity index test results of each embodiment and comparative example are shown in Table 2. The semi-calcined dolomite powder that was only calcined in Comparative Example 2 and the dolomite powder that was only ground in Comparative Example 4 can only play a filling effect in cement mortar, and the activity index at each age is <70% and shows a shrinking trend with increasing age. The late activity of the composite admixture can be effectively improved by compounding with metakaolin and fly ash. The activity index can be increased from 63~63% before compounding to more than 85% at 360d. At the same time, the rapid hydration of the glass phase on the surface of the shell-core structure semi-calcined dolomite powder can also improve the activity index in the early stage of hydration to a certain extent. Compared with Comparative Examples 1~4, the 3d activity index of Examples 1~5 is increased by 5%~14%.
[0067] Table 2 Activity index test results of various embodiments and comparative examples
[0068]
[0069] The test results of the restricted expansion rate of each embodiment and comparative example are shown in Table 3. For Examples 1 to 5, a semi-calcined dolomite powder with a core-shell structure is prepared by adding low-melting point glass during the calcination process. The glass phase coated on its surface can effectively inhibit the hydration expansion of magnesium oxide before 3 days, delaying the expansion effect to 3 days to 7 days, and the delayed effect is stronger as the dosage increases. The results show that at a glass powder compounding ratio of 5 to 15%, the contribution rate of the restricted expansion rate of 3 to 7 days accounts for 45 to 57% of the total restricted expansion rate of 28 days. For Comparative Examples 1 and 2, which have only been calcined but have not formed a core-shell structure, the expansion efficiency of magnesium oxide has been fully exerted before 3 days, and most of it is wasted in the plastic stage and cannot produce an expansion effect. Therefore, after the restricted expansion rate reaches the maximum at 3 days, it gradually decreases with the extension of age.
[0070] Table 3 Test results of the limited expansion ratio of each embodiment and comparative example
[0071]
[0072] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a dolomite-based composite mineral admixture, characterized in that: The following steps are involved: S1. Mechanically crush and grind natural dolomite to obtain a specific surface area of 450~600 m 2 / kg of dolomite powder; S2, mixing dolomite powder and low-melting-point glass powder into a raw material in a weight ratio of 95:5-85:15, calcining at 650-750° C. for 0.5-2 h, cooling naturally in air, and grinding to obtain semi-calcined dolomite powder with a shell-core structure and a glass phase coated on the surface; S3, mixing the shell-core structure semi-calcined dolomite powder and the high-alumina active admixture in a ratio of 70:30 to 80:20 to obtain a finished dolomite-based composite mineral admixture; The low melting point glass powder is a mixture of one or more of phosphate series and borate series, with a total content of calcium oxide and bismuth oxide ≥ 20%, a softening temperature ≤ 600°C, a crystallization temperature ≥ 750°C, and a maximum particle size ≤ 45 μm.
2. The preparation method according to claim 1, characterized in that: The total content of calcium carbonate and magnesium carbonate in the dolomite is ≥90%, and the content of magnesium carbonate is ≥30%.
3. The preparation method according to claim 1, characterized in that: The shell-core structure semi-calcined dolomite powder has a 45 μm sieve residue fineness of ≤5.0%, a magnesium oxide content of ≥15%, and a free calcium oxide content of ≤1.0%.
4. The preparation method according to claim 1, characterized in that: The high-alumina active admixture is one or more of metakaolin, calcined bauxite, natural volcanic ash material, fly ash, and slag powder, and the alumina content is ≥20%.
5. A dolomite-based composite mineral admixture, characterized in that: The method is prepared by any one of claims 1 to 4.