A permeability testing device and testing method for non-metallic pipelines for pure hydrogen transportation
By designing a test device for sealing shells and gas chromatographs, the hydrogen concentration of non-metallic pipelines is detected in real time, and the problem of difficulty in comprehensively detecting local permeability in the prior art is solved, and accurate permeability detection of various parts of non-metallic pipelines is achieved. Improves safety and detection efficiency.
Patent Information
- Application Number
- CN202411163395.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The prior art is difficult to comprehensively detect the local permeability of non-metallic pipelines, which makes possible safety hazards difficult to eliminate and the detection is not accurate enough.
A test device including a sealing shell, a gas chromatograph and a hydrogen-filling pipeline was designed. The non-metallic pipeline sample was clamped through the sealing shell, and the gas chromatograph detected the hydrogen concentration in the sealing chamber in real time, and calculated the hydrogen permeation of each section to be tested. improve detection accuracy.
The permeability detection of each part of the non-metal pipeline is achieved, which improves the accuracy of the detection, can accurately calculate the permeability of each section, reduces the risk of local permeability not meeting the standards, and the design of the shell improves installation convenience and Substitutability reduces the cost of testing.
Smart Images

Figure CN118688069B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-metallic pipeline penetration detection, in particular to a permeability testing device and a testing method for a non-metallic pipeline for pure hydrogen transportation. Background Art
[0002] In the process of hydrogen transportation, in order to avoid the risk of leakage caused by corrosion of metal pipelines, non-metallic pipelines with higher corrosion resistance are mostly used for transportation at this stage. In addition to high corrosion resistance, non-metallic pipelines also have advantages such as earthquake resistance, good flexibility, and long life. Therefore, non-metallic pipelines are widely used in the field of hydrogen transportation.
[0003] However, since hydrogen molecules are small and diffuse quickly, non-metallic pipelines face a greater risk of penetration when transporting hydrogen. And since hydrogen has low ignition energy and is flammable and explosive, this will cause a large amount of leaked hydrogen to accumulate in a limited space, which in turn poses a great safety hazard. Therefore, hydrogen penetration testing is required for existing or newly built non-metallic pipelines to ensure safe use.
[0004] Patent CN114813452B discloses a non-metallic pipe hydrogen permeability test device and method. In the non-metallic pipe hydrogen permeability test device proposed in the patent, the annular reinforcement of the tested tube of the tested tube is reinforced, and the axial reinforcement of the tested tube of the tested tube is reinforced. Therefore, a hydrogen pressure far higher than its pressure strength can be applied to the pipe during the test, and the amount of hydrogen that penetrates into the sealed test chamber per unit time is significantly increased. Therefore, the pressure sensor can measure a significant change in hydrogen pressure in a relatively short time, thereby improving the test efficiency. In the actual detection process, while the entire pipeline is subjected to a permeability test, it is also necessary to detect a part of the pipeline to avoid the situation where the local permeability is greater than the set standard. However, the above-mentioned prior art is mainly used to detect the entire pipeline, so it is difficult to detect the local pipeline, which leads to incomplete detection and inability to comprehensively eliminate possible safety hazards. Summary of the invention
[0005] In order to avoid and overcome the technical problems existing in the prior art, the present invention provides a permeability testing device and a testing method for a non-metallic pipeline for pure hydrogen transportation. The present invention can perform permeability testing on each part of the non-metallic pipeline separately, thereby improving the accuracy of the testing.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A permeability testing device for a non-metallic pipeline for pure hydrogen transportation comprises a non-metallic pipeline sample as a test object and sealed at both ends, a hydrogen filling pipeline for filling hydrogen into the tube cavity of the non-metallic pipeline sample, a sealed cavity sealed and coated on the outside of the non-metallic pipeline sample to be tested, a gas chromatograph for detecting the concentration of hydrogen leaked in the sealed cavity from the non-metallic pipeline sample to be tested, and an environmental box for sealing and storing the non-metallic pipeline sample.
[0008] As a further solution of the present invention: it includes a hollow sealing shell, and a positioning hole is opened on the sealing shell through its shell cavity; the non-metallic pipeline sample is coaxially sealed and penetrated in the positioning hole, and the section of the non-metallic pipeline sample to be tested is located in the shell cavity of the sealing shell, and the shell cavity of the sealing shell constitutes the sealing cavity.
[0009] As a further solution of the present invention: the sealing shell includes two shells with the same structure, and a groove with sealed ends is formed on the shell, and positioning grooves are recessed on the two sealed ends of the groove; the two shells are sealed together, and the corresponding positioning grooves cooperate to form the positioning hole, and the two grooves cooperate to form the sealing cavity.
[0010] As a further solution of the present invention: both sides of the groove on the shell extend outward to form folded edges, and a plurality of locking holes are opened on the folded edges; sealing gaskets are arranged at the joints of the two shells arranged up and down, and at the joints between the positioning groove and the non-metallic pipe sample, and bolts and nuts passing through the two locking holes aligned up and down form a threaded fit to seal and fix the two shells to each other.
[0011] As a further solution of the present invention: the gas chromatograph is communicated with the groove of the shell located at the lower side in the sealed shell through the gas guide tube.
[0012] As a further solution of the present invention: the hydrogen filling pipeline includes a hydrogen source for providing hydrogen, which is arranged in sequence along the gas supply direction, a hydrogen compressor for compressing the hydrogen provided by the hydrogen source, a high-pressure buffer tank for storing the hydrogen compressed by the hydrogen compressor, a flow solenoid valve for controlling the gas supply flow of the high-pressure buffer tank, a pressure transmitter for detecting and controlling the pressure of the hydrogen filled in the non-metallic pipe sample, a flow meter for measuring the total amount of hydrogen filled in the non-metallic pipe sample, and a pressure relief valve installed at the other end of the non-metallic pipe sample.
[0013] As a further solution of the present invention: the environmental chamber includes a chamber body and a chamber cover which can be sealed on the chamber body; the shell located on the lower side of the sealed shell is installed on the inner bottom surface of the chamber body; the hydrogen filling pipeline is located on the outside of the environmental chamber, and the flow meter and the non-metallic pipeline sample are connected to each other through an air pipe passing through the chamber wall of the environmental chamber, and the penetration point between the air pipe and the chamber wall is in a sealed state.
[0014] The test method uses the above-mentioned non-metallic pipeline permeability test device for pure hydrogen transportation, and is characterized in that the test method comprises the following steps:
[0015] S1. Place the non-metallic pipeline sample on the shell at the lower side, place the shell at the upper side on the side, and keep the environmental box open; at the same time, connect the non-metallic pipeline sample to the hydrogen filling pipeline; then open the pressure relief valve, and fill the non-metallic pipeline sample with hydrogen for a set number of times through the hydrogen filling pipeline until the hydrogen purity at each position inside the non-metallic pipeline sample reaches the set value, and then close the pressure relief valve;
[0016] S2. Evenly charge the non-metallic pipe sample with hydrogen through the hydrogen charging pipeline, and observe the hydrogen pressure in the non-metallic pipe sample through the pressure transmitter until the hydrogen pressure in the non-metallic pipe sample reaches and remains stable at the set pressure value; then check whether there is leakage at the connection between the non-metallic pipe sample and the hydrogen charging pipeline, the seals at both ends of the non-metallic pipe sample, and the connection inside the hydrogen charging pipeline; if there is leakage, find the specific location and repair it; otherwise, the test device has no leakage and meets the sealing requirements;
[0017] S3. After the leak detection is completed, use nitrogen to clean the hydrogen in the environmental box and the shell to make the inside of the environmental box in a hydrogen-free state; then, the other shell is sealed on the lower shell through the matching sealing cover of bolts and nuts, and the section to be tested of the non-metallic pipe sample is located in the sealed cavity; then, the box cover is closed to make the environmental box in a sealed state; the sealed environmental box is evacuated, and then nitrogen is filled into the environmental box to normal pressure;
[0018] S4, placing the environmental box in a normal pressure state at a set temperature and keeping it warm for a set time, then filling the non-metallic pipe sample with hydrogen through the hydrogen filling pipeline, and maintaining the hydrogen pressure in the non-metallic pipe sample at the set pressure value;
[0019] S5. Turn on the gas chromatograph, detect the hydrogen concentration in the sealed cavity in real time through the gas chromatograph, and calculate the change of the hydrogen concentration in real time;
[0020] S6. Linearly fit the data detected by the gas chromatograph to obtain a hydrogen concentration change curve. When the slope change amplitude of the hydrogen concentration change curve is within the set amplitude range, it is considered that the non-metallic pipeline sample has reached a stable permeation state; otherwise, the detection is repeated according to the contents of step S1 to step S5 until the non-metallic pipeline sample reaches a stable permeation state;
[0021] S7. Detect non-metallic pipe samples that have reached a stable penetration state in the time period t The real-time hydrogen concentration within the time period is calculated tThe average value of hydrogen concentration in the environmental chamber is calculated; then, the hydrogen permeability of the non-metallic pipe sample is calculated in combination with the temperature detected by the temperature sensor inside the environmental chamber. The calculation formula is as follows: ;
[0022] In the formula, Le Indicates the hydrogen permeability of non-metallic pipe specimens; Indicates that the non-metallic pipe sample reaches the stable state of penetration in the time period t The average hydrogen concentration in V 1 represents the volume of the sealed chamber; V 2 represents the volume of the non-metallic pipe sample; T Indicates the temperature inside the environmental chamber.
[0023] As a further solution of the present invention: the set pressure values in step S2 and step S4 are both 1.25 times the rated pressure of the non-metallic pipeline; in step S2, hydrogen is uniformly charged into the non-metallic pipeline sample through the hydrogen charging pipeline, and the hydrogen charging speed is 1MPa / min; in step S4, after the environmental box is kept at the set temperature, the temperature in the environmental box is T That is the set temperature, and the set temperature range is [-40℃,55℃].
[0024] As a further solution of the present invention: the insulation time in step S4 is set to 24 hours.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention sets a sealed cavity on the outside of the non-metallic pipe section to be detected to collect the hydrogen that permeates therefrom, detects the hydrogen concentration in the sealed cavity by a gas chromatograph, and calculates the permeation of the section to be detected based on time. Each section to be detected can be detected in sequence according to a certain order; or a sealed cavity can be set on the outside of each section to be detected and detected at the same time. It can be seen that the present invention can detect each section of the non-metallic pipe to more accurately calculate the permeability of each section, improve the accuracy of the detection, and avoid the risk of the local permeability of the non-metallic pipe not meeting the standard.
[0027] 2. The present invention adopts a method of two shells cooperating with each other to clamp the non-metallic pipe sample, so as to form a corresponding sealed cavity. On the one hand, the convenience and stability of installation can be improved by clamping up and down; on the other hand, when one of the shells is damaged, it can be replaced separately to reduce the cost of the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the overall structure of the present invention.
[0029] Figure 2It is a schematic diagram of the structure of the shell in the present invention.
[0030] Figure 3 It is a structural schematic diagram of the sealing shell in the present invention.
[0031] In the figure: 1. Environmental chamber; 11. Box body; 12. Box cover; 2. Non-metallic pipe sample; 3. Sealing shell; 31. Sealing cavity; 32. Shell; 321. Groove; 322. Positioning groove; 323. Folding edge; 324. Locking hole; 33. Positioning hole; 4. Gas chromatograph; 41. Air guide tube; 5. Hydrogen filling pipeline; 51. Hydrogen source; 52. Hydrogen compressor; 53. High-pressure buffer tank; 54. Flow solenoid valve; 55. Pressure transmitter; 56. Flow meter; 57. Pressure relief valve; 58. Sealing plug; 6. Base. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] See also Figure 1 to Figure 3 In an embodiment of the present invention, a permeability testing device for a non-metallic pipeline for pure hydrogen transportation includes a non-metallic pipeline sample 2 as a test object and sealed at both ends, a hydrogen filling pipeline 5 for filling hydrogen into the tube cavity of the non-metallic pipeline sample 2, a sealed cavity 31 sealed and coated on the outside of the to-be-tested section of the non-metallic pipeline sample 2, a gas chromatograph 4 for detecting the concentration of hydrogen leaked in the sealed cavity 31 from the to-be-tested section of the non-metallic pipeline sample 2, and an environmental box 1 for sealingly storing the non-metallic pipeline sample 2.
[0034] The cylindrical non-metallic pipe sample 2 has an appropriate length, and multiple sections to be tested can be planned on it and tested in sequence. The rated pressure of the non-metallic pipe used in the present invention is 5MPa. When sealing the two ends of the non-metallic pipe sample 2, a sealing plug 58 of a suitable size can be used to plug the two end ports of the non-metallic pipe sample 2. At the same time, the corresponding air pipe interface and pressure relief valve 57 need to be installed on the sealing plug 58 to facilitate the charging and discharging of hydrogen. The two-port sealing method of the pipeline commonly used in the prior art can also be used, which can achieve sealing while also being able to charge and discharge gas.
[0035] The environmental chamber 1 comprises a chamber body 11 and a chamber cover 12 which can be sealed on the chamber body 11. One side of the chamber cover 12 is hinged on the chamber body 11. When sealing is required, the chamber cover 12 is closed and locked with a conventional lock to put the environmental chamber 1 in a sealed state.
[0036] The sealing shell 3 includes two shells 32 of the same structure. A groove 321 with sealed ends is formed on the shell 32. A positioning groove 322 is recessed on both sealed ends of the groove 321. The cross-sections of the positioning groove 322 and the groove 321 are both semicircular and coaxially arranged. Both sides of the shell 32 located at the groove 321 extend outward to form a folded edge 323, and a plurality of locking holes 324 are opened on the folded edge 323. When in use, firstly, a shell 32 is fixedly installed on the inner bottom surface of the environmental chamber 1 through the base 6, and then the non-metallic pipe sample 2 is coaxially placed in the positioning groove 322, and the section to be tested is located above the groove 321. Then, another shell 32 for use in conjunction is covered on the shell 32 on the lower side. At the same time, sealing gaskets need to be arranged at the joints of the two shells 32 arranged up and down, and at the joints between the positioning groove 322 and the non-metallic pipe sample 2. Finally, the two shells 32 are fixed together using bolts and nuts, and the two grooves 321 cooperate to form the corresponding sealing cavity 31, and the corresponding positioning grooves 322 cooperate to form the positioning hole 33.
[0037] The gas chromatograph 4 is connected to the groove 321 of the shell 32 located on the lower side of the sealed shell 3 through the air duct 41. The air duct 41 passes through the through hole on the wall of the environmental box 1 and is sealed to the through hole to avoid leakage when the environmental box 1 is evacuated.
[0038] The hydrogen filling pipeline 5 includes a hydrogen source 51 for providing hydrogen, a hydrogen compressor 52 for compressing the hydrogen provided by the hydrogen source 51, a high-pressure buffer tank 53 for storing the hydrogen compressed by the hydrogen compressor 52, a flow solenoid valve 54 for controlling the gas supply flow of the high-pressure buffer tank 53, a pressure transmitter 55 for detecting and controlling the pressure of the hydrogen filled in the non-metallic pipeline sample 2, a flow meter 56 for measuring the total amount of hydrogen filled in the non-metallic pipeline sample 2, and a pressure relief valve 57 installed at the other end of the non-metallic pipeline sample 2. A hydrogen storage bottle is usually used as the hydrogen source 51.
[0039] The present invention adopts the following test method to perform permeability test on each section to be tested on the non-metallic pipe sample 2.
[0040] The test method includes the following steps:
[0041] S1. Place the non-metallic pipe sample 2 on the lower shell 32, place the upper shell 32 on the side, and keep the environmental box 1 open. At the same time, connect the non-metallic pipe sample 2 to the hydrogen filling pipeline 5, then open the pressure relief valve 57, and intermittently perform hydrogen filling three times on the non-metallic pipe sample 2 through the hydrogen filling pipeline 5 until the hydrogen purity at each position inside the non-metallic pipe sample 2 reaches the set value, and then close the pressure relief valve 57; through the three hydrogen fillings, the air in the non-metallic pipe sample 2 can be effectively removed to ensure that the hydrogen purity inside the non-metallic pipe sample 2 is maintained at an appropriate level.
[0042] S2. The non-metallic pipe sample 2 is uniformly charged with hydrogen through the hydrogen charging pipeline 5, and the speed of hydrogen charging is 1MPa / min. The hydrogen pressure in the non-metallic pipe sample 2 is observed in real time through the pressure transmitter 55 until the hydrogen pressure in the non-metallic pipe sample 2 reaches and remains stable at 1.25 times the rated pressure of the non-metallic pipe, that is, 6.25MPa. Then check whether there is leakage at the connection between the non-metallic pipe sample 2 and the hydrogen charging pipeline 5, the seals at both ends of the non-metallic pipe sample 2, and the connection inside the hydrogen charging pipeline 5. If there is a leak, find the specific location and repair it; otherwise, the test device has no leakage and meets the sealing requirements.
[0043] S3. After the leak detection is completed, nitrogen is used to clean the hydrogen inside the environmental box 1 and the shell 32 to make the inside of the environmental box 1 in a hydrogen-free state, thereby reducing the interference of residual hydrogen during the side leakage process and improving the accuracy of the gas chromatograph 4 detection. Then, the other shell 32 is sealed on the lower shell 32 through the matching sealing cover of bolts and nuts, and the section to be tested of the non-metallic pipe sample 2 is located in the sealed cavity 31. Then, the box cover 12 is covered to make the environmental box 1 in a sealed state. The environmental box 1 in a sealed state is evacuated, and then nitrogen is filled into the environmental box 1 to normal pressure.
[0044] S4, placing the environmental box 1 in a normal pressure state at a set temperature and keeping it warm for a set insulation time, then filling hydrogen into the non-metallic pipe sample 2 through the hydrogen filling pipeline 5, and maintaining the hydrogen pressure in the non-metallic pipe sample 2 at a set pressure value. The set temperature range is [-40°C, 55°C], the set temperature in this embodiment is 18°C, and the set insulation time is 24 hours.
[0045] S5. Turn on the gas chromatograph 4, detect the hydrogen concentration in the sealed cavity 31 in real time through the gas chromatograph 4, and calculate the change of the hydrogen concentration in real time.
[0046] S6. Linear fitting is performed on the data detected by the gas chromatograph 4 to obtain a hydrogen concentration change curve. When the slope change amplitude of the hydrogen concentration change curve is within the set amplitude range, it is considered that the non-metallic pipe sample 2 has reached a stable permeation state, that is, when the hydrogen concentration inside the sealed cavity 31 is in a uniform change, it means that the non-metallic pipe sample 2 is uniformly permeating. Otherwise, the detection is repeated according to the contents of step S1 to step S5 until the non-metallic pipe sample 2 reaches a stable permeation state.
[0047] S7. Detect the non-metallic pipe sample 2 that has reached the stable state of penetration in the time period t The real-time hydrogen concentration within the time period is calculated t The average value of hydrogen concentration in the chamber 1 is calculated; then, the hydrogen permeability of the non-metallic pipe sample 2 is calculated in combination with the temperature detected by the temperature sensor inside the environmental chamber 1. The data of one of the tests is as follows: The volume of the sealed chamber 31 V 1 is 11437.8L, the temperature in environmental chamber 1 T At 18°C, the volume of non-metallic pipe sample 2 V 2 is 45L, and the average hydrogen concentration of the sealed chamber 31 measured by the gas chromatograph 4 within 0.25h is 1.355ppm. Then the hydrogen permeability of the current section to be tested of the non-metallic pipe sample 2 within 0.25h is calculated as follows:
[0048] ;
[0049] It can be seen that the hydrogen permeability of the current section to be tested of non-metallic pipe sample 2 within 0.25h is .
[0050] By adopting the above steps, the hydrogen permeability of each section to be tested can be calculated.
[0051] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for testing the permeability of a non-metallic pipeline for pure hydrogen transportation, characterized in that: The following steps are involved: S1. Place the non-metallic pipeline sample (2) on the shell (32) located at the lower side of the permeability test device, place the shell (32) located at the upper side on the side, and keep the environmental chamber (1) open; at the same time, connect the non-metallic pipeline sample (2) to the hydrogen filling pipeline (5); then open the pressure relief valve (57), and fill the non-metallic pipeline sample (2) with hydrogen for a set number of times through the hydrogen filling pipeline (5), until the hydrogen purity at each position inside the non-metallic pipeline sample (2) reaches the set value, and then close the pressure relief valve (57); S2. The non-metallic pipe sample (2) is uniformly charged with hydrogen through the hydrogen charging pipeline (5), and the hydrogen pressure in the non-metallic pipe sample (2) is observed through the pressure transmitter (55) until the hydrogen pressure in the non-metallic pipe sample (2) reaches and remains stable at a set pressure value, wherein the set pressure value is 1.25 times the rated pressure of the non-metallic pipe; then, the connection between the non-metallic pipe sample (2) and the hydrogen charging pipeline (5), the sealing parts at both ends of the non-metallic pipe sample (2), and the connection inside the hydrogen charging pipeline (5) are checked for leaks; if there is a leak, the specific location is found and repaired; otherwise, the test device is leak-free and meets the sealing requirements; S3. After the leak detection is completed, nitrogen is used to purge the hydrogen inside the environmental box (1) and the shell (32) so that the interior of the environmental box (1) is in a hydrogen-free state; then the other shell (32) is sealed on the lower shell (32) by means of bolts and nuts, and the section to be tested of the non-metallic pipe sample (2) is located in the sealed cavity (31); then the box cover (12) is closed so that the environmental box (1) is in a sealed state; the sealed environmental box (1) is evacuated, and then nitrogen is filled into the environmental box (1) to normal pressure; S4, placing the environmental box (1) in a normal pressure state at a set temperature and maintaining the temperature for a set time, then filling the non-metallic pipe sample (2) with hydrogen through the hydrogen filling pipeline (5), and maintaining the hydrogen pressure in the non-metallic pipe sample (2) at a set pressure value, which is 1.25 times the rated pressure of the non-metallic pipe; S5, turning on the gas chromatograph (4), detecting the hydrogen concentration in the sealed chamber (31) in real time through the gas chromatograph (4), and calculating the change of the hydrogen concentration in real time; S6. Performing linear fitting on the data detected by the gas chromatograph (4) to obtain a hydrogen concentration change curve. When the slope change amplitude of the hydrogen concentration change curve is within a set amplitude range, it is considered that the non-metallic pipe sample (2) has reached a stable permeation state. Otherwise, repeating the detection according to the contents of steps S1 to S5 until the non-metallic pipe sample (2) has reached a stable permeation state. S7. Detect non-metallic pipe samples that have reached a stable permeability state (2) in the time period t The real-time hydrogen concentration within the time period is calculated t The average value of the hydrogen concentration inside the environmental chamber (1) is calculated; then, the hydrogen permeability of the non-metallic pipe sample (2) is calculated in combination with the temperature detected by the temperature sensor inside the environmental chamber (1). The calculation formula is as follows: ; In the formula, Le represents the hydrogen permeability of the non-metallic pipe specimen (2); Indicates that the non-metallic pipe specimen (2) has reached a stable state of penetration in the time period t The average hydrogen concentration in V 1 represents the volume of the sealed chamber (31); V 2 represents the volume of the non-metallic pipe specimen (2); T represents the temperature in the environmental chamber (1); The permeability testing device comprises a non-metallic pipe sample (2) as a test object and sealed at both ends, a hydrogen filling pipeline (5) for filling hydrogen into the pipe cavity of the non-metallic pipe sample (2), a sealed cavity (31) sealed around the outside of the test section of the non-metallic pipe sample (2), a gas chromatograph (4) for detecting the concentration of hydrogen leaking from the test section of the non-metallic pipe sample (2) in the sealed cavity (31), and an environmental chamber (1) capable of sealing and storing the non-metallic pipe sample (2); The invention comprises a hollow sealing shell (3), wherein a positioning hole (33) is provided on the sealing shell (3) and penetrates through its shell cavity; the non-metallic pipeline sample (2) is coaxially sealed and penetrated in the positioning hole (33), and the section to be tested of the non-metallic pipeline sample (2) is located in the shell cavity of the sealing shell (3), and the shell cavity of the sealing shell (3) constitutes the sealing cavity (31); The sealing shell (3) comprises two shells (32) of the same structure, a groove (321) with sealed ends at both ends is formed on the shells (32), and positioning grooves (322) are recessed on the two sealed ends of the groove (321); the two shells (32) are sealed together, the corresponding positioning grooves (322) cooperate to form the positioning hole (33), and the two grooves (321) cooperate to form the sealing cavity (31); Both sides of the recess (321) on the shell (32) extend outward to form folded edges (323), and a plurality of locking holes (324) are provided on the folded edges (323); sealing gaskets are arranged at the joints of the two shells (32) arranged up and down, and at the joints between the positioning groove (322) and the non-metallic pipe sample (2); bolts passing through the two locking holes (324) aligned up and down form threaded engagement with nuts, so as to seal and fix the two shells (32) to each other; The gas chromatograph (4) is in communication with the groove (321) of the housing (32) located at the lower side of the sealing shell (3) through the gas guide tube (41); The hydrogen filling pipeline (5) comprises a hydrogen source (51) for providing hydrogen, a hydrogen compressor (52) for compressing the hydrogen provided by the hydrogen source (51), a high-pressure buffer tank (53) for storing the hydrogen compressed by the hydrogen compressor (52), a flow solenoid valve (54) for controlling the flow rate of the gas supply of the high-pressure buffer tank (53), a pressure transmitter (55) for detecting and controlling the pressure of the hydrogen filled into the non-metallic pipeline sample (2), a flow meter (56) for measuring the total amount of hydrogen filled into the non-metallic pipeline sample (2), and a pressure relief valve (57) installed at the other end of the non-metallic pipeline sample (2); The environmental box (1) comprises a box body (11) and a box cover (12) which can be sealed on the box body (11); a shell (32) located at the lower side of the sealing shell (3) is installed on the inner bottom surface of the box body (11); the hydrogen filling pipeline (5) is located outside the environmental box (1), and the flow meter (56) and the non-metallic pipe sample (2) are connected to each other through an air pipe passing through the box wall of the environmental box (1), and the penetration point between the air pipe and the box wall is in a sealed state.
2. The method for testing the permeability of a non-metallic pipeline for pure hydrogen transportation according to claim 1, characterized in that: In step S2, hydrogen is uniformly charged into the non-metallic pipe sample (2) through the hydrogen charging pipeline (5) at a rate of 1 MPa / min. In step S4, after the environmental box (1) is kept at a set temperature, the temperature in the environmental box (1) is T That is the set temperature, and the set temperature range is [-40℃,55℃].
3. The method for testing the permeability of a non-metallic pipeline for pure hydrogen transportation according to claim 2, characterized in that: The set holding time in step S4 is 24 hours.