A preparation method of TMDs alloy nanosheets and high-performance photodetector using the same as passivation layer and gain layer
WS2(1-x)WSe2x alloy nanosheets were prepared by bidirectional airflow physical vapor deposition as passivation and gain layers, and combined with In2S3 heterojunction, solving the application problem of WS2 and WSe2 alloy nanosheets in photodetectors and realizing the construction of high-performance photodetectors.
Patent Information
- Application Number
- CN202411216597.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-02
AI Technical Summary
How to construct high-performance photodetectors by combining them with other two-dimensional materials, especially the application of WS2 and WSe2 alloy nanosheets in photodetectors.
WS2(1-x)WSe2x alloy nanosheets were prepared by bidirectional airflow physical vapor deposition and used as passivation and gain layers. Combined with In2S3 heterojunction, a high-performance photodetector was constructed.
This significantly improves the performance of the photodetector, achieving an on/off ratio of 2.02×10⁴, and enhancing photocurrent and photoelectric conversion efficiency.
Smart Images

Figure CN118763152B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of two-dimensional material photoelectric detectors, and in particular to a method for preparing a TMDs alloy nanosheet and a high-performance photoelectric detector using the nanosheet as a passivation layer and a gain layer. Background Art
[0002] With the rapid development of imaging and communication technologies, the demand for high-performance photodetectors with high responsiveness, high detection rate, and fast response speed has gradually increased. Due to the unique electrical and optical properties of two-dimensional materials, people have aroused great interest and brought a new platform for the design of optoelectronic devices. Two-dimensional materials have the advantages of atomic-level thickness, strong light-matter interaction, and mechanical flexibility. In addition, two-dimensional materials have self-passivating surfaces and can be freely stacked or stitched to form van der Waals heterostructures without being constrained by lattice matching, achieving excellent photoelectric response characteristics that surpass those of a single material.
[0003] As an important member of two-dimensional materials, WS 2 and WSe 2 It has excellent physical properties and a wide range of device applications, and has good stability, good thermal properties and chemical stability, which is conducive to building long-term stable device performance and has high adaptability to substrates of other materials. However, how to build a high-performance photodetector by combining it with other two-dimensional materials has become a key technical issue. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing transition metal dichalcogenide (TMDs) alloy nanosheets and a high-performance photodetector as a passivation layer and a gain layer, specifically a WS 2(1-x) Wlq 2x The invention discloses a method for preparing alloy nanosheets and a high-performance photodetector using the alloy nanosheets as a passivation layer and a gain layer to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is to provide a WS 2(1-x) Wlq 2x The preparation method of alloy nanosheets comprises the following steps:
[0007] WS 2 and WSe 2 After mixing, it is used as reactants, with inert gas as carrier gas and SiO 2 The two-dimensional WS was prepared by physical vapor deposition with bidirectional gas flow. 2(1-x) Wlq 2x Alloy nanosheets.
[0008] Furthermore, the WS 2(1-x) Wlq 2x The value range of X is 0.25~0.75.
[0009] Furthermore, the SiO 2 SiO / Si substrate 2 Face up.
[0010] Furthermore, the WS 2 and WSe 2 The mixing mass ratio is 1~3:1~3.
[0011] Furthermore, the distance between the support and the reactant is 8 to 10 cm.
[0012] Furthermore, the physical vapor deposition step of the bidirectional airflow includes:
[0013] The air was exhausted by an inert gas with a flow rate of 120-150 sccm, and the air flow direction was from the carrier to the reactant. The flow rate was then adjusted to 30-40 sccm, and the temperature was raised to 1100-1130°C at a heating rate of 10-13°C / min. The air flow direction was changed from the reactant to the carrier, and the flow rate was adjusted to 100-120 sccm. The temperature was kept for 8-15 minutes, and the flow rate was finally adjusted to 20-30 sccm. The mixture was cooled to room temperature, and a two-dimensional WS was prepared on the surface of the carrier. 2(1-x) Wlq 2x Alloy nanosheets.
[0014] The present invention adopts a bidirectional gas flow physical vapor deposition method, which reduces unnecessary nucleation during the heating process and excess nucleation during the cooling process by changing the flow direction of the inert gas and regulating its flow rate. Compared with the previous physical vapor deposition technology, it is easier to achieve large-size and uniform-thickness two-dimensional WS 2(1-x) Wlq 2x Preparation of alloys, specifically:
[0015] First, adjust the gas flow direction from the carrier to the reactant, and then start to increase the temperature to prevent the growth temperature WS from being reached. 2(1-x) Wlq 2x The alloy begins to grow; when the temperature rises to 1100-1130℃, change the direction of the inert gas flow from the reactant to the carrier, adjust the gas flow rate to 100-120sccm, and keep the temperature within this range to make WS 2(1-x) Wlq 2x Start to grow on the surface of the carrier; after the insulation is completed, the temperature starts to drop naturally, and the air flow rate is adjusted to 20~30sccm to reduce WS 2(1-x) Wlq 2xThe purpose of these operations is to increase WS 2(1-x) Wlq 2x The grain size is small while maintaining the uniformity of thickness; the substrate is taken out after cooling to room temperature, and a two-dimensional layered WS is prepared on the surface of the carrier. 2(1-x) Wlq 2x Alloy nanosheets.
[0016] The second technical solution of the present invention is to provide a WS prepared by the above preparation method. 2(1-x) Wlq 2x Application of alloy nanosheets in photodetectors.
[0017] The third technical solution of the present invention is to provide a high-performance photoelectric detector, wherein the high-performance photoelectric detector is based on the above-mentioned WS 2(1-x) Wlq 2x The alloy nanosheets serve as the passivation layer and the gain layer.
[0018] Technical solution 4 of the present invention: Provide a method for preparing the above-mentioned high-performance photodetector, the steps comprising:
[0019] The above two-dimensional layered WS 2(1-x) Wlq 2x Alloy nanosheets transferred to new SiO 2 / Si substrate surface, and then the two-dimensional In 2 S 3 Transfer to WS 2(1-x) Wlq 2x On the alloy nanosheet, a two-dimensional WS 2(1-x) Wlq 2x Alloy / In 2 S 3 Heterojunction;
[0020] In the two-dimensional WS 2(1-x) Wlq 2x Alloy / In 2 S 3 The heterojunction surface is spin-coated with photoresist, and after alignment, exposure, and development by a photolithography machine, titanium / gold electrodes are plated to obtain a photodetector.
[0021] Furthermore, the transfer to the new SiO 2 The steps on the surface of the Si substrate are:
[0022] Two-dimensional layered WS on the support surface 2(1-x) Wlq 2x The alloy nanosheets were spin-coated with PMMA solution, baked at 100 °C for 10 min, and then immersed in BOE solution for 5 min to obtain a PMMA film / 2D WS separated from the support. 2(1-x) Wlq 2xAlloy nanosheets;
[0023] PMMA film / 2D WS 2(1-x) Wlq 2x Alloy nanosheets attached to new SiO 2 / Si substrate, baked at 100-120°C for 30-40 min, immersed in acetone to remove the PMMA film, and dried with nitrogen to complete the WS 2(1-x) Wlq 2x Alloy nanosheets to new SiO 2 / Transfer to the Si substrate surface.
[0024] Furthermore, the two-dimensional In 2 S 3 Transfer to WS 2(1-x) Wlq 2x The steps on the alloy nanosheets are:
[0025] Spin coating PVA onto 2D In 2 S 3 Heat at 110℃ for 4min, tear off, and complete the two-dimensional In 2 S 3 Transfer to the PVA film, and then stick to the In 2 S 3 PVA film and WS 2(1-x) Wlq 2x The alloy nanosheets were stacked, heated at 110°C for 4 min, and then immersed in deionized water at 55°C for 30 min to remove PVA, thus completing the two-dimensional In 2 S 3 To WS 2(1-x) Wlq 2x alloy nanosheets to obtain two-dimensional WS 2(1-x) Wlq 2x Alloy / In 2 S 3 Heterojunction.
[0026] The present invention uses two-dimensional WS 2(1-x) Wlq 2x The alloy nanosheets serve as the substrate passivation layer and gain layer to reduce the harmful effects on the substrate and reduce the upper two-dimensional In 2 S 3 In the recombination of photocarriers; at the same time, In 2 S 3 The photogenerated holes in WS 2(1-x) Wlq 2x alloy and is bound, reducing its 2 S 3 The recombination probability of photogenerated electrons in the 2 S3 Photodetector performance, constructing high-performance WS 2(1-x) Wlq 2x / In 2 S 3 Photodetector.
[0027] The present invention discloses the following technical effects:
[0028] The present invention adopts a bidirectional gas flow physical vapor deposition method, and reduces unnecessary nucleation during the heating process and excess nucleation during the cooling process by changing the flow direction of the inert gas and regulating its flow rate, thereby achieving large-size and uniform-thickness two-dimensional WS 2(1-x) Wlq 2x The alloy can be prepared with a size of up to 400 μm. 2(1-x) Wlq 2x The alloy acts as a passivation layer and gain layer to reduce the harmful effects of the substrate and reduce the upper two-dimensional In 2 S 3 The recombination probability of photon carriers in the 2 S 3 Photodetector performance, constructing high-performance WS 2(1-x) Wlq 2x / In 2 S 3 The photodetector has an experimentally measured light on / off ratio of up to 2.02×10 4 . BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 Preparation of WS for the present invention 2(1-x) Wlq 2x Schematic diagram of the device for alloy nanosheets;
[0031] Figure 2 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets;
[0032] Figure 3 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2xHigh-angle annular dark field scanning transmission electron microscopy and element mapping of alloy nanosheets, where (a) is a high-angle annular dark field scanning transmission electron microscopy image, (b) to (d) are element mapping maps of W, S, and Se, respectively;
[0033] Figure 4 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2x Photoluminescence mapping (PL Mapping) of alloy nanosheets at 690nm;
[0034] Figure 5 The two-dimensional WS prepared in Examples 1 to 3 and Comparative Examples 1 to 2 2(1-x) Wlq 2x Photoluminescence spectra of alloy nanosheets;
[0035] Figure 6 This is an optical microscope image of the photodetector prepared in Example 4;
[0036] Figure 7 This is an optical microscope image of the photodetector prepared in Example 5;
[0037] Figure 8 This is an optical microscope image of the photodetector prepared in Example 6;
[0038] Fig. 9 is the on / off ratio of the photodetector prepared in Examples 4 to 6;
[0039] Fig.10 The two-dimensional WS prepared in Example 2 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets;
[0040] Fig.11 The two-dimensional WS prepared in Example 2 2(1-x) Wlq 2x PL Mapping of alloy nanosheets at 656nm;
[0041] Fig.12 The two-dimensional WS prepared in Example 3 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets;
[0042] Fig.13 The two-dimensional WS prepared in Example 3 2(1-x) Wlq 2x PL Mapping of alloy nanosheets at 720nm;
[0043] Fig.14This is an optical microscope image of the photodetector prepared in Comparative Example 3;
[0044] Fig.15 This is an optical microscope image of the photodetector prepared in Comparative Example 4;
[0045] Fig.16 It is the on / off ratio of the photodetector prepared in Comparative Examples 3-4. DETAILED DESCRIPTION
[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0047] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0051] The raw materials used in the present invention are all commercially available products, among which WS 2 Powder and WSe 2 The powders were purchased from Aladdin with a purity of 99.99%.
[0052] Figure 1 Preparation of WS for the present invention2(1-x) Wlq 2x Schematic diagram of the device for alloy nanosheets.
[0053] Example 1
[0054] WS 2(1-x) Wlq 2x Preparation of alloy nanosheets:
[0055] S1. WS 2 Powder and WSe 2 Prepare 50 mg of each powder, stir and mix evenly to obtain a reactant;
[0056] S2, reactants and SiO 2 The SiO / Si substrate is placed at the center and edge of the heating zone of a single-temperature-zone horizontal tube furnace. 2 SiO / Si substrate 2 Face up, reactants and SiO in the center 2 / Si substrate distance is 10cm;
[0057] S3, first pass nitrogen at a gas flow rate of 150 sccm for 20 minutes to exhaust the air in the quartz tube of the horizontal tube furnace, then adjust the flow rate to 40 sccm and start heating, and heat it uniformly for 1.5 hours to 1130°C. The gas flow direction in this step is from the substrate to the reactant;
[0058] S4. When the temperature reaches 1130°C, change the nitrogen flow direction from the reactant to the substrate, and then adjust the flow rate to 120 sccm and keep warm for 12 minutes, so that WS 2(1-x) Wlq 2x The alloy begins to grow on the substrate;
[0059] S5. After the insulation is completed, adjust the gas flow rate to 25sccm and reduce WS 2(1-x) Wlq 2x The excess growth, natural cooling, on the SiO 2 Two-dimensional WS prepared on Si substrate surface 2(1-x) Wlq 2x Alloy nanosheets (X=0.5).
[0060] Figure 2 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets. Figure 2 It can be seen that the two-dimensional WS 2(1-x) Wlq 2x The alloy nanosheets are regular triangular in shape and have a size of up to 400 μm.
[0061] Figure 3 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2x High-angle annular dark field scanning transmission electron microscopy and element mapping of alloy nanosheets, where (a) is a high-angle annular dark field scanning transmission electron microscopy image, and (b) to (d) are element mapping maps of Se, S, and W, respectively. Figure 3 It can be seen that Se, S, and W elements are evenly distributed, indicating that the prepared WS 2(1−x) Se 2x The alloy has good homogeneity and high quality.
[0062] Figure 4 The two-dimensional WS prepared in Example 1 2(1-x) Wlq 2x PL Mapping of alloy nanosheets at 690nm, Figure 4 It can be seen that the uniform PL intensity across the entire triangular flake indicates its high uniformity.
[0063] Example 2
[0064] Compared with Example 1, the only difference is that WS 2 Powder and WSe 2 The mass ratio of the powder is 1:3, specifically, WS 2 Powder 20mg, WSe 2 Powder 60mg, in SiO 2 Two-dimensional WS prepared on Si substrate surface 2(1-x) Wlq 2x Alloy nanosheets (X=0.75).
[0065] Fig.10 The two-dimensional WS prepared in Example 2 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets; Fig.11 The two-dimensional WS prepared in Example 2 2(1-x) Wlq 2x PL mapping of alloy nanosheets at 656nm.
[0066] Depend on Figures 10-11 It can be seen that the two-dimensional WS prepared in Example 2 2(1-x) Wlq 2x The alloy nanosheets have good uniformity, high crystallinity, and a size of up to 300μm.
[0067] Example 3
[0068] Compared with Example 1, the only difference is that WS 2 Powder and WSe 2The mass ratio of the powder is 3:1, specifically, WS 2 Powder 60mg, WSe 2 Powder 20mg, in SiO 2 Two-dimensional WS prepared on Si substrate surface 2(1-x) Wlq 2x Alloy nanosheets (X=0.25).
[0069] Fig.12 The two-dimensional WS prepared in Example 3 2(1-x) Wlq 2x Optical microscope image of alloy nanosheets; Fig.13 The two-dimensional WS prepared in Example 3 2(1-x) Wlq 2x PL mapping of alloy nanosheets at 720nm.
[0070] Depend on Figures 12-13 It can be seen that the two-dimensional WS prepared in Example 3 2(1-x) Wlq 2x The alloy nanosheets have good uniformity, high crystallinity, and a size of up to 200 μm.
[0071] Example 4
[0072] The preparation steps of the photodetector are:
[0073] S1. In Example 1, SiO 2 2D WS on Si substrate 2(1-x) Wlq 2x The alloy nanosheets were spin-coated with PMMA at a speed of 2000 rpm for 120 s. After the spin coating was completed, they were baked at 100 °C for 10 min and then immersed in BOE solution for 5 min. 2(1-x) Wlq 2x The PMMA film of the alloy nanosheet is separated from the substrate, and the separated WS 2(1-x) Wlq 2x The alloy nanosheet / PMMA film was washed with deionized water three times and then attached to a new SiO 2 / Si substrate, heated at 100 °C on a hot plate for 30 min, and finally immersed in acetone for 30 min to remove the PMMA film, and dried with nitrogen to complete the two-dimensional WS 2(1-x) Wlq 2x Transfer of alloy nanosheets to new substrates;
[0074] S2, spin coating PVA onto the two-dimensional In 2 S 3 Then heat at 110℃ for 4min and tear off slowly. 2 S3 That is, it is transferred to the PVA film, and then the In 2 S 3 PVA film and WS on substrate 2(1-x) Wlq 2x The alloy nanosheets were stacked, heated at 110 °C for 4 min, and then immersed in deionized water at 55 °C for 30 min to remove PVA and achieve In 2 S 3 Transfer in WS 2(1-x) Wlq 2x On the alloy nanosheet, a two-dimensional layered WS is formed 2(1-x) Wlq 2x Alloy / In 2 S 3 Heterojunction;
[0075] S3, in two-dimensional layered WS 2(1-x) Wlq 2x Alloy / In 2 S 3 The heterojunction surface is spin-coated with photoresist, and the device pattern is formed after plate alignment, exposure, and development by a photolithography machine, and then titanium / gold electrodes are plated to obtain a photodetector (the relevant steps are conventional methods in the field and are not described in detail here).
[0076] Example 5
[0077] Compared with Example 4, the only difference is that step S1 uses SiO 2 2D WS on Si substrate 2(1-x) Wlq 2x Alloy nanosheets.
[0078] Example 6
[0079] Compared with Example 4, the only difference is that step S1 uses SiO 2 2D WS on Si substrate 2(1-x) Wlq 2x Alloy nanosheets.
[0080] Figure 6 This is an optical microscope image of the photodetector prepared in Example 4; Figure 7 This is an optical microscope image of the photodetector prepared in Example 5; Figure 8 This is an optical microscope image of the photodetector prepared in Example 6.
[0081] Depend on Figures 6-8 It can be seen that the photodetector is a two-dimensional WS 2(1-x) Wlq 2x Alloy nanosheets are the bottom material, two-dimensional In 2 S3 As the upper material, titanium and gold are the source and drain electrodes, placed on the two-dimensional WS 2(1-x) Wlq 2x Alloy Nanostructures and Two-Dimensional In 2 S 3 Overlapping positions.
[0082] Fig. 9 is the on / off ratio of the photodetector prepared in Examples 4 to 6, Fig. 9 It can be seen that WS 2(1-x) Wlq 2x (X=0.25, 0.75) alloy and In 2 S 3 The on / off ratios of the prepared photodetectors were 3.29×10 3 4.38×10 3 Compared with WS 2(1-x) Wlq 2x (X=0.25, 0.75) alloy and In 2 S 3 The prepared photodetector, WS 2(1-x) Wlq 2x (X=0.5) alloy and In 2 S 3 The on / off ratio of the prepared photodetector reaches 2.02×10 4 , which is improved by an order of magnitude. This shows that the photocurrent generated when the unit light power is incident is larger, the photoelectric conversion efficiency is higher, and the sensitivity is higher.
[0083] Comparative Example 1
[0084] Compared with Example 1, the only difference is that WS 2 Powder and WSe 2 The mass ratio of the powder is 1:0, specifically, WS 2 Powder 80mg, WSe 2 Powder 0mg, in SiO 2 Two-dimensional WS prepared on Si substrate surface 2(1-x) Wlq 2x Alloy nanosheets (X=0).
[0085] Comparative Example 2
[0086] Compared with Example 1, the only difference is that WS 2 Powder and WSe 2 The mass ratio of the powder is 0:1, specifically, WS 2 Powder 0mg, WSe 2 Powder 80mg, in SiO 2 Two-dimensional WS prepared on Si substrate surface 2(1-x) Wlq2x Alloy nanosheets (X=1).
[0087] Figure 5 The two-dimensional WS prepared in Examples 1 to 3 and Comparative Examples 1 to 2 2(1-x) Wlq 2x Photoluminescence spectra of alloy nanosheets, by Figure 5 It can be seen that with WSe 2 Increase of powder, WS 2(1-x) Wlq 2x The photoluminescence peak position of the alloy gradually shifts to WS 2(1-x) Wlq 2x (X=1) peak position shift.
[0088] Comparative Example 3
[0089] Compared with Example 4, the only difference is that step S1 uses SiO 2 2D WS on Si substrate 2(1-x) Wlq 2x Alloy nanosheets.
[0090] Comparative Example 4
[0091] Compared with Example 4, the only difference is that step S1 uses SiO 2 2D WS on Si substrate 2(1-x) Wlq 2x Alloy nanosheets.
[0092] Fig.14 This is an optical microscope image of the photodetector prepared in Comparative Example 3; Fig.15 This is an optical microscope image of the photodetector prepared in Comparative Example 4. Figures 14 and 15 It can be seen that the photodetector is a two-dimensional WS 2(1-x) Wlq 2x Alloy nanosheets are the bottom material, two-dimensional In 2 S 3 As the upper material, titanium and gold are the source and drain electrodes, placed on the two-dimensional WS 2(1-x) Wlq 2x Alloy Nanostructures and Two-Dimensional In 2 S 3 Overlapping positions.
[0093] Fig.16 is the on / off ratio of the photodetector prepared in Comparative Examples 3-4, Fig.16 It can be seen that the comparison sample WS 2(1-x) Wlq 2x (X=0, 1) alloy and In 2 S 3The on / off ratios of the prepared photodetectors are 1.56×10 3 4.84×10 3 , compared to WS 2(1-x) Wlq 2x (X=0.25, 0.5, 0.75) alloy and In 2 S 3 The photoelectric detector produced has been improved by 1 to 2 orders of magnitude.
[0094] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A large size, uniform thickness WS 2(1-x) Wlq 2x The method for preparing alloy nanosheets is characterized by the following steps: include: WS2 and WSe2 were mixed as reactants, inert gas was used as carrier gas, SiO2 / Si substrate was used as carrier, and two-dimensional WS was prepared by physical vapor deposition with bidirectional gas flow. 2(1-x) Wlq 2x Alloy nanosheets; The WS 2(1-x) Wlq 2x The value range of X is 0.25~0.75; The physical vapor deposition step of the bidirectional airflow comprises: The air was exhausted by an inert gas with a flow rate of 120-150 sccm, and the air flow direction was from the carrier to the reactant. The flow rate was then adjusted to 30-40 sccm, and the temperature was raised to 1100-1130°C at a heating rate of 10-13°C / min. The air flow direction was changed from the reactant to the carrier, and the flow rate was adjusted to 100-120 sccm. The temperature was kept for 8-15 minutes, and the flow rate was finally adjusted to 20-30 sccm. The mixture was cooled to room temperature, and a two-dimensional WS was prepared on the surface of the carrier. 2(1-x) Wlq 2x Alloy nanosheets.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the WS2 and WSe2 mixture is 1~3:1~3.
3. The preparation method according to claim 1, characterized in that: The SiO2 surface of the SiO2 / Si substrate faces upward.
4. The preparation method according to claim 1, characterized in that: The distance between the support and the reactant is 8-10 cm.
5. WS prepared by the preparation method according to any one of claims 1 to 4 2(1-x) Wlq 2x Application of alloy nanosheets in photodetectors.
6. A high performance photodetector, characterized in that: The high-performance photodetector is a WS prepared by the preparation method according to any one of claims 1 to 4. 2(1-x) Wlq 2x The alloy nanosheets serve as the passivation layer and the gain layer.
7. A method for preparing a high-performance photodetector as claimed in claim 6, comprising: The two-dimensional layered WS 2(1-x) Wlq 2x The alloy nanosheets were transferred to the new SiO2 / Si substrate surface, and then the two-dimensional In2S3 was transferred to WS 2(1-x) Wlq 2x Alloy nanosheets to obtain two-dimensional WS 2(1-x) Wlq 2x Alloy / In2S3 heterojunction; In the two-dimensional WS 2(1-x) Wlq 2x The surface of the alloy / In2S3 heterojunction is spin-coated with photoresist, and after alignment, exposure and development by a photolithography machine, titanium / gold electrodes are plated to obtain a photodetector.
8. The preparation method according to claim 7, characterized in that: The steps of transferring to the new SiO2 / Si substrate surface are: Two-dimensional layered WS on the support surface 2(1-x) Wlq 2x The alloy nanosheets were spin-coated with PMMA solution, baked at 100 °C for 10 min, and then immersed in BOE solution for 5 min to obtain a PMMA film / 2D WS separated from the support. 2(1-x) Wlq 2x Alloy nanosheets; PMMA film / 2D WS 2(1-x) Wlq 2x The alloy nanosheets were attached to a new SiO2 / Si substrate, baked at 100-120°C for 30-40 min, immersed in acetone to remove the PMMA film, and dried with nitrogen to complete the WS. 2(1-x) Wlq 2x Transfer of alloy nanosheets to new SiO2 / Si substrate surface.
9. The preparation method according to claim 7, characterized in that: The transfer of two-dimensional In2S3 to WS 2(1-x) Wlq 2x The steps on the alloy nanosheets are: PVA was spin-coated onto the two-dimensional In2S3, heated at 110°C for 4 min, and peeled off to complete the transfer of the two-dimensional In2S3 onto the PVA film. Then, the PVA film with In2S3 adhered to it was bonded to the WS film. 2(1-x) Wlq 2x The alloy nanosheets were stacked, heated at 110 °C for 4 min, and then immersed in deionized water at 55 °C for 30 min to remove PVA, completing the two-dimensional In2S3 to WS 2(1-x) Wlq 2x alloy nanosheets to obtain two-dimensional WS 2(1-x) Wlq 2x Alloy / In2S3 heterojunction.