Method for producing high-grade needle coke raw material

Through the thermal polycondensation reaction of hydrogenated diesel and catalyzed diesel, the sulfur and nitrogen contents are reduced. Combined with the catalytic oil slurry, the problem of sulfur and nitrogen heteroatoms in the residual oil raw material is solved, and needle coke with low sulfur, low nitrogen and high aromatics is provided. The raw materials meet the special grade standards and improve the quality and safety of the raw materials.

CN118725908AActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310330948.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

It is difficult to effectively utilize residual oil raw materials to produce high-grade needle coke raw materials with low sulfur, low nitrogen and high aromatic hydrocarbons with existing technology, resulting in the presence of sulfur and nitrogen heteroatoms affecting the performance of graphite electrodes and increasing safety risks.

Method used

Hydrogenated diesel and catalytic diesel are subjected to a thermal polycondensation reaction to reduce the sulfur and nitrogen content, and then mixed with catalytic cracking oil slurry, and then enter the delayed coking unit as a raw material for the production of high-grade needle coke.

Benefits of technology

The mixture of heavy components and catalytic oil slurry obtained after thermal polycondensation has significantly reduced sulfur and nitrogen contents, meeting the standards of super-grade needle coke, providing better quality needle coke raw materials, and solving the problem of sulfur and nitrogen heteroatoms in the raw materials. question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725908A_ABST
    Figure CN118725908A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a high-grade needle coke raw material, which comprises the following steps of: feeding hydrogenated diesel oil from a residual oil hydrogenation device and catalytic diesel oil from a catalytic cracking device into a thermal polycondensation device for thermal polycondensation reaction to obtain a thermal polycondensation product, and mixing heavy components of the thermal polycondensation product obtained by cutting with filtered catalytic cracking slurry oil, the mixture is used as a raw material for producing high-grade needle coke. According to the invention, the hydrogenated diesel oil and the catalytic diesel oil are subjected to moderate thermal polycondensation to obtain low-sulfur polycyclic aromatic hydrocarbon, so that not only is the diesel oil outlet problem solved, but also a higher-quality needle coke raw material is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of residual oil raw material processing, and in particular to a method for producing high-grade needle coke raw material from residual oil raw material. Background Art

[0002] Needle coke has a series of advantages such as low thermal expansion coefficient, low porosity, low sulfur, low ash, low metal content, high conductivity and easy graphitization. Its graphitized products have good chemical stability, corrosion resistance, high thermal conductivity, good mechanical strength at low and high temperatures, and good electrochemical comprehensive performance. Needle coke is mainly used for ultra-high power graphite electrodes and negative electrode materials for lithium-ion batteries. The country continues to promote the adjustment and transformation and upgrading of the industrial structure of the steel and automobile industries, vigorously promotes the application of energy-saving, low-carbon and green environmental protection technologies, and promotes the rapid development of electric arc furnace steelmaking and new energy vehicles. The demand for raw material needle coke is also growing rapidly.

[0003] According to the properties and formation mechanism of needle coke, raw materials with high content of polycyclic aromatic hydrocarbons should be selected. Catalytic cracking slurry is a low value-added product of catalytic cracking unit. It has high content of polycyclic aromatic hydrocarbons and is suitable as a raw material for producing needle coke. The sulfur and nitrogen impurity contents of slurry produced by catalytic cracking unit in my country are both high. The presence of sulfur and nitrogen heteroatoms in the needle coke carbonization reaction will cause unnecessary cross-linking reactions, resulting in the loss of planarity of the molecules to form a cross-linked structure, thereby destroying the planarity of the intermediate product and being unfavorable for the formation of a wide-area intermediate phase. Moreover, sulfur and nitrogen are released under high temperature during the graphitization of needle coke and the use of electrodes, which will cause crystal expansion, which will not only affect the performance of graphite electrodes, but also cause graphite electrodes to break, resulting in production accidents. Therefore, whether it is used as a raw material for graphite electrodes or lithium battery negative electrode materials, there are clear requirements for the sulfur and nitrogen heteroatom content of needle coke. The China Carbon Industry Association Standard (T / ZGTS 002-2019) stipulates that the sulfur content of special grade needle coke is ≯0.35% and the nitrogen content is ≯0.10%. Therefore, raw materials with low sulfur, low nitrogen and high aromatics are suitable for producing high-grade needle coke.

[0004] CN1872963A discloses a pretreatment method for raw materials for producing needle coke. In this method, the raw oil is first filtered and vacuum distilled to remove heavy non-ideal components such as asphaltene, colloid and part of ash, and light non-ideal components such as diesel fraction, wherein the light non-ideal components are extracted from the top and the first vacuum tower, the heavy non-ideal components are extracted from the bottom of the tower, and the remaining ideal components are extracted from the tower to contact with hydrogen and hydrogenation catalyst, and the hydrogenation reaction flow is separated to obtain the raw materials for producing needle coke.

[0005] CN103666556A discloses a method for preparing petroleum coke, comprising: (1) performing vacuum distillation on catalytic cracking slurry, wherein the catalytic cracking slurry has a sulfur content of 0.50% to 2.5% by weight, an ash content of 0.01% to 1% by weight, and an asphaltene content of 1% to 20% by weight; (2) mixing the distillate oil obtained in step (1) with hydrogen, and then contacting with a hydrogenation protective agent and a hydrogenation and hydrogenation refining agent in sequence; (3) inputting the hydrogenated liquid product obtained in step (2) into a delayed coking device for thermal cracking reaction to obtain petroleum coke.

[0006] CN103013567A discloses a method for producing needle coke raw material from catalytic cracking oil slurry. In this method, a hydrogenation protection reaction zone is set before a hydrogenation reaction zone. The catalytic cracking oil slurry first enters the protection zone to absorb most of the catalytic cracking catalyst powder, then is mixed with hydrogen and enters a heating furnace, and after heating, enters the hydrogenation reaction zone for hydrogenation treatment reaction. By hydrogenation refining of the catalytic cracking oil slurry, most of the sulfur in the catalytic cracking oil slurry is removed, and a qualified needle coke raw material is produced. Summary of the invention

[0007] The invention aims to solve the technical problem of how to effectively utilize residual oil raw materials to produce high-grade needle coke raw materials in maximum quantity.

[0008] The present invention provides a method for producing high-grade needle coke raw materials, comprising:

[0009] (1) The hydrogenated diesel from the residue oil hydrogenation unit and the catalytic diesel from the catalytic cracking unit enter the thermal polycondensation unit for thermal polycondensation reaction to obtain a thermal polycondensation product;

[0010] (2) distilling and cutting the thermal polycondensation product into a heavy component and a light component, and returning the light component to the inlet of the thermal polycondensation device;

[0011] (3) The heavy component obtained in step (2) is mixed with the filtered catalytic cracking oil slurry, and the mixture is fed into a delayed coking unit as a raw material for producing high-grade needle coke.

[0012] In one embodiment of the present invention, the distillation range of hydrogenated diesel is 160-350° C., the sulfur content is 0.001%-0.050% by weight, and the nitrogen content is 0.001%-0.050% by weight. The distillation range of catalytic diesel is 160-350° C., the sulfur content is 0.0105%-0.200% by weight, and the nitrogen content is 0.010%-0.200% by weight. The mixing mass ratio of hydrogenated diesel and catalytic diesel is 1:1-1:4.

[0013] In the present invention, hydrogenated diesel and catalytic diesel are sent to a thermal polycondensation device for thermal polycondensation reaction, the purpose of which is to reasonably utilize the aromatic components in diesel, and to make it a high-quality needle coke raw material by thermal polycondensation to a certain degree of condensed aromatics. And because the sulfur content and nitrogen content in hydrogenated diesel and catalytic diesel are lower than the sulfur content and nitrogen content of catalytic oil slurry, the heavy components obtained after thermal polycondensation of the two are also components with low sulfur content and nitrogen content, which are mixed with catalytic oil slurry, thereby effectively reducing the sulfur content and nitrogen content of the final mixture. Therefore, the present invention not only solves the diesel outlet, but also obtains high-quality raw materials for producing high-grade needle coke.

[0014] In one embodiment of the present invention, the thermal polycondensation device in step (1) is a tubular reactor to accurately control the temperature and time of the thermal polycondensation.

[0015] In one embodiment of the present invention, the thermal polycondensation reaction temperature in step (1) is 400°C to 480°C, and the reaction time is 0.1h to 2h. Preferably, the thermal polycondensation reaction temperature is 440°C to 470°C, and the reaction time is 0.2h to 1h.

[0016] In one embodiment of the present invention, the cut point between the light component and the heavy component of the thermal polycondensation product in step (2) is 370°C to 470°C, preferably 420°C to 460°C.

[0017] In one embodiment of the present invention, the heavy component obtained in step (2) is composed of three to six-ring condensed aromatic hydrocarbons.

[0018] In one embodiment of the present invention, the initial boiling point of the filtered catalytic cracking slurry is greater than or equal to 350°C, the sulfur content is not more than 0.50% by weight, the nitrogen content is not more than 0.10%, and the content of three-ring and four-ring aromatic hydrocarbons is not less than 30%.

[0019] In one embodiment of the present invention, the mixing mass ratio of the filtered catalytic cracking oil slurry and the heavy component is 1:1 to 1:4.

[0020] In one embodiment of the present invention, the residual oil feedstock and hydrogen enter a fixed bed residual oil hydrogenation unit, and pass through a hydrogenation protective agent, a hydrogenation demetallization agent, a hydrogenation desulfurization agent and a hydrogenation denitrogenation agent in sequence. The resulting hydrogenated oil is separated to obtain dry gas, hydrogenated gasoline, hydrogenated diesel and hydrogenated residual oil. The resulting hydrogenated residual oil enters a catalytic cracking unit, and undergoes a catalytic cracking reaction under the action of a catalytic cracking catalyst to obtain dry gas, catalytic gasoline, catalytic diesel and catalytic oil slurry.

[0021] In one embodiment of the present invention, the process conditions for fixed bed residue hydrogenation are: reaction temperature between 300°C and 430°C, preferably 350°C to 390°C; reaction pressure between 13.0MPa and 19.0MPa, preferably 15.0MPa to 18.0MPa; volume space velocity between 0.10h -1 ~0.50h -1 Between, preferably 0.15h -1 ~0.40h -1 ; The volume ratio of hydrogen to oil is between 500 and 1500, preferably 800 to 1200.

[0022] The hydrogenation protective agent and hydrogenation demetallization agent loaded in the fixed bed residue oil hydrogenation reactor can be commercially available residue oil hydrogenation protective agent and hydrogenation demetallization agent. The purpose of loading the hydrogenation demetallization agent is to remove metal impurities in the raw material and to protect the downstream hydrogenation desulfurization agent and hydrogenation denitrification agent.

[0023] The hydrodesulfurization agent can adopt a commercially available fixed-bed residue oil hydrodesulfurization catalyst, and preferably the active metal of the hydrodesulfurization agent is cobalt-molybdenum, that is, the hydrodesulfurization agent is a cobalt-molybdenum type catalyst. The hydrodenitrification agent can adopt a commercially available fixed-bed residue oil hydrodenitrification catalyst, and preferably the active metal of the hydrodenitrification agent is nickel-tungsten, that is, the hydrodenitrification agent is a nickel-tungsten type catalyst. The present invention comprehensively determines the loading ratio of the hydrodesulfurization agent and the hydrodenitrification agent based on the sulfur content and nitrogen content in the raw material and the reaction conditions.

[0024] In one embodiment of the present invention, based on the entire residual oil hydrogenation catalyst, the filling ratio of the hydrogenation protective agent is between 1% and 10% by volume, the filling ratio of the hydrogenation demetallization agent is between 5% and 50%, the filling ratio of the hydrogenation desulfurization agent is between 5% and 50%, and the filling ratio of the hydrogenation denitrification agent is between 5% and 50%.

[0025] In the present invention, there is no limitation on the catalytic cracking unit, but a catalytic cracking unit that produces more light olefins is preferred.

[0026] The characteristics of the present invention are as follows: hydrogenated diesel and catalytic diesel are subjected to moderate thermal polycondensation to obtain low-sulfur condensed ring aromatics, which not only solves the diesel outlet problem but also provides a better quality needle coke raw material. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of one embodiment of the method for producing high-grade needle coke raw material provided by the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the accompanying drawings, but the present invention is not limited thereby.

[0029] Figure 1 FIG. 1 is a schematic diagram of one embodiment of the method for producing high-grade needle coke raw material provided by the present invention. Figure 1 As shown, the residual oil raw material and hydrogen from pipeline 1 enter the fixed bed residual oil hydrogenation device 2 together, and the hydrogenation reaction is carried out under the action of the hydrogenation catalyst to remove most of the impurities such as sulfur and nitrogen in the residual oil. The hydrogenation product oil enters the separation system 4 through pipeline 3, and the gas and hydrogenated gasoline obtained by separation are discharged from the device through pipelines 5 and 6 respectively, and the hydrogenated diesel enters the thermal polycondensation device 19 through pipeline 7. The hydrogenated residual oil enters the catalytic cracking device 9 through pipeline 8, and the cracking reaction is carried out under the action of the catalytic cracking catalyst. The catalytic cracking product oil enters the separation system 11 through pipeline 10, and the dry gas, liquefied gas and catalytic gasoline obtained by separation are discharged from the device through pipelines 12, 13 and 14 respectively, and the catalytic oil slurry enters the filtering device 17 through pipeline 16. The catalytic diesel is mixed with the hydrogenated diesel from pipeline 7 through pipeline 15 and enters the thermal polycondensation device 19 to carry out the thermal polycondensation reaction. The thermal polycondensation product is fractionated to obtain light and heavy components, and the light component returns to the thermal polycondensation device 19 through pipeline 20. The heavy component is mixed with the catalytic oil slurry filtered by the filter device 17, and then leaves the device through the pipeline 18 to enter the delayed coking device as a raw material for producing high-grade needle coke.

[0030] The present invention will be further described below in conjunction with embodiments, but the present invention is not limited thereto.

[0031] The properties of the residual oil raw materials A and B used in the examples and comparative examples are shown in Table 1. The trade names of the hydrogenation protective agent, hydrogenation demetallization agent, hydrogenation desulfurization agent and hydrogenation denitrification agent used in the fixed bed residual oil hydrogenation unit are RG-30B, RDM-202, RMS-30 and RSN-1 respectively, and the trade name of the hydrogenation desulfurization denitrification agent used in the comparative example is RCS-31, all of which are produced by the Changling Catalyst Plant of Sinopec Catalyst Branch. The main properties of the hydrogenation catalyst are shown in Table 2. The trade name of the catalytic cracking catalyst used is MLC500, which is produced by Sinopec Catalyst Changling Branch.

[0032] Example 1

[0033] The residual oil raw material A enters the residual oil hydrogenation unit together with hydrogen, and passes through the hydrogenation protective agent RG-30B, the hydrogenation demetallization agent RDM-202, the hydrodesulfurization agent RMS-30 and the hydrodenitrogenation catalyst RSN-1 in sequence to remove most of the sulfur and nitrogen heteroatoms in the residual oil. The hydrogenated oil is separated to obtain dry gas, hydrogenated gasoline, hydrogenated diesel and hydrogenated residual oil. The hydrogenated residual oil enters the catalytic cracking unit, and under the action of the catalytic cracking catalyst, catalytic cracking reaction is carried out to obtain dry gas, catalytic gasoline, catalytic diesel and catalytic oil slurry. The hydrogenated diesel and catalytic diesel enter the thermal polycondensation unit for thermal polycondensation reaction to obtain thermal polycondensation products. The thermal polycondensation products are distilled and cut into heavy components and light components, and the light components are returned to the thermal polycondensation unit. The heavy components are mixed with the filtered catalytic oil slurry and enter the delayed coking unit as the raw material for producing high-grade needle coke.

[0034] The main operating conditions, main product properties and yields of the residue oil hydrotreating unit and catalytic cracking unit are shown in Tables 3 and 4.

[0035] Example 2

[0036] The residual oil raw material B enters the residual oil hydrogenation unit together with hydrogen, and passes through the hydrogen protection agent RG-30B, the hydrodemetallization agent RDM-202, the hydrodesulfurization agent RMS-30 and the hydrodenitrogenation catalyst RSN-1 in sequence to remove most of the sulfur and nitrogen heteroatoms in the residual oil. The hydrogenated oil is separated to obtain dry gas, hydrogenated gasoline, hydrogenated diesel and hydrogenated residual oil. The hydrogenated residual oil enters the catalytic cracking unit, and under the action of the catalytic cracking catalyst, catalytic cracking reaction is carried out to obtain dry gas, catalytic gasoline, catalytic diesel and catalytic oil slurry. The hydrogenated diesel and catalytic diesel enter the thermal polycondensation unit for thermal polycondensation reaction to obtain thermal polycondensation products. The thermal polycondensation products are distilled and cut into heavy components and light components, and the light components are returned to the thermal polycondensation unit. The heavy components are mixed with the filtered catalytic oil slurry and enter the delayed coking unit as the raw material for producing high-grade needle coke.

[0037] The main operating conditions, main product properties and yields of the residue oil hydrotreating unit and catalytic cracking unit are shown in Tables 3 and 4.

[0038] As can be seen from Table 4, the sulfur content of the high-grade needle coke raw materials obtained in Example 1 and Example 2 is both less than 0.10% by weight, and the nitrogen content is both less than 0.05% by weight, and can be used as raw materials for producing high-grade needle coke. The raw materials enter the delayed coking device, and after coking treatment, the properties of the needle coke obtained are listed in Table 4, and the carbon industry association standard (T / ZGTS 002-2019) is listed in Table 6. It can be seen from Table 4 that the properties of the obtained needle coke meet the index requirements of special grade coke.

[0039] The total yields of Example 1 and Example 2 are listed in Table 5, wherein dry gas, liquefied gas and gasoline refer to the sum of the relevant products of the residue oil hydrogenation unit and the catalytic cracking unit, and the needle coke raw material refers to the mixture of the heavy components obtained from the thermal polycondensation unit and the filtered catalytic oil slurry.

[0040] Comparative Example 1

[0041] The residual oil raw material A enters the residual oil hydrogenation unit together with hydrogen, and passes through the hydrogenation protective agent RG-30B, the hydrogenation demetallization agent RDM-202, and the hydrogenation desulfurization and denitrification agent RCS-31 in sequence to remove most of the sulfur and nitrogen heteroatoms in the residual oil. The hydrogenated oil is separated to obtain dry gas, hydrogenated gasoline, hydrogenated diesel and hydrogenated residual oil. The hydrogenated residual oil enters the catalytic cracking unit, and undergoes catalytic cracking reaction under the action of the catalytic cracking catalyst to obtain dry gas, catalytic gasoline, catalytic diesel and catalytic oil slurry. The hydrogenated diesel and catalytic diesel enter the thermal polycondensation unit for thermal polycondensation reaction to obtain thermal polycondensation products. The thermal polycondensation products are distilled and cut into heavy components and light components, and the light components are returned to the thermal polycondensation unit. The heavy components are mixed with the filtered catalytic oil slurry and enter the delayed coking unit as a raw material for producing high-grade needle coke.

[0042] The main operating conditions, main product properties and yields of the residue oil hydrotreating unit and catalytic cracking unit are shown in Tables 3 and 4, and the total yield is listed in Table 5.

[0043] The needle coke raw material obtained in Comparative Example 1 enters a delayed coking device. After coking treatment, the properties of the needle coke obtained are listed in Table 4. It can be seen from Table 4 that the properties of the obtained needle coke meet the index requirements of Class I coke.

[0044] Table 1

[0045] Crude oil number Residue A Residue B <![CDATA[Density (20 °C), kg / m 3 > 955 960 <![CDATA[Kinematic viscosity (at 100 °C), mm 2 / s]]> 32 40 Carbon residue, weight % 6.3 8.5 Nitrogen, weight % 0.15 0.23 Sulfur, weight % 1.7 2.0 <![CDATA[Asphaltenes (C7 insolubles)]]> 1.5 2.1 Metal (nickel + vanadium) content, ppm 20 43

[0046] Table 2

[0047]

[0048]

[0049] Table 3

[0050]

[0051]

[0052] Table 4

[0053]

[0054]

[0055] Table 5

[0056]

[0057]

[0058] Table 6

[0059]

Claims

1. A method for producing high-grade needle coke raw material, comprising: (1) The hydrogenated diesel from the residue oil hydrogenation unit and the catalytic diesel from the catalytic cracking unit enter the thermal polycondensation unit for thermal polycondensation reaction to obtain a thermal polycondensation product; (2) distilling and cutting the thermal polycondensation product into a heavy component and a light component, and returning the light component to the inlet of the thermal polycondensation device; (3) The heavy component obtained in step (2) is mixed with the filtered catalytic cracking oil slurry, and the mixture is fed into a delayed coking unit as a raw material for producing high-grade needle coke.

2. The method according to claim 1, characterized in that The distillation range of hydrogenated diesel is 160-350°C, and the sulfur content is 0.001%-0.050% by weight, and the nitrogen content is 0.001%-0.050% by weight. The distillation range of catalytic diesel is 160-350°C, and the sulfur content is 0.0105%-0.200% by weight, and the nitrogen content is 0.010%-0.200% by weight. The mixing mass ratio of hydrogenated diesel and catalytic diesel is 1:1-1:

4.

3. The method according to claim 1, characterized in that The thermal polycondensation device in step (1) is a tubular reactor, the thermal polycondensation reaction temperature is 400° C. to 480° C., and the reaction time is 0.1 h to 2 h.

4. The method according to claim 1, characterized in that: In step (1), the thermal polycondensation reaction temperature is 440° C. to 470° C., and the reaction time is 0.2 h to 1 h.

5. The method according to claim 1, characterized in that The cutting point between the light component and the heavy component of the thermal polycondensation product in step (2) is 370°C to 470°C.

6. The method according to claim 1, characterized in that The cutting point between the light component and the heavy component of the thermal polycondensation product in step (2) is 420°C to 460°C.

7. The method according to claim 1, characterized in that The heavy component obtained in step (2) is composed of three-ring to six-ring condensed aromatic hydrocarbons.

8. The method according to claim 1, characterized in that The initial boiling point of the filtered catalytic cracking oil slurry is greater than or equal to 350° C., and the sulfur content is not more than 0.50% by weight, the nitrogen content is not more than 0.10% by weight, and the content of three-ring and four-ring aromatic hydrocarbons is not less than 30%.

9. The method according to claim 1, characterized in that: The mixing mass ratio of the catalytic cracking oil slurry and the heavy component after filtration is 1:1 to 1:

4.

10. The method according to claim 1, characterized in that The residual oil feedstock and hydrogen enter the fixed bed residual oil hydrogenation unit, and pass through the hydrogenation protective agent, hydrogenation demetallization agent, hydrogenation desulfurization agent and hydrogenation denitrogenation agent in sequence. The resulting hydrogenated oil is separated to obtain dry gas, hydrogenated gasoline, hydrogenated diesel and hydrogenated residual oil. The obtained hydrogenated residual oil enters the catalytic cracking unit, and undergoes catalytic cracking reaction under the action of the catalytic cracking catalyst to obtain dry gas, catalytic gasoline, catalytic diesel and catalytic oil slurry.

11. The method according to claim 10, characterized in that Based on the whole residual oil hydrogenation catalyst, the filling ratio of the hydrogenation protective agent is between 1% and 10% by volume, the filling ratio of the hydrogenation demetallization agent is between 5% and 50%, the filling ratio of the hydrogenation desulfurization agent is between 5% and 50%, and the filling ratio of the hydrogenation denitrification agent is between 5% and 50%.

12. The method according to claim 10 or 11, characterized in that: The active metals of the hydrodesulfurization agent are cobalt-molybdenum; the active metals of the hydrodenitrogenation agent are nickel-tungsten.

Citation Information

Patent Citations

  • Method and equipment for preparing needle coke crude materials

    CN107987875A

  • Delayed coking process for preparing coal-based needle coke

    CN109370642A

  • Method and equipment for preparing needle coke raw material

    CN112745916A

  • Method for preparing needle coke

    CN114479921A

  • Petroleum needle coke for graphite electrode and method of producing the same

    EP3130652A1