Scale and corrosion inhibition composition as well as preparation method and water treatment application thereof

Through the combination of modified copolymers and functional additives, a scale and corrosion inhibitor is formed, which solves the problems of narrow application range and difficulty in compounding of scale and corrosion inhibitors in the existing technology, and achieves excellent scale inhibition and mitigation at high temperatures. The corrosion effect reduces the dosage requirement.

CN118724302AActive Publication Date: 2024-10-01SHENZHEN AIKANGQUAN WATER TREATMENT SERVICE CO LTD

Patent Information

Application Number
CN202410823844.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-01
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Existing scale and corrosion inhibitors have a narrow applicable range of temperature and water quality, poor scale inhibition effect, high difficulty in compounding, and large amounts of compounding, making it difficult to effectively prevent corrosion and scaling of boilers and pipes.

Method used

Using modified copolymer, long-chain alkyl alcohol amine, acrylic acid-acrylamide copolymer, metal salt, water-soluble zinc salt and functional additive composition, through the chelation effect of the modified copolymer and the barrier of functional additives Film formation promotes chelate precipitation, avoids contact with corrosive ions, forms a loose scale particle system, prevents the growth of calcium carbonate and magnesium crystals, and improves scale and corrosion inhibition effects.

Benefits of technology

It improves the temperature stability and water quality adaptability of scale and corrosion inhibitors, reduces the dosage requirements, significantly enhances the scale and corrosion inhibition effects at high temperatures, and solves the problems of narrow range and complex formulation of scale and corrosion inhibitors in the existing technology. Difficulty issue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004909863000000141
    Figure BDA0004909863000000141
Patent Text Reader

Abstract

The invention relates to the field of industrial water treatment, in particular to a scale and corrosion inhibition composition as well as a preparation method and water treatment application thereof. The scale and corrosion inhibition composition is prepared from the following raw materials in percentage by mass: 10 to 20 percent of modified copolymer, 5 to 10 percent of long-chain alkyl alcohol amine, 5 to 10 percent of acrylic acid-acrylamide copolymer, 1 to 2 percent of metal salt, 1 to 3 percent of water-soluble zinc salt, 1 to 6 percent of functional additive and the balance of deionized water. The scale and corrosion inhibition composition prepared in the invention not only has excellent scale and corrosion inhibition effects, but also can reduce the requirements of the scale and corrosion inhibition composition on temperature, water quality and dosage, still has excellent scale and corrosion inhibition effects at a relatively high temperature, and has very excellent market use prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of industrial water treatment, and in particular to a scale and corrosion inhibitor composition, a preparation method thereof, and water treatment applications. Background Art

[0002] Industrial circulating water accounts for more than 50% of industrial water. If it is not treated during use, equipment and pipelines will have problems such as corrosion, scaling and microbial slime, which will affect the efficiency and service life of equipment and pipelines. Taking boiler water as an example, boiler steam condensate is high-quality boiler feed water containing thermal energy. Recycling steam condensate is the most effective measure for boiler water and energy saving. If it is recycled and utilized, it can significantly reduce boiler fuel consumption, reduce the amount of softened water, reduce steam production costs, and improve boiler water quality. However, when the pH of condensate is low, corrosion products dissolve and condensate is contaminated by iron ions. When untreated condensate is used as boiler feed water, the large amount of iron ions contained in the water will cause secondary scaling and under-scale corrosion on the boiler heat transfer surface, causing greater harm, making it technically difficult to directly recycle steam condensate.

[0003] On the other hand, even if the recycling of circulating water is further considered during use, the lack of good anti-corrosion and anti-scaling measures for pipelines leads to serious corrosion of pipelines, and deposition and scaling are easily generated. Although the commonly used aeration and filtration measures can reduce the concentration of scaling and corrosive metal ions to a certain extent, they still cannot effectively reduce the probability of corrosion and scaling of pipelines. Therefore, the use of scale inhibitors and corrosion inhibitors has become the most important solution to the above technical problems in the domestic industrial field.

[0004] However, due to their formula, existing scale inhibitors and corrosion inhibitors have high requirements for temperature, water quality, and dosage. In particular, some non-phosphorus scale inhibitors have a narrow range of application for water quality and temperature, and the scale inhibition effect is poor outside the range. They also have problems such as high difficulty in compounding and large compounding dosage. Therefore, in order to solve the above problems, the present application provides a scale inhibitor and corrosion inhibitor composition and a preparation method thereof. The scale inhibitor and corrosion inhibitor composition prepared in the present application not only has excellent scale inhibition and corrosion inhibition effects, but also can reduce the scale inhibitor and corrosion inhibitor slow-release composition requirements for temperature, water quality, and dosage. It still has excellent scale inhibition and corrosion inhibition effects at higher temperatures, and has very excellent market prospects. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present application provides a scale and corrosion inhibition composition, which includes, by mass percentage, 10-20% modified copolymer, 5-10% long-chain alkyl alcohol amine, 5-10% acrylic acid-acrylamide copolymer, 1-2% metal salt, 1-3% water-soluble zinc salt, 1-6% functional additive, and the balance deionized water.

[0006] As a preferred solution, the mass ratio of the modified copolymer, the long-chain alkyl alcohol amine and the acrylic acid-acrylamide copolymer is (15-20): (6-10): (8-10).

[0007] As a preferred solution, the mass ratio of the modified copolymer, the long-chain alkyl alcohol amine and the acrylic acid-acrylamide copolymer is (16-19): (6-8): (9-10).

[0008] As a preferred scheme, the preparation method of the modified copolymer comprises the following steps: S1: adding epoxysuccinic acid to an organic solvent, preheating the temperature to 60-65°C and stirring for 0.5-1h; S2: adding a reaction aid after stirring, and dripping a mixed solution of methacrylic acid and maleic acid into the S1 solution, the dripping temperature is 65-70°C, the dripping reaction time is 0.5-1h, heating to 80-85°C after the dripping is completed, and keeping the temperature for reaction for 2-3h, after the reaction is completed, filtering, washing and drying the product.

[0009] As a preferred solution, the mass ratio of epoxysuccinic acid, reaction aid, methacrylic acid and maleic acid is (10-15): (0.2-0.4): (3-4): (4-5).

[0010] As a preferred solution, the mass ratio of the epoxysuccinic acid, the reaction aid, the methacrylic acid and the maleic acid is (12-14): (0.2-0.3): (3-3.5): (4-4.5).

[0011] As a preferred solution, the reaction aids are potassium persulfate and triethylamine.

[0012] As a preferred solution, the mass ratio of potassium persulfate to triethylamine is (1-1.5):(0.8-1).

[0013] As a preferred solution, the organic solvent is ethyl acetate.

[0014] In the present application, by adding the above-mentioned modified copolymer, the scale inhibition and anti-corrosion functions of the scale inhibition and corrosion inhibition composition can be greatly improved, and it can effectively adapt to the high-temperature action environment of the water system, improve the action stability, and reduce the water quality selection requirements. The modified copolymer can utilize the chelation effect of the carboxylic acid groups of methacrylic acid and maleic acid on its molecular chain with metal ions, greatly improving the generation efficiency of chelates in the water system and promoting the precipitation of chelates; on the other hand, the modified copolymer can also form a barrier film with a certain thickness on the metal surface through the joint action of the functional additives of the present application, and the modified copolymer can produce an effective and uniform adsorption effect on the corrosive ions on the film surface, avoiding the direct contact between the corrosive ions and the metal surface, and can also strengthen the binding effect of polyepoxysuccinic acid on calcium and magnesium ions, thereby forming tiny scale particles in the water droplet phase, and then forming a loose system of tiny scale particles, avoiding their aggregation and structural phenomena on the metal surface, and the loose chelate particles formed by the combination with calcium and magnesium ions can hinder the growth of calcium carbonate and magnesium crystal structures, and cannot form solid particles with a stable form and precipitate, and can enhance the above-mentioned blocking effect at high temperatures, thereby obtaining excellent performance stability at high temperatures.

[0015] As a preferred solution, the long-chain alkyl alcohol amine is at least one of dodecyl alcohol amine, hexadecyl alcohol amine and octadecyl alcohol amine.

[0016] As a preferred solution, the long-chain alkyl alcoholamine is a combination of dodecyl alcoholamine and octadecyl alcoholamine.

[0017] As a preferred solution, the mass ratio of the dodecyl alcoholamine to the octadecyl alcoholamine is (1-1.2):(3-4.5).

[0018] As a preferred solution, the acrylic acid-acrylamide copolymer is acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.

[0019] As a preferred solution, the limiting viscosity of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 0.075 to 0.15 (30°C) / dl·g -1 .

[0020] As a preferred solution, the limiting viscosity of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 0.08 to 0.1 (30°C) / dl·g -1 .

[0021] As a preferred solution, the metal salt is at least one of metal molybdate, metal silicate, metal borate and metal chloride.

[0022] As a preferred solution, the metal salts are sodium silicate and magnesium chloride.

[0023] As a preferred solution, the mass ratio of sodium silicate to magnesium chloride is (3-4): (0.5-1).

[0024] As a preferred solution, the mass ratio of sodium silicate to magnesium chloride is (3-3.5):(0.6-0.8).

[0025] As a preferred solution, the water-soluble zinc salt is at least one of zinc chloride, zinc sulfate, zinc gluconate, zinc acetate and zinc citrate.

[0026] As a preferred solution, the water-soluble zinc salt is a combination of zinc sulfate and zinc gluconate.

[0027] As a preferred solution, the mass ratio of zinc sulfate to zinc gluconate is (2-2.5):(0.8-1).

[0028] As a preferred solution, the functional additive is at least one of a dispersant, a wetting agent, a defoaming agent, a cosolvent, and a stabilizer.

[0029] As a preferred solution, the functional auxiliary agent at least includes a dispersant.

[0030] As a preferred solution, the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether.

[0031] As a preferred solution, the mass ratio of the fatty alcohol polyoxyethylene ether to the block polyether is (2-2.2): (0.5-0.8).

[0032] As a preferred solution, the fatty alcohol polyoxyethylene ether is isomeric 13 fatty alcohol polyoxyethylene ether.

[0033] As a preferred solution, the hydroxyl value of the isomeric 13-fatty alcohol polyoxyethylene ether is 70 to 90 mgKOH / g.

[0034] As a preferred solution, the weight average molecular weight of the block polyether is 1200-5000.

[0035] As a preferred solution, the block polyether is a composition of a block polyether with a weight average molecular weight of 1400-1800 and a block polyether with a weight average molecular weight of 4500-5000.

[0036] As a preferred solution, the mass ratio of the block polyether with a weight average molecular weight of 1400-1800 to the block polyether with a weight average molecular weight of 4500-5000 is (2-3.5):(1-1.8).

[0037] As a preferred solution, the mass ratio of the block polyether with a weight average molecular weight of 1400-1800 to the block polyether with a weight average molecular weight of 4500-5000 is (2.5-3.2):(1.2-1.5).

[0038] In the present application, the addition of the above-mentioned compound dispersant can not only play an excellent role in dispersing the raw materials of the scale inhibitor and corrosion inhibitor, but also can further improve the stability and scale inhibition effect of the scale inhibitor and corrosion inhibitor under high temperature, reduce its requirements for temperature and water quality, and effectively reduce the amount of scale inhibitor and corrosion inhibitor. When the above-mentioned specific fatty alcohol polyoxyethylene ether and block polyether are used, it can form a multilayer oily droplet formed by different viscosity phases in the water system. The presence of the droplet phase can effectively avoid excessive aggregation of active reaction molecules in the water system, thereby greatly reducing the probability of adverse chemical reactions in a high-temperature active environment, thereby avoiding the formation of other complex scaling, and can also improve the stability of the scale inhibitor and corrosion inhibitor in high-temperature water quality.

[0039] Secondly, the presence of the droplet phase can greatly reduce the intermolecular attraction between scale components, attract the formation of tiny water slag particles into the droplet phase, help disperse the scaling particles and tiny scale particles in the water, and greatly reduce their aggregation and deposition in the water system; finally, the use of the above scheme can also effectively enhance the spreadability of water on the metal surface, increase the thickness of the surface protective film, thereby reducing the adhesion of the scale layer, isolating the metal and the corrosive medium, and the directional film layer structure formed on the metal surface can effectively prevent the chemical corrosive medium from contacting the metal surface, thereby playing an excellent anti-scaling and corrosion-inhibiting role.

[0040] The second aspect of the present application provides a method for preparing the above-mentioned scale and corrosion inhibition composition, and the preparation method comprises the following steps: S1: adding water-soluble zinc salt, metal salt and functional additive into deionized water and stirring evenly for use; S2: sequentially adding modified copolymer, long-chain alkyl alcohol amine and acrylic acid-acrylamide copolymer, heating to 50-60°C, stirring evenly at a high speed of 200-300rpm until the product becomes viscous and uniform, then taking out, vacuum drying at 40-50°C, and then crushing through a 200-400 mesh sieve to obtain the product.

[0041] The third aspect of the present application provides an application of the above-mentioned scale and corrosion inhibition composition in water treatment.

[0042] The beneficial effects of this application are:

[0043] 1. A scale inhibition and corrosion inhibition composition provided in the present application, the prepared scale inhibition and corrosion inhibition composition not only has excellent scale inhibition and corrosion inhibition effect, but also can reduce the requirements of the scale inhibition and corrosion inhibition composition for temperature, water quality and dosage. It still has excellent scale inhibition and corrosion inhibition effect at higher temperature, and has very excellent market use prospects.

[0044] 2. A scale and corrosion inhibitor composition provided in the present application can greatly improve the scale inhibition and anti-corrosion functions of the scale and corrosion inhibitor composition by adding a modified copolymer, and can effectively adapt to the high temperature environment of the water system, improve the stability of the action, and reduce the water quality selection requirements; the modified copolymer can utilize the chelation effect of the carboxylic acid groups of methacrylic acid and maleic acid on its molecular chain with metal ions, greatly improving the formation efficiency of chelates in the water system and promoting the precipitation of chelates; on the other hand, the modified copolymer can also form a barrier film with a certain thickness on the metal surface through the joint action of the functional additives of the present application, and the modified copolymer can produce an effective and uniform adsorption effect on the corrosive ions on the film surface, avoiding direct contact between the corrosive ions and the metal surface, and can also enhance the binding effect of polyepoxysuccinic acid on calcium and magnesium ions.

[0045] 3. A scale and corrosion inhibition composition provided in the present application promotes the formation of tiny scale particles in the aqueous droplet phase by adding a modified copolymer, thereby forming a loose system of tiny scale particles, avoiding their aggregation and structural phenomena on the metal surface. The loose chelate particles formed by combining with calcium and magnesium ions can hinder the growth of calcium carbonate and magnesium crystal structures, and cannot form solid particles with a stable form and precipitate. Moreover, the above-mentioned inhibitory effect can be enhanced at high temperatures, thereby obtaining excellent performance stability at high temperatures.

[0046] 4. The scale inhibitor and corrosion inhibitor composition provided in the present application, the addition of the compound dispersant can not only play an excellent role in dispersing the scale inhibitor and corrosion inhibitor raw materials, but also can further improve the stability of the scale inhibitor and corrosion inhibitor under high temperature and the scale inhibitor and corrosion inhibitor effect, reduce its requirements for temperature and water quality, and effectively reduce the amount of scale inhibitor and corrosion inhibitor. When the above-mentioned specific fatty alcohol polyoxyethylene ether and block polyether are used, it can form a multilayer oil droplet formed by different viscosity phases in the water system. The presence of the droplet phase can effectively avoid excessive aggregation of active reaction molecules in the water system, thereby greatly reducing the probability of adverse chemical reactions in a high-temperature active environment, thereby avoiding the formation of other complex scales, and can also improve the stability of the scale inhibitor and corrosion inhibitor in high-temperature water quality. DETAILED DESCRIPTION

[0047] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.

[0048] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.

[0049] Example 1

[0050] Example 1 The first aspect provides a scale and corrosion inhibition composition, in which the raw materials include, by mass percentage: 18% modified copolymer, 7.5% long-chain alkyl alcohol amine, 9% acrylic acid-acrylamide copolymer, 1.2% metal salt, 2.1% water-soluble zinc salt, 5.5% functional additive, and the balance deionized water.

[0051] The preparation method of the modified copolymer comprises the following steps, calculated by mass: S1: adding 13.4 parts of cis-epoxysuccinic acid to 180 parts of ethyl acetate, preheating to 60°C and stirring for 0.6h; S2: adding 0.23 parts of a reaction aid after stirring, and dripping a mixed ethyl acetate solution of 3.25 parts of methacrylic acid and 4.2 parts of maleic acid (60 parts in total) into the S1 solution, the dripping temperature is 65°C, the dripping reaction time is 0.8h, the temperature is raised to 80°C after the dripping is completed, and the reaction is kept warm for 2.5h, and the product is filtered, washed and dried after the reaction is completed.

[0052] The reaction aids are potassium persulfate and triethylamine; the mass ratio of potassium persulfate to triethylamine is 1.3:1.

[0053] The long-chain alkyl alcohol amine is a composition of dodecyl alcohol amine and octadecyl alcohol amine, and the mass ratio of dodecyl alcohol amine to octadecyl alcohol amine is 1.1:3.8.

[0054] The acrylic acid-acrylamide copolymer is acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, and the limiting viscosity is 0.085 (30°C) / dl·g -1 , purchased the corresponding products sold by Shandong Xingrui Environmental Technology Co., Ltd.

[0055] The metal salts are sodium silicate and magnesium chloride, and the mass ratio of sodium silicate to magnesium chloride is 3.2:0.65.

[0056] The water-soluble zinc salt is a composition of zinc sulfate and zinc gluconate, and the mass ratio of zinc sulfate to zinc gluconate is 2.1:0.9.

[0057] The functional auxiliary agent is a dispersant, and the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether, and the mass ratio of fatty alcohol polyoxyethylene ether to block polyether is 2.2:0.6.

[0058] The fatty alcohol polyoxyethylene ether is isomeric 13 fatty alcohol polyoxyethylene ether, the hydroxyl value of isomeric 13 fatty alcohol polyoxyethylene ether is 88 mgKOH / g, and it is purchased from E-1310 product sold by Hai'an Guoyun Chemical Co., Ltd.

[0059] The block polyether is a composition of a block polyether with a weight average molecular weight of 1600 and a block polyether with a weight average molecular weight of 4600, and the mass ratio of the two is 2.8:1.3. The block polyether with a weight average molecular weight of 1600 and the block polyether with a weight average molecular weight of 4600 are purchased from BASF as L42 and L85 block polyether products, respectively.

[0060] The second aspect of this embodiment provides a method for preparing the above-mentioned scale and corrosion inhibition composition, and the preparation method comprises the following steps: S1: adding water-soluble zinc salt, metal salt and functional additive into deionized water and stirring evenly for use; S2: adding modified copolymer, long-chain alkyl alcohol amine and acrylic acid-acrylamide copolymer in sequence, heating to 55°C, stirring evenly at a high speed of 280rpm until the product becomes viscous and uniform, then taking out, vacuum drying at 50°C, and then crushing through a 250-mesh sieve to obtain the product.

[0061] Example 2

[0062] Example 2 The first aspect provides a scale and corrosion inhibition composition, in which the raw materials include, by mass percentage: 15% modified copolymer, 8.5% long-chain alkyl alcohol amine, 10% acrylic acid-acrylamide copolymer, 1.4% metal salt, 2.2% water-soluble zinc salt, 5% functional additive, and the balance deionized water.

[0063] The preparation method of the modified copolymer comprises the following steps, calculated by mass: S1: adding 13.4 parts of cis-epoxysuccinic acid to 180 parts of ethyl acetate, preheating to 60°C and stirring for 0.6h; S2: adding 0.23 parts of a reaction aid after stirring, and dripping a mixed ethyl acetate solution of 3.25 parts of methacrylic acid and 4.2 parts of maleic acid (60 parts in total) into the S1 solution, the dripping temperature is 65°C, the dripping reaction time is 0.8h, the temperature is raised to 80°C after the dripping is completed, and the reaction is kept warm for 2.5h, and the product is filtered, washed and dried after the reaction is completed.

[0064] The reaction aids are potassium persulfate and triethylamine; the mass ratio of potassium persulfate to triethylamine is 1.3:1.

[0065] The long-chain alkyl alcohol amine is a composition of dodecyl alcohol amine and octadecyl alcohol amine, and the mass ratio of dodecyl alcohol amine to octadecyl alcohol amine is 1:4.5.

[0066] The acrylic acid-acrylamide copolymer is acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, and the limiting viscosity is 0.085 (30°C) / dl·g -1 , purchased the corresponding products sold by Shandong Xingrui Environmental Technology Co., Ltd.

[0067] The metal salts are sodium silicate and magnesium chloride, and the mass ratio of the sodium silicate to the magnesium chloride is 3:0.8.

[0068] The water-soluble zinc salt is a composition of zinc sulfate and zinc gluconate, and the mass ratio of zinc sulfate to zinc gluconate is 2.5:0.8.

[0069] The functional auxiliary agent is a dispersant, and the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether, and the mass ratio of fatty alcohol polyoxyethylene ether to block polyether is 2:0.5.

[0070] The fatty alcohol polyoxyethylene ether is isomeric 13 fatty alcohol polyoxyethylene ether, the hydroxyl value of isomeric 13 fatty alcohol polyoxyethylene ether is 88 mgKOH / g, and it is purchased from E-1310 product sold by Hai'an Guoyun Chemical Co., Ltd.

[0071] The block polyether is a composition of a block polyether with a weight average molecular weight of 1600 and a block polyether with a weight average molecular weight of 4600, and the mass ratio of the two is 2:1.6. The block polyether with a weight average molecular weight of 1600 and the block polyether with a weight average molecular weight of 4600 are purchased from BASF as L42 and L85 block polyether products, respectively.

[0072] The second aspect of this embodiment provides a method for preparing the above-mentioned scale and corrosion inhibition composition, and the preparation method comprises the following steps: S1: adding water-soluble zinc salt, metal salt and functional additive into deionized water and stirring evenly for use; S2: adding modified copolymer, long-chain alkyl alcohol amine and acrylic acid-acrylamide copolymer in sequence, heating to 55°C, stirring evenly at a high speed of 280rpm until the product becomes viscous and uniform, then taking out, vacuum drying at 50°C, and then crushing through a 250-mesh sieve to obtain the product.

[0073] Comparative Example 1

[0074] The specific implementation of this comparative example is basically the same as that of Example 1, except that:

[0075] The scale and corrosion inhibition composition comprises, by weight percentage, 12% of modified copolymer, 12% of long-chain alkyl alcohol amine, 4.5% of acrylic acid-acrylamide copolymer, 1.2% of metal salt, 2.1% of water-soluble zinc salt, 5.5% of functional additive, and the balance of deionized water.

[0076] Comparative Example 2

[0077] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified copolymer comprises the following steps, calculated by mass: S1: adding 22.4 parts of cis-epoxysuccinic acid to 240 parts of ethyl acetate, preheating to 60°C and stirring for 0.8h; S2: after stirring, adding 0.35 parts of a reaction aid, and dropping a mixed ethyl acetate solution of 1.5 parts of methacrylic acid and 2.1 parts of maleic acid (40 parts in total) into the S1 solution, the dropping temperature is 65°C, the dropping reaction time is 0.6h, after the dropping is completed, the temperature is raised to 80°C, and the reaction is kept warm for 2.5h. After the reaction is completed, the product is filtered, washed, and dried.

[0078] Comparative Example 3

[0079] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified copolymer comprises the following steps, calculated by mass: S1: adding 8.5 parts of cis-epoxysuccinic acid to 150 parts of ethyl acetate, preheating to 60°C and stirring for 0.6h; S2: after stirring, adding 0.23 parts of a reaction aid, and dropping a mixed ethyl acetate solution of 4.8 parts of methacrylic acid and 6.5 parts of maleic acid (a total of 80 parts) into the S1 solution, the dropping temperature is 65°C, the dropping reaction time is 1h, after the dropping is completed, the temperature is raised to 80°C, and the reaction is kept warm for 3h. After the reaction is completed, the product is filtered, washed, and dried.

[0080] Comparative Example 4

[0081] The specific implementation of this comparative example is basically the same as that of Example 1, except that the limiting viscosity of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 0.055 (30°C) / dl·g -1 , purchased the corresponding products sold by Shandong Xingrui Environmental Technology Co., Ltd.

[0082] Comparative Example 5

[0083] The specific implementation of this comparative example is basically the same as that of Example 1, except that the functional auxiliary agent is a dispersant, the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether, and the mass ratio of fatty alcohol polyoxyethylene ether to block polyether is 8:1.

[0084] Comparative Example 6

[0085] The specific implementation of this comparative example is basically the same as that of Example 1, except that the functional auxiliary agent is a dispersant, the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether, and the mass ratio of fatty alcohol polyoxyethylene ether to block polyether is 1:1.

[0086] Comparative Example 7

[0087] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the fatty alcohol polyoxyethylene ether is isomeric 13 fatty alcohol polyoxyethylene ether, the hydroxyl value of isomeric 13 fatty alcohol polyoxyethylene ether is 150 mgKOH / g, and it is purchased from E-1304 product sold by Hai'an Guoyun Chemical Co., Ltd.

[0088] Comparative Example 8

[0089] The specific implementation of this comparative example is basically the same as that of Example 1, except that the block polyether is a composition of a block polyether with a weight average molecular weight of 8400 and a block polyether with a weight average molecular weight of 10000, and the mass ratio of the two is 2:1.6. The block polyether with a weight average molecular weight of 8400 and the block polyether with a weight average molecular weight of 10000 are purchased from BASF as L68 and L88 block polyether products, respectively.

[0090] Performance Evaluation

[0091] Scale inhibition rate: The scale inhibition rate of the scale inhibition and corrosion inhibition composition of the embodiment and the comparative example was tested with reference to HG / T3924-2007 standard. The temperature of boiler return water was 72-75°C, the dosage of the scale inhibition and corrosion inhibition composition was 10 mg / L, and the test value was the average value of 10 tests and recorded in Table 1.

[0092] Corrosion inhibition rate: The corrosion inhibition rate of the scale and corrosion inhibition composition of the embodiment and the comparative example was tested with reference to HG / T3924-2007 standard. The test items were carbon steel and copper. The temperature of boiler return water was 72-75°C. The dosage of the scale and corrosion inhibition composition was 10 mg / L. The test value was the average value of 10 tests and recorded in Table 1.

[0093] Corrosion rate: The corrosion inhibition effect of the scale and corrosion inhibition composition was tested using a carbon steel test piece. The rotating hanging piece test was performed. The dosage of the scale and corrosion inhibition composition was 15 mg / L. The temperature of the boiler return water was 72-75°C. The test value was the average of 10 tests and recorded in Table 1.

[0094] Table 1 Performance test results

[0095]

[0096] From the examples and comparative examples of the present application and the data results in Table 1, it can be seen that examples 1 and 2 of the present application can have obvious performance advantages in scale inhibition, corrosion inhibition and stability by adopting the unique technical solution defined in the present application, and solve the technical problem that the existing scale inhibitors and corrosion inhibitors have too narrow requirements for water temperature, water quality, etc. However, comparative examples 1 to 8 are significantly worse than examples 1 and 2 in the above performance tests because they do not correctly adopt the corresponding defined technical solutions, which just proves the necessity of the technical solutions adopted in examples 1 and 2 for the technical effects of the present application.

Claims

1. A scale and corrosion inhibition composition, characterized in that: The raw materials include, by mass percentage: 10-20% modified copolymer, 5-10% long-chain alkyl alcohol amine, 5-10% acrylic acid-acrylamide copolymer, 1-2% metal salt, 1-3% water-soluble zinc salt, 1-6% functional additive, and the balance deionized water; The preparation method of the modified copolymer comprises the following steps: S1: adding epoxy succinic acid to an organic solvent, preheating the temperature to 60-65° C., and stirring for 0.5-1h; S2: adding a reaction aid after stirring, and dripping a mixed solution of methacrylic acid and maleic acid into the S1 solution, the dripping temperature is 65-70° C., the dripping reaction time is 0.5-1h, and after the dripping is completed, the temperature is increased to 80-85° C., and the reaction is kept for 2-3h. After the reaction is completed, the product is filtered, washed, and dried to obtain the product; The mass ratio of epoxysuccinic acid, reaction aid, methacrylic acid and maleic acid is (10-15): (0.2-0.4): (3-4): (4-5); The reaction aids are potassium persulfate and triethylamine; the mass ratio of potassium persulfate to triethylamine is (1-1.5): (0.8-1); The long-chain alkyl alcohol amine is at least one of dodecyl alcohol amine, hexadecanolamine, and octadecyl alcohol amine; The acrylic acid-acrylamide copolymer is acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer; The limiting viscosity of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 0.075 to 0.15 (30° C.) / dl·g -1 ; The metal salt is at least one of metal molybdate, metal silicate, metal borate and metal chloride; The water-soluble zinc salt is at least one of zinc chloride, zinc sulfate, zinc gluconate, zinc acetate, and zinc citrate; The functional additive is at least one of a dispersant, a wetting agent, a defoaming agent, a cosolvent and a stabilizer.

2. The scale and corrosion inhibition composition according to claim 1, characterized in that: The mass ratio of the modified copolymer, the long-chain alkyl alcohol amine and the acrylic acid-acrylamide copolymer is (15-20): (6-10): (8-10).

3. The scale and corrosion inhibition composition according to claim 2, characterized in that: The long-chain alkyl alcohol amine is a combination of dodecyl alcohol amine and octadecyl alcohol amine.

4. The scale and corrosion inhibition composition according to claim 3, characterized in that: The mass ratio of the dodecyl alcohol amine to the octadecyl alcohol amine is (1-1.2):(3-4.5).

5. The scale and corrosion inhibition composition according to claim 4, characterized in that: The limiting viscosity of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 0.08 to 0.1 (30° C.) / dl·g -1 .

6. The scale and corrosion inhibition composition according to claim 5, characterized in that: The metal salts are sodium silicate and magnesium chloride; the mass ratio of the sodium silicate to the magnesium chloride is (3-4): (0.5-1).

7. The scale and corrosion inhibition composition according to claim 6, characterized in that: The water-soluble zinc salt is a composition of zinc sulfate and zinc gluconate; the mass ratio of the zinc sulfate to the zinc gluconate is (2-2.5):(0.8-1).

8. The scale and corrosion inhibition composition according to claim 7, characterized in that: The functional auxiliary agent at least includes a dispersant; the dispersant is a composition of fatty alcohol polyoxyethylene ether and block polyether.

9. A method for preparing the scale and corrosion inhibitor composition according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: S1: adding water-soluble zinc salt, metal salt and functional additive into deionized water, stirring evenly and setting aside; S2: sequentially adding modified copolymer, long-chain alkyl alcohol amine and acrylic acid-acrylamide copolymer, heating to 50-60°C, stirring evenly at a high speed of 200-300rpm until the product is viscous and uniform, then taking out, vacuum drying at 40-50°C, and then crushing through a 200-400 mesh sieve to obtain the product.

10. Use of the scale and corrosion inhibitor composition according to any one of claims 1 to 8 in water treatment.

Citation Information

Patent Citations

  • Composition for scale and corrosion inhibitor of industrial boiler feed water and condensed water system and application of composition

    CN106186376A

  • Recovery method and recovery device for discharged cooling water

    CN107735365A

  • Corrosion and scale inhibitor composition and application thereof

    CN113185008A

Cited By

  • Scale inhibitor used in ultrafiltration and reverse osmosis processes, and preparation method and application thereof

    CN119591262A

  • Antiscalant for use in ultrafiltration and reverse osmosis processes, and method for its preparation and use

    CN119591262B