Curable resin film, composite sheet, semiconductor chip, and method for producing semiconductor chip
By applying a curable resin film with high transmittance and black pigment on the bump formation surface of the semiconductor chip, the problem of malfunction caused by near-infrared rays is solved, and the semiconductor chip is effectively shielded and strengthened.
Patent Information
- Application Number
- CN202380018739.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-28
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology has not fully studied how to prevent problems caused by malfunctions of semiconductor chips in near-infrared communications through protective films.
Provided is a curable resin film that forms a protective film on a bump formation surface of a semiconductor chip and performs thermal curing treatment at 130°C and 0.5MPa for 240 minutes so that the near-infrared transmittance at 940nm is less than 13%, and Contains black pigment, has a thickness of 1 μm or more, and is used to suppress malfunction of semiconductor chips.
It realizes the near-infrared shielding function of the semiconductor chip, prevents malfunctions, and improves the strength and processability of the chip.
Smart Images

Figure CN118743014A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin film, a composite sheet, a semiconductor chip, and a method for manufacturing a semiconductor chip. More specifically, the present invention relates to a curable resin film, a composite sheet having the curable resin film, a semiconductor chip using the curable resin film as a protective film, and a method for manufacturing the semiconductor chip. Background Art
[0002] In recent years, semiconductor devices have been manufactured using a mounting method called a flip-chip method. In the flip-chip method, a semiconductor chip having bumps on a circuit surface and a substrate for mounting the semiconductor chip are stacked in such a manner that the circuit surface of the semiconductor chip faces the substrate, thereby mounting the semiconductor chip on the substrate.
[0003] It should be noted that, generally, the semiconductor chip is obtained by dividing a semiconductor wafer having bumps on a circuit surface into individual pieces.
[0004] A semiconductor wafer having bumps may be provided with a protective film for the purpose of protecting a bonding portion between the bump and the semiconductor wafer (hereinafter also referred to as a “bump base”).
[0005] For example, in Patent Document 1, after a stacked body formed by stacking a supporting substrate, an adhesive layer and a curable resin layer in sequence is pressed and adhered to the bump forming surface of a semiconductor chip having bumps with the curable resin layer as a bonding surface, the curable resin layer is heated and cured, thereby forming a protective film.
[0006] In the method described in Patent Document 1, after a protective film is formed on a wafer with bumps, the wafer with bumps is diced together with the protective film to obtain individual semiconductor chips.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2015-092594 Summary of the invention
[0010] Problems to be solved by the invention
[0011] On the other hand, in recent years, the technology of sending and receiving data by infrared rays (hereinafter also referred to as "infrared communication") has been used in various devices. Therefore, for semiconductor devices equipped with semiconductor chips, it is required to prevent malfunctions caused by near infrared rays (750nm to 1500nm band) used in infrared communication.
[0012] Therefore, the inventors of the present invention thought that if the protective film of a semiconductor chip formed with a protective film is given a function of preventing malfunctions caused by near infrared rays, the semiconductor chip formed with a protective film can be easily given a function of preventing malfunctions caused by near infrared rays. However, the actual situation is that the technology of preventing malfunctions caused by near infrared rays using the protective film has not been fully studied.
[0013] Therefore, the subject of the present invention is to provide a curable resin film for forming a protective film on a bump forming surface of a semiconductor chip having a bump forming surface with bumps, and the curable resin film is capable of suppressing malfunction of the above-mentioned semiconductor chip caused by near-infrared rays, a composite sheet having the curable resin film, a semiconductor chip, and a method for manufacturing the semiconductor chip.
[0014] Solution to the problem
[0015] According to the present invention, the following [1] to
[16] can be provided.
[0016] [1] A curable resin film for forming a protective film on a bump formation surface of a semiconductor chip having a bump formation surface with bumps,
[0017] The curable resin film satisfies the following requirement (1).
[0018] Requirement (1): The near-infrared transmittance at 940 nm after heat curing treatment at 130° C. and 0.5 MPa for 240 minutes is less than 13%.
[0019] [2] The curable resin film according to [1] above, comprising a black pigment.
[0020] [3] The curable resin film according to [2] above, wherein the content of the black pigment is greater than 0.5% by mass based on the total amount of the curable resin film.
[0021] [4] The curable resin film according to any one of [1] to [3] above, wherein the thickness is 1 μm or more.
[0022] [5] The curable resin film according to any one of [1] to [4], which is used to form the curable resin film as the protective film on both the bump formation surface and the side surface of the semiconductor chip.
[0023] [6] A composite sheet having a laminated structure in which the curable resin film according to any one of [1] to [5] and a release sheet are laminated.
[0024] [7] The composite sheet according to [6] above, wherein the release sheet has a base material and a release layer, and the release layer faces the curable resin film.
[0025] [8] The composite sheet according to [7] above, wherein the release sheet further has an intermediate layer between the substrate and the release layer.
[0026] [9] The composite sheet according to [7] or [8] above, wherein the release layer is a layer formed from a composition containing an ethylene-vinyl acetate copolymer.
[0027]
[10] A method for manufacturing a semiconductor chip, the method comprising the following steps (V1) to (V4) in sequence.
[0028] Step (V1): Step of preparing a semiconductor wafer having a bump formation surface with bumps
[0029] Step (V2): a step of pressing and pasting the curable resin film described in any one of [1] to [4] above onto the bump-forming surface of the semiconductor wafer to cover the bump-forming surface of the semiconductor wafer with the curable resin film
[0030] Step (V3): a step of curing the curable resin film to obtain a semiconductor wafer with a cured resin film
[0031] Step (V4): a step of singulating the semiconductor wafer with the cured resin film to obtain semiconductor chips in which the bump formation surface is covered with the cured resin film.
[0032]
[11] A method for manufacturing a semiconductor chip, the method comprising the following steps (S1), (S2), (S3) and (S4) in sequence,
[0033] Step (S1): a step of preparing a wafer for manufacturing a semiconductor chip, wherein the semiconductor chip manufacturing wafer has a bump forming surface of a semiconductor wafer having bumps and has grooves serving as scheduled division lines formed on the bump forming surface so as not to reach the back surface;
[0034] Step (S2): a step of pressing and sticking the curable resin film described in [5] above to the bump forming surface of the semiconductor chip manufacturing wafer, covering the bump forming surface of the semiconductor chip manufacturing wafer with the curable resin film, and embedding the curable resin film in the groove portion formed in the semiconductor chip manufacturing wafer;
[0035] Step (S3): a step of curing the curable resin film to obtain a wafer for semiconductor chip production with a cured resin film;
[0036] Step (S4): a step of singulating the semiconductor chip manufacturing wafer with the cured resin film along the predetermined division line to obtain semiconductor chips in which at least the bump forming surface and the side surface are covered with the cured resin film.
[0037] Furthermore, the following step (S-BG) is included after the step (S2) and before the step (S3), after the step (S3) and before the step (S4), or during the step (S4).
[0038] Step (S-BG): a step of grinding the back surface of the semiconductor chip manufacturing wafer.
[0039]
[12] The method for manufacturing a semiconductor chip according to the above
[10] further includes the following step (TA).
[0040] Step (TA): a step of forming a back surface protective film on the back surface of the semiconductor wafer
[0041]
[13] The method for manufacturing a semiconductor chip according to the above
[11] further includes the following step (TB).
[0042] Step (TB): a step of forming a back surface protective film on the back surface of the wafer for manufacturing a semiconductor chip.
[0043]
[14] A semiconductor chip having a bump forming surface with bumps, wherein the bump forming surface of the semiconductor chip has a cured resin film formed by curing the curable resin film described in any one of [1] to [4] above, and the semiconductor chip has a near infrared shielding function.
[0044]
[15] A semiconductor chip having a bump forming surface with bumps and having a cured resin film formed by curing the curable resin film described in [5] above on both the bump forming surface and the side surface of the semiconductor chip, the near infrared shielding function being imparted thereto.
[0045]
[16] The semiconductor chip according to
[14] or
[15] , further comprising a back surface protective film on the back surface of the semiconductor chip.
[0046] Effects of the Invention
[0047] According to the present invention, there can be provided a curable resin film that can be used to form a protective film on the bump forming surface of a semiconductor chip having a bump forming surface with bumps, a curable resin film that can suppress malfunction of the semiconductor chip due to infrared rays, a composite sheet having the curable resin film, a semiconductor chip, and a method for manufacturing the semiconductor chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a cross-sectional schematic diagram showing the structure of a composite sheet according to one embodiment.
[0049] Figure 2 It is a schematic cross-sectional view showing the structure of a composite sheet according to another embodiment.
[0050] Figure 3 1 is a schematic cross-sectional view showing an example of a wafer for semiconductor chip production prepared in step ( S1 ).
[0051] Figure 4 It is a figure which shows the outline of a process (S2).
[0052] Figure 5 This is a diagram showing an overview of step (S3).
[0053] Figure 6 This is a diagram showing an outline of step (S4).
[0054] Figure 7 It is a diagram showing an outline of the step (S-BG).
[0055] Figure 8 This is a diagram showing an overview of step (V4).
[0056] Fig. 9 The image is obtained by photographing the semiconductor chip manufacturing wafer with a cured resin film from the cured resin film side in the evaluation of “4-2. Notch Visibility”, and is an image showing an example of a case where the irregularities of the notch can be clearly recognized.
[0057] Fig.10 The image obtained by photographing the semiconductor chip manufacturing wafer with a cured resin film from the cured resin film side in the evaluation of “4-2. Notch Visibility” is an image showing an example of a case where the irregularities of the notch cannot be clearly recognized.
[0058] Explanation of symbols
[0059] 10, 20 composite sheets
[0060] 30, 30' wafer for semiconductor chip manufacturing
[0061] 40, 40' semiconductor chip
[0062] 1, 11, 11' stripping film
[0063] 2.12 Thermosetting resin film
[0064] 3.13 Base material
[0065] 4.14 Peeling layer
[0066] 15 Middle Layer
[0067] 21, 21' semiconductor wafer
[0068] 21a, 21a' bump forming surface
[0069] 21b Back
[0070] 22, 22' bump
[0071] 23 Groove
[0072] X1 Thermosetting resin film
[0073] Y1 Peel Sheet
[0074] r1 Cured resin film
[0075] α1 First composite sheet
[0076] X2 Curable resin film for back side
[0077] Y2 Second peeling sheet
[0078] r2 Cured resin film for back surface, back surface protective film
[0079] α2 Second composite sheet DETAILED DESCRIPTION
[0080] In the present specification, the "active ingredient" refers to the ingredients contained in the target composition excluding diluent solvents such as water and organic solvents.
[0081] In addition, in this specification, "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid", and the same applies to other similar terms.
[0082] In addition, in this specification, a weight average molecular weight and a number average molecular weight are polystyrene conversion values measured by gel permeation chromatography (GPC) method.
[0083] In addition, in this specification, regarding the preferred numerical range (for example, the range of content, etc.), the lower limit and upper limit described in stages can be independently combined. For example, according to the description of "preferably 10 to 90, more preferably 30 to 60", "preferable lower limit (10)" and "more preferably upper limit (60)" can also be combined to obtain "10 to 60".
[0084] In addition, in this specification, "the content of each component in the total amount of the effective components of the curable resin composition" and "the content of each component in the curable resin film formed from the curable resin composition" have the same meaning.
[0085] [Aspects of the curable resin film of this embodiment]
[0086] The curable resin film of the present embodiment is used to form a protective film on a bump formation surface of a semiconductor chip having a bump formation surface provided with bumps, wherein the curable resin film satisfies the following requirement (1).
[0087] Requirement (1): The near-infrared transmittance at 940 nm after heat curing treatment at 130° C. and 0.5 MPa for 240 minutes is less than 13%.
[0088] When the near-infrared transmittance at 940 nm specified in the above requirement (1) is 13% or more, it is difficult to suppress malfunction of the semiconductor chip due to the near-infrared rays.
[0089] Here, from the viewpoint of further suppressing malfunction of the semiconductor chip caused by near-infrared rays, the near-infrared transmittance at 940 nm specified in the above requirement (1) is preferably 10% or less, more preferably 7.0% or less, further preferably 5.0% or less, and further preferably 3.0% or less.
[0090] From the viewpoint of further facilitating suppression of malfunction of the semiconductor chip due to near infrared rays, the near infrared transmittance at 800 nm is preferably 30% or less, more preferably 26% or less, and even more preferably 25% or less.
[0091] In this specification, the infrared transmittance refers to the near-infrared transmittance measured by the method described in Examples described later.
[0092] The method for producing the curable resin film satisfying the above requirement (1) is not particularly limited, and an example thereof includes a method of adding near infrared shielding particles to the curable resin film.
[0093] As the near-infrared shielding particles, various known particles may be used, and the near-infrared shielding particles may be of a near-infrared absorbing type or a near-infrared reflecting type. In addition, the near-infrared shielding particles may be used alone or in combination of two or more.
[0094] Examples of near-infrared shielding particles include precious metal particles such as gold and silver; tin-doped indium oxide particles (ITO particles); antimony-doped tin oxide particles; cesium-doped tungsten oxide particles; lanthanum hexaboride; dyes; pigments; aluminum oxide; silicon carbide, etc.
[0095] Among them, from the viewpoint of easy acquisition, etc., pigments are preferred. In addition, among pigments, black pigments are preferred from the aspect of excellent near-infrared shielding performance. That is, the curable resin film of the present embodiment preferably contains a pigment, and more preferably contains a black pigment.
[0096] Examples of the black pigment include carbon black, copper oxide, ferroferric oxide, manganese dioxide, aniline black, and activated carbon.
[0097] Among them, carbon black is preferred from the viewpoint of availability and the like.
[0098] From the viewpoint of easily satisfying the above requirement (1), the content of the black pigment in the curable resin film is preferably greater than 0.5% by mass, more preferably 0.7% by mass or more, further preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more, based on the total amount of the curable resin film.
[0099] From the viewpoint of ensuring the film-forming property of the curable resin film, the content of the black pigment is preferably less than 35% by mass, more preferably 30% by mass or less, and even more preferably 25% by mass or less, based on the total amount of the curable resin film.
[0100] In order to facilitate good uniform dispersion of the black pigment in the curable resin film, the particle size of the black pigment is preferably 1 nm to 1 μm, more preferably 10 nm to 500 nm, and even more preferably 10 nm to 100 nm.
[0101] In this specification, the particle size of the black pigment refers to an arithmetic average particle size obtained by randomly selecting and measuring the particle sizes of a plurality of primary particles of the black pigment observed with an electron microscope and calculating the average value thereof.
[0102] In addition, as a method for producing a curable resin film that satisfies the above requirement (1), a method of increasing the film thickness of the curable resin film can also be mentioned.
[0103] As the thickness of the curable resin film increases, the infrared shielding performance of the cured resin film after thermal curing slightly improves, and the above requirement (1) can be easily satisfied.
[0104] Specifically, the thickness of the curable resin film is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more.
[0105] From the viewpoint of suppressing contamination due to bleeding during pasting, the thickness of the curable resin film is preferably 250 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less.
[0106] The curable resin film may be a single layer (monolayer) or may be a multilayer of two or more layers. When the curable resin film is a multilayer, the multilayers may be the same or different from each other, and the combination of the multilayers is not particularly limited.
[0107] For example, the curable resin film may be composed of multiple layers, and near-infrared shielding particles such as a black pigment may be contained only in at least one layer (for example, the outermost layer).
[0108] It should be noted that the “thickness of the curable resin film” refers to the thickness of the entire curable resin film. For example, the thickness of a multi-layered curable resin film refers to the total thickness of all layers constituting the curable resin film.
[0109] <Preferred use of the curable resin film of the present embodiment>
[0110] The curable resin film of the present embodiment can be used to form a cured resin film as a protective film on the bump formation surface of a semiconductor chip having a bump formation surface provided with bumps.
[0111] Here, from the perspective of improving the strength of the semiconductor chip and making it easier to suppress malfunctions of the semiconductor chip caused by near-infrared rays, the curable resin film of this embodiment is preferably used to form a curable resin film as a protective film on both the bump forming surface and the side surface of a semiconductor chip having a bump forming surface with bumps.
[0112] From such a viewpoint, the curable resin film of the present embodiment preferably satisfies the requirement (2) described below in addition to the requirement (1) described above.
[0113] (Requirement (2))
[0114] Requirement (2) is defined as follows.
[0115] Requirement (2): A test piece of the curable resin film having a diameter of 25 mm and a thickness of 1 mm is strained under the conditions of a temperature of 90°C and a frequency of 1 Hz, and the storage modulus of the test piece is measured. The storage modulus of the test piece when the strain of the test piece is 1% is set to Gc1, and the storage modulus of the test piece when the strain of the test piece is 300% is set to Gc300. At this time, the value of X calculated by the following formula (i) is greater than 10 and less than 10,000.
[0116] X=Gc1 / Gc300····(i)
[0117] From the viewpoint of forming a protective film with excellent coating properties, the upper limit of the X value specified in requirement (2) is preferably 5,000 or less, more preferably 2,000 or less, further preferably 1,000 or less, further preferably 500 or less, further preferably 300 or less, further preferably 100 or less, further preferably 80 or less.
[0118] In addition, from the viewpoint of improving embedding properties of the semiconductor chip manufacturing wafer into the groove portion, the lower limit of the value of X specified in the requirement (2) is preferably 20 or more, and more preferably 30 or more.
[0119] In the curable resin film of the present embodiment, Gc1 is not particularly limited as long as the value of X defined in the requirement (2) is 10 or more and less than 10,000.
[0120] Among them, Gc1 is preferably 1×10 2 ~1×10 6 Pa, more preferably 2×10 3 ~7×10 5 Pa, more preferably 3×10 3 ~5×10 5 Pa.
[0121] In the curable resin film of the present embodiment, Gc300 is not particularly limited as long as the X value is 10 or more and less than 10,000.
[0122] Among them, from the viewpoint of improving the embedding property of the curable resin film into the bump base and into the groove of the wafer for manufacturing the semiconductor chip after the bump penetrates the curable resin film, Gc300 is preferably 10 to 15,000 Pa, more preferably 30 to 10,000 Pa, and further preferably 60 to 5,000 Pa.
[0123] The curable resin film of the present embodiment is formed into a cured resin film by curing based on heating or energy ray irradiation. The curable resin film of the present embodiment may be a thermosetting resin film cured by heating, or an energy ray curable resin film cured by energy ray irradiation, and is preferably a thermosetting resin film from the viewpoint of operability, etc.
[0124] Hereinafter, the configuration of the thermosetting resin film of the present embodiment will be described in detail in conjunction with conditions for satisfying the above requirement (I) and further satisfying the above requirement (2).
[0125] [Thermosetting resin film]
[0126] The thermosetting resin film of the present embodiment forms a cured resin film by curing by heating.
[0127] The thermosetting resin film of the present embodiment contains a polymer component (A) and a thermosetting component (B). The thermosetting resin film of the present embodiment can be formed from, for example, a thermosetting resin composition containing a polymer component (A) and a thermosetting component (B).
[0128] The polymer component (A) is a component that can be regarded as a polymerizable compound formed by a polymerization reaction. In addition, the thermosetting component (B) is a component that can be triggered by heat to undergo a curing (polymerization) reaction. It should be noted that the curing (polymerization) reaction also includes a condensation reaction.
[0129] <Polymer component (A)>
[0130] The thermosetting resin film and the thermosetting resin composition contain a polymer component (A).
[0131] The polymer component (A) is a polymer compound for imparting film-forming properties, flexibility, etc. to the thermosetting resin film. One polymer component (A) may be used alone or in combination of two or more. When two or more polymer components (A) are used in combination, their combination and ratio may be arbitrarily selected.
[0132] Examples of the polymer component (A) include acrylic resins, polyarylate resins, polyvinyl acetal, polyester, urethane resins (resins having urethane bonds), acrylic urethane resins, silicone resins (resins having siloxane bonds), rubber resins (resins having rubber structures), phenoxy resins, and thermosetting polyimides.
[0133] Among them, acrylic resins, polyarylate resins, and polyvinyl acetal are preferred.
[0134] Examples of the acrylic resin include known acrylic polymers.
[0135] The weight average molecular weight (Mw) of the acrylic resin is preferably 10,000 to 2,000,000, more preferably 300,000 to 1,500,000, and even more preferably 500,000 to 1,000,000.
[0136] By making the weight average molecular weight of the acrylic resin above the above lower limit, it is easy to improve the shape stability (time stability during storage) of the thermosetting resin film. In addition, by making the weight average molecular weight of the acrylic resin below the above upper limit, the thermosetting resin film is easy to follow the concave-convex surface of the adherend, for example, it is easy to suppress the generation of gaps between the adherend and the thermosetting resin film. Therefore, the coating property of the bump forming surface of the semiconductor wafer becomes good, and the embedding property into the groove portion is also easy to improve. Therefore, it is easy to meet the above requirement (2).
[0137] The glass transition temperature (Tg) of the acrylic resin is preferably -60 to 70°C, more preferably -40 to 50°C, and even more preferably -30 to 30°C from the viewpoint of adhesion and handling properties of the thermosetting resin film.
[0138] Examples of acrylic resins include polymers of one or more (meth)acrylates, and copolymers of two or more monomers selected from (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-methylol acrylamide.
[0139] Examples of the (meth)acrylates constituting the acrylic resin include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and isononyl (meth)acrylate. , alkyl (meth)acrylates whose alkyl groups constituting the alkyl esters are chain structures having 1 to 18 carbon atoms, such as decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate);
[0140] Cycloalkyl (meth)acrylates such as isobornyl (meth)acrylate and dicyclopentyl (meth)acrylate;
[0141] Aralkyl (meth)acrylates such as benzyl (meth)acrylate;
[0142] Cycloalkenyl (meth)acrylates such as dicyclopentenyl (meth)acrylate;
[0143] Cycloalkenyloxyalkyl (meth)acrylates such as dicyclopentenyloxyethyl (meth)acrylate;
[0144] (Meth)acrylic acid imide;
[0145] Glycidyl (meth)acrylates such as glycidyl (meth)acrylate;
[0146] (meth)acrylates containing a hydroxy group, such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate;
[0147] (Meth)acrylates containing a substituted amino group such as N-methylaminoethyl (meth)acrylate, and the like.
[0148] In the present specification, the "substituted amino group" refers to a group in which one or two hydrogen atoms of an amino group are substituted with a group other than a hydrogen atom.
[0149] Among them, from the viewpoint of the film-forming property of the thermosetting resin film and the adhesion of the thermosetting resin film to the protective film-forming surface of the semiconductor chip, a copolymer composed of a (meth)acrylic acid alkyl ester whose alkyl group constituting the alkyl ester is a chain structure with 1 to 18 carbon atoms, a glycidyl group-containing (meth)acrylic acid ester, and a hydroxyl-containing (meth)acrylic acid ester is preferably used. A copolymer composed of a (meth)acrylic acid alkyl ester whose alkyl group constituting the alkyl ester is a chain structure with 1 to 4 carbon atoms, a glycidyl group-containing (meth)acrylic acid ester, and a hydroxyl-containing (meth)acrylic acid ester is more preferably used. A copolymer composed of a combination of butyl acrylate, methyl acrylate, glycidyl acrylate, and 2-hydroxyethyl acrylate is further preferred.
[0150] The acrylic resin may be, for example, a resin obtained by copolymerizing, in addition to (meth)acrylate, one or more monomers selected from (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-methylol acrylamide.
[0151] The monomers constituting the acrylic resin may be used alone or in combination of two or more. When the monomers constituting the acrylic resin are two or more, the combination and ratio thereof may be arbitrarily selected.
[0152] As the polyarylate resin in the polymer component (A), known polyarylate resins can be mentioned, for example, resins having a basic structure of polycondensation of dihydric phenol and dibasic acid such as phthalic acid and carboxylic acid, among which polycondensation products of bisphenol A and phthalic acid, poly-4,4'-isopropylidene diphenylene terephthalate / isophthalate copolymers, and derivatives thereof are preferred.
[0153] Examples of the polyvinyl acetal in the polymer component (A) include known polyvinyl acetals.
[0154] Among them, preferred examples of polyvinyl acetal include polyvinyl formal and polyvinyl butyral, and polyvinyl butyral is more preferred.
[0155] Examples of the polyvinyl butyral include polyvinyl butyrals having structural units represented by the following formulae (i)-1, (i)-2, and (i)-3.
[0156] [Chemical formula 1]
[0157]
[0158] (wherein, l, m and n are each independently an integer greater than 1.)
[0159] The weight average molecular weight (Mw) of polyvinyl acetal is preferably 5,000 to 200,000, more preferably 8,000 to 100,000. By making the weight average molecular weight of polyvinyl acetal above the above lower limit, it is easy to improve the shape stability (time stability during storage) of the thermosetting resin film. In addition, by making the weight average molecular weight of polyvinyl acetal below the above upper limit, the thermosetting resin film is easy to follow the uneven surface of the adherend, for example, it is easy to suppress the generation of gaps between the adherend and the thermosetting resin film. Therefore, the coating of the bump forming surface of the semiconductor chip becomes good, and it is also easy to improve the embedding property into the groove portion. Therefore, the above requirement (2) can be easily met.
[0160] The glass transition temperature (Tg) of polyvinyl acetal is preferably 40 to 80°C, more preferably 50 to 70°C, from the viewpoint of film-forming properties of a thermosetting resin film and protrusion properties of the bump head tops.
[0161] Here, in this specification, "bump head protrusion" refers to the performance of the bump penetrating the thermosetting resin film for forming a protective film when the thermosetting resin film is attached to the wafer with bumps, also called the bump head penetration.
[0162] The ratio of three or more monomers constituting polyvinyl acetal can be arbitrarily selected.
[0163] The content of the polymer component (A) is preferably 2 to 30% by mass, more preferably 3 to 25% by mass, and even more preferably 3 to 15% by mass, based on the total amount of the effective ingredients of the thermosetting resin composition.
[0164] The polymer component (A) may also belong to the thermosetting component (B). In the present embodiment, when the thermosetting resin composition contains such components belonging to both the polymer component (A) and the thermosetting component (B), the thermosetting resin composition is regarded as containing both the polymer component (A) and the thermosetting component (B).
[0165] <Thermosetting component (B)>
[0166] The thermosetting resin film and the thermosetting resin composition contain a thermosetting component (B).
[0167] The thermosetting component (B) is a component for curing the thermosetting resin film to form a hard cured resin film.
[0168] The thermosetting component (B) may be used alone or in combination of two or more. When two or more thermosetting components (B) are used, the combination and ratio thereof may be arbitrarily selected.
[0169] As the thermosetting component (B), for example, epoxy thermosetting resin, thermosetting polyimide, polyurethane, unsaturated polyester and silicone resin can be listed. Among them, epoxy thermosetting resin is preferred. When the thermosetting component (B) is epoxy thermosetting resin, the protectiveness of the cured resin film and the protrusion of the top of the bump head can be improved, and the warping of the cured resin film can be suppressed.
[0170] The epoxy thermosetting resin comprises an epoxy resin (B1) and a thermosetting agent (B2).
[0171] The epoxy thermosetting resin may be used alone or in combination of two or more. When two or more epoxy thermosetting resins are used, their combination and ratio may be arbitrarily selected.
[0172] (Epoxy resin (B1))
[0173] The epoxy resin (B1) is not particularly limited, but from the viewpoint of more easily exerting the effects of the present invention, it is preferred to use a combination of an epoxy resin that is solid at room temperature (hereinafter also referred to as a solid epoxy resin) and an epoxy resin that is liquid at room temperature (hereinafter also referred to as a liquid epoxy resin).
[0174] In addition, in this specification, "normal temperature" means 5-35 degreeC, Preferably it is 15-25 degreeC.
[0175] The liquid epoxy resin is not particularly limited as long as it is liquid at room temperature, and examples thereof include bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, glycidyl ester epoxy resin, biphenyl epoxy resin, phenylene skeleton epoxy resin, etc. Among them, bisphenol A epoxy resin is preferred.
[0176] The liquid epoxy resin may be used alone or in combination of two or more. When two or more liquid epoxy resins are used, their combination and ratio may be arbitrarily selected.
[0177] The epoxy equivalent of the liquid epoxy resin is preferably 200 to 600 g / eq, more preferably 250 to 550 g / eq, and further preferably 300 to 500 g / eq.
[0178] In addition, the epoxy equivalent in this embodiment can be measured according to JIS K 7236:2009.
[0179] The solid epoxy resin is not particularly limited as long as it is solid at room temperature, and examples thereof include biphenyl epoxy resin, bisphenol A epoxy resin, bisphenol F epoxy resin, o-cresol novolac epoxy resin, dicyclopentadiene epoxy resin, naphthalene epoxy resin, anthracene epoxy resin, fluorene epoxy resin, etc. Among them, naphthalene epoxy resin, dicyclopentadiene epoxy resin, and fluorene epoxy resin are preferred, and naphthalene epoxy resin and dicyclopentadiene epoxy resin are more preferred.
[0180] The solid epoxy resin may be used alone or in combination of two or more. When two or more solid epoxy resins are used, their combination and ratio may be arbitrarily selected.
[0181] The epoxy equivalent of the solid epoxy resin is preferably 150 to 450 g / eq, more preferably 150 to 400 g / eq.
[0182] The ratio [(x) / (y)] of the content of the liquid epoxy resin (x) to the content of the solid epoxy resin (y) is preferably 0.01 to 10.0, more preferably 0.02 to 8.0, and even more preferably 0.03 to 6.0 in terms of mass ratio. When the ratio [(x) / (y)] is within the above range, it is easy to suppress the generation of cutting chips when the cured resin film is cut with a cutter, thereby improving processability.
[0183] The number average molecular weight of the epoxy resin (B1) is not particularly limited, but is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000 from the viewpoint of curability of the thermosetting resin film and strength and heat resistance of the cured resin film after curing.
[0184] (Thermosetting agent (B2))
[0185] The thermosetting agent (B2) functions as a curing agent for the epoxy resin (B1).
[0186] As the thermosetting agent (B2), for example, a compound having two or more functional groups capable of reacting with an epoxy group in one molecule can be cited. As the above functional group, for example, a phenolic hydroxyl group, an alcoholic hydroxyl group, an amino group, a carboxyl group, and a group formed by an acid anhydride of an acid group can be cited, preferably a phenolic hydroxyl group, an amino group, or a group formed by an acid anhydride of an acid group, more preferably a phenolic hydroxyl group or an amino group.
[0187] Examples of the phenolic curing agent having a phenolic hydroxyl group in the thermosetting agent (B2) include polyfunctional phenolic resins, biphenol, novolac-type phenolic resins, dicyclopentadiene-based phenolic resins, and aralkylphenolic resins.
[0188] Among the thermosetting agents (B2), examples of amine-based curing agents having an amino group include dicyandiamide (hereinafter, sometimes abbreviated to "DICY") and the like.
[0189] Among them, a phenolic curing agent having a phenolic hydroxyl group is preferred, and a novolac-type phenolic resin is more preferred.
[0190] In the thermosetting agent (B2), for example, the number average molecular weight of resin components such as polyfunctional phenol resins, novolac phenol resins, dicyclopentadiene phenol resins and aralkylphenol resins is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000.
[0191] In the thermosetting agent (B2), the molecular weight of non-resin components such as biphenol and dicyandiamide is not particularly limited, but is preferably 60 to 500, for example.
[0192] The thermosetting agent (B2) may be used alone or in combination of two or more. When two or more thermosetting agents (B2) are used, their combination and ratio may be arbitrarily selected.
[0193] In the thermosetting resin composition, the content of the thermosetting agent (B2) is preferably 0.010 to 200 parts by mass, more preferably 0.020 to 150 parts by mass, further preferably 0.050 to 100 parts by mass, and further preferably 0.10 to 77 parts by mass, relative to 100 parts by mass of the epoxy resin (B1). By making the content of the thermosetting agent (B2) above the above lower limit, the curing of the thermosetting resin film is easier to carry out. In addition, by making the content of the thermosetting agent (B2) below the above upper limit, the moisture absorption rate of the thermosetting resin film is reduced, and the reliability of the package obtained using the thermosetting resin film is further improved.
[0194] In the thermosetting resin composition, from the viewpoint of improving the protective properties of the cured resin film, the content of the thermosetting component (B) (the total content of the epoxy resin (B1) and the thermosetting agent (B2)) is preferably 200 to 10,000 parts by mass, more preferably 300 to 5,000 parts by mass, further preferably 400 to 2,000 parts by mass, and further preferably 500 to 1,000 parts by mass, relative to 100 parts by mass of the polymer component (A).
[0195] <Curing accelerator (C)>
[0196] The thermosetting resin film and the thermosetting resin composition may contain a curing accelerator (C).
[0197] The curing accelerator (C) is a component for adjusting the curing speed of the thermosetting resin composition.
[0198] Preferred curing accelerators (C) include, for example, tertiary amines such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; imidazoles (imidazoles in which one or more hydrogen atoms are replaced by groups other than hydrogen atoms) such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; organic phosphines (phosphines in which one or more hydrogen atoms are replaced by organic groups) such as tributylphosphine, diphenylphosphine, and triphenylphosphine; tetraphenylphosphine; Tetraphenyl borate, triphenylphosphine tetraphenyl borate and other tetraphenyl borate, etc.
[0199] Among them, from the viewpoint of more easily exerting the effects of the present invention, imidazoles are preferred, and 2-phenyl-4,5-dihydroxymethylimidazole is more preferred.
[0200] The curing accelerator (C) may be used alone or in combination of two or more. When two or more curing accelerators (C) are used, their combination and ratio may be arbitrarily selected.
[0201] In the thermosetting resin composition, when a curing accelerator (C) is used, the content of the curing accelerator (C) is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the content of the thermosetting component (B). By making the content of the curing accelerator (C) above the above lower limit, it is easy to more significantly obtain the effect brought about by the use of the curing accelerator (C). In addition, by making the content of the curing accelerator (C) below the above upper limit, for example, the inhibitory effect of the high-polarity curing accelerator (C) moving toward the bonding interface side with the adherend in the thermosetting resin film under high temperature / high humidity conditions and segregation is increased, and the reliability of the package obtained using the thermosetting resin film is further improved.
[0202] <Filling material (D)>
[0203] The thermosetting resin film and the thermosetting resin composition may contain a filler (D).
[0204] By containing the filler (D), it is easy to adjust the thermal expansion coefficient of the cured resin film obtained by curing the thermosetting resin film to an appropriate range, and the reliability of the package obtained using the thermosetting resin film is further improved. In addition, by making the thermosetting resin film contain the filler (D), the moisture absorption rate of the cured resin film can also be reduced and the heat dissipation can be improved.
[0205] The filler (D) may be any of an organic filler and an inorganic filler, and is preferably an inorganic filler. Preferred inorganic fillers include, for example, powders of silica, talc, calcium carbonate, boron nitride, etc.; beads obtained by sphericalizing these inorganic fillers; surface-modified products of these inorganic fillers; single crystal fibers of these inorganic fillers; glass fibers, etc. Among them, the inorganic filler is preferably silica.
[0206] The filler (D) may be used alone or in combination of two or more.
[0207] When there are two or more fillers (D), their combination and ratio can be arbitrarily selected.
[0208] From the viewpoint of suppressing the peeling of the cured resin film from the chip due to thermal expansion and thermal contraction, when the filler (D) is used, the content of the filler (D) is preferably 5 to 50% by mass, more preferably 7 to 40% by mass, and even more preferably 10 to 30% by mass, based on the total amount of the effective ingredients of the thermosetting resin composition.
[0209] The average particle size of the filler (D) is preferably 5 nm to 1000 nm, more preferably 5 nm to 500 nm, and even more preferably 10 nm to 300 nm.
[0210] In the present specification, the particle size of the filler (D) refers to an arithmetic average particle size obtained by randomly selecting and measuring the particle sizes of a plurality of primary particles of the filler (D) observed with an electron microscope and calculating the average value thereof.
[0211] (Energy ray curable resin (E))
[0212] The thermosetting resin film and the thermosetting resin composition may contain an energy ray curable resin (E).
[0213] When the thermosetting resin film contains the energy ray-curable resin (E), the properties can be changed by irradiation with energy rays.
[0214] The energy-curable resin (E) is a resin obtained by polymerizing (curing) an energy-curable compound. Examples of the energy-curable compound include compounds having at least one polymerizable double bond in the molecule, preferably acrylate compounds having a (meth)acryloyl group.
[0215] Examples of the acrylate compounds include (meth)acrylates containing a chain aliphatic skeleton such as trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate; (meth)acrylates containing a cyclic aliphatic skeleton such as dicyclopentyl di(meth)acrylate; polyalkylene glycol (meth)acrylates such as polyethylene glycol di(meth)acrylate; oligoester (meth)acrylates; urethane (meth)acrylate oligomers; epoxy-modified (meth)acrylates; polyether (meth)acrylates other than the above-mentioned polyalkylene glycol (meth)acrylates; itaconic acid oligomers, and the like.
[0216] The weight average molecular weight of the energy ray curable compound is preferably 100 to 30,000, more preferably 300 to 10,000.
[0217] The energy-ray-curable compound used for polymerization may be used alone or in combination of two or more. When two or more energy-ray-curable compounds are used for polymerization, their combination and ratio may be arbitrarily selected.
[0218] When an energy-ray curable resin (E) is used, the content of the energy-ray curable resin (E) is preferably 1 to 95% by mass, more preferably 5 to 90% by mass, and even more preferably 10 to 85% by mass based on the total amount of the active ingredients of the thermosetting resin composition.
[0219] <Photopolymerization initiator (F)>
[0220] When the thermosetting resin film and the thermosetting resin composition contain an energy-ray curable resin (E), the thermosetting resin film and the thermosetting resin composition may contain a photopolymerization initiator (F) in order to efficiently carry out the polymerization reaction of the energy-ray curable resin (E).
[0221] Examples of the photopolymerization initiator (F) include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzil, bibenzyl, diacetyl, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-chloroanthraquinone.
[0222] The photopolymerization initiator (F) may be used alone or in combination of two or more. When two or more photopolymerization initiators (F) are used, the combination and ratio thereof may be arbitrarily selected.
[0223] In the thermosetting resin composition, the content of the photopolymerization initiator (F) is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 2 to 5 parts by mass, based on 100 parts by mass of the energy ray curable resin (E).
[0224] <Near infrared shielding particles (G)>
[0225] As described above, from the viewpoint of easily satisfying the above requirement (1), the thermosetting resin film and the thermosetting resin composition preferably contain near-infrared shielding particles (G).
[0226] As the near infrared shielding particles (G), there can be mentioned the examples given above as the near infrared shielding particles, and among them, the black pigment (G1) is preferred.
[0227] Preferred black pigments (G1) and the content of the black pigment (G1) are as described above.
[0228] <Additives (H)>
[0229] The thermosetting resin film and the thermosetting resin composition may contain an additive (H) within a range not impairing the effects of the present invention. The additive (H) may be a known additive and may be arbitrarily selected according to the purpose without particular limitation.
[0230] Preferred examples of the additive (H) include coupling agents, crosslinking agents, surfactants, plasticizers, antistatic agents, antioxidants, leveling agents, and gettering agents.
[0231] The additive (H) may be used alone or in combination of two or more. When two or more general-purpose additives (H) are used, their combination and ratio may be arbitrarily selected.
[0232] The content of the additive (H) is not particularly limited and can be appropriately selected according to the purpose.
[0233] <Solvent>
[0234] The thermosetting resin composition preferably further contains a solvent.
[0235] The thermosetting resin composition containing a solvent has good handleability.
[0236] The solvent is not particularly limited. Preferred solvents include, for example, hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutanol (2-methylpropane-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; amides (compounds having an amide bond) such as dimethylformamide and N-methylpyrrolidone, etc.
[0237] The solvent may be used alone or in combination of two or more. When two or more solvents are used, the combination and ratio thereof may be arbitrarily selected.
[0238] From the viewpoint of being able to more uniformly mix the components contained in the thermosetting resin composition, the solvent is preferably methyl ethyl ketone or the like.
[0239] <Method for preparing thermosetting resin composition>
[0240] The thermosetting resin composition can be prepared by blending the components constituting the composition.
[0241] The order of addition of each component when being matched is not particularly limited, and two or more components can also be added simultaneously. When a solvent is used, the solvent can be mixed with any matching component other than the solvent and the matching component can be diluted in advance and used, or any matching component other than the solvent can be mixed with the solvent and these matching components without diluting them in advance.
[0242] The method for mixing the components during compounding is not particularly limited, and can be appropriately selected from known methods such as a method of mixing by rotating a stirring bar or a stirring blade, a method of mixing using a stirrer, and a method of mixing by applying ultrasonic waves.
[0243] The temperature and time during addition and mixing of the components are not particularly limited as long as the components are not degraded, and may be appropriately adjusted, but the temperature is preferably 15 to 30°C.
[0244] [Compound sheet]
[0245] The curable resin film of this embodiment can be made into a composite sheet having a laminated structure in which the curable resin film and a release sheet are laminated. By making it into a composite sheet, the curable resin film can be stably supported / protected when the curable resin film is transported as a product package or when the curable resin film is transported in the manufacturing process of a semiconductor chip.
[0246] Figure 1 is a schematic cross-sectional view showing the structure of a composite sheet according to one embodiment, Figure 2 It is a schematic cross-sectional view showing the structure of a composite sheet in another embodiment.
[0247] Figure 1The composite sheet 10 includes a release sheet 1 and a curable resin film 2 provided on the release sheet 1. The release sheet 1 includes a substrate 3 and a release layer 4 provided to face the curable resin film 2.
[0248] Figure 2 The composite sheet 20 includes a release sheet 11 and a curable resin film 12 provided on the release sheet 11. The release sheet 11 may include an intermediate layer 15 between a substrate 13 and a release layer 14.
[0249] It should be noted that a laminated body in which the base material 13 , the intermediate layer 15 , and the release layer 14 are laminated in this order is suitable for use as a back grinding sheet.
[0250] Hereinafter, each layer constituting the release sheet used in the composite sheet of the present embodiment will be described.
[0251] <Base material>
[0252] The substrate is in a sheet or film shape, and examples of its constituent material include the following various resins.
[0253] Examples of the resin constituting the substrate include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylenes such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resins; ethylene copolymers (copolymers obtained using ethylene as a monomer) such as ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylate copolymers, and ethylene-norbornene copolymers; and vinyl chlorides such as polyvinyl chloride and vinyl chloride copolymers. Polyesters such as polyethylene terephthalate, polyethylene terephthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene 2,6-naphthalate, and fully aromatic polyesters in which all structural units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylates; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene ethers; polyphenylene sulfides; polysulfones; polyether ketones, etc.
[0254] In addition, examples of the resin constituting the substrate include polymer alloys such as a mixture of the above polyester and other resins. In the polymer alloy of the above polyester and other resins, the amount of the other resin is preferably small.
[0255] In addition, examples of the resin constituting the substrate include crosslinked resins obtained by crosslinking one or more of the resins listed above; and modified resins such as ionomers using one or more of the resins listed above.
[0256] The resin constituting the substrate may be used alone or in combination of two or more. When there are two or more resins constituting the substrate, the combination and ratio thereof may be arbitrarily selected.
[0257] The substrate may be a single layer (monolayer) or may be a plurality of layers of two or more. When the substrate is a plurality of layers, the plurality of layers may be the same or different from each other, and the combination of the plurality of layers is not particularly limited.
[0258] The thickness of the substrate is preferably 5 μm to 1,000 μm, more preferably 10 μm to 500 μm, further preferably 15 μm to 300 μm, and further preferably 20 μm to 150 μm.
[0259] Here, the “thickness of the substrate” refers to the thickness of the entire substrate. For example, the thickness of a substrate including multiple layers refers to the total thickness of all layers constituting the substrate.
[0260] The substrate is preferably a substrate with high thickness accuracy, that is, a substrate in which thickness deviation is suppressed regardless of the location. Among the above-mentioned constituent materials, as such a material with high thickness accuracy that can be used to constitute the substrate, for example, polyethylene, polyolefins other than polyethylene, polyethylene terephthalate, polybutylene terephthalate, ethylene-vinyl acetate copolymer, etc. can be cited.
[0261] The base material may contain various known additives such as a filler, a colorant, an antistatic agent, an antioxidant, an organic lubricant, a catalyst, a softener (plasticizer), etc., in addition to the above-mentioned main constituent materials such as the resin.
[0262] The substrate may be transparent or opaque, may be colored according to the purpose, or may have other layers deposited thereon.
[0263] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the above resin.
[0264] <Peeling layer>
[0265] The release layer has a function of imparting releasability to the release sheet. The release layer can be formed, for example, from a cured product of a release layer-forming composition containing a release agent.
[0266] The release agent is not particularly limited, and examples thereof include silicone resins, alkyd resins, acrylic resins, ethylene-vinyl acetate copolymers, etc. Among them, ethylene-vinyl acetate copolymers are preferred from the viewpoint of improving the protrusion of the bump head top and the peelability from the cured resin film.
[0267] The release layer may be a single layer (monolayer) or may be a plurality of layers. When the release layer is a plurality of layers, the plurality of layers may be the same or different from each other, and the combination of the plurality of layers is not particularly limited.
[0268] From the viewpoint of peelability and handling, the thickness of the peeling layer is preferably 3 to 50 μm, more preferably 5 to 30 μm. Here, the “thickness of the peeling layer” refers to the thickness of the entire peeling layer. For example, the thickness of a peeling layer composed of multiple layers refers to the total thickness of all layers constituting the peeling layer.
[0269] <Middle layer>
[0270] The intermediate layer is in the form of a sheet or a film, and its constituent material can be appropriately selected according to the purpose, and is not particularly limited. For example, in the case where the purpose is to suppress the deformation of the cured resin film caused by the shape of the bumps present on the semiconductor surface reflected in the protective film covering the semiconductor surface, as the preferred constituent material of the intermediate layer, from the viewpoint of high concave-convex tracking and further improved adhesion of the intermediate layer, a resin containing a structural unit derived from a monomer component such as urethane (meth) acrylate, olefin monomers such as α-olefins, etc. can be cited.
[0271] The intermediate layer may be a single layer (single layer) or may be a plurality of layers of two or more. When the intermediate layer is a plurality of layers, the plurality of layers may be the same or different from each other, and the combination of the plurality of layers is not particularly limited.
[0272] The thickness of the intermediate layer can be appropriately adjusted according to the height of the bump on the surface of the semiconductor to be protected. From the perspective of being able to easily absorb the impact of the high bump, it is preferably 50 μm to 600 μm, more preferably 70 μm to 500 μm, and further preferably 80 μm to 400 μm. Here, the "thickness of the intermediate layer" refers to the thickness of the entire intermediate layer. For example, the thickness of the intermediate layer composed of multiple layers refers to the total thickness of all layers constituting the intermediate layer.
[0273] <Method for producing composite sheet>
[0274] The composite sheet can be produced by sequentially laminating the above-mentioned layers in a corresponding positional relationship.
[0275] For example, when manufacturing a composite sheet, when a release layer or an intermediate layer is stacked on a substrate, the release layer or the intermediate layer can be stacked by coating a release layer forming composition or an intermediate layer forming composition on the substrate and drying it as needed or irradiating it with energy rays.
[0276] Examples of the coating method include spin coating, spray coating, bar coating, knife coating, roll coating, roll knife coating, blade coating, die coating, and gravure coating.
[0277] On the other hand, for example, when a thermosetting resin film is further laminated on a release layer laminated on a substrate, a thermosetting resin composition may be applied on the release layer to directly form a curable resin film.
[0278] Similarly, when a release layer is further laminated on the intermediate layer laminated on the substrate, the release layer can be directly formed by coating the release layer-forming composition on the intermediate layer.
[0279] As such, when a continuous two-layer laminated structure is formed using any composition, a composition can be further applied on the layer formed by the above-mentioned composition to form a new layer. Among these two layers, the layer to be laminated later is preferably formed in advance on another release film using the above-mentioned composition, and the exposed surface of the layer formed on the opposite side of the contact side with the above-mentioned release film is bonded to the exposed surface of the remaining layer formed, thereby forming a continuous two-layer laminated structure. At this time, the above-mentioned composition is preferably applied to the release treatment surface of the release film. The release film can be removed as needed after the laminated structure is formed.
[0280] [Method for manufacturing the first semiconductor chip]
[0281] The manufacturing method of the first semiconductor chip of the present embodiment is a manufacturing method of a semiconductor chip using the above-mentioned curable resin film, which can be applied when a curable resin film is formed as a protective film on both the bump forming surface and the side surface of a semiconductor chip having a bump forming surface with bumps. The manufacturing method of the first semiconductor chip generally includes: a step (S1) of preparing a wafer for semiconductor chip manufacturing, a step (S2) of pasting a curable resin film, a step (S3) of curing the curable resin film, and a step (S4) of singulation, and further includes: a step (S-BG) of grinding the back side of the wafer for semiconductor chip manufacturing.
[0282] Specifically, the method for manufacturing the first semiconductor chip of the present embodiment includes the following steps (S1) to (S4) in sequence.
[0283] Step (S1): a step of preparing a wafer for manufacturing a semiconductor chip, wherein a groove portion serving as a predetermined dividing line is formed on the bump forming surface of a semiconductor wafer having a bump forming surface with bumps so as not to reach the back surface;
[0284] Step (S2): a step of pressing and pasting the curable resin film on the bump-forming surface of the semiconductor chip manufacturing wafer, covering the bump-forming surface of the semiconductor chip manufacturing wafer with the curable resin film, and embedding the curable resin film in the groove portion formed in the semiconductor chip manufacturing wafer;
[0285] Step (S3): a step of curing the curable resin film to obtain a wafer for semiconductor chip production with a cured resin film;
[0286] Step (S4): a step of singulating the semiconductor chip manufacturing wafer with the cured resin film along the predetermined division line to obtain semiconductor chips in which at least the bump forming surface and the side surface are covered with the cured resin film.
[0287] Furthermore, the following step (S-BG) is included after the step (S2) and before the step (S3), after the step (S3) and before the step (S4), or during the step (S4).
[0288] Step (S-BG): a step of grinding the back surface of the semiconductor chip manufacturing wafer.
[0289] In the first semiconductor chip manufacturing method of this embodiment, a semiconductor chip can be manufactured in which both the bump formation surface and the side surface are covered and protected by the cured resin film and the near infrared shielding performance is imparted to both the bump formation surface and the side surface by the cured resin film.
[0290] It should be noted that "covered" here means that a cured resin film is formed along the shape of the semiconductor chip on at least the bump formation surface and side surfaces of one semiconductor chip. That is, the present invention is clearly different from a sealing technique in which a plurality of semiconductor chips are encapsulated in resin.
[0291] Hereinafter, the method for manufacturing the first semiconductor chip of the present embodiment will be described in detail step by step.
[0292] It should be noted that in the following description, a "semiconductor chip" is also simply referred to as a "chip", and a "semiconductor wafer" is also simply referred to as a "wafer".
[0293] In the following description, a curable resin film (curable resin film of the present embodiment) used to form a cured resin film as a protective film on both the bump forming surface and the side surface of a semiconductor chip is also referred to as a "curable resin film (X1)". Furthermore, a cured resin film formed by curing the "curable resin film (X1)" is also referred to as a "curable resin film (r1)". In addition, a curable resin film used to form a cured resin film as a protective film on the surface (back side) of a semiconductor chip opposite to the bump forming surface is also referred to as a "curable resin film for back side (X2)". Furthermore, a cured resin film formed by curing the "curable resin film for back side (X2)" is also referred to as a "curable resin film for back side (r2)".
[0294] In addition, a composite sheet for forming a cured resin film (r1) as a protective film on both the bump forming surface and the side surface of the semiconductor chip is also referred to as a "first composite sheet (α1)". The "first composite sheet (α1)" has a laminated structure in which a "first peeling sheet (Y1)" and a "curable resin film (X1)" are laminated.
[0295] In addition, the composite sheet for forming the back surface cured resin film (r2) as a protective film on the back surface of the semiconductor chip is also referred to as the "second composite sheet (α2)". The "second composite sheet (α2)" has a laminated structure in which the "second release sheet (Y2)" and the "back surface curable resin film (X2)" are laminated.
[0296] <Step (S1)>
[0297] For an example of a semiconductor wafer prepared in step (S1), Figure 3 A schematic cross-sectional view is shown in FIG.
[0298] In step ( S1 ), a semiconductor chip manufacturing wafer 30 is prepared in which grooves 23 serving as scheduled division lines are formed on the bump forming surface 21 a of a semiconductor wafer 21 having a bump forming surface 21 a with bumps 22 so as not to reach the back surface 21 b .
[0299] The shape of the bump 22 is not particularly limited, and can be any shape as long as it can contact and fix with the electrode on the substrate for chip mounting. Figure 3 In the embodiment, the bump 22 is set to be spherical, but the bump 22 may be a spheroid. The spheroid may be, for example, a spheroid extending in a vertical direction relative to the bump forming surface 21a of the wafer 21, or a spheroid extending in a horizontal direction relative to the bump forming surface 21a of the wafer 21. In addition, the bump 22 may be in a pillar shape.
[0300] The height of the bump 22 is not particularly limited and can be appropriately changed according to design requirements.
[0301] As an example, it is 30 μm to 300 μm, preferably 60 μm to 250 μm, and more preferably 80 μm to 200 μm.
[0302] It should be noted that the “height of the bump 22 ” refers to the height of a portion that is located at the highest position from the bump formation surface 21 a when focusing on one bump.
[0303] The number of the bumps 22 is not particularly limited and can be appropriately changed according to design requirements.
[0304] The wafer 21 is, for example, a semiconductor wafer having circuits such as wiring, capacitors, diodes, and transistors formed on its surface. The material of the wafer is not particularly limited, and examples thereof include silicon wafers, silicon carbide wafers, compound semiconductor wafers, glass wafers, and sapphire wafers.
[0305] The size of the wafer 21 is not particularly limited, but is generally 8 inches (200 mm in diameter) or larger, preferably 12 inches (300 mm in diameter) or larger, from the viewpoint of improving the batch processing efficiency. It should be noted that the shape of the wafer 21 is not limited to a circle, and may be a square, such as a square or a rectangle. In the case of a square wafer, the size of the wafer 21 is preferably such that the length of the longest side is larger than the above-mentioned size (diameter) from the viewpoint of improving the batch processing efficiency.
[0306] The thickness of the chip 21 is not particularly limited. From the viewpoint of easily suppressing the warping associated with the shrinkage when the curable resin film (X1) is cured and from the viewpoint of suppressing the grinding amount of the back side 21b of the chip 21 in the subsequent process and shortening the time required for back side grinding, the thickness is preferably 100 μm to 1,000 μm, more preferably 200 μm to 900 μm, and further preferably 300 μm to 800 μm.
[0307] The bump forming surface 21a of the semiconductor chip manufacturing wafer 30 prepared in step (S1) has a plurality of grooves 23 formed in a grid shape as predetermined division lines when the semiconductor chip manufacturing wafer 30 is singulated. The plurality of grooves 23 are cut grooves formed by using the dicing before grinding method, and are formed with a depth shallower than the thickness of the wafer 21 so that the deepest part of the groove 23 does not reach the back side 21b of the wafer 21. The plurality of grooves 23 can be formed by cutting using a conventionally known wafer cutting device equipped with a dicing blade.
[0308] It should be noted that the plurality of grooves 23 may be formed so that the manufactured semiconductor chip has a desired size and shape. The size of a semiconductor chip is generally about 0.5 mm×0.5 mm to 1.0 mm×1.0 mm, but is not limited to this size.
[0309] From the viewpoint of improving embedding properties of the curable resin film (X1), the width of the groove 23 is preferably 10 to 2,000 μm, more preferably 30 to 1,000 μm, further preferably 40 to 500 μm, and further preferably 50 to 300 μm.
[0310] The depth of the groove 23 can be adjusted according to the thickness of the wafer used and the required chip thickness, and is preferably 30 μm to 700 μm, more preferably 60 μm to 600 μm, and further preferably 100 μm to 500 μm.
[0311] The semiconductor chip manufacturing wafer 30 prepared in the step ( S1 ) is supplied to the step ( S2 ).
[0312] <Step (S2)>
[0313] Figure 4 The outline of step (S2) is shown in FIG.
[0314] In step ( S2 ), the curable resin film ( X1 ) is pressed and attached to the bump formation surface 21 a of the wafer 30 for semiconductor chip fabrication.
[0315] Here, from the viewpoint of operability, the curable resin film (X1) can be used as a first composite sheet (α1) having a laminated structure in which a first peeling sheet (Y1) and a curable resin film (X1) are laminated. When the first composite sheet (α1) is used, the curable resin film (X1) of the first composite sheet (α1) is pressed and pasted on the bump forming surface 21a of the semiconductor chip manufacturing wafer 30 as an adhesive surface.
[0316] Through step (S2), Figure 4 As shown, the bump formation surface 21 a of the semiconductor chip manufacturing wafer 30 is covered with the curable resin film ( X1 ), and the curable resin film ( X1 ) is embedded in the groove portion 23 formed in the semiconductor chip manufacturing wafer 30 .
[0317] From the perspective of improving the embedding property of the curable resin film (X1) into the groove 23, the pressing pressure when the curable resin film (X1) is pasted to the wafer 30 for semiconductor chip manufacturing is preferably 1 kPa to 200 kPa, more preferably 5 kPa to 150 kPa, and further preferably 10 kPa to 100 kPa.
[0318] It should be noted that the pressing force when the curable resin film (X1) is pasted to the semiconductor chip manufacturing wafer 30 can be appropriately changed from the initial stage to the final stage of pasting. For example, from the perspective of making the embedding property of the curable resin film (X1) into the groove portion 23 better, it is preferred to make the pressing force lower at the initial stage of pasting and gradually increase the pressing force.
[0319] In addition, when the curable resin film (X1) is pasted onto the wafer 30 for manufacturing a semiconductor chip, if the curable resin film (X1) is a thermosetting resin film, it is preferably heated from the perspective of making the curable resin film (X1) better embedded in the groove portion 23.
[0320] As a specific heating temperature (sticking temperature), 50°C to 150°C is preferable, 60°C to 130°C is more preferable, and 70°C to 110°C is further preferable.
[0321] In addition, the said heat treatment performed on the curable resin film (X1) is not included in the curing process of the curable resin film (X1).
[0322] In addition, when the curable resin film (X1) is attached to the semiconductor chip manufacturing wafer 30, it is preferably carried out in a reduced pressure environment. As a result, the groove 23 becomes negative pressure, and it is easy to make the curable resin film (X1) spread throughout the entire groove 23. As a result, the embedding property of the curable resin film (X1) into the groove 23 becomes better. As a specific pressure of the reduced pressure environment, it is preferably 0.001kPa to 50kPa, more preferably 0.01kPa to 5kPa, and further preferably 0.05kPa to 1kPa.
[0323] <Step (S3)>
[0324] Figure 5 The outline of step (S3) is shown in FIG.
[0325] In step ( S3 ), the curable resin film ( X1 ) is cured to obtain a semiconductor chip manufacturing wafer 30 with a cured resin film ( r1 ).
[0326] The cured resin film (r1) formed by curing the curable resin film (X1) is stronger than the curable resin film (X1) at room temperature. Therefore, the bump base portion is well protected by forming the cured resin film (r1).
[0327] Depending on the type of curable component contained in the curable resin film (X1), curing of the curable resin film (X1) can be performed by either thermal curing or curing by irradiation with energy rays.
[0328] It should be noted that, in the present specification, "energy rays" refer to rays having energy quanta among electromagnetic waves or charged particle beams, and examples thereof include ultraviolet rays and electron beams, and ultraviolet rays are preferred.
[0329] As conditions for thermal curing, the curing temperature is preferably 90° C. to 200° C., and the curing time is preferably 1 hour to 3 hours.
[0330] The conditions for curing by energy ray irradiation can be appropriately set according to the type of energy ray used. For example, when ultraviolet rays are used, the illuminance is preferably 170 mw / cm 2 ~250mw / cm 2 The light intensity is preferably 300 mJ / cm 2 ~3,000mJ / cm 2 .
[0331] Here, in the process of curing the curable resin film (X1) to form the cured resin film (r1), from the perspective of removing bubbles that may enter when the groove portion 23 is buried with the curable resin film (X1) in the removal step (S2), it is preferred that the curable resin film (X1) is a thermosetting resin film.
[0332] <Step (S4)>
[0333] Figure 6 The outline of step (S4) is shown in FIG.
[0334] In step ( S4 ), the portion of the cured resin film ( r1 ) formed in the groove portion 23 of the semiconductor chip manufacturing wafer 30 with the cured resin film ( r1 ) is cut along the planned dividing line.
[0335] The cutting is performed, for example, by knife dicing, etc. Thus, a semiconductor chip 40 in which at least the bump formation surface 21 a and the side surfaces are covered with the cured resin film ( r1 ) can be obtained.
[0336] Since the bump forming surface 21a and the side of the semiconductor chip 40 are covered by the cured resin film (r1), they have excellent strength. In addition, since the bump forming surface 21a and the side are continuously covered by the cured resin film (r1) without gaps, the bonding surface (interface) between the bump forming surface 21a and the cured resin film (r1) is not exposed on the side of the semiconductor chip 40. In the bonding surface (interface) between the bump forming surface 21a and the cured resin film (r1), the exposed portion exposed on the side of the semiconductor chip 40 is likely to become the starting point of film peeling. Since the semiconductor chip 40 of this embodiment does not have this exposed portion, during the process of cutting the semiconductor chip manufacturing wafer 30 to manufacture the semiconductor chip 40 and after manufacturing, film peeling caused by the exposed portion is not likely to occur. Therefore, a semiconductor chip 40 in which the peeling of the cured resin film (r1) as a protective film is suppressed can be obtained.
[0337] Here, when the curable resin film (X1) of the present embodiment contains a black pigment, the unevenness caused by the cut groove (hereinafter also referred to as "cut") defined by the groove portion 23 can be clearly identified on the wafer surface, so the processability in the step (S4) is improved. That is, the black pigment can achieve the effect of killing two birds with one stone, that is, making the near-infrared light shielding property of the curable resin film (r1) good and improving the processability.
[0338] It should be noted that from the perspective of improving the incision recognition and the perspective of improving the near-infrared light-shielding property, the content of the black pigment in the curable resin film is preferably 0.7% by mass or more, more preferably 1.0% by mass or more, and further preferably 1.5% by mass or more, based on the total amount of the curable resin film.
[0339] <Process (S-BG)>
[0340] Figure 7 An overview of the step (S-BG) is shown in FIG.
[0341] In the process (S-BG), if Figure 7 As shown in (1-a), first, the back surface 21b of the semiconductor chip manufacturing wafer 30 is ground in a state where the first composite sheet (α1) is attached. Figure 7 The "BG" in the formula refers to back grind. Figure 7 As shown in (1-b), the first release sheet (Y1) is peeled off from the first composite sheet (α1).
[0342] When grinding the back side 21b of the semiconductor chip manufacturing wafer 30, the grinding amount only needs to be enough to expose at least the bottom of the groove 23 of the semiconductor chip manufacturing wafer 30. Further grinding may be performed to grind the curable resin film (X1) or the cured resin film (r1) embedded in the groove 23 together with the semiconductor chip manufacturing wafer 30.
[0343] It should be noted that, in the present embodiment, the above-mentioned step (S-BG) is performed after the above-mentioned step (S2) and before the above-mentioned step (S3), but the above-mentioned step (S-BG) may also be performed after the above-mentioned step (S3) and before the above-mentioned step (S4), or may also be performed during the above-mentioned step (S4).
[0344] <Process (TB)>
[0345] In one aspect of the method for manufacturing the first semiconductor chip of the present embodiment, it is preferable to further include the following step (TB).
[0346] Step (TB): a step of forming a back surface protective film on the back surface of the wafer for manufacturing a semiconductor chip.
[0347] According to the manufacturing method of the above embodiment, a semiconductor chip 40 can be obtained in which at least the bump forming surface 21a and the side surface are covered with a cured resin film (r1). However, the back surface of the semiconductor chip 40 is exposed. Therefore, from the viewpoint of protecting the back surface of the semiconductor chip 40 and further improving the strength of the semiconductor chip 40, it is preferable to implement the above step (TB).
[0348] More specifically, the step (TB) preferably includes the following step (TB1) and the following step (TB2) in this order.
[0349] Step (TB1): Step of attaching a back surface curable resin film (X2) to the back surface of a wafer for producing a semiconductor chip
[0350] Step (TB2): a step of curing the back surface curable resin film (X2) to form a back surface cured resin film (r2)
[0351] It should be noted that step (TB1) is performed after step (S-BG). In addition, step (TB2) is performed before step (S4). Thus, in step (S4), the semiconductor wafer with a cured resin film whose back side is protected by the back side cured resin film (r2) is singulated to obtain a semiconductor chip whose bump forming surface and side surfaces are protected by the cured resin film (r1) and whose back side is protected by the back side cured resin film (r2).
[0352] In addition, in step (TB1), a second composite sheet (α2) having a laminated structure formed by laminating a second release sheet (Y2) and a curable resin film (X2) for the back surface can be used. Specifically, step (TB1) is preferably a step of laminating a second composite sheet (α2) having a laminated structure formed by laminating a second release sheet (Y2) and a curable resin film (X2) for the back surface to the back surface of a wafer for semiconductor chip manufacturing with the curable resin film (X2) for the back surface as the adhesive surface.
[0353] In this case, the timing of peeling the second release sheet (Y2) from the second composite sheet (α2) may be between the step (TB1) and the step (TB2) or after the step (TB2).
[0354] Here, when the second composite sheet (α2) is used in step (TB1), the release sheet (Y2) of the second composite sheet (α2) preferably functions as a dicing sheet while supporting the back surface curable resin film (X2).
[0355] In addition, by adhering the second composite sheet (α2) to the back side 21b of the semiconductor chip 30 with the cured resin film (r1) in step (S4), the second peeling sheet (Y2) functions as a cutting sheet during singulation based on dicing, making dicing easier.
[0356] Here, when the step (S3) is performed after the step (S-BG), the step (TB1) can be performed before the step (S3), and then the step (S3) and the step (TB2) can be performed simultaneously. That is, the curable resin film (X1) and the second curable resin film (X2) can be cured at the same time. Thus, the number of curing treatments can be reduced.
[0357] (Curable resin film for back surface (X2))
[0358] The second curable resin film (X2) may be any general curable resin film used to form a back surface protective film of a semiconductor chip, and may be, for example, the same material and structure as those of the curable resin film (X1).
[0359] However, since the back side of the semiconductor wafer is generally smooth without bumps or grooves, the back side curable resin film (X2) is not required to satisfy the requirement (2) which is a preferred condition for the curable resin film (X1). Therefore, the X value of the back side curable resin (X2) may be 18 or less, and may be 10,000 or more.
[0360] Here, from the viewpoint of imparting near infrared shielding performance also to the back surface side of the semiconductor chip, it is preferred that the second curable resin film (X2) also satisfies the above requirement (1).
[0361] Therefore, the second curable resin film (X2) preferably contains near-infrared shielding particles (G).
[0362] As the near infrared shielding particles (G), the examples given above as the near infrared shielding particles can be cited, and among them, the black pigment (G1) is preferred.
[0363] Preferred black pigments (G1) and the content of the black pigment (G1) are as described above.
[0364] <Process (U)>
[0365] One aspect of the method for manufacturing the first semiconductor chip of the present embodiment may further include the following step (U).
[0366] Step (U): a step of removing the cured resin film (r1) including the top of the bump or a portion of the cured resin film (r1) attached to the top of the bump to expose the top of the bump
[0367] Examples of the exposure process for exposing the top of the bump include etching processes such as wet etching processes and dry etching processes.
[0368] Here, as the dry etching process, for example, a plasma etching process or the like can be cited.
[0369] In addition, when the top of the bump is not exposed on the surface of the protective film, an exposure process may be performed for the purpose of retreating the protective film until the top of the bump is exposed.
[0370] The timing for carrying out step (U) is not particularly limited as long as the cured resin film (r1) is exposed, but is preferably after step (S3) and before step (S4) when the release sheet (Y1) and back grinding sheet are not attached.
[0371] [Method for manufacturing the second semiconductor chip]
[0372] The manufacturing method of a semiconductor chip using the above-mentioned curable resin film is not limited to a manufacturing method adopted when a cured resin film is formed as a protective film on both the bump forming surface and the side surface of a semiconductor chip having a bump forming surface with bumps as in the manufacturing method of the first semiconductor chip, but may also be a manufacturing method adopted when a cured resin film is formed as a protective film only on the bump forming surface of a semiconductor chip having a bump forming surface with bumps.
[0373] Hereinafter, a method for manufacturing the second semiconductor chip will be described as a manufacturing method used when a cured resin film as a protective film is formed only on the bump formation surface of a semiconductor chip having a bump formation surface provided with bumps.
[0374] The method for manufacturing the second semiconductor chip of the present embodiment includes the following steps (V1) to (V4) in sequence.
[0375] Step (V1): a step of preparing a semiconductor wafer having a bump formation surface having bumps;
[0376] Step (V2): a step of pressing and sticking the curable resin film onto the bump-forming surface of the semiconductor wafer to cover the bump-forming surface of the semiconductor wafer with the curable resin film;
[0377] Step (V3): a step of curing the curable resin film to obtain a semiconductor wafer with a cured resin film;
[0378] Step (V4): a step of dividing the semiconductor wafer with the cured resin film into individual pieces to obtain semiconductor chips in which the bump formation surfaces are covered with the cured resin film.
[0379] As the semiconductor wafer prepared in the step (V1), for example, there can be mentioned a semiconductor wafer similar to the semiconductor wafer 21 having the bump formation surface 21a having the bumps 22 described in the step (S1).
[0380] Step (V2) is the same as step (S2). It should be noted that by pressing and sticking the curable resin film to the bump formation surface of the semiconductor wafer, the entire bump formation surface including the bump base can be well covered with the curable resin film.
[0381] In addition, similarly to step (S2), from the viewpoint of workability, the curable resin film (X1) can be used as a first composite sheet (α1) having a laminated structure in which the first release sheet (Y1) and the curable resin film (X1) are laminated.
[0382] Step (V3) is the same as step (S3).
[0383] Figure 8 The outline of step (V4) is shown in FIG. Figure 8 In the process (S4) of the manufacturing method of the first semiconductor chip shown above, Figure 6 The components shown in FIG. 1 correspond to the components in FIG. 1 . Figure 6 Symbols with an apostrophe at the end of each symbol.
[0384] In step (V4), the semiconductor chip manufacturing wafer 30' with the first cured resin film (r1') is divided into individual pieces by cutting the semiconductor wafer 21' and the first cured resin film (r1') along imaginary planned dividing lines.
[0385] The singulation of the semiconductor wafer with the cured resin film in step (V4) can be performed by various methods used when semiconductor wafers are chipped (for example, blade dicing, laser dicing, stealth dicing (registered trademark) method, blade first dicing method, stealth first dicing method).
[0386] Here, the following step (V-BG) may be included after the step (V2) and before the step (V3), or after the step (V3) and before the step (V4).
[0387] Step (V-BG): a step of grinding the back surface of the semiconductor chip manufacturing wafer.
[0388] Among them, in the above-mentioned step (V4), when the stealth dicing (registered trademark) method, the blade first dicing method, or the stealth first dicing method is adopted, the above-mentioned step (V-BG) is preferably performed in the above-mentioned step (V4). Thereby, the semiconductor wafer with a cured resin film can be singulated and the semiconductor wafer can be thinned at the same time.
[0389] It should be noted that the method for manufacturing the second semiconductor chip of the present embodiment may include either or both of the step (TB) and the step (U).
[0390] When the above step (TB) is used, the back surface protective film can be formed on the back surface of the semiconductor wafer having the bump forming surface having the bumps. Therefore, the above step (TB) can be used after being changed to the following step (TA).
[0391] Step (TA): a step of forming a back surface protective film on the back surface of the semiconductor wafer having the bump formation surface having bumps.
[0392] In addition, more specifically, the step (TA) preferably includes the following step (TA1) and the following step (TA2) in this order.
[0393] Step (TA1): a step of attaching a back surface curable resin film (X2) to the back surface of the semiconductor wafer;
[0394] Step (TA2): a step of curing the curable resin film for back surface (X2) to form a cured resin film for back surface (r2).
[0395] [Semiconductor Chip]
[0396] The semiconductor chip of the present embodiment has a bump formation surface having bumps, and has a cured resin film formed by curing the curable resin film of the present embodiment on the bump formation surface.
[0397] Therefore, according to the present embodiment, a semiconductor chip having a bump forming surface with bumps can be provided, wherein the bump forming surface of the semiconductor chip has a cured resin film formed by curing the curable resin film and has a near infrared shielding function.
[0398] In addition, a semiconductor chip having a bump forming surface with bumps can be provided, wherein the bump forming surface of the semiconductor chip has a cured resin film formed by curing the curable resin film, and has a near infrared shielding function, and further has a back surface protective film.
[0399] The semiconductor chip of the present embodiment has a bump formation surface having bumps, and has a cured resin film formed by curing the curable resin film of the present embodiment on both the bump formation surface and the side surfaces.
[0400] The semiconductor chip of the present embodiment can be obtained by cutting the cured resin film embedded in the groove portion formed on the semiconductor chip manufacturing wafer along the planned dividing line and dividing the cured resin film into individual pieces. The cured resin film is a cured product of the curable resin film.
[0401] Therefore, according to the present embodiment, a semiconductor chip having a bump forming surface with bumps can be provided, wherein both the bump forming surface and the side surfaces of the semiconductor chip have a cured resin film formed by curing the curable resin film, and a near infrared shielding function is imparted.
[0402] In addition, a semiconductor chip having a bump forming surface with bumps can be provided, wherein both the bump forming surface and the side surface of the semiconductor chip have a cured resin film formed by curing the curable resin film, and a near infrared shielding function is imparted, and the semiconductor chip further has a back surface protective film.
[0403] In addition, when both the curable resin film and the back curable resin film contain black pigment, a sense of unity in color tone can be observed between the curable resin film formed by curing the curable resin film and the back curable resin film formed by curing the back curable resin film, which can improve the design. Moreover, near-infrared shielding properties can be imparted not only to the bump-forming surface and side surfaces of the semiconductor chip, but also to the back surface. That is, a semiconductor chip with excellent design and excellent near-infrared shielding properties can be obtained.
[0404] Example
[0405] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the following examples.
[0406] 1. Raw materials for producing the thermosetting resin film-forming composition
[0407] The raw materials used for producing the thermosetting resin film-forming composition are shown below.
[0408] (1) Polymer component (A)
[0409] (A)-1: Polyvinyl butyral having structural units represented by the following formulae (i)-1, (i)-2 and (i)-3 ("S-LEC BL-10" manufactured by Sekisui Chemical Co., Ltd., weight average molecular weight 25,000, glass transition temperature 59°C)
[0410] [Chemical formula 2]
[0411]
[0412] (Where, l 1 About 28 m 1 1 to 3, n 1 An integer between 68 and 74. )
[0413] (A)-2: Polyarylate ("Unifiner (registered trademark) M-2040" manufactured by Unitika Co., Ltd.)
[0414] (2) Epoxy resin (B1)
[0415] [Liquid epoxy resin]
[0416] (B1)-1: Liquid modified bisphenol A type epoxy resin ("EPICLON EXA-4850-150" manufactured by DIC Corporation, number average molecular weight 900, epoxy equivalent 450 g / eq)
[0417] [Solid epoxy resin]
[0418] (B1)-2: dicyclopentadiene type epoxy resin ("EPICLONHP-7200HH" manufactured by DIC Corporation, weight average molecular weight less than 20,000, epoxy equivalent 255 to 260 g / eq)
[0419] (B1)-3: Naphthalene-type epoxy resin ("EPICLON HP-5000" manufactured by DIC Corporation, epoxy equivalent 252 g / eq)
[0420] (B1)-4: Naphthalene-type epoxy resin ("EPICLON HP-4710" manufactured by DIC Corporation, epoxy equivalent 170 g / eq)
[0421] (B1)-5: Fluorene type epoxy resin ("OGSOL CG500" manufactured by Osaka Gas Chemical Co., Ltd., epoxy equivalent 300 g / eq)
[0422] (3) Thermal curing agent (B2)
[0423] (B2)-1: o-cresol type novolac resin ("PHENOLITE KA-1160" manufactured by DIC Corporation, hydroxyl equivalent 117 g / eq)
[0424] (4) Curing accelerator (C)
[0425] (C)-1: 2-phenyl-4,5-dihydroxymethylimidazole ("CUREZOL 2PHZ-PW" manufactured by Shikoku Chemical Industry Co., Ltd.)
[0426] (5) Filler (D)
[0427] (D)-1: Spherical silica modified with epoxy group (Admanano YA050C-MKK manufactured by Admatechs, average particle size 50 nm)
[0428] The average particle size of the filler (D) is an arithmetic average particle size obtained by randomly selecting and measuring the particle sizes of a plurality of primary particles of the black pigment observed with an electron microscope and calculating the average value thereof.
[0429] (6) Black pigment (G1)
[0430] (G1)-1: Carbon black (manufactured by Mitsubishi Chemical Corporation, “MA600B”, particle size 20 nm)
[0431] (G1)-2: Carbon black (Mitsubishi Chemical Corporation "#20", particle size 50 nm)
[0432] The particle size of the black pigment (G1) is an arithmetic average particle size obtained by randomly selecting and measuring the particle sizes of a plurality of primary particles of the black pigment observed with an electron microscope and calculating the average value thereof.
[0433] (7) Additives (H)
[0434] (H)-1: Surfactant (acrylic acid polymer, BYK-361N)
[0435] (H)-2: Silicone oil (aralkyl-modified silicone oil, "XF42-334" manufactured by Momentive Performance Materials Japan LLC)
[0436] 2. Production Examples 1 to 12 and Comparative Production Examples 1 to 8
[0437] 2-1-1. Production Example 1
[0438] (1) Production of Thermosetting Resin Film-Forming Composition (1)
[0439] By dissolving or dispersing the compounding formula 1 shown in Table 1 in methyl ethyl ketone and stirring at 23°C, a thermosetting resin film-forming composition (1) (hereinafter also referred to as "composition (1)") having a total concentration of all components other than the solvent of 60% by mass was obtained. It should be noted that the compounding amounts of the components other than the solvent shown here are all the compounding amounts of the target product without the solvent.
[0440] (2) Manufacturing of thermosetting resin film
[0441] A release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film having one side treated with silicone and subjected to a release treatment was used, the composition (1) obtained above was applied to the above-mentioned release-treated surface, and heated and dried at 120°C for 2 minutes, thereby forming a thermosetting resin film with a thickness of 45 μm (hereinafter also referred to as "F(1)-45").
[0442] In addition, in this Example, the thickness of each layer was measured at 23 degreeC using the constant pressure thickness gauge (model: "PG-02J", based on standard specification: JIS K 6783:2009, Z 1702:1994, Z 1709:1995) manufactured by Teclock Co., Ltd.
[0443] 2-1-2. Production Example 2
[0444] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(1)-10”) was formed by the same method as in Production Example 1 except that the application amount of the composition (1) was changed.
[0445] 2-1-3. Production Example 3
[0446] A thermosetting resin film having a thickness of 5 μm (hereinafter also referred to as “F(1)-5”) was formed by the same method as in Production Example 1 except that the application amount of the composition (1) was changed.
[0447] 2-1-4. Production Example 4
[0448] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(2)-45”) was formed by the same method as in Production Example 1 except that the compounding formula 1 shown in Table 1 was changed to the compounding formula 2.
[0449] 2-1-5. Production Example 5
[0450] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(2)-10”) was formed by the same method as in Production Example 4 except that the application amount of the composition (1) was changed.
[0451] 2-1-6. Production Example 6
[0452] A thermosetting resin film having a thickness of 5 μm (hereinafter also referred to as “F(2)-5”) was formed by the same method as in Production Example 4 except that the application amount of the composition (1) was changed.
[0453] 2-1-7. Production Example 7
[0454] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(3)-45”) was formed by the same method as in Production Example 1 except that the compounding formulation 1 shown in Table 1 was changed to the compounding formulation 3.
[0455] 2-1-8. Production Example 8
[0456] A thermosetting resin film having a thickness of 30 μm (hereinafter also referred to as “F(3)-30”) was formed by the same method as in Production Example 7 except that the application amount of the composition (1) was changed.
[0457] 2-1-9. Production Example 9
[0458] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(7)-45”) was formed by the same method as in Production Example 1 except that the compounding formulation 1 shown in Table 1 was changed to the compounding formulation 7.
[0459] 2-1-10. Production Example 10
[0460] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(7)-10”) was formed in the same manner as in Production Example 9 except that the application amount of the composition (1) was changed.
[0461] 2-1-11. Production Example 11
[0462] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(8)-45”) was formed by the same method as in Production Example 1 except that the compounding formulation 1 shown in Table 1 was changed to the compounding formulation 8.
[0463] 2-1-12. Production Example 12
[0464] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(8)-10”) was formed by the same method as in Production Example 11 except that the application amount of the composition (1) was changed.
[0465] 2-2-1. Comparative Manufacturing Example 1
[0466] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(3)-10”) was formed by the same method as in Production Example 7 except that the application amount of the composition (1) was changed.
[0467] 2-2-2. Comparative Manufacturing Example 2
[0468] A thermosetting resin film having a thickness of 5 μm (hereinafter also referred to as “F(3)-5”) was formed by the same method as in Production Example 7 except that the application amount of the composition (1) was changed.
[0469] 2-2-3. Comparative Manufacturing Example 3
[0470] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(4)-45”) was formed by the same method as in Production Example 1 except that the compounding formula 1 shown in Table 1 was changed to the compounding formula 4.
[0471] 2-2-4. Comparative Manufacturing Example 4
[0472] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(4)-10”) was formed in the same manner as in Comparative Production Example 3 except that the coating amount of the composition (1) was changed.
[0473] 2-2-5. Comparative Manufacturing Example 5
[0474] A thermosetting resin film having a thickness of 5 μm (hereinafter also referred to as “F(4)-5”) was formed in the same manner as in Comparative Production Example 3 except that the application amount of the composition (1) was changed.
[0475] 2-2-6. Comparative Manufacturing Example 6
[0476] A thermosetting resin film having a thickness of 45 μm (hereinafter also referred to as “F(5)-45”) was formed by the same method as in Production Example 1 except that the compounding formulation 1 shown in Table 1 was changed to the compounding formulation 5.
[0477] 2-2-7. Comparative Manufacturing Example 7
[0478] A thermosetting resin film having a thickness of 10 μm (hereinafter also referred to as “F(5)-10”) was formed in the same manner as in Comparative Production Example 6 except that the application amount of the composition (1) was changed.
[0479] 2-2-8. Comparative Manufacturing Example 8
[0480] A thermosetting resin film having a thickness of 5 μm (hereinafter also referred to as “F(5)-5”) was formed in the same manner as in Comparative Production Example 7 except that the application amount of the composition (1) was changed.
[0481] In addition, the description of "-" in the column of the contained component in Table 1 means that the compounding formulas 1 to 8 do not contain the component.
[0482] color
[0483]
[0484] 3. Evaluation 1 (Examples 1 to 12, Comparative Examples 1 to 8)
[0485] The following evaluations were performed using the thermosetting resin films obtained in Production Examples 1 to 12 and Comparative Production Examples 1 to 8.
[0486] 3-1. Evaluation of transmittance
[0487] A glass plate (manufactured by Matsunami Glass Industries, Ltd., "White Edge Polished No. 1", length 76 mm×width 26 mm×thickness 1 mm) was prepared and cut into half the length for use.
[0488] Then, the surface of the thermosetting resin film opposite to the surface provided with the release film was bonded to the glass plate under the following conditions using a laminating device ("Roll Laminator RSL-382S" manufactured by Japan Office Laminator Co., Ltd.).
[0489] Paste temperature: 60℃
[0490] Pasting speed: 1mm / sec
[0491] ·Paste pressure: 0.3MPa
[0492] Next, the release film was peeled off from the thermosetting resin film, heated for 240 minutes at 130°C and 0.5 MPa to be thermally cured, and naturally cooled to return to room temperature (25°C) to prepare a glass plate with a cured resin film. Then, the transmittance at 940nm and 800nm of the glass plate with the cured resin film was measured under the following conditions. It should be noted that when measuring the transmittance, the glass plate with the cured resin film was set so that the cured resin film side was the light-receiving surface.
[0493] ·Measurement device: UV-3600 series manufactured by Shimadzu Corporation
[0494] ·Measurement wavelength range: 190nm~2,000nm
[0495] Detector unit: Direct light reception
[0496] ·Measurement temperature: 25℃
[0497] 3-2. Evaluation of near infrared shielding properties 1
[0498] The glass plate with a cured resin film produced in the above-mentioned "3.1 Evaluation of transmittance" was used as a test piece.
[0499] Then, the test piece was placed 5 cm away from the laser output part of the laser device described below so that the surface direction of the test piece was perpendicular to the output direction of the laser. The test piece was placed so that the cured resin film side was the laser irradiation surface.
[0500] Laser irradiation device: Cobolt multi-wavelength laser (wavelength: 730nm, 760nm, 785nm, 808nm, 830nm, 940nm, 975nm)
[0501] Output wavelength: 940nm
[0502] Next, the test piece was irradiated with a laser beam having a wavelength of 940 nm, and the front camera of an iPhone 7 (manufactured by Apple) was activated to photograph the test piece from a position 10 cm away from the test piece (i.e., a position 15 cm away from the laser output portion), thereby evaluating the shielding property of near infrared rays. The evaluation was carried out at room temperature (23°C).
[0503] Then, the case where the infrared laser cannot be confirmed by the front camera is regarded as acceptable (A), and the case where the infrared laser is confirmed by the front camera is regarded as unacceptable (F).
[0504] If infrared laser light is not detected in the front camera, it means that the cured resin film has excellent near-infrared shielding properties. Conversely, if infrared laser light is detected in the front camera, it means that the cured resin film has poor near-infrared shielding properties.
[0505] 3-3. Evaluation of near infrared shielding properties 2
[0506] Two PHSs (personal handy-phone system, manufactured by DOCOMO, product name "AQUOS", receiving wavelength: 800 nm) were placed on a flat surface at a distance of 15 cm. Next, a glass plate with a cured resin film prepared in "3.1 Transmittance Evaluation" was used as a test piece and placed in front of one of the PHSs. The two PHSs were shielded by the test piece to confirm whether transmission and reception could be performed between the two PHSs.
[0507] Furthermore, the case where transmission and reception cannot be performed between the two PHSs is regarded as acceptable (A), and the case where transmission and reception can be performed between the two PHSs is regarded as unacceptable (F).
[0508] If transmission and reception cannot be performed between two PHSs, it means that the near-infrared shielding property of the cured resin film is excellent. On the contrary, if transmission and reception can be performed between two PHSs, it means that the near-infrared shielding property of the cured resin film is poor.
[0509] 4. Evaluation 2 (Examples 1, 4, 7, 9 and 11, and Comparative Examples 3 and 6)
[0510] The following evaluation was performed using the thermosetting resin films having a thickness of 45 μm obtained in Production Examples 1, 4 and 7, 9 and 11, and Comparative Production Examples 3 and 6.
[0511] 4-1. Measurement of Gc1 and Gc300 of Thermosetting Resin Film and Calculation of X Value
[0512] Twenty thermosetting resin films having a thickness of 45 μm were produced. Next, these thermosetting resin films were stacked, and the obtained stacked film was cut into a disk shape having a diameter of 25 mm, thereby producing a test piece of a thermosetting resin film having a thickness of 1 mm.
[0513] The setting position of the test piece in the viscoelasticity measuring device ("MCR301" manufactured by Anton Paar) is preheated at 80°C, the test piece of the thermosetting resin film obtained above is placed on the setting position, and the measuring fixture is abutted against the upper surface of the test piece, thereby fixing the test piece to the above setting position.
[0514] Next, the strain applied to the test piece was gradually increased within a range of 0.01% to 1000% at a temperature of 90°C and a measurement frequency of 1 Hz, and the storage modulus Gc of the test piece was measured. Then, the X value was calculated from the measured values of Gc1 and Gc300.
[0515] 4-2. Evaluation of incision identification
[0516] (1) Preparation of wafers for semiconductor chip production
[0517] As a wafer for producing semiconductor chips, a 12-inch silicon wafer (wafer thickness 750 μm) cut in half along a planned dividing line was used. The width of the half-cut portion (width of the groove portion) of the silicon wafer was 60 μm, and the depth of the groove was 230 μm.
[0518] (2) Evaluation method
[0519] One surface of a 45 μm-thick thermosetting resin film was pressed and bonded to the front surface side (half-cut formation surface) of a wafer for semiconductor chip production under the following conditions.
[0520] · Pasting device: BG tape laminator ("RAD-3510F / 8" manufactured by Lintec Corporation)
[0521] ·Paste pressure: 0.5MPa
[0522] Paste time: 43 seconds
[0523] Pasting speed: 7mm / sec
[0524] Paste temperature: 80℃
[0525] ·Roller pasting height: -200mm
[0526] Next, the wafer for semiconductor chip production to which the thermosetting resin film was attached was heated for 4 hours under the conditions of a temperature of 130° C. and a pressure of 0.5 MPa to be cured, thereby forming a cured resin film.
[0527] Then, the wafer for semiconductor chip production with the cured resin film was fixed to a dicing table of a dicing machine ("DFD6362" manufactured by DISCO Corporation), and it was confirmed whether the cut could be recognized by a camera attached to the dicing machine.
[0528] The case where the projections and recesses of the cut can be clearly identified is considered qualified "A", the case where the projections and recesses of the cut are generally clearly identified but not qualified "A" is considered qualified "B", and the case where the projections and recesses of the cut cannot be clearly identified is considered unqualified "F".
[0529] It should be noted that an example of an image (photograph) of a qualified "A" is shown in Fig. 9 , an example of an image (photo) of the case of unqualified "B" is shown in Fig.10 .
[0530] 4-3. Evaluation of design and film peeling
[0531] (1) Sample preparation
[0532] The wafer for semiconductor chip production with a cured resin film prepared in the above-mentioned "4-2. Evaluation of incision visibility" was ground on the back side of the wafer so that the thickness of the wafer for semiconductor chip production became 200 μm.
[0533] Using RAD-3600, a roll-shaped thermosetting resin film with a thickness of 25 μm sandwiched by a peeling film was pasted on the back of a wafer for semiconductor chip manufacturing at a workbench temperature of 70°C. Heating was performed at 130°C for 2 hours to obtain a cured resin film for the back. DC tape D-686H (manufactured by Lintec Co., Ltd.) was pasted on the side of the cured resin film for the back, and a blade cutter DFG6362 was used to cut along the predetermined dividing line by blade cutting, and the chip size was singulated into 6 mm square chips. The chip was peeled off from the DC tape, and the chip was observed using an optical microscope ("VHX-1000" manufactured by Keyence).
[0534] The thermosetting resin film for the back surface in a roll shape and having a thickness of 25 μm sandwiched between release films was produced by the following procedure.
[0535] The polymer component (a), epoxy resin (b1)-1, epoxy resin (b1)-2, curing agent (b2), curing accelerator (c), filler (d), coupling agent (e) and colorant (J) are dissolved or dispersed in methyl ethyl ketone in such a manner that their contents (solid content, parts by mass) are 150 / 70 / 30 / 5 / 2 / 320 / 2 / 18 (solid weight ratio), and stirred at 23°C to prepare a composition (2) for forming a thermosetting resin film for the back surface having a solid content concentration of 52% by mass (hereinafter also referred to as "composition (2)").
[0536] (1) Polymer component (a)
[0537] An acrylic resin (weight average molecular weight 800,000, glass transition temperature -28°C) obtained by copolymerizing butyl acrylate (55 parts by mass), methyl acrylate (10 parts by mass), glycidyl methacrylate (20 parts by mass), and 2-hydroxyethyl acrylate (15 parts by mass).
[0538] (2) Epoxy resin (b)
[0539] (b1)-1: Bisphenol A type epoxy resin (jER828 manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 184 to 194 g / eq)
[0540] (b1)-2: dicyclopentadiene type epoxy resin (EPICLON HP-7200HH manufactured by DIC Corporation, epoxy equivalent 255 to 260 g / eq)
[0541] (3) Curing agent (b2)
[0542] Biphenyl aralkyl type phenolic resin (produced by Meiwa Chemicals Co., Ltd., MEHC-7851-H, hydroxyl equivalent 218 g / eq)
[0543] (4) Curing accelerator (c)
[0544] 2-Phenyl-4,5-dihydroxymethylimidazole ("CUREZOL 2PHZ-PW" manufactured by Shikoku Chemical Industry Co., Ltd.)
[0545] (5) Filler (d)
[0546] Epoxy-modified spherical silica (5SE-CH1 manufactured by Admatechs, average particle size 500 nm)
[0547] (6) Coupling agent (e)
[0548] 3-Glycidoxypropyltrimethoxysilane (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0549] (7) Colorant (j)
[0550] Black pigment (Multi Rack A903 Black manufactured by Toyo Ink Co., Ltd.)
[0551] Next, a release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film having one side subjected to release treatment by silicone treatment was used, the composition (2) obtained above was applied to the release-treated surface, another release film ("SP-PET382150" manufactured by Lintec Corporation) was attached to the exposed surface, and then heated and dried at 120° C. for 2 minutes, thereby forming a 25 μm thick thermosetting resin film for the back surface sandwiched between the release films. This was used in the above test in the form of a roll.
[0552] The design properties were evaluated according to the following criteria.
[0553] Evaluation "A": The cured resin film was formed on the entire bump formation surface and side surface of the semiconductor chip, and a sense of unity in color tone was observed between the cured resin film and the second cured resin film formed on the back surface, indicating high design properties.
[0554] Evaluation "F": Although the cured resin film was formed on the entire bump formation surface and side surfaces of the semiconductor chip, there was no sense of unity in color tone between the cured resin film and the second cured resin film formed on the back surface, and the designability was low.
[0555] Film peeling was evaluated based on the following criteria.
[0556] Evaluation "A": The following three conditions are met.
[0557] (1) No film peeling of the cured resin film from the semiconductor chip was observed on the bump formation surface and side surfaces of the semiconductor chip.
[0558] (2) Film peeling of the second cured resin film from the semiconductor chip was not observed on the back surface of the semiconductor chip.
[0559] (3) Film peeling between the cured resin film and the second cured resin film was also not observed.
[0560] Evaluation "F": at least one of the above conditions (1) to (3) is not satisfied.
[0561] 4-4. Evaluation of warpage
[0562] A composite sheet having a thermosetting resin film with a thickness of 45 μm formed on the release-treated surface of a release film (“SP-PET381031” manufactured by Lintec Corporation, with a thickness of 38 μm) was heat-bonded (bonding pressure 0.3 MPa, bonding temperature 60°C, bonding speed 1 mm / sec, 1 reciprocating) to an electrolytic copper foil (thickness 35 μm, manufactured by Kansai Electronics Industry Co., Ltd.) cut into a circular size of 8 inches using a tabletop laminator (product name: “LPD3212”, manufactured by FUJIPULA Co., Ltd.). After visually confirming that the test piece had no warpage, the release film was peeled off and then heat-cured for 240 minutes at a temperature of 130°C and a pressure of 0.5 MPa. Then, after cooling naturally and returning to room temperature (25°C), tape (manufactured by NICHIBAN Co., Ltd., trade name "SELLOTAPE (registered trademark) LP-24", tape width 24 mm) was pasted at positions (three locations) where the periphery of the copper foil with the thermosetting resin film pasted thereon was divided into three parts substantially equally, and the warpage at a given position (the location with the largest warpage) was measured. It should be noted that a warpage of less than 15 mm was considered acceptable "A", and a warpage of more than 15 mm was considered unacceptable "F".
[0563]
[0564] The following can be seen from the results shown in Table 2.
[0565] The results shown in Examples 1 to 8 show that a thermosetting resin film having an infrared transmittance of less than 13% at 940 nm after heat curing at 130° C. and 0.5 MPa for 240 minutes has excellent near infrared shielding properties and can prevent malfunctions caused by near infrared rays.
[0566] In addition, according to the results shown in Examples 1, 4, 7, 9 and 11, when the thermosetting resin films of F(1)-45, F(2)-45, F(3)-45, F(7)-45 and F(8)-45 were used, the X value satisfied the above-mentioned requirement (2), and all the evaluation results of the incision recognition, design, film peeling and warping were good.
[0567] It should be noted that, for Comparative Example 6, although the projections and depressions of the cut can be identified due to the transparency of the cured resin film, in Comparative Examples 6 to 8, the viscosity reduction of the curable resin film when it is pasted to the semiconductor chip is greater than that of the embodiment and other comparative examples. It can be seen that due to the increase in the amount of curable resin film filled into the groove, etc., a portion where a protective film is not formed is generated at the end of the semiconductor chip when the cured resin film is made.
Claims
1. A curable resin film for forming a protective film on a bump-forming surface of a semiconductor chip having a bump-forming surface with bumps, The curable resin film satisfies the following requirement (1): Requirement (1): The near-infrared transmittance at 940 nm after heat curing treatment at 130° C. and 0.5 MPa for 240 minutes is less than 13%. The curable resin film according to claim 1 , comprising a black pigment.
3. The curable resin film according to claim 2, in, The content of the black pigment is more than 0.5% by mass based on the total amount of the curable resin film. The curable resin film according to claim 1 or 2, which has a thickness of 1 μm or more. 5 . The curable resin film according to claim 1 , which is used to form the cured resin film as the protective film on both the bump formation surface and the side surface of the semiconductor chip. 6 . A composite sheet having a laminated structure in which the curable resin film according to claim 1 or 2 and a release sheet are laminated.
7. The composite sheet according to claim 6, in, The release sheet includes a base material and a release layer, and the release layer faces the curable resin film.
8. The composite sheet according to claim 7, in, The release sheet further includes an intermediate layer between the base material and the release layer.
9. The composite sheet according to claim 7, in, The release layer is a layer formed of a composition including an ethylene-vinyl acetate copolymer.
10. A method for manufacturing a semiconductor chip, the method comprising the following steps (V1) to (V4) in sequence: Step (V1): a step of preparing a semiconductor wafer having a bump formation surface having bumps; Step (V2): a step of pressing and sticking the curable resin film according to claim 1 or 2 onto the bump-forming surface of the semiconductor wafer, thereby covering the bump-forming surface of the semiconductor wafer with the curable resin film; Step (V3): a step of curing the curable resin film to obtain a semiconductor wafer with a cured resin film; Step (V4): a step of dividing the semiconductor wafer with the cured resin film into individual pieces to obtain semiconductor chips in which the bump formation surfaces are covered with the cured resin film.
11. A method for manufacturing a semiconductor chip, the method comprising the following steps (S1), (S2), (S3) and (S4) in sequence, Step (S1): a step of preparing a wafer for manufacturing a semiconductor chip, wherein the semiconductor chip manufacturing wafer has a bump forming surface of a semiconductor wafer having bumps and has grooves serving as scheduled division lines formed on the bump forming surface so as not to reach the back surface; Step (S2): a step of pressing and sticking the curable resin film according to claim 5 to the bump forming surface of the semiconductor chip manufacturing wafer, covering the bump forming surface of the semiconductor chip manufacturing wafer with the curable resin film, and embedding the curable resin film in the groove portion formed in the semiconductor chip manufacturing wafer; Step (S3): a step of curing the curable resin film to obtain a wafer for semiconductor chip production with a cured resin film; Step (S4): a step of singulating the semiconductor chip manufacturing wafer with the cured resin film along the predetermined division line to obtain semiconductor chips in which at least the bump forming surface and the side surface are covered with the cured resin film. Further, after the step (S2) and before the step (S3), after the step (S3) and before the step (S4), or during the step (S4), the following step (S-BG) is included: Step (S-BG): a step of grinding the back surface of the semiconductor chip manufacturing wafer.
12. The method for manufacturing a semiconductor chip according to claim 10, further comprising the following step (TA): Step (TA): a step of forming a back surface protective film on the back surface of the semiconductor wafer.
13. The method for manufacturing a semiconductor chip according to claim 11, further comprising the following step (TB): Step (TB): a step of forming a back surface protective film on the back surface of the wafer for manufacturing the semiconductor chip. 14 . A semiconductor chip having a bump formation surface provided with bumps, wherein the bump formation surface of the semiconductor chip has a cured resin film obtained by curing the curable resin film according to claim 1 , and the semiconductor chip has a near infrared shielding function. 15 . A semiconductor chip having a bump formation surface with bumps, wherein the semiconductor chip has a cured resin film obtained by curing the curable resin film according to claim 5 on both the bump formation surface and the side surface thereof, and the semiconductor chip has a near infrared shielding function. 16 . The semiconductor chip according to claim 14 , further comprising a back surface protective film on the back surface of the semiconductor chip.