Preparation method and application of super-hydrophobic gray zinc-aluminum-magnesium coated steel plate
Through the hydrothermal steam method and organic silicon molecular self-assembly technology, the problem of gray coloration and super-hydrophobicity on the surface of zinc-aluminum-magnesium coated steel plates has been solved, achieving environmentally friendly, low-cost, self-cleaning effects, simplifying the process and reducing environmental pollution. Suitable for high-end consumer market.
Patent Information
- Application Number
- CN202410731337.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-09-24
AI Technical Summary
When trying to prepare a gray surface on existing zinc-aluminum-magnesium alloy-coated steel plates, the coating process is complex and costly. The electroplating process consumes a lot of energy and causes serious environmental pollution. The surface is easy to pollute, difficult to clean, and has a short aesthetic life. At the same time, existing superhydrophobic materials using fluoropolymers pose environmental health risks, are expensive, and have poor heat resistance.
The hydrothermal steam method is used to prepare a gray oxide film layer on the surface of the zinc-aluminum-magnesium coated steel plate, and the self-assembly process of organic silicon molecules is used to obtain a super-hydrophobic gray coated steel plate. This simplifies the process, avoids the use of toxic chemical reagents, and achieves environmentally friendly and low-cost self-assembly. Cleaning effect.
It achieves uniform coloring, durability and super-hydrophobic self-cleaning on the surface of zinc-aluminum-magnesium coated steel sheets, simplifies the process, reduces production costs, reduces environmental pollution, and is suitable for high-end home appliances, automobiles and construction fields.
Smart Images

Figure CN118685772A
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zinc-aluminum-magnesium coated steel plates, and specifically relates to a preparation method and application of a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate. Background Art
[0002] Hot-dip galvanized aluminum-magnesium alloy coated steel plates are widely used in home appliances, automobiles, and construction fields due to their excellent corrosion resistance, self-healing properties after cutting, and good processing formability. The current user market tends to be younger, and consumer products tend to have more personalized aesthetic needs. Hot-dip galvanized aluminum-magnesium alloy coated steel plates present a single silver-white color, and their aesthetics are relatively poor. This problem limits their development. Gray symbolizes texture and high-end in the fashion field. The development of a gray series of steel plates can significantly expand the application prospects of coated steel plates in the high-end consumer market. At present, gray steel plates are often prepared by processes such as coating and electroplating. The utility model patent CN211334934U provides a method for preparing a twilight gray series PCM composite steel plate, which is prepared by compounding a polyurethane primer layer, a twilight gray polyester resin layer on a galvanized substrate, and compounding an acrylic adhesive layer and a PE layer on the twilight gray polyester resin layer to obtain a twilight gray composite steel plate. Invention patent CN 116641108A discloses a fingerprint-resistant porous gray composite coating, which is prepared by electroplating a copper layer, a nickel layer, and a porous gray layer on a substrate in sequence, and then immersing in dimethyl silicone oil for 30 seconds and calcining at 300°C for 30 minutes. Although the steel plate prepared in this way meets the user market's demand for color decoration, it still has the following shortcomings: the gray steel plate prepared based on the coating coating process, because the surface of the zinc-aluminum-magnesium alloy coated steel plate presents a bright metallic luster of silver-white, has strong reflectivity, and needs to be brushed with a thick coating for multiple times to mask the metal base color, there are problems such as complex process control, high overall coating cost, and a large amount of carcinogenic organic solvent volatilization; the gray coated steel plate prepared based on the electroplating process needs to be repeatedly electroplated, the electroplating formula is complex, and many types of chemical agents are required. The process is energy-consuming and costly, and the electroplating waste liquid is harmful to the environment and difficult to recycle. In addition, the surface of common gray steel plates is a high-energy surface that is easily contaminated by dust and oil droplets. Once contaminated, it is difficult to clean, which shortens its service life.
[0003] Superhydrophobic materials have attracted wide attention in self-cleaning applications due to their extraordinary hydrophobic ability on the surface. However, in the prior art, fluorinated polymers are often used to modify the surface of materials to be superhydrophobic. These fluorinated polymers are expensive, have poor heat resistance, and are often toxic, which can easily cause serious environmental health risks during production and use. Therefore, the research and development of an environmentally friendly, low-cost, self-cleaning superhydrophobic gray aluminum-magnesium coated steel plate for use in the fields of home appliances, automobiles, and construction has become an important topic that needs to be studied urgently. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate and its application. The present invention adopts a hydrothermal steam method, without complex chemical reagents, and uses water as the only reaction solvent to prepare a gray oxide film on the surface of the zinc-aluminum-magnesium coated steel plate, and then a super-hydrophobic gray coated steel plate can be obtained by a simple organic silicon molecule self-assembly process, thereby improving the comprehensive performance of the coated steel plate surface, improving the universality of the coated steel plate surface coloring process, and expanding the function of the zinc-aluminum-magnesium coated steel plate surface, which has good application prospects.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] The present invention provides a method for preparing a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate, comprising the following steps:
[0007] (1) grinding the surface of the zinc-aluminum-magnesium coated steel plate with sandpaper of different mesh sizes in turn to remove the surface oxide film, and then degreasing, cleaning and drying the surface of the zinc-aluminum-magnesium coated steel plate with an alkaline degreasing solution;
[0008] (2) adding a certain amount of deionized water into a polytetrafluoroethylene reactor, suspending the zinc-aluminum-magnesium coated steel plate pretreated in step (1) above the reactor, performing a hydrothermal reaction at 100-160° C., washing with water, and drying to obtain a gray zinc-aluminum-magnesium coated steel plate sample;
[0009] (3) Immersing the zinc-aluminum-magnesium coated steel plate sample obtained in step (2) in a siloxane solution, and obtaining a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate after curing.
[0010] Based on the above technical solution, further, the zinc-aluminum-magnesium coating composition of the zinc-aluminum-magnesium coated steel plate described in step (1) is Al: 6-12%, Mg: 2-4%, and the rest is Zn and unavoidable impurities.
[0011] Based on the above technical solution, further, in step (1), the surface of the zinc-aluminum-magnesium coated steel plate is polished with 800#, 1500#, and 3000# sandpaper in sequence until the alloy surface is bright and has no obvious scratches. The purpose of polishing the coating surface is to remove the surface oxide film and reduce the roughness to obtain a smoother original surface of the zinc-aluminum-magnesium coating.
[0012] Based on the above technical solution, further, the alkaline degreasing liquid described in step (1) is a mixed aqueous solution of sodium hydroxide and sodium bicarbonate, and based on 100 parts by weight of water, 20-40 parts by weight of sodium bicarbonate and 1-5 parts by weight of sodium hydroxide are dissolved in the alkaline degreasing liquid.
[0013] Based on the above technical solution, further, the degreasing treatment in step (1) is specifically to put the zinc-aluminum-magnesium coated steel plate with the surface oxide film removed into an alkaline degreasing solution, and wipe the surface of the zinc-aluminum-magnesium coated steel plate with a cotton cloth at 20-40°C. The degreasing and cleaning of the zinc-aluminum-magnesium coated steel plate is mainly to remove carbonaceous pollutants on the surface of the steel plate, reduce the dissolution of Al to a certain extent, increase the surface wettability, so as to facilitate subsequent surface treatment and improve the surface quality.
[0014] Based on the above technical solution, further, the cleaning described in step (1) is specifically to use anhydrous ethanol and deionized water to repeatedly rinse 3 to 10 times in sequence.
[0015] Based on the above technical solution, further, in step (2), the deionized water occupies 10%-40% of the volume of the hydrothermal reactor, the hydrothermal reaction temperature is 100-130° C., and the hydrothermal reaction time is 12-24 hours.
[0016] Based on the above technical solution, further, the silicone solution in step (3) is a methyl silicone ethanol solution with a concentration of 10-100 mg / mL.
[0017] Based on the above technical solution, further, in step (3), the immersion time is 5-30 minutes, the curing temperature is 150-250° C., and the curing time is 5-30 minutes.
[0018] On the other hand, the present invention also provides a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate, which is prepared by using any of the above-mentioned methods for preparing the super-hydrophobic gray zinc-aluminum-magnesium coated steel plate.
[0019] On the other hand, the present invention also provides the application of the above-mentioned super-hydrophobic gray zinc-aluminum-magnesium coated steel plate in the fields of home appliances, automobiles, and construction.
[0020] Based on the above technical solution, further application in the field of home appliances is the application of super hydrophobic gray zinc-aluminum-magnesium coated steel plate as steel for home appliance panels.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention adopts an environmentally friendly low-temperature hydrothermal steam method to modify the zinc-aluminum-magnesium coated steel plate, and only uses water as a modification solvent to obtain a coated steel plate with a gray appearance, and the surface coloring is uniform, and the color is long-lasting and uniform; after a simple self-assembly treatment of environmentally friendly siloxane, a super-hydrophobic and self-cleaning gray zinc-aluminum-magnesium coated steel plate can be prepared, and the prepared steel plate has super-hydrophobicity and anti-pollution self-cleaning properties.
[0023] 2. The preparation method of the present invention is simple, does not require additives, is free of chromium and other toxic reagents, is environmentally friendly and pollution-free, harmless to the human body, and is easy to mass-automatically produce industrially. It solves the problems of complex chemical composition of the coloring liquid, complex process, volatilization of organic solvents, serious environmental pollution, and easy pollution of the surface of the gray zinc-aluminum-magnesium coated steel plate and short aesthetic life in the existing zinc-aluminum-magnesium steel plate surface coloring process. It can be applied to high-end home appliances, automobiles, and construction materials, and therefore has very significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0025] Figure 1 This is a static contact angle test diagram of the super-hydrophobic gray zinc-aluminum-magnesium coated steel plate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0027] Embodiment 1:
[0028] This embodiment provides a method for preparing a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate, comprising the following steps:
[0029] (1) The hot-dip galvanized aluminum-magnesium coated steel sheet is cut into a sample of 4*5 cm in size, wherein the hot-dip galvanized aluminum-magnesium coated steel sheet has a composition of Al: 11%, Mg: 3%, and the rest is Zn and unavoidable impurities.
[0030] (2) Use 800#, 1500#, and 3000# sandpaper to polish the surface of the sample until the alloy surface is bright and has no obvious scratches.
[0031] (3) Prepare an alkaline degreasing solution based on 100 parts by weight of water, including 3 parts of sodium hydroxide and 30 parts of sodium bicarbonate, and mix them evenly. Place the sample in the alkaline degreasing solution, scrub and degrease with cotton cloth at room temperature for 3 minutes, then repeatedly wash with anhydrous ethanol and deionized water, and blow dry with cold air.
[0032] (4) Weigh 20 ml of deionized water into a 100 ml polytetrafluoroethylene hydrothermal autoclave, hang the dried sample in step (3) in the hydrothermal autoclave, react at 110° C. for 18 h, take out the reacted sample, wash it with deionized water, and dry it with cold air to obtain the gray zinc-aluminum-magnesium coated steel plate sample.
[0033] (5) A methylsiloxane ethanol solution was prepared with a concentration of 50 mg / mL, and the gray coated steel plate sample was immersed in the methylsiloxane ethanol solution for 10 minutes, and then placed in a 200°C oven for curing for 10 minutes to obtain a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate.
[0034] The results are as follows Figure 1 As shown, the surface water contact angle of the zinc-aluminum-magnesium coated steel plate prepared in this embodiment is 155.3°, which is super hydrophobic. The modified coated steel plate appears gray in macroscopic view, and the blackness value L*<50.
[0035] Example 2
[0036] Different from Example 1, the hydrothermal temperature in step (3) of this embodiment is 120° C. and the reaction time is 18 h.
[0037] Comparative Example 1
[0038] Different from Example 1, in step (2) of this comparative example, the coating surface is not ground or polished, and the process directly proceeds to step (3).
[0039] Comparative Example 2
[0040] Different from Example 1, in this comparative example, step (2) does not involve grinding and polishing the coating surface, and step (3) does not involve degreasing and cleaning the sample, and the process directly starts from step (4).
[0041] Table 1 is the test results of the surface blackness value of the samples prepared in Examples 1-2 and Comparative Examples 1-2
[0042] serial number L* a* b* Example 1 49.04 -1.42 0.28 Example 2 48.18 -1.6 0.08 Comparative Example 1 65.69 -0.78 1.68 Comparative Example 2 59.13 -0.78 0.46
[0043] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate, characterized in that: The following steps are involved: (1) grinding the surface of the zinc-aluminum-magnesium coated steel plate with sandpaper of different mesh sizes in turn to remove the surface oxide film, and then degreasing, cleaning and drying the surface of the zinc-aluminum-magnesium coated steel plate with an alkaline degreasing solution; (2) adding a certain amount of deionized water into a reaction kettle, suspending the zinc-aluminum-magnesium coated steel plate pretreated in step (1) above the reaction kettle, performing a hydrothermal reaction at 100-160° C., washing with water, and drying to obtain a gray zinc-aluminum-magnesium coated steel plate sample; (3) Immersing the zinc-aluminum-magnesium coated steel plate sample obtained in step (2) in a siloxane solution, and obtaining a super-hydrophobic gray zinc-aluminum-magnesium coated steel plate after curing.
2. The preparation method according to claim 1, characterized in that: The zinc-aluminum-magnesium coating composition of the zinc-aluminum-magnesium coated steel plate in step (1) is Al: 6-12%, Mg: 2-4%, and the rest is Zn and unavoidable impurities.
3. The preparation method according to claim 1, characterized in that: In step (1), the surface of the zinc-aluminum-magnesium coated steel plate is polished with 800#, 1500# and 3000# sandpaper in sequence until the alloy surface is bright and has no obvious scratches; the alkaline degreasing solution is a mixed aqueous solution of sodium hydroxide and sodium bicarbonate, and based on 100 parts by weight of water, 20-40 parts by weight of sodium bicarbonate and 1-5 parts by weight of sodium hydroxide are dissolved in the alkaline degreasing solution; the degreasing treatment is specifically to put the zinc-aluminum-magnesium coated steel plate with the surface oxide film removed into the alkaline degreasing solution, and wipe the surface of the zinc-aluminum-magnesium coated steel plate with cotton cloth at 20-40°C.
4. The preparation method according to claim 1, characterized in that: The cleaning described in step (1) is specifically to rinse with anhydrous ethanol and deionized water repeatedly for 3 to 10 times.
5. The preparation method according to claim 1, characterized in that: In step (2), the volume of the hydrothermal reactor is 10%-40% of deionized water, the hydrothermal reaction temperature is 100-130° C., and the hydrothermal reaction time is 12-24 hours.
6. The preparation method according to claim 1, characterized in that: The siloxane solution in step (3) is a methylsiloxane ethanol solution with a concentration of 10-100 mg / mL.
7. The preparation method according to claim 1, characterized in that: In step (3), the soaking time is 5-30 minutes, the curing temperature is 150-250° C., and the curing time is 5-30 minutes.
8. A super hydrophobic gray zinc-aluminum-magnesium coated steel plate, characterized in that: The super-hydrophobic gray zinc-aluminum-magnesium coated steel plate is prepared by the preparation method of any one of claims 1 to 7.
9. Application of the super-hydrophobic gray zinc-aluminum-magnesium coated steel sheet according to claim 8 in the fields of home appliances, automobiles and construction.
10. The use according to claim 9, characterized in that: The application in the home appliance field is the use of super-hydrophobic gray zinc-aluminum-magnesium coated steel plates as steel for home appliance panels.
Citation Information
Patent Citations
Method for preparing superhydrophobic surface
CN102632031A
Method for producing black-plated steel sheet, and method for producing molded article of black-plated steel sheet
CN104246014A
Method for producing black-plated steel sheet, and method for producing molded article of black-plated steel sheet
CN104271801A
Method for manufacturing black plated steel sheet, apparatus for manufacturing black plated steel sheet, and system for manufacturing black plated steel sheet
CN108699666A
HIGH-STRENGTH Zn-Al-Mg-BASED SURFACE-COATED STEEL SHEET AND METHOD FOR PRODUCING SAME
CN110678571A