Polyester composite material as well as preparation method and application thereof

By optimizing the structure of the extruder hopper and the way of adding raw materials, the problem of consistency and stability of polyester composite materials during the injection molding process has been solved, the process capability index has been improved, the needs of intelligent manufacturing have been met, and higher production efficiency has been achieved. and product consistency.

CN118752736APending Publication Date: 2024-10-11NANTONG ZHONGLAN ENGINEERING PLASTICS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311260246.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing polyester composite materials have material consistency and stability problems during the injection molding process, resulting in a decrease in product yield and production efficiency. Especially in automated manufacturing environments, it is difficult to meet the needs of modern intelligent manufacturing.

Method used

By optimizing the structure of the collecting hopper at the feeding port of the extruder, the order, position and angle of adding granular and powdery raw materials are changed, so that they can enter the extruder evenly and stably, and the accumulation of powdery raw materials on the inner wall of the collecting hopper is reduced. Inverted cones are used The solid structure of the collecting hopper and the specific discharge angle design ensure that the raw materials flow in a clockwise or counterclockwise rotation to wash away the inner wall of the collecting hopper and achieve uniform addition of components.

Benefits of technology

Improved the process capability index (CPK) of polyester composite materials, including mechanical properties, consistency, processing performance and laser marking consistency, to meet the stability requirements of intelligent manufacturing, expand the scope of material application, and is suitable for automation and intelligence Production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752736A_ABST
    Figure CN118752736A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer composite materials, and particularly relates to a polyester composite material and a preparation method and application thereof. The preparation method comprises the following steps: adding the polybutylene terephthalate particles and the additive particles into a collection hopper through a first feeding pipe, adding the additive powder into the collection hopper through a second feeding pipe, and then feeding the additive powder into a screw extruder through a discharge port of the collection hopper for melt extrusion. The polyester composite material prepared by the preparation method has very high consistency, in the automatic production of downstream customers, the processing stability of processing equipment is very high, the size consistency of prepared parts is very high, the consistency of laser marking is very high, the yield of products is very high, the effectiveness of the process is improved, and the production cost is reduced. And a better choice is provided for automatic production of intelligent equipment and new energy automobiles in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer composite materials, and specifically to a polyester composite material and a preparation method and application thereof. Background Art

[0002] Polyester and its products (resins, fibers, films and engineering plastics, etc.) are among the polymer products with the largest production volume, the widest application and the fastest development speed in the world. Among thermoplastic polyester resins, polybutylene terephthalate (PBT) material, as a representative engineering plastic, is widely used in automotive parts, electronics and electrical, lighting, machinery, spinning, communications, films and instrumentation due to its advantages such as ease of molding and processing, excellent mechanical and physical properties, heat resistance, drug resistance and chemical resistance. At the same time, new application areas are constantly expanding.

[0003] During the processing, PBT materials are modified with various additives and blended with other resins to obtain better comprehensive properties such as heat resistance, flame retardancy, electrical insulation and good processing performance. For example, after being modified with glass fiber, PBT can be used to manufacture electronic components that require long-term operation at high temperatures and high dimensional stability. PBT has a high breakdown voltage and is suitable for making high-voltage resistant parts. Due to its good fluidity in the molten state, it is suitable for injection processing of electrical parts with complex structures, such as integrated circuit sockets, printed circuit boards, computer keyboards, electrical switches, fuses, temperature control switches, protectors, etc. Automobile bumpers, carburetors, spark plugs, fuel supply system components, igniters, etc. In the field of communications, PBT is widely used in integrated modules, wiring boards, power tools, etc. for programmable telephones.

[0004] The above materials are usually used to obtain products through injection molding, which is also called injection molding. It is a molding method that combines injection and molding. The advantages of injection molding are fast production speed, high efficiency, automated operation, a wide variety of colors, shapes from simple to complex, sizes from large to small, and precise product size. The product is easy to update and can be made into complex-shaped parts. Injection molding is suitable for mass production and complex-shaped products and other molding and processing fields.

[0005] The injection molding process can be roughly divided into the following six stages: mold closing, injection, pressure holding, cooling, mold opening, and product removal. By repeating this process, products can be produced in batches and periodically. The adjustable parameters in the injection molding process include the control of temperature, pressure and time. By adjusting the injection pressure, injection time, injection temperature, pressure holding and back pressure in various ways, qualified parts that meet the production requirements can be obtained. Generally speaking, there are three main aspects for evaluating the performance of plastic products: first, appearance quality, including integrity, color, and gloss; second, the accuracy between size and relative position, that is, dimensional accuracy and position accuracy; third, mechanical properties, chemical properties, electrical properties, etc. corresponding to the purpose, that is, functionality. Therefore, if there is a problem in any of the above three aspects, it will lead to the generation and expansion of product defects.

[0006] With the application of automation technology, the production and manufacturing process has gradually been transformed by automated equipment. More and more factories have reduced the number of workers and used equipment to automate the entire process. Changes in the production and manufacturing environment have put forward high requirements on the consistency of materials, including the consistency of mechanical properties, electrical properties, processing properties, secondary processing properties, and laser marking effects.

[0007] Regarding the processing consistency of materials, taking the injection molding process as an example, in the injection molding process of PBT materials, the more sensitive the injection molding process is, the more directly it affects the stability of mass production, directly leading to reduced production efficiency and a decrease in the injection molding yield rate. Therefore, solving the above injection molding problems and improving the yield rate of products are the basic demands of the PBT material injection molding industry. Improving the injection molding consistency of PBT materials is particularly important for molding, stable production, and improving processing capabilities. Injection molding consistency is mainly reflected in the stability of various parameters in the injection molding production process, including injection volume, metering stroke (pre-plastic stroke), residual material, etc. For materials, the most intuitive expression is: the difference in fluidity directly leads to fluctuations in injection molding parameters. Many factors, such as whether the dispersion of each component in the composite material is uniform and the stability of the raw materials, directly affect the injection molding consistency of the material.

[0008] For the consistency of material performance, the proportion of each component added to the material must be consistent, and the dispersion of each component in the composite material must be uniform. If a certain component is sometimes more and sometimes less, the consistency of the material will be reduced. For example, uneven distribution of glass fiber will lead to unstable mechanical strength of PBT glass fiber composite material, with large fluctuations; uneven distribution of toughening agent, notch sensitivity, large difference between samples; uneven addition and dispersion of lubricant will cause unstable flow performance of composite material, which will be good at one time and bad at another, and the consistency of processing will be poor; unstable addition and uneven dispersion of laser additive will cause instability of laser marking of subsequent parts, and serious consequences of automatic production line shutdown.

[0009] At present, the main process for manufacturing the above polyester composite material is to use a twin-screw extruder for extrusion preparation. In the process of extrusion preparation, there are two methods; the first method is that all the components are weighed manually, and then all are added to a mixing tank. After being mixed evenly, they are added to the inlet (collection hopper) of the extruder by free fall. This method requires a lot of manual weighing operations, which is prone to manual errors, and it is impossible to trace and analyze the causes. The product quality is difficult to control. At the same time, there are granular and powdery forms in the various components. During the descent process, the granules fall faster and enter the extruder first. The powdery raw materials fall slower and are easy to accumulate and enter the extruder later, so the stability and consistency of the produced products are poor. The second method is that all the raw materials are automatically weighed by their own weighing scales and then added to the extruder. Some of the raw materials are added to the side feed port, and the rest of the raw materials slide into the feed port (collection hopper) of the extruder through a round tube; this method solves the manual problem in the first method, and also solves the problem of inconsistent feeding speeds of granular raw materials and powdery raw materials. The stability and consistency of the polyester composite material prepared by this method are improved.

[0010] However, since the extruder generally has no more than two side feed ports, one raw material (such as flame retardant epoxy bromide) is added to the first side feed port, and another raw material (such as glass fiber) is added to the second side feed port. The remaining raw materials are still automatically weighed by the metering scale and added to the extruder's feed port - the collection hopper, and then added to the extruder as the twin screws of the extruder rotate. Although this method has made some progress, it still has some disadvantages, causing challenges to the consistency and stability of the materials. Figure 1 As shown, the added raw materials are granular and powdery. The granular raw materials have better fluidity and can easily slide into the extruder mouth. The powdery raw materials are easy to accumulate on the inner wall of the hopper, part of which enters the extruder, and part of which suddenly enters the extruder after accumulating to a certain thickness, resulting in poor consistency and stability of the material.

[0011] In response to the needs of the above applications and to meet the development requirements of the industry, a method for preparing a modified PBT material with stable processing and uniform dispersion is developed, which meets the development needs of today's industrial society and can improve the injection molding consistency and production efficiency during the production process, and is of great practical significance.

[0012] Patent CN201820340775.7 proposes a method that uses injection molding equipment with a specific structure to reduce the scrap rate, improve stability and injection uniformity during injection molding, and achieve stable product quality. However, this method has no clear requirements on the type and quality of materials and has application limitations.

[0013] Patent CN201280010137.4 proposes to obtain polyester with excellent mechanical properties and molding stability by controlling the conductivity of the diol composition used as the polyester raw material. However, this solution to the material consistency is only applicable to the processing and uniform mixing of materials in a liquid state, not to the processing and mixing of solid materials, and has certain limitations.

[0014] Patent CN2021121544825.1 proposes a three-layer co-extrusion feeding device, which adopts pneumatic feeding and driving parts to drive mixing, which can reduce manual labor intensity and improve production efficiency. However, this method of improving the degree of automation has certain limitations, as the mixing and discharging and subsequent production processes are intermittent, and the stratification of granular and powdered materials in the discharging process still needs to be considered.

[0015] Patent CN202120630802.6 proposes an efficient mixing device for modified plastic production. Through a specific structural design, it not only improves the mixing efficiency, but also realizes the automatic unloading of materials. However, the mixing device is a sealed operation, and the process is that the device runs alone, which cannot achieve continuous automatic production, and the subsequent processing process still has certain limitations.

[0016] Patent CN201911234924.7 proposes to solve the problem of product color consistency in the diisocyanate production field by mixing a functional color reducing agent with diisocyanate.

[0017] In summary, the above patents are all committed to making certain improvements in their respective local areas. However, how to improve the performance consistency and processing stability of polyester composite materials, improve the process capability index (CPK) of materials, expand the application areas of materials, and widely use them in the field of intelligent manufacturing in a manufacturing environment where automation continues to become popular, remains to be explored. Summary of the invention

[0018] In view of the deficiencies of the prior art, the present invention provides a polyester composite material and a preparation method and application thereof. The preparation method changes the order, position and angle of addition of the existing granular raw materials and powdered raw materials so that they are added to the feed port of the extruder in a uniform and stable manner, thereby reducing the accumulation on the inner wall of the collecting hopper and avoiding the problem of uneven addition of some powdered raw materials. The polyester composite material prepared by the preparation method has an excellent process capability index (CPK), including mechanical property consistency, processing performance consistency, laser marking consistency and other characteristics, thereby expanding more application fields, especially providing new stable materials that meet the requirements for the development of the upcoming automated manufacturing and intelligent manufacturing, and has strong competitiveness.

[0019] To achieve the above objectives, the technical solutions adopted by the present invention are:

[0020] The present invention first provides a method for preparing a polyester composite material. The raw materials for preparing the polyester composite material include: polybutylene terephthalate (PBT) particles, additive particles, and additive powder;

[0021] The preparation method comprises the following steps: adding the polybutylene terephthalate particles and the additive particles into a collecting hopper through a first feeding pipe, adding the additive powder into the collecting hopper through a second feeding pipe, and then entering the screw extruder through a discharge port of the collecting hopper for melt extrusion;

[0022] The aggregate hopper is an inverted cone structure;

[0023] The discharge position of the first feeding pipe on the collecting hopper is in the upper part of the collecting hopper; the discharge angle of the first feeding pipe in the vertical direction on the collecting hopper is -40 degrees to +40 degrees;

[0024] The discharge position of the second feeding pipe on the collecting hopper is in the lower half of the collecting hopper; the discharge angle of the second feeding pipe in the vertical direction on the collecting hopper is -5 degrees to +5 degrees.

[0025] The present invention optimizes the shape of a collecting hopper of an extruder feeding port, optimizes the position of raw materials added to the collecting hopper, and optimizes the angle of the raw materials added to the collecting hopper, so as to achieve real-time addition of raw materials to the extruder and ensure the consistency and stability of the prepared polyester composite material.

[0026] like Figure 2 As shown, the collecting hopper of the feeding port of the screw extruder described in the present invention is an inverted cone structure, which is more conducive to the granular raw materials to form a clockwise or counterclockwise rotating flow to flush the inner wall of the collecting hopper compared to the collecting hopper using a quadrilateral cone, and the powdered raw materials adhered to the inner wall of the collecting hopper are brought into the extruder in time.

[0027] like Figure 3 As shown, the lower half of the collecting hopper described in the present invention refers to the part of the collecting hopper corresponding to the circle within 50% of the distance between the upper cover surface of the collecting hopper and the center point, which is suitable for arranging the discharge position of the second feeding pipe of the powdered raw material; the upper half of the collecting hopper refers to the part of the collecting hopper outside 50% of the distance between the upper cover surface of the collecting hopper and the center point, which is suitable for arranging the discharge position of the first feeding pipe of the granular raw material.

[0028] like Figure 4 As shown, the vertical discharge angle of the present invention represents the angle between the discharge direction and the vertical direction, wherein, when α1-α5 is a positive value, it indicates that the material flows into the collecting hopper in a clockwise direction, conversely, when α1-α5 is a negative value, it indicates that the material flows into the collecting hopper in a counterclockwise direction; when the α1-α5 angle is 0 degrees, it indicates that the material enters the collecting hopper vertically.

[0029] The purpose of the present invention is to allow powdered raw materials to enter from the center of the upper cover of the collecting hopper and enter the bottom of the collecting hopper as much as possible to reduce the accumulation on the inner wall of the collecting hopper, and the granular raw materials to enter from the periphery of the upper cover of the collecting hopper to form a clockwise or counterclockwise rotating flow to flush the inner wall of the collecting hopper as much as possible, and bring the materials adhered to the inner wall of the collecting hopper into the extruder in time, so that various components can be added to the prepared polyester composite material in time and accurately.

[0030] The discharge angle of the first feeding pipe on the collecting hopper in the vertical direction is +18 degrees to +22 degrees; the discharge angle of the second feeding pipe on the collecting hopper in the vertical direction is -2 degrees to +2 degrees.

[0031] Preferably, the discharge angle of the first feeding pipe on the collecting hopper in the vertical direction is 20 degrees; the discharge angle of the second feeding pipe on the collecting hopper in the vertical direction is 0 degrees. The present invention finds that the polyester composite material prepared by adopting the above discharge angle has the best CPK value of various properties, has good consistency, and meets the production needs of modern intelligent manufacturing.

[0032] Preferably, when the discharge angle of the first feeding pipe or the second feeding pipe is not 0 degrees, the projection of its discharge direction on the cross section of the collecting hopper is located in the tangent direction of the collecting hopper.

[0033] Preferably, the number of the first feeding pipes is more than two. In practical applications, the PBT particles and the additive particles can be fed separately through different first feeding pipes, thereby avoiding the premixing step before feeding.

[0034] Preferably, the particle size of the polybutylene terephthalate particles is 2 to 4 mm.

[0035] Preferably, the particle size of the additive particles is 2 to 4 mm.

[0036] Preferably, the particle size of the additive powder is 20 to 400 μm.

[0037] Preferably, the raw materials for preparing the polyester composite material include: 50 to 98 parts of polybutylene terephthalate (PBT) particles, 0.01 to 40 parts of additive particles, and 0.01 to 25 parts of additive powder.

[0038] The present invention further improves the CPK values ​​of various properties of the polyester composite material by optimizing the particle sizes and proportions of polybutylene terephthalate particles, additive particles, and additive powder.

[0039] The present invention has no special limitation on additives, and examples thereof include toughening agents, compatibilizers, masterbatches, antioxidants, lubricants, flame retardants, etc., and can be added in the form of additive particles or additive powders according to actual needs. For example, toughening agents, compatibilizers, masterbatches, etc. are added in the form of additive particles, and antioxidants, lubricants, flame retardants, etc. are added in the form of additive powders.

[0040] Preferably, the preparation method further comprises: sequentially cooling, pelletizing and uniformly mixing the product after melt extrusion to obtain a polyester composite material.

[0041] The present invention also provides a polyester composite material, which is prepared by the above preparation method.

[0042] The present invention also provides application of the polyester composite material or the polyester composite material prepared by the preparation method in the field of automated manufacturing or intelligent manufacturing.

[0043] The beneficial effects of the present invention are at least:

[0044] The preparation method of the polyester composite material provided by the present invention changes the order, position and angle of addition of the existing granular raw materials and powdered raw materials so that they are added to the feed port of the extruder evenly and stably, thereby reducing the accumulation on the inner wall of the collecting hopper and avoiding the problem of adding more or less of some powdered raw materials. Thus, it is ensured that the high-performance polyester composite material prepared has stable mechanical properties, the consistency of the prepared parts is good, and the application range of the existing polyester can be greatly expanded, especially suitable for intelligent manufacturing equipment; it has stable processing performance, good consistency in the process of automated manufacturing of injection molding machines, stable parts, stable process, suitable for batch and automated production and manufacturing, and suitable for the gradually intelligent and automated production and manufacturing environment in the future; at the same time, the preparation method has simple equipment, easy to control parameters, easy to implement, and convenient for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0046] Figure 1 This is a schematic diagram of powdered and granular raw materials entering the inner wall of the collecting hopper at the feed inlet of an existing extruder.

[0047] Figure 2 The following are the reference diagrams for the shape of the aggregate hopper; the left diagram is an inverted cone structure, and the right diagram is a quadrilateral vertebral structure.

[0048] Figure 3 It is a schematic diagram of the discharge position of the feeding pipe on the upper cover of the collecting hopper of the present invention; wherein ①, ②, ③, ④, ⑤ correspond to the pipe openings of 1# pipe, 2# pipe, 3# pipe, 4# pipe, and 5# pipe respectively, wherein 1# pipe, 2# pipe, and 3# pipe are the first feeding pipes, and 4# pipe and 5# pipe are the second feeding pipes.

[0049] Figure 4 It is a schematic diagram of the discharge angle of the feeding pipe of the present invention, ①, ②, ③, ④, ⑤ refer to the same as above, α1, α2, α3, α4, α5 correspond to the discharge angles of 1# pipeline, 2# pipeline, 3# pipeline, 4# pipeline, 5# pipeline respectively.

[0050] Figure 5 Process capability report for the melt index of Example 1.

[0051] Figure 6 These are the test data of Examples 1-10 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0052] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0053] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the art or the product instructions shall be followed.

[0054] The raw materials or instruments used without indicating the manufacturer are all conventional products that can be purchased through regular channels.

[0055] The following detection methods were used for the relevant tests of the present invention:

[0056] Melt index: measured according to ISO 1133 standard, test temperature is 250℃, load is 2.16kg;

[0057] Melt viscosity: measured according to ASTM D445 standard, the test condition is Ubbelohde viscometer, 25℃;

[0058] Flame retardant performance: measured in accordance with UL 94 standard, the test condition is vertical combustion;

[0059] Low temperature impact strength: measured according to ASTM D256 standard, the specimen is placed in a low temperature box (-40℃) for 24 hours to test the low temperature notched impact strength of the material;

[0060] Bending strain: measured according to ASTM D790 standard, the test environment temperature is 25℃, and the test speed is 10mm / s;

[0061] Processing stability performance: injection molding by injection molding machine and testing and evaluation records of processing performance, filling pressure, metering time and filling stroke;

[0062] Laser marking stability: The laser marking machine sets the laser conditions, performs laser engraving on the material surface, and evaluates and compares the records;

[0063] Color difference: The L, a, and b values ​​of the material color plate are tested by Datacolor colorimeter, and the color difference ΔE is calculated. The calculation formula is as follows And compare the records.

[0064] Example 1

[0065] A preparation method of a laser-marked polyester composite material includes the following steps, which can be partially referred to Figure 3 and Figure 4 :

[0066] Raw material feeding and extrusion:

[0067] 84 portions of 3mm raw material PBT particles enter the hopper through the 1# and 2# pipe ports, 6 portions of 4mm additive particles (toughener, compatibilizer, masterbatch) enter the hopper through the 3# pipe port, and 10 portions of about 250μm powdered additives (antioxidants, lubricants, flame retardants) enter the hopper through the 4# and 5# pipe ports, and the inclination angles α1-α5 of the 1# to 5# pipes are all 0, that is, the materials enter the hopper vertically, and the materials are gathered to the extruder feed port through the hopper, and are processed and pelletized by the twin-screw extruder to obtain plastic particles. The hopper is an inverted cone structure; the discharge position of the 1# to 3# pipe ports on the hopper is in the upper half of the hopper; the discharge position of the 4# and 5# pipe ports on the hopper is in the lower half of the hopper;

[0068] The length-to-diameter ratio of the twin-screw extruder is 40:1, the extrusion temperature is 170° C.-260° C., the screw speed is 300 rpm, and the product is prepared through extrusion, cooling, pelletizing, homogenizing and packaging.

[0069] Injection molding:

[0070] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0071] Taking the melt index as an example, the test data is shown in Table 1 below, and the process capability index (CPK) analysis is as follows: Figure 5 .

[0072] Table 1

[0073]

[0074] Comparative Example 1

[0075] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0076] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0077] The raw material PBT particles are fed into the collecting hopper through the 4# and 5# pipe ports, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 1# and 2# pipe ports respectively, and the pipe inclination angles α1-α5 are all 0, the materials enter the collecting hopper vertically, and the materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained through extrusion, cooling, pelletizing, homogenizing, and packaging.

[0078] Injection molding:

[0079] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0080] Example 2

[0081] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0082] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0083] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +10 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0084] Injection molding:

[0085] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0086] Example 3

[0087] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0088] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0089] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +20 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0090] Injection molding:

[0091] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0092] Example 4

[0093] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0094] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0095] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +30 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0096] Injection molding:

[0097] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0098] Example 5

[0099] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0100] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0101] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +20 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all +5 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0102] Injection molding:

[0103] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0104] Example 6

[0105] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0106] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0107] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles enter the collecting hopper through the 3# pipe port, and the powdered additive raw materials enter the collecting hopper through the 4# pipe port and the 5# pipe port respectively. The inclination angles α1-α of the granular raw material pipeline are all -30 degrees (counterclockwise), and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0108] Injection molding:

[0109] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0110] Example 7

[0111] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0112] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0113] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles enter the collecting hopper through the 3# pipe port, and the powdered additive raw materials enter the collecting hopper through the 4# pipe port and the 5# pipe port respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +40 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0114] Injection molding:

[0115] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0116] Example 8

[0117] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0118] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0119] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles enter the collecting hopper through the 3# pipe port, and the powdered additive raw materials enter the collecting hopper through the 4# pipe port and the 5# pipe port respectively. The inclination angle α1 of the granular raw material pipeline is +10 degrees, α2 is +20 degrees, α3 is -10 degrees (counterclockwise), and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0120] Injection molding:

[0121] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0122] Example 9

[0123] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0124] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0125] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively. The inclination angle α1 of the granular raw material pipeline is +10 degrees, α2 is +20 degrees, α3 is +30 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all 0 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0126] Injection molding:

[0127] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0128] Example 10

[0129] A preparation method of a laser-marked polyester composite material comprises the following steps:

[0130] Raw material feeding and extrusion (the composition, particle size and weight ratio of the raw materials are the same as those in Example 1):

[0131] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles enter the collecting hopper through the 3# pipe port, and the powdered additive raw materials enter the collecting hopper through the 4# pipe port and the 5# pipe port respectively. The inclination angles α1-α3 of the granular raw material pipeline are all +25 degrees, and the inclination angles α4-α5 of the powdered raw material pipeline are all +5 degrees. The materials are gathered to the extruder feed port through the collecting hopper, and processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained by extrusion, cooling, pelletizing, homogenizing, and packaging.

[0132] Injection molding:

[0133] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0134] Comparative Example 2

[0135] A preparation method for a laser-marked polyester composite material, wherein the raw material system of the composite material is different from that in Example 1 in that the particle sizes of the raw material PBT particles and the additive particles are changed, specifically, the PBT particles are 4.5 mm, the additive particles are 4.5 mm, and the powdered additive is about 250 μm. The preparation method comprises the following steps:

[0136] Raw material feeding and extrusion (the composition and weight ratio of the raw materials are the same as those in Example 1):

[0137] The raw material PBT particles are fed into the collecting hopper through the 1# pipe port and the 2# pipe port, the additive particles are fed into the collecting hopper through the 3# pipe port, and the powdered additive raw materials are fed into the collecting hopper through the 4# pipe port and the 5# pipe port, respectively, and the pipe inclination angles α1-α5 are all 0, the materials enter the collecting hopper vertically, and the materials are gathered to the extruder feed port through the collecting hopper, and are processed and pelletized by a twin-screw extruder to obtain plastic particles. The twin-screw extruder has an aspect ratio of 40:1, an extrusion temperature of 170°C-260°C, a screw speed of 300rpm, and is obtained through extrusion, cooling, pelletizing, homogenizing, and packaging.

[0138] Injection molding:

[0139] After the plastic particles obtained by extrusion are dried at 120°C for 4 hours, the moisture content is controlled to be less than 0.05%. They are then injection molded by an injection molding machine, and standard specimens are obtained for testing. A total of 20 parallel samples are used, and 20 data are tested to calculate the CPK value. In addition, the melt index is tested and the data is recorded in accordance with the ISO 1133 standard. During the injection molding process, four data records, namely processing performance, filling pressure, metering time and filling stroke, are used to evaluate the injection molding stability. 20 groups are injected in parallel and the CPK value is calculated. The standard sample obtained by injection molding is laser engraved on the surface of the material and the clarity is evaluated and compared. The color plate obtained by injection molding is tested by a Datacolor colorimeter to obtain the L, a, and b values ​​of the material color plate, and the color difference ΔE is calculated. 20 groups are recorded in parallel and the CPK value is calculated.

[0140] From the test data of the embodiments and comparative examples Figure 6 The following results were obtained:

[0141] Comparing Example 1 with Comparative Example 1, when the powdered raw materials of Comparative Example 1 were discharged from feed pipes No. 1 and No. 2, the raw materials hit the side wall of the collecting hopper and then were drawn into the bottom of the collecting hopper. No granular raw materials were washed away, and the raw materials accumulated on the inner wall of the collecting hopper. The CPK values ​​of various performance properties of the material were less than 1, which was not suitable for modern intelligent manufacturing production.

[0142] It can be seen from the test results of Examples 1-10 that the granular raw materials are discharged from 1# pipe, 2# pipe, and 3# pipe, and the powdered raw materials are discharged from 4# pipe and 5# pipe. The powdered raw materials enter from the center of the upper cover of the collecting hopper and enter the bottom of the collecting hopper. The granular raw materials enter from the periphery of the upper cover of the collecting hopper, forming a clockwise or counterclockwise rotating flow mode to flush the inner wall of the collecting hopper, and the materials adhered to the inner wall of the collecting hopper are brought into the extruder in time, so that various components are added to the prepared polyester composite material in time and accurately, and the CPK values ​​of various properties of the material are significantly improved. When α4 and α5 have an inclination angle of 5°, the powdered raw materials do not directly enter the bottom of the collecting hopper, and the CPK values ​​of various properties of the prepared materials decrease slightly. At the same time, when the inclination angles of α1, α2, and α3 are 20°, and the inclination angles of α4 and α5 are 0°, the CPK values ​​of various properties of the prepared materials are the best, reaching more than 1.67, with good consistency, meeting the production needs of modern intelligent manufacturing.

[0143] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a polyester composite material, characterized in that: The raw materials for preparing the polyester composite material include: polybutylene terephthalate particles, additive particles, additive powder; The preparation method comprises the following steps: adding the polybutylene terephthalate particles and the additive particles into a collecting hopper through a first feeding pipe, adding the additive powder into the collecting hopper through a second feeding pipe, and then entering the screw extruder through a discharge port of the collecting hopper for melt extrusion; The aggregate hopper is an inverted cone structure; The discharge position of the first feeding pipe on the collecting hopper is in the upper part of the collecting hopper; the discharge angle of the first feeding pipe in the vertical direction on the collecting hopper is -40 degrees to +40 degrees; The discharge position of the second feeding pipe on the collecting hopper is in the lower half of the collecting hopper; the discharge angle of the second feeding pipe in the vertical direction on the collecting hopper is -5 degrees to +5 degrees.

2. The method for preparing the polyester composite material according to claim 1, characterized in that: The discharge angle of the first feeding pipe on the collecting hopper in the vertical direction is +18 degrees to +22 degrees; the discharge angle of the second feeding pipe on the collecting hopper in the vertical direction is -2 degrees to +2 degrees.

3. The method for preparing the polyester composite material according to claim 2, characterized in that: The discharge angle of the first feeding pipe in the vertical direction on the collecting hopper is +20 degrees; the discharge angle of the second feeding pipe in the vertical direction on the collecting hopper is 0 degrees.

4. The method for preparing the polyester composite material according to any one of claims 1 to 3, characterized in that: The number of the first feeding tubes is two or more.

5. The method for preparing the polyester composite material according to any one of claims 1 to 4, characterized in that: The particle size of the polybutylene terephthalate particles is 2 to 4 mm.

6. The method for preparing the polyester composite material according to any one of claims 1 to 5, characterized in that: The particle size of the additive particles is 2 to 4 mm.

7. The method for preparing the polyester composite material according to any one of claims 1 to 6, characterized in that: The particle size of the additive powder is 20 to 400 μm.

8. The method for preparing the polyester composite material according to any one of claims 1 to 7, characterized in that: The raw materials for preparing the polyester composite material include, by weight: 50 to 98 parts of polybutylene terephthalate particles, 0.01 to 40 parts of additive particles, and 0.01 to 25 parts of additive powder.

9. A polyester composite material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the polyester composite material according to any one of claims 1 to 8, or the polyester composite material prepared by the preparation method according to claim 9 in the field of automated manufacturing or intelligent manufacturing.

Citation Information

Patent Citations

  • Diol composition and polyester

    CN103391957A

  • Functional color reducing agent, and method for stabilizing color number of diisocyanate product

    CN110878033A

  • Stability of mould plastics is improved electronic power assisted steering ware bush of tubular column formula

    CN208198570U

  • Efficient mixing device for modified plastic production

    CN214982308U

  • Feeding device of extruder

    CN218928560U