Composition, protective layer, laminate, and display device

By using a protective layer composition containing multifunctional polymeric compounds without luminescent inorganic semiconductor particles on the wavelength conversion layer, the problem of decreased luminous intensity caused by heat in the wavelength conversion layer is solved, thereby improving the luminous performance of the display device.

CN118786366APending Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380020547.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-17
Filing Date
2023-01-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In existing technologies, wavelength conversion layers containing quantum dots are susceptible to thermal effects, which can lead to a decrease in luminescence intensity.

Method used

A protective layer composition without luminescent inorganic semiconductor particles is used, comprising a multifunctional polymeric compound or its polymer having two or more olefinic unsaturated bonds within the molecule, forming a protective layer disposed on the wavelength conversion layer to suppress the decrease in luminescence intensity caused by heat.

Benefits of technology

It effectively suppressed the decrease in luminous intensity of the wavelength conversion layer due to heat, thereby improving the luminous performance of the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786366A_ABST
    Figure CN118786366A_ABST
Patent Text Reader

Abstract

Provided is a composition for forming a protective layer disposed on a wavelength conversion layer containing light-emitting inorganic semiconductor particles, the composition containing a polyfunctional polymerizable compound having two or more ethylenically unsaturated bonds in each molecule, or a polymer thereof, without containing light-emitting inorganic semiconductor particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition and a protective layer formed therefrom, and also to a laminate including the protective layer and a display device including the laminate. Background Art

[0002] Patent Document 1 describes a curable resin composition containing quantum dots and a wavelength conversion film formed using the curable resin composition.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-065178 Summary of the invention

[0006] The wavelength conversion layer containing light-emitting inorganic semiconductor particles such as quantum dots is susceptible to deterioration of light-emitting properties due to heat.

[0007] One object of the present invention is to provide a composition for forming a protective layer disposed on a wavelength conversion layer, which can form a protective layer capable of suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat. Another object of the present invention is to provide a protective layer formed from the composition, a laminate including the protective layer, and a display device including the laminate.

[0008] The present invention provides the following contents.

[0009] [1] A composition for forming a protective layer disposed on a wavelength conversion layer containing light-emitting inorganic semiconductor particles,

[0010] The above composition does not contain luminescent inorganic semiconductor particles,

[0011] Furthermore, it includes a polyfunctional polymerizable compound having two or more ethylenically unsaturated bonds in the molecule or a polymer thereof.

[0012] [2] The composition according to [1], wherein the polyfunctional polymerizable compound is a polyfunctional (meth)acrylic compound.

[0013] [3] The composition according to [1] or [2], wherein the polyfunctional polymerizable compound has an acidic functional group.

[0014] [4] The composition according to any one of [1] to [3], wherein the polyfunctional polymerizable compound has three or more ethylenically unsaturated bonds in the molecule.

[0015] [5] A protective layer formed from the composition according to any one of [1] to [4].

[0016] [6] A laminate comprising:

[0017] A wavelength conversion layer containing light-emitting inorganic semiconductor particles, and

[0018] The protective layer described in [5] is arranged on the wavelength conversion layer.

[0019] [7] A display device comprising the laminated body described in [6].

[0020] [8] A method for forming a protective layer disposed on a wavelength conversion layer containing light-emitting inorganic semiconductor particles,

[0021] The protective layer is formed of a composition,

[0022] The composition does not contain light-emitting inorganic semiconductor particles and contains a polyfunctional polymerizable compound having two or more ethylenically unsaturated bonds in a molecule or a polymer thereof.

[0023] [9] Use of a composition for forming a protective layer disposed on a wavelength conversion layer containing light-emitting inorganic semiconductor particles,

[0024] The composition does not contain light-emitting inorganic semiconductor particles and contains a polyfunctional polymerizable compound having two or more ethylenically unsaturated bonds in a molecule or a polymer thereof.

[0025] The present invention can provide a composition for forming a protective layer disposed on a wavelength conversion layer, which can form a protective layer capable of suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat. In addition, the present invention can also provide a protective layer formed from the composition, a laminate comprising the protective layer, and a display device comprising the laminate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic cross-sectional view showing an example of the laminated body according to the present invention.

[0027] Figure 2 This is a schematic cross-sectional view showing another example of the laminated body according to the present invention.

[0028] Figure 3 This is a schematic cross-sectional view showing another example of the laminated body according to the present invention.

[0029] Figure 4 This is a schematic cross-sectional view showing another example of the laminated body according to the present invention.

[0030] Figure 5This is a schematic cross-sectional view showing an example of a display device according to the present invention. DETAILED DESCRIPTION

[0031] The present invention relates to a composition for forming a protective layer disposed on a wavelength conversion layer, a protective layer (covering layer) formed from the composition, a laminate comprising the protective layer, and a display device comprising the laminate. In addition, the present invention relates to a method for forming a protective layer using the composition and the use of the composition for forming a protective layer.

[0032] <Composition for forming wavelength conversion layer and wavelength conversion layer>

[0033] (1) Composition for forming wavelength conversion layer I

[0034] The wavelength conversion layer is a layer that absorbs primary light from a primary light source and emits light of a wavelength different from that of the primary light, and preferably converts the wavelength of blue light, which is the primary light, into a wavelength of light of a different color. The wavelength conversion layer is preferably a layer that emits green or red light.

[0035] The wavelength conversion layer can be formed by a composition for forming a wavelength conversion layer (hereinafter also referred to as "composition I"), which contains luminescent inorganic semiconductor particles (A) (hereinafter referred to as "semiconductor particles (A)") that absorb the above-mentioned primary light and generate light with a wavelength different from that of the primary light. Composition I may contain components other than semiconductor particles (A). Composition I may also be a curable composition that is cured by light irradiation or heat. Composition I is described in more detail below.

[0036] (1-1) Luminescent Inorganic Semiconductor Particles (A)

[0037] The semiconductor particles (A) contained in the composition I emit light of a wavelength different from the primary light, preferably converting the wavelength of blue light as the primary light into a wavelength of light of a color different from the primary light. The semiconductor particles (A) preferably emit green or red light, more preferably absorb blue light and emit green or red light.

[0038] In this specification, "blue" refers to all light that is visually discerned as blue (all light that has intensity in the blue wavelength region, such as 380nm to 495nm), and is not limited to light of a single wavelength. "Green" refers to all light that is visually discerned as green (all light that has intensity in the green wavelength region, such as 495nm to 585nm), and is not limited to light of a single wavelength. "Red" refers to all light that is visually discerned as red (all light that has intensity in the red wavelength region, such as 585nm to 780nm), and is not limited to light of a single wavelength. "Yellow" refers to all light that is visually discerned as yellow (all light that has intensity in the yellow wavelength region, such as 560nm to 610nm), and is not limited to light of a single wavelength.

[0039] The luminescence spectrum of the semiconductor particles (A) emitting green light preferably includes a peak having a maximum value in the wavelength region of 500nm to 560nm, more preferably includes a peak having a maximum value in the wavelength region of 520nm to 545nm, and further preferably includes a peak having a maximum value in the wavelength region of 525nm to 535nm. Thus, the luminous intensity of the green light of the display device can be further improved. The peak preferably has a full width at half maximum of 15nm to 80nm, more preferably 15nm to 60nm, further preferably 15nm to 50nm, and particularly preferably 15nm to 45nm. Thus, the luminous intensity of the green light of the display device can be further improved.

[0040] The luminescent spectrum of the semiconductor particles (A) emitting red light preferably includes a peak having a maximum value in the wavelength region of 610nm to 750nm, more preferably includes a peak having a maximum value in the wavelength region of 620nm to 650nm, and further preferably includes a peak having a maximum value in the wavelength region of 625nm to 645nm. Thus, the luminescent intensity of the red light of the display device can be further improved. The peak preferably has a full width at half maximum of 15nm to 80nm, more preferably 15nm to 60nm, further preferably 15nm to 50nm, and particularly preferably 15nm to 45nm. Thus, the luminescent intensity of the red light of the display device can be further improved.

[0041] The emission spectrum of the semiconductor particles (A) can be measured by the method described in the section of Examples described later.

[0042] As semiconductor particles (A), quantum dots and particles composed of compounds having a perovskite crystal structure (hereinafter also referred to as "perovskite compounds") can be cited, preferably quantum dots. Quantum dots are luminescent semiconductor microparticles with a particle size of 1 nm to 100 nm, which utilize the band gap of the semiconductor to absorb ultraviolet light or visible light (e.g., blue light) and emit light.

[0043] Examples of quantum dots include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe , CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS , HgZnSeTe, HgZnSTe, etc. compounds of group 12 elements and group 16 elements; compounds of group 13 elements and group 15 elements such as GaN, GaP, GaAs, AlN, AlP, AlAs, InN, InP, InAs, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; compounds of group 14 elements and group 16 elements such as PdS, PbSe, etc.

[0044] When the quantum dots contain S and Se, they may be surface-modified with metal oxides or organic substances. By using surface-modified quantum dots, it is possible to prevent S and Se from being extracted by components contained in composition I or reactive components that may be contained.

[0045] In addition, quantum dots can also be combined with the above compounds to form a core-shell structure. Examples of such a combination include microparticles with a CdSe core and a ZnS shell, and microparticles with an InP core and a ZnSeS shell.

[0046] The energy state of quantum dots depends on their size, so by changing the particle size, the emission wavelength can be freely selected. In addition, since the spectrum width of the light emitted from quantum dots is narrow, it is beneficial to the wide color gamut of display devices. Furthermore, since quantum dots have high responsiveness, they are also beneficial in terms of the utilization efficiency of primary light.

[0047] The perovskite compound is a compound having A, B, and X as components and having a perovskite-type crystal structure.

[0048] A is a component located at each vertex of a hexahedron centered at B in the perovskite crystal structure, and is a monovalent cation.

[0049] X represents a component located at each vertex of an octahedron centered at B in a perovskite crystal structure, and is at least one ion selected from a halide ion and a thiocyanate ion.

[0050] B is a component located at the center of a hexahedron having A at its vertices and an octahedron having X at its vertices in the perovskite crystal structure, and is a metal ion.

[0051] The perovskite compound having A, B, and X as components is not particularly limited, and may be a compound having any of a three-dimensional structure, a two-dimensional structure, and a quasi-two-dimensional structure.

[0052] In the case of a three-dimensional structure, the perovskite compound consists of ABX (3+δ) express.

[0053] In the case of a two-dimensional structure, the perovskite compound consists of A2BX (4+δ) express.

[0054] Here, δ is a number that can be appropriately changed according to the charge balance of B, and is in the range of −0.7 to 0.7.

[0055] As a perovskite compound and composed of ABX (3+δ) Preferred specific examples of the compound having a three-dimensional perovskite-type crystal structure represented by include:

[0056] CH3NH3PbBr3, CH3NH3PbCl3, CH3NH3PbI3, CH3NH3PbBr (3-y) I y (0<y<3), CH3NH3PbBr (3-y) Cl y (0<y<3), (H2N=CH-NH2)PbBr3, (H2N=CH-NH2)PbCl3, (H2N=CH-NH2)PbI3;

[0057] CH3NH3Pb (1-a) Ca a Br3(0<a≤0.7), CH3NH3Pb (1-a) Sr a Br3(0<a≤0.7), CH3NH3Pb (1-a) La a Br (3+δ) (0<a≤0.7, 0<δ≤0.7), CH3NH3Pb (1-a) Ba a Br3(0<a≤0.7), CH3NH3Pb (1-a) Dy a Br (3+δ)(0<a≤0.7、0<δ≤0.7);

[0058] CH3NH3Pb (1-a) Na a Br (3+δ) (0<a≤0.7、-0.7≤δ<0)、CH3NH3Pb (1-a) LI a Br (3+δ) (0<a≤0.7、-0.7≤δ<0);

[0059] CsPb (1-a) Na a Br (3+δ) (0<a≤0.7、-0.7≤δ<0)、CsPb (1-a) LI a Br (3+δ) (0<a≤0.7、-0.7≤δ<0);

[0060] CH3NH3Pb (1-a) Na a Br (3+δ-y) I y (0<a≤0.7、-0.7≤δ<0、0<y<3)、CH3NH3Pb (1-a) LI a Br (3+δ-y) I y (0<a≤0.7、-0.7≤δ<0、0<y<3)、CH3NH3Pb (1-a) Na a Br (3+δ-y) Cl y (0<a≤0.7、-0.7≤δ<0、0<y<3)、CH3NH3Pb (1-a) LI a Br (3+δ-y) Cl y (0<a≤0.7、-0.7≤δ<0、0<y<3);

[0061] (H2N=CH-NH2)Pb (1-a) Na a Br (3+δ) (0<a≤0.7、-0.7≤δ<0)、(H2N=CH-NH2)Pb (1-a) LI a Br (3+δ) (0<a≤0.7、-0.7≤δ<0)、(H2N=CH-NH2)Pb (1-a) Na a Br (3+δ-y) I y(0<a≤0.7、-0.7≤δ<0、0<y<3)、(H2N=CH-NH2)Pb (1-a) Na a Br (3+δ-y) Cl y (0<a≤0.7、-0.7≤δ<0、0<y<3);

[0062] CsPbBr3、CsPbCl3、CsPbI3、CsPbBr (3-y) I y (0<y<3)、CsPbBr (3-y) Cl y (0<y<3)、CH3NH3PbBr (3-y) Cl y (0<y<3);

[0063] CH3NH3Pb (1-a) Zn a Br3(0<a≤0.7)、CH3NH3Pb (1-a) Al a Br (3+δ) (0<a≤0.7、0≤δ≤0.7)、CH3NH3Pb (1-a) Co a Br3(0<a≤0.7)、CH3NH3Pb (1-a) Mn a Br3(0<a≤0.7)、CH3NH3Pb (1-a) Mg a Br3(0<a≤0.7)、CsPb (1-a) Zn a Br3(0<a≤0.7)、CsPb (1-a) Al a Br (3+δ) (0<a≤0.7、0<δ≤0.7)、CsPb (1-a) Co a Br3(0<a≤0.7)、CsPb (1-a) Mn a Br3(0<a≤0.7)、CsPb (1-a) Mg a Br3(0<a≤0.7)、CH3NH3Pb (1-a) Zn a Br (3-y) I y (0<a≤0.7、0<y<3);

[0064] CH3NH3Pb (1-a) Al a Br (3+δ-y) Iy (0 < a ≤ 0.7, 0 < δ ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Co a Br (3-y) I y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mn a Br (3-y) I y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mg a Br (3-y) I y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Zn a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Al a Br (3+δ-y) Cl y (0 < a ≤ 0.7, 0 < δ ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Co a Br (3+δ-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mn a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mg a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3);

[0065] (H2N=CH-NH2)Zn a (0 < a ≤ 0.7), (H2N=CH-NH2)MgBr3 a (0 < a ≤ 0.7), (H2N=CH-NH2)PbBr3 (1-a) Zn a Br (3-y) I y (0 < a ≤ 0.7, 0 < y < 3), (H2N=CH-NH2)Pb (1-a) Zn a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), etc.

[0066] As a perovskite compound and composed of A2BX (4+δ) Preferred specific examples of the compound having a two-dimensional perovskite-type crystal structure represented by include:

[0067] (C4H9NH3)2PbBr4, (C4H9NH3)2PbCl4, (C4H9NH3)2PbI4, (C7H 15 NH3)2PbBr4、(C7H 15 NH3)2PbCl4、(C7H 15 NH3)2PbI4, (C4H9NH3)2Pb (1-a) LI a Br (4+δ) (0<a≤0.7, -0.7≤δ<0), (C4H9NH3)2Pb (1-a) Na a Br (4+δ) (0<a≤0.7, -0.7≤δ<0), (C4H9NH3)2Pb (1-a) R a Br (4+δ) (0<a≤0.7, -0.7≤δ<0);

[0068] (C7H 15 NH3)2Pb (1-a) Na a Br (4+δ) (0<a≤0.7, -0.7≤δ<0), (C7H 15 NH3)2Pb (1-a) LI a Br (4+δ) (0<a≤0.7, -0.7≤δ<0), (C7H 15 NH3)2Pb (1-a) BnB (4+δ) (0<a≤0.7, -0.7≤δ<0);

[0069] (C4H9NH3)2Pb (1-a) Na a Br (4+δ-y) I y (0<a≤0.7, -0.7≤δ<0, 0<y<4), (C4H9NH3)2Pb (1-a) LI a Br (4+δ-y) I y (0<a≤0.7, -0.7≤δ<0, 0<y<4), (C4H9NH3)2Pb (1-a) R a Br (4+δ-y) Iy (0.a≤0.7、-0.7≤δ<0、0<y<4)?

[0070] (C4H9NH3)2Pb (1-a) Ankle a Br (4+δ-y) Cl y (0<a≤0.7、-0.7≤δ<0、0<y<4)、(C4H9NH3)2Pb (1-a) LI a Br (4+δ-y) Cl y (0<a≤0.7、-0.7≤δ<0、0<y<4)、(C4H9NH3)2Pb (1-a) Rb a Br (4+δ-y) Cl y (0.a≤0.7、-0.7≤δ<0、0<y<4)?

[0071] (C4H9NH3)2PbBr4、(C7H 15 NH3)2PbBr4

[0072] (C4H9NH3)2PbBr (4-y) Cl y (0<y<4)、(C4H9NH3)2PbBr (4-y) I y (0<y<4);

[0073] (C4H9NH3)2Pb (1-a) Zn a Br4(0<a≤0.7)、(C4H9NH3)2Pb (1-a) Mg a Br4(0<a≤0.7)、(C4H9NH3)2Pb (1-a) Co a Br4(0<a≤0.7)、(C4H9NH3)2Pb (1-a) Mn a Br4(0<a≤0.7)?

[0074] (C7H 15 NH3)2Pb (1-a) Zn a Br4(0<a≤0.7)、(C7H 15 NH3)2Pb (1-a) Mg a Br4(0<a≤0.7)、(C7H 15 NH3)2Pb (1-a) Co aBr4(0<a≤0.7),(C7H 15 NH3)2Pb (1-a) Mn a Br4(0<a≤0.7);

[0075] (C4H9NH3)2Pb (1-a) Zn a Br (4-y) I y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Mg a Br (4-y) I y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Co a Br (4-y) I y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Mn a Br (4-y) I y (0<a≤0.7, 0<y<4);

[0076] (C4H9NH3)2Pb (1-a) Zn a Br (4-y) Cl y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Mg a Br (4-y) Cl y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Co a Br (4-y) Cl y (0<a≤0.7, 0<y<4), (C4H9NH3)2Pb (1-a) Mn a Br (4-y) Cl y (0<a≤0.7, 0<y<4), etc.

[0077] Composition I may contain two or more semiconductor particles (A). For example, composition I may contain only one semiconductor particle (A) that absorbs primary light and emits green light, or it may contain two or more in combination. Composition I may contain only one semiconductor particle (A) that absorbs primary light and emits red light, or it may contain two or more in combination.

[0078] The content of the semiconductor particles (A) in composition I, relative to the total amount of the solid components of composition I, is, for example, 1 mass % to 60 mass %, preferably 10 mass % to 50 mass %, more preferably 15 mass % to 50 mass %, further preferably 20 mass % to 50 mass %, and further preferably 20 mass % to 40 mass %.

[0079] When composition I contains two or more semiconductor particles (A), the content of the semiconductor particles (A) refers to the total content of the two or more semiconductor particles (A). The same applies to the components contained or may be contained in composition I other than the semiconductor particles (A) described later. When the composition contains two or more, the content or content of the component refers to their total content or total content. The same applies to composition II described later.

[0080] In this specification, the total amount of solid content of the composition refers to the total amount of components contained in the composition after removing the solvent (J). The content of the solid content of the composition can be measured by a known analytical method such as liquid chromatography or gas chromatography. The content of each component in the solid content of the composition can be calculated based on the formulation when the composition is prepared.

[0081] (1-2) Organic ligand (G)

[0082] Composition I may further include an organic ligand (G), and the semiconductor particles (A) may also be present in composition I in a state coordinated with the organic ligand (G). The organic ligand (G) is, for example, an organic compound having a polar group that exhibits coordination ability to the semiconductor particles (A). The organic ligand (G) may, for example, be coordinated to the surface of the semiconductor particles (A). Composition I may include one or more organic ligands (G).

[0083] In composition I, the organic ligand (G) preferably has at least a portion of its molecules coordinated to the semiconductor particles (A), and may have all or substantially all of its molecules coordinated to the semiconductor particles (A). From the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, it is advantageous to include an organic ligand (G) coordinated to the semiconductor particles (A).

[0084] The above-mentioned polar group of the organic ligand (G) is, for example, at least one group selected from a thiol group (-SH), a carboxyl group (-COOH) and an amino group (-NH2). The polar group selected from this group is advantageous in improving the coordination with the semiconductor particles (A). High coordination helps to improve the stability and dispersibility of the semiconductor particles (A) in the composition I, and to improve the luminous intensity of the wavelength conversion layer. Among them, the polar group is more preferably at least one group selected from a thiol group and a carboxyl group. The organic ligand (G) may have one or more polar groups.

[0085] The organic ligand (G) can be, for example, represented by the following formula (x):

[0086] X A -R X (x)

[0087] An organic compound represented by A is the above polar group, R X It is a monovalent hydrocarbon group that may contain heteroatoms (N, O, S, halogen atoms, etc.). The hydrocarbon group may have one or more unsaturated bonds such as carbon-carbon double bonds. The hydrocarbon group may have a linear, branched or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, or 1 to 30. The methylene group contained in the hydrocarbon group may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc.

[0088] Group R X It may contain a polar group. As a specific example of the polar group, the polar group X A The description involved.

[0089] As having carboxyl group as polar group X A Specific examples of organic ligands include formic acid, acetic acid, propionic acid, and other saturated or unsaturated fatty acids. Specific examples of saturated or unsaturated fatty acids include saturated fatty acids such as butyric acid, valeric acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, arachidic acid, behenic acid, and tetradecanoic acid; monovalent unsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, eicosenoic acid, erucic acid, and nervonic acid; polyvalent unsaturated fatty acids such as linoleic acid, α-linolenic acid, γ-linolenic acid, octadecatetraenoic acid, dihomo-γ-linolenic acid, arachidic acid, eicosatetraenoic acid, docosadienoic acid, and adrenic acid (docosatetraenoic acid).

[0090] Having a thiol group or an amino group as the polar group X A Specific examples of the organic ligand include the above-exemplified organic ligands having a carboxyl group as a polar group X A An organic ligand in which the carboxyl group of the organic ligand is replaced by a thiol group or an amino group.

[0091] In addition to the above, examples of the organic ligand represented by the above formula (x) include compound (G-1) and compound (G-2).

[0092] [Compound (G-1)]

[0093] Compound (G-1) is a compound having a first functional group and a second functional group. The first functional group is a carboxyl group (-COOH), and the second functional group is a carboxyl group or a thiol group (-SH). Compound (G-1) has a carboxyl group and / or a thiol group, and thus can become a ligand coordinated to the semiconductor particle (A). Composition I may contain only one compound (G-1) or two or more.

[0094] An example of compound (G-1) is a compound represented by the following formula (G-1a). Compound (G-1) may be an acid anhydride of the compound represented by formula (G-1a).

[0095]

[0096] [Where R B represents a divalent hydrocarbon group. B When there are multiple substituents, they may be the same or different. The above hydrocarbon group may also have one or more substituents. When there are multiple substituents, they may be the same or different, and they may be bonded to each other to form a ring together with the atoms to which they are bonded. The -CH2- contained in the above hydrocarbon group may be substituted with at least one of -O-, -S-, -SO2-, -CO- and -NH-.

[0097] p represents an integer from 1 to 10.]

[0098] As R B Examples of the divalent hydrocarbon group represented by include a chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group.

[0099] Examples of the chain hydrocarbon group include linear or branched alkanediyl groups, which usually have 1 to 50 carbon atoms, preferably 1 to 20 carbon atoms, and more preferably 1 to 10 carbon atoms. Examples of the alicyclic hydrocarbon group include monocyclic or polycyclic cycloalkanediyl groups, which usually have 3 to 50 carbon atoms, preferably 3 to 20 carbon atoms, and more preferably 3 to 10 carbon atoms. Examples of the aromatic hydrocarbon group include monocyclic or polycyclic arenediyl groups, which usually have 6 to 20 carbon atoms.

[0100] Examples of the substituent that the hydrocarbon group may have include an alkyl group having 1 to 50 carbon atoms, a cycloalkyl group having 3 to 50 carbon atoms, an aryl group having 6 to 20 carbon atoms, a carboxyl group, an amino group, a halogen atom, etc. The substituent that the hydrocarbon group may have is preferably a carboxyl group, an amino group or a halogen atom.

[0101] When -CH2- contained in the above hydrocarbon group is substituted with at least one of -O-, -CO- and -NH-, the substitution for -CH2- is preferably at least one of -CO- and -NH-, more preferably -NH-. p is preferably 1 or 2.

[0102] Examples of the compound represented by formula (G-1a) include compounds represented by the following formulae (1-1) to (1-9).

[0103]

[0104] Specific examples of the compound represented by formula (G-1a) when represented by chemical names include mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, 4-mercaptobutyric acid, mercaptosuccinic acid, mercaptostearic acid, mercaptooctanoic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-methoxybutyl 3-mercaptopropionate, 3-mercapto-2-methylpropionic acid, etc. Among them, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.

[0105] Another example of the compound (G-1) is a polycarboxylic acid compound, and preferably a compound (G-1b) in which -SH in the formula (G-1a) is substituted with a carboxyl group (-COOH) among the compounds represented by the above formula (G-1a).

[0106] Examples of the compound (G-1b) include the following compounds.

[0107] Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, dodecafluorooctanedioic acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenedioic acid, sebacic acid, hexadecanoic acid, acetylene dicarboxylic acid, trans-guanosine, 1,3-adamantanedioic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1, 4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalene dicarboxylic acid, 2,3-norbornene dicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroisophthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, 2,5-furanone carboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-pyridinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 3,4-pyridinedicarboxylic acid, pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-stilbene dicarboxylic acid, anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, chelidonic acid monohydrate, azobenzene-4,4'-dicarboxylic acid, azobenzene-3,3'-dicarboxylic acid, chlorendic acid, 1H-imidazole-4,5-dicarboxylic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 1,10 -bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutyric acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl) ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropyldiphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl)isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.

[0108] From the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescent intensity of the wavelength conversion layer, the molecular weight of the compound (G-1) is preferably 3000 or less, more preferably 2500 or less, further preferably 2000 or less, further preferably 1000 or less, particularly preferably 800 or less, and most preferably 500 or less. The molecular weight of the compound (G-1) is usually 100 or more.

[0109] The molecular weight may be a number average molecular weight or a weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are respectively the number average molecular weight and the weight average molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC).

[0110] When the composition I contains the compound (G-1), the content ratio of the compound (G-1) to the semiconductor particles (A) in the composition I is preferably 0.001 to 1, more preferably 0.01 to 0.5, and further preferably 0.02 to 0.45, in terms of mass ratio. If the content ratio is within this range, it is advantageous from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer.

[0111] When composition I contains compound (G-1), from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the content of compound (G-1) in composition I is preferably 0.1 mass % to 20 mass % relative to the total amount of solid components of composition I, more preferably 0.2 mass % to 20 mass %, further preferably 0.2 mass % to 10 mass %, further preferably 0.5 mass % to 10 mass %, particularly preferably 0.5 mass % to 8 mass %.

[0112] [Compound (G-2)]

[0113] Compound (G-2) is a compound different from compound (G-1), and is a compound containing a polyalkylene glycol structure and having a polar group at a molecular terminal. The molecular terminal is preferably the terminal of the longest carbon chain (carbon atoms in the carbon chain may be substituted with other atoms such as oxygen atoms) in compound (G-2).

[0114] Composition I may contain only one compound (G-2) or two or more compounds. Composition I may contain compound (G-1) or compound (G-2), or compound (G-1) and compound (G-2).

[0115] In addition, the compound which contains a polyalkylene glycol structure and has the said 1st functional group and 2nd functional group belongs to compound (G-1).

[0116] The polyalkylene glycol structure is defined by the following formula:

[0117]

[0118] The structure represented by (n is an integer greater than 2). C The alkylene group includes, for example, an ethylene group and a propylene group.

[0119] Specific examples of the compound (G-2) include polyalkylene glycol compounds represented by the following formula (G-2a).

[0120]

[0121] In formula (G-2a), X is a polar group, Y is a monovalent group, and Z is C is a divalent or trivalent group. n is an integer greater than 2. m is 1 or 2. C It is an alkylene group.

[0122] The polar group X is preferably selected from at least one of a thiol group (-SH), a carboxyl group (-COOH) and an amino group (-NH2). The polar group selected from this group is advantageous in improving the coordination with the semiconductor particles (A). Among them, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the polar group X is more preferably selected from at least one of a thiol group and a carboxyl group.

[0123] The group Y is a monovalent group. The group Y is not particularly limited, and examples thereof include monovalent hydrocarbon groups that may have substituents (N, O, S, halogen atoms, etc.). The -CH2- contained in the hydrocarbon group may also be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The number of carbon atoms in the above hydrocarbon group is, for example, 1 to 12. The hydrocarbon group may also have an unsaturated bond.

[0124] As the group Y, there can be mentioned an alkyl group having 1 to 12 carbon atoms in a straight chain, branched chain or cyclic structure; an alkoxy group having 1 to 12 carbon atoms in a straight chain, branched chain or cyclic structure, etc. The number of carbon atoms of the alkyl group and the alkoxy group is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The -CH2- contained in the alkyl group and the alkoxy group may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. Among them, the group Y is preferably a straight chain or branched chain alkoxy group having 1 to 4 carbon atoms, and more preferably a straight chain alkoxy group having 1 to 4 carbon atoms.

[0125] The group Y may contain a polar group. As the polar group, at least one group selected from a thiol group (-SH), a carboxyl group (-COOH) and an amino group (-NH2) may be cited. Among them, as described above, a compound containing a polyalkylene glycol structure and having the first functional group and the second functional group belongs to compound (G-1). The polar group is preferably disposed at the end of the group Y.

[0126] Group Z C is a divalent or trivalent group. C , is not particularly limited, and examples thereof include divalent or trivalent hydrocarbon groups which may contain heteroatoms (N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may further have an unsaturated bond.

[0127] The group Z as a divalent group C , examples include alkylene groups having 1 to 24 carbon atoms and having a linear, branched or cyclic structure; alkenylene groups having 1 to 24 carbon atoms and having a linear, branched or cyclic structure. The number of carbon atoms of the alkyl and alkenylene groups is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4. The -CH2- contained in the alkyl and alkenylene groups may be substituted by -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. The group Z as a trivalent group C Examples of the divalent group Z include C A group formed by removing a hydrogen atom.

[0128] Group Z C It may have a straight chain structure. C In a branch chain other than the branch chain including the polyalkylene glycol structure represented by the above formula (G-2a), another polyalkylene glycol structure different from the polyalkylene glycol structure represented by the above formula (G-2a) may be included.

[0129] Among them, group Z C The linear or branched alkylene group having 1 to 6 carbon atoms is preferred, and the linear alkylene group having 1 to 4 carbon atoms is more preferred.

[0130] R C The alkylene group is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.

[0131] In the formula (G-2a), n is an integer of 2 or more, preferably 2-540, more preferably 2-120, and even more preferably 2-60.

[0132] The molecular weight of compound (G-2) can be, for example, about 150 to 10,000, but from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, it is preferably 150 to 5,000, and more preferably 150 to 4,000. The molecular weight can be a number average molecular weight or a weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight respectively measured by GPC in terms of standard polystyrene.

[0133] When the composition I contains the compound (G-2), the content ratio of the compound (G-2) relative to the semiconductor particles (A) in the composition I is preferably 0.001 to 2, more preferably 0.01 to 1.5, and further preferably 0.1 to 1. If the content ratio is within this range, it is advantageous from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer.

[0134] When composition I contains compound (G-2), from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the content of compound (G-2) in composition I is preferably 0.1 mass % to 40 mass % relative to the total amount of solid components of composition I, more preferably 0.1 mass % to 20 mass %, further preferably 1 mass % to 15 mass %, and further preferably 2 mass % to 12 mass %.

[0135] When composition I contains an organic ligand (G), the ratio of the content of the organic ligand (G) to the content of the semiconductor particles (A) in composition I is preferably 0.001 to 1, more preferably 0.01 to 0.8, and further preferably 0.02 to 0.5, in terms of mass ratio. If the content ratio is within this range, it is advantageous from the perspective of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer. The content of the organic ligand (G) mentioned here refers to the total content of all organic ligands contained in composition I.

[0136] From the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the total content of the semiconductor particles (A) and the organic ligands (G) in composition I is preferably 10% by mass to 75% by mass, more preferably 12% by mass to 70% by mass, and further preferably 15% by mass to 65% by mass, relative to the total amount of solid components of composition I.

[0137] (1-3) Light scattering agent (B)

[0138] Composition I may further contain a light scattering agent (B). The wavelength conversion layer formed by the composition may exhibit light scattering properties. Composition I may contain two or more light scattering agents (B). From the viewpoint of increasing the luminous intensity of the wavelength conversion layer, composition I preferably further contains a light scattering agent (B).

[0139] As the light scattering agent (B), inorganic particles such as particles of metal or metal oxide, glass particles, etc. can be cited. As metal oxides, TiO2, SiO2, BaTiO3, ZnO, etc. can be cited. From the perspective of efficient light scattering, particles of TiO2 are preferred. The particle size of the light scattering agent (B) is, for example, about 0.03 μm to 20 μm, preferably 0.05 μm to 1 μm, and more preferably 0.05 μm to 0.5 μm.

[0140] As the light scattering agent (B), a light scattering agent obtained by pre-dispersing the light scattering agent in a part or all of the solvent (J) using a dispersant can also be used. As the dispersant, a commercially available product can be used. Examples of commercially available products include:

[0141] BYK-Chemie Japan Co., Ltd. DISPERBYK-101, 102, 103, 106, 107, 108, 109, 110, 111, 116, 118, 130, 140, 154, 161, 162, 163, 164, 165, 166, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 192, 2000, 2001, 2020, 2025, 2050, 2070, 2095, 2150, 2155; ANTI-TERRA-U, U100, 203, 204, 250,; B YK-P104, P104S, P105, 220S, 6919; BYK-LPN6919, 21116; LACTIMON, LACTIMON-WS; Bykumen, etc.;

[0142] SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36600, 38500, 41000, 41090, 53095, 55000, 76500, etc. manufactured by Japan Lubrizol;

[0143] EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 4402, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 4550, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, 1503, etc. manufactured by BASF;

[0144] Ajisper PA111, PB711, PB821, PB822, PB824, etc. manufactured by Ajinomoto Fine-Techno.

[0145] The content of the light scattering agent (B) in the composition I is, for example, 0.001% by mass to 50% by mass, and is preferably 1% by mass to 30% by mass, more preferably 2% by mass to 20% by mass, further preferably 2% by mass to 15% by mass, and further preferably 3% by mass to 10% by mass, relative to the total amount of solid components of the composition I, from the viewpoint of improving the light scattering ability and luminous intensity of the wavelength conversion layer.

[0146] (1-4) Resin (C)

[0147] Composition I may further contain a resin (C). From the viewpoint of forming a wavelength conversion layer from composition I, composition I preferably contains a resin (C). Resin (C) may contain one or more resins. Examples of resin (C) include the following resins [K1] to [K4].

[0148] Resin [K1]: a copolymer of at least one (a) selected from unsaturated carboxylic acids and unsaturated carboxylic anhydrides (hereinafter, also referred to as “(a)”), and a monomer (c) copolymerizable with (a) (but different from (a)) (hereinafter, also referred to as “(c)”);

[0149] Resin [K2]: a resin obtained by reacting a monomer (b) having a cyclic ether structure having 2 to 4 carbon atoms and an ethylenically unsaturated bond (hereinafter also referred to as "(b)") with a copolymer of (a) and (c);

[0150] Resin [K3]: a resin obtained by reacting a copolymer of (a) and (b) with (c);

[0151] Resin [K4]: A resin obtained by reacting a copolymer of (a), (b) and (c), and further reacting the copolymer with a carboxylic anhydride.

[0152] Examples of (a) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid;

[0153] Unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, 3-vinylphthalic acid, 4-vinylphthalic acid, 3,4,5,6-tetrahydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, dimethyltetrahydrophthalic acid, and 1,4-cyclohexenedicarboxylic acid;

[0154] Bicyclic unsaturated compounds containing a carboxyl group, such as methyl-5-norbornene-2,3-dicarboxylic acid, 5-carboxybicyclo[2.2.1]hept-2-ene, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene, 5-carboxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-methylbicyclo[2.2.1]hept-2-ene and 5-carboxy-6-ethylbicyclo[2.2.1]hept-2-ene;

[0155] Unsaturated dicarboxylic anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride;

[0156] Unsaturated mono[(meth)acryloyloxyalkyl] esters of divalent or higher polyvalent carboxylic acids such as mono[2-(meth)acryloyloxyethyl] succinate and mono[2-(meth)acryloyloxyethyl] phthalate;

[0157] Unsaturated (meth)acrylates containing a hydroxyl group and a carboxyl group in the same molecule such as α-(hydroxymethyl) (meth)acrylic acid, and the like.

[0158] Among these, (meth)acrylic acid, maleic anhydride, and the like are preferred from the viewpoint of copolymerization reactivity and the like.

[0159] In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid, and the same applies to "(meth)acryloyl", "(meth)acrylate" and the like.

[0160] (b) is, for example, a monomer having a cyclic ether structure having 2 to 4 carbon atoms (e.g., at least one selected from an oxirane ring, an oxetane ring, and a tetrahydrofuran ring) and an ethylenically unsaturated bond. (b) is preferably a monomer having a cyclic ether structure having 2 to 4 carbon atoms and a (meth)acryloyloxy group.

[0161] The number of carbon atoms in the cyclic ether structure refers to the number of carbon atoms in a condensed ring when a ring including an ether bond such as an oxirane ring, an oxetane ring or a tetrahydrofuran ring forms a condensed ring with another ring.

[0162] Examples of (b) include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, glycidyl vinyl ether, o-vinyl benzyl glycidyl ether, m-vinyl benzyl glycidyl ether, p-vinyl benzyl glycidyl ether, α-methyl-o-vinyl benzyl glycidyl ether, α-methyl-m-vinyl benzyl glycidyl ether, α-methyl-p-vinyl benzyl glycidyl ether, 2,3-bis(glycidyloxymethyl)styrene, 2,4-bis(glycidyloxymethyl)styrene, Monomers having an ethylene oxide ring and an ethylenically unsaturated bond, such as 2,5-bis(glycidyloxymethyl)styrene, 2,6-bis(glycidyloxymethyl)styrene, 2,3,4-tri(glycidyloxymethyl)styrene, 2,3,5-tri(glycidyloxymethyl)styrene, 2,3,6-tri(glycidyloxymethyl)styrene, 3,4,5-tri(glycidyloxymethyl)styrene, and 2,4,6-tri(glycidyloxymethyl)styrene;

[0163] Monomers having an oxetane ring and an ethylenically unsaturated bond, such as 3-methyl-3-methacryloyloxymethyloxetane, 3-methyl-3-acryloyloxymethyloxetane, 3-ethyl-3-acryloyloxymethyloxetane, 3-methyl-3-acryloyloxyethyloxetane, 3-methyl-3-acryloyloxyethyloxetane, 3-ethyl-3-acryloyloxyethyloxetane, and 3-ethyl-3-acryloyloxyethyloxetane;

[0164] Monomers having a tetrahydrofuran ring and an ethylenically unsaturated bond, such as tetrahydrofurfuryl acrylate (for example, Viscoat V#150, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and tetrahydrofurfuryl methacrylate, etc.

[0165] As (b), a monomer having an ethylene oxide ring and an ethylenically unsaturated bond is preferred because (b) has high reactivity during the production of the resins [K2] to [K4] and is less likely to remain unreacted.

[0166] Examples of (c) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0](meth)acrylate. 2,6 ] decane-8-yl ester (in the technical field, as a common name, it is called "dicyclopentyl (meth)acrylate". In addition, it is sometimes called "tricyclodecyl (meth)acrylate"), tricyclo[5.2.1.0 2,6 ] (meth)acrylates such as decane-8-yl ester (in the art, commonly known as "dicyclopentenyl (meth)acrylate"), dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, allyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate;

[0167] (Meth)acrylates containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate;

[0168] Diethyl maleate, diethyl fumarate, diethyl itaconate and other dicarboxylic acid diesters;

[0169] Bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxybicyclo[2.2.1]hept-2-ene, 5-hydroxymethylbicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-methoxybicyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-bis(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-bis(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5,6-dimethoxy Bicyclic unsaturated compounds such as bicyclo[2.2.1]hept-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2-ene, 5-cyclohexyloxycarbonylbicyclo[2.2.1]hept-2-ene, 5-phenoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-bis(tert-butoxycarbonyl)bicyclo[2.2.1]hept-2-ene, and 5,6-bis(cyclohexyloxycarbonyl)bicyclo[2.2.1]hept-2-ene;

[0170] Dicarbonyl imide derivatives such as N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidohexanoate, N-succinimidyl-3-maleimidopropionate, and N-(9-acridinyl)maleimide;

[0171] Styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylic acid amide, methacrylamide, vinyl acetate, 1,3-butadiene isoprene, 2,3-dimethyl-1,3-butadiene;

[0172] Acrylic acid 3,4-epoxy tricyclic [5.2.1.0 2,6 ]Decan-8-yl ester, 3,4-epoxytricyclic acrylate [5.2.1.0 2,6 ] Monomers having a cyclic ether structure having more than 4 carbon atoms and an ethylenically unsaturated bond, such as decane-9-yl ester, etc.

[0173] The number of carbon atoms in the cyclic ether structure refers to the number of carbon atoms in a condensed ring when a ring including an ether bond such as an oxirane ring, an oxetane ring or a tetrahydrofuran ring forms a condensed ring with another ring.

[0174] Among the above, from the perspective of copolymerization reactivity and heat resistance of the resin (C), preferred (c) are styrene, vinyltoluene, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, bicyclo[2.2.1]hept-2-ene, etc. Also preferred as (c) are monomers having a cyclic ether structure having more than 4 carbon atoms and an ethylenically unsaturated bond.

[0175] Among all the constituent units constituting the resin [K1], the ratio derived from each constituent unit in the resin [K1] is preferably:

[0176] Constituent units derived from (a): 2 mol% to 60 mol%,

[0177] Constituent units derived from (c): 40 mol% to 98 mol%,

[0178] More preferably:

[0179] Constituent units derived from (a): 10 mol% to 50 mol%,

[0180] Constituent units derived from (c): 50 mol% to 90 mol%.

[0181] When the ratio of the structural unit of the resin [K1] is within the above range, the storage stability of the composition I and the solvent resistance of the wavelength conversion layer tend to be excellent.

[0182] The resin [K1] can be produced by referring to the method described in the document "Experimental Methods for Polymer Synthesis" (Otsu Takayuki Publishing Co., Ltd., Chemical Dojin, 1st edition, 1st printing, published on March 1, 1972) and the cited documents described in the document.

[0183] Specifically, a method is exemplified in which predetermined amounts of (a) and (c), a polymerization initiator, a solvent, etc. are added to a reaction vessel, oxygen is replaced with nitrogen gas, for example, to create a deoxygenated atmosphere, and heating and heat-retaining are performed while stirring.

[0184] The polymerization initiator and solvent used are not particularly limited, and those commonly used in the art can be used. For example, as the polymerization initiator, there can be mentioned azo compounds (2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), etc.), organic peroxides (benzoyl peroxide, etc.), and as the solvent, any solvent that dissolves each monomer can be used, and the solvents described later as the solvent (J) that can be included in the composition I can be mentioned.

[0185] The obtained copolymer may be used directly as a solution after the reaction, or as a concentrated or diluted solution, or as a solid (powder) obtained by reprecipitation or the like. If a solvent (J) described later is used as a solvent during polymerization, the solution after the reaction can be used directly in the preparation of composition I, thereby simplifying the manufacturing process of composition I.

[0186] The resin [K2] can be produced by adding the cyclic ether having 2 to 4 carbon atoms contained in (b) to the carboxylic acid and / or carboxylic anhydride contained in (a), to the copolymer of (a) and (c).

[0187] First, a copolymer of (a) and (c) is produced in the same manner as described as the method for producing resin [K1]. In this case, the ratio derived from each structural unit is preferably the same as the ratio described for resin [K1].

[0188] Next, the cyclic ether having 2 to 4 carbon atoms contained in (b) is reacted with a part of the carboxylic acid and / or carboxylic anhydride derived from (a) in the above copolymer.

[0189] After the production of the copolymer of (a) and (c), the atmosphere in the flask is replaced by air from nitrogen, and the resin [K2] can be produced by reacting at 60°C to 130°C for 1 to 10 hours in the presence of (b), a reaction catalyst (e.g., an organic phosphorus compound, a metal complex, an amine compound, etc.) of a carboxylic acid or a carboxylic anhydride and a cyclic ether, and an inhibitor (e.g., hydroquinone, etc.).

[0190] The amount of (b) used is preferably 5 to 80 mol, more preferably 10 to 75 mol, relative to 100 mol of (a). By setting it within this range, the storage stability of the composition I and the balance of the solvent resistance, heat resistance and mechanical strength of the wavelength conversion layer tend to be improved.

[0191] As the organic phosphorus compound of the reaction catalyst, for example, triphenylphosphine can be mentioned. As the amine compound of the reaction catalyst, for example, aliphatic tertiary amine compounds or aliphatic quaternary ammonium salt compounds can be used, and as specific examples thereof, for example, tris(dimethylaminomethyl)phenol, triethylamine, tetrabutylammonium bromide, tetrabutylammonium chloride can be mentioned. The reaction catalyst is preferably an organic phosphorus compound.

[0192] The amount of the reaction catalyst used is preferably 0.001 to 5 parts by mass based on 100 parts by mass of the total amount of (a), (b), and (c).

[0193] The amount of the polymerization inhibitor used is preferably 0.001 to 5 parts by mass based on 100 parts by mass of the total amount of (a), (b), and (c).

[0194] The reaction conditions such as the charging method, reaction temperature and time can be appropriately adjusted in consideration of the production equipment, the heat generated by polymerization, etc. It should be noted that the polymerization conditions can also be appropriately adjusted in consideration of the production equipment, the heat generated by polymerization, etc., in the charging method and reaction temperature.

[0195] As a first step, the resin [K3] is subjected to the same method as the above-mentioned method for producing the resin [K1] to obtain a copolymer of (b) and (c). As above, the obtained copolymer may be used directly as a solution after the reaction, or may be used as a concentrated or diluted solution, or may be used as a solid (powder) obtained by a method such as reprecipitation.

[0196] The ratios of the constituent units derived from (b) and (c) relative to the total number of moles of all constituent units constituting the copolymer are preferably:

[0197] Constituent units derived from (b): 5 mol% to 95 mol%,

[0198] Constituent units derived from (c): 5 mol% to 95 mol%,

[0199] More preferably:

[0200] Constituent units derived from (b): 10 mol% to 90 mol%,

[0201] Constituent units derived from (c): 10 mol% to 90 mol%.

[0202] Resin [K3] can be obtained by reacting the carboxylic acid or carboxylic anhydride contained in (a) with the cyclic ether derived from (b) contained in the copolymer of (b) and (c) under the same conditions as those for producing resin [K2].

[0203] The amount of (a) to be reacted with the copolymer is preferably 5 to 80 mol relative to 100 mol of (b).

[0204] The resin [K4] is a resin obtained by further reacting a carboxylic acid anhydride with the resin [K3]. The carboxylic acid anhydride and the hydroxyl group generated by the reaction of the cyclic ether with the carboxylic acid or the carboxylic acid anhydride are reacted.

[0205] Examples of the carboxylic anhydride include maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride.

[0206] The amount of the carboxylic anhydride used is preferably 0.5 to 1 mol relative to 1 mol of the amount of (a) used.

[0207] Examples of the resin [K1], resin [K2], resin [K3], and resin [K4] include resin [K1] such as benzyl (meth)acrylate / (meth)acrylic acid copolymer and styrene / (meth)acrylic acid copolymer;

[0208] Resins such as a resin obtained by adding glycidyl (meth)acrylate to a benzyl (meth)acrylate / (meth)acrylic acid copolymer, a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / styrene / (meth)acrylic acid copolymer, and a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer [K2];

[0209] Resins such as a resin obtained by reacting (meth)acrylic acid with a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate, and a resin obtained by reacting (meth)acrylic acid with a copolymer of tricyclodecyl (meth)acrylate / styrene / glycidyl (meth)acrylate [K3];

[0210] Resins [K4] and the like obtained by further reacting tetrahydrophthalic anhydride with a resin obtained by reacting (meth)acrylic acid with a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate.

[0211] The resin (C) preferably contains the resin [K1].

[0212] As a further example of resin (C), the resin described in Japanese Patent Publication No. 2018-123274 can be cited. As the resin, a polymer having a double bond in the side chain and a structural unit (α) represented by the following formula (I) and a structural unit (β) represented by the following formula (II) on the main chain, and further comprising an acid group (hereinafter also referred to as "resin (Ca)").

[0213] The acid group can be introduced into the resin by, for example, the resin (Ca) containing a structural unit (γ) derived from a monomer containing an acid group (eg, (meth)acrylic acid, etc.) The resin (Ca) preferably contains structural units (α), (β), and (γ) in the main chain skeleton.

[0214]

[0215] [Where R A and R Bare the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms. n represents the average number of repeating units of the constituent unit represented by formula (I), and is a number greater than 1.]

[0216]

[0217] [Where R C The same or different, represents a hydrogen atom or a methyl group. D are the same or different and represent a linear or branched hydrocarbon group having 4 to 20 carbon atoms. m represents the average number of repeating units of the constituent unit represented by formula (II), and is a number greater than 1.]

[0218] From the viewpoint of heat resistance and storage stability of the resin (Ca), the content ratio of the constituent unit (α) in the resin (Ca) is, for example, 0.5% to 50% by mass, preferably 1% to 40% by mass, and more preferably 5% to 30% by mass, relative to the total amount of all monomer units providing the main chain skeleton of the resin (Ca) (100% by mass). n in formula (I) represents the average number of repeating units of the constituent unit (α) in the resin (Ca), and n can be set so that the content ratio of the constituent unit (α) is within the above range.

[0219] From the viewpoint of solvent resistance of the wavelength conversion layer, the content ratio of the constituent unit (β) is, for example, 10% to 90% by mass, preferably 20% to 80% by mass, and more preferably 30% to 75% by mass, relative to the total amount 100% by mass of all monomer units providing the main chain skeleton of the resin (Ca). m in formula (II) represents the average number of repeating units of the constituent unit (β) in the resin (Ca), and m can be set so that the content ratio of the constituent unit (β) is within the above range.

[0220] From the viewpoint of the solubility of the resin (Ca) in the solvent (J), the content ratio of the constituent unit (γ) is, for example, 0.5% by mass to 50% by mass, preferably 2% by mass to 50% by mass, and more preferably 5% by mass to 45% by mass, relative to 100% by mass of the total amount of all monomer units providing the main chain skeleton of the resin (Ca).

[0221] The resin (C) may include one or more selected from the above-mentioned resin [K1], resin [K2], resin [K3], resin [K4] and resin (Ca).

[0222] The weight average molecular weight Mw of the resin (C) measured by GPC in terms of standard polystyrene is, for example, 1000 to 20000, preferably 2000 to 15000, and more preferably 3000 to 13000 from the viewpoint of the developability of the composition I and the luminous intensity of the wavelength conversion layer. The Mw of the resin (C) can be adjusted by appropriately combining the selection of the raw materials used, the charging method, the reaction temperature and time, and other reaction conditions. The Mw of the resin (C) can be measured according to the measurement method described in the Example column described later. Alternatively, the Mw of the resin (C) contained in the composition I can be measured by GPC.

[0223] The molecular weight distribution [weight average molecular weight (Mw) / number average molecular weight (Mn)] of the resin (C) measured by GPC is, for example, 1.0 to 6.0, and preferably 1.2 to 4.0 from the viewpoint of improving the light emission intensity of the wavelength conversion layer.

[0224] From the viewpoint of the developability of composition I and the solvent resistance of the wavelength conversion layer, the acid value of resin (C) is preferably 90 mgKOH / g to 150 mgKOH / g, more preferably 95 mgKOH / g to 140 mgKOH / g, and further preferably 100 mgKOH / g to 130 mgKOH / g. The acid value of resin (C) can be adjusted by the content of the monomer component having an acid group (e.g., the above (a)).

[0225] The acid value of the resin (C) is a value measured as the amount (mg) of potassium hydroxide required to neutralize 1 g of the resin (C), and can be determined, for example, by titration using an aqueous potassium hydroxide solution. Specifically, it can be measured according to the measurement method described in the Example column described later. Alternatively, the acid value of the resin (C) contained in the composition I can be determined, for example, by performing a structural analysis thereof.

[0226] From the viewpoint of increasing the luminous intensity of the wavelength conversion layer, the resin (C) preferably contains a resin having a double bond equivalent of 300 g / eq to 2000 g / eq, and more preferably contains a resin having a double bond equivalent of 500 g / eq to 1500 g / eq. As a resin having a double bond equivalent of 300 g / eq to 2000 g / eq, a (meth) acrylic resin can be cited. The resin (C) is preferably composed of a (meth) acrylic resin.

[0227] The content of the resin (C) in the composition I is, for example, 5% to 80% by mass, preferably 10% to 70% by mass, more preferably 13% to 60% by mass, and further preferably 17% to 55% by mass, relative to the total amount of the solid content of the composition I. When the content of the resin (C) is within the above range, the semiconductor particles (A) tend to be easily dispersed, and the luminous intensity of the wavelength conversion layer tends to be improved.

[0228] In composition I, the mass ratio (solid content ratio) of the resin (C) to the polymerizable compound (D) described later is, for example, 1 or more, preferably 1.5 or more, and more preferably 2 or more from the viewpoint of the developability of composition I and the luminous intensity of the wavelength conversion layer.

[0229] (1-5) Polymerizable compound (D)

[0230] Composition I may further contain a polymerizable compound (D). The polymerizable compound (D) is a compound obtained by polymerization of active free radicals, acids, etc. generated by the polymerization initiator (E) described later. Examples of the polymerizable compound (D) include photopolymerizable compounds such as compounds having ethylenically unsaturated bonds, such as (meth)acrylate compounds. Another example of a polymerizable compound (D) is a thermally polymerizable compound. Composition I may also contain two or more polymerizable compounds (D).

[0231] The polymerizable compound (D) is preferably a photopolymerizable compound having three or more ethylenically unsaturated bonds in the molecule. The weight average molecular weight of the polymerizable compound (D) is preferably 150 to 2,900, more preferably 250 to 1,500.

[0232] Examples of photopolymerizable compounds having three or more ethylenically unsaturated bonds in the molecule include a compound (Da) having three or more ethylenically unsaturated bonds in the molecule and having an acidic functional group, and a compound (Db) having three or more ethylenically unsaturated bonds in the molecule but not having an acidic functional group. The polymerizable compound (D) preferably includes at least one of the compound (Da) and the compound (Db), and may also include two or more compounds (Da), two or more compounds (Db), or at least one of the compounds (Da) and at least one of the compounds (Db).

[0233] Examples of the acidic functional group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, etc. Among them, the acidic functional group is preferably a carboxyl group.

[0234] By including the compound (Da) in the polymerizable compound (D), the dispersibility of the semiconductor particles (A) in the composition I can be improved, and the luminous intensity of the wavelength conversion layer can be improved. In addition, by including the compound (Da) in the polymerizable compound (D), the curability and heat resistance of the composition I can be improved.

[0235] The ethylenically unsaturated bond possessed by the compound (Da) is preferably a (meth)acryloyloxy group. The number of ethylenically unsaturated bonds possessed by one molecule of the compound (Da) is preferably 3 to 5, more preferably 3. The number of acidic functional groups possessed by one molecule of the compound (Da) is 1 or more. When there are 2 or more acidic functional groups, each acidic functional group may be different or the same, but preferably has at least one carboxyl group.

[0236] Examples of the compound (Da) include compounds obtained by polyacid-modifying a compound having three or more (meth)acryloyloxy groups and hydroxyl groups, such as pentaerythritol tri(meth)acrylate or dipentaerythritol penta(meth)acrylate. Examples of the compound include compounds obtained by monoesterifying pentaerythritol (meth)acrylate triester with a dibasic acid (e.g., succinic acid, maleic acid) or an anhydride thereof, and compounds obtained by monoesterifying dipentaerythritol penta(meth)acrylate with a dibasic acid (e.g., succinic acid, maleic acid) or an anhydride thereof.

[0237] The ethylenically unsaturated bond contained in the compound (Db) is preferably a (meth)acryloyloxy group. The number of ethylenically unsaturated bonds contained in one molecule of the compound (Db) is preferably 3 to 6.

[0238] Examples of the compound (Db) include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tris(2-(meth)acryloyloxyethyl)isocyanurate, ethylene glycol-modified pentaerythritol tetra(meth)acrylate, ethylene glycol-modified dipentaerythritol hexa(meth)acrylate, propylene glycol-modified pentaerythritol tetra(meth)acrylate, propylene glycol-modified dipentaerythritol hexa(meth)acrylate, caprolactone-modified pentaerythritol tetra(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among them, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and the like are preferred.

[0239] The content of the polymerizable compound (D) in the composition I is preferably 7% to 60% by mass, more preferably 10% to 45% by mass, and further preferably 13% to 30% by mass, relative to the total amount of solid components of the composition I. When the content of the polymerizable compound (D) is within the above range, the developability of the composition I and the solvent resistance of the wavelength conversion layer tend to be improved.

[0240] The polymerizable compound (D) preferably contains 50% by mass or more of the compound (Db) from the viewpoint of improving the developability of the composition I. The polymerizable compound (D) preferably contains the compound (Da) and the compound (Db) from the viewpoint of improving the solvent resistance of the wavelength conversion layer.

[0241] (1-6) Polymerization initiator (E)

[0242] Composition I may further contain a polymerization initiator (E). The polymerization initiator (E) is a compound that can generate active free radicals, acids, etc. by the action of light or heat to initiate polymerization of the polymerizable compound (D). Composition I may contain one or more polymerization initiators (E).

[0243] Examples of the polymerization initiator (E) include photopolymerization initiators such as oxime compounds, biimidazole compounds, triazine compounds, and acylphosphine compounds; and thermal polymerization initiators such as azo compounds and organic peroxides.

[0244] An example of the oxime compound is an oxime compound having a first molecular structure represented by the following formula (1). Hereinafter, this oxime compound is also referred to as "oxime compound (1)".

[0245]

[0246] From the viewpoint of increasing the luminous intensity of the wavelength conversion layer, it is advantageous to include an oxime compound (1) as a polymerization initiator (E). It is speculated that one factor that can exert such an effect is that due to the unique molecular structure of the oxime compound (1), the absorption wavelength of the oxime compound (1) changes significantly before and after the cleavage (decomposition) of the oxime compound (1) required when the oxime compound (1) initiates photopolymerization, and therefore the oxime compound (1) has a high ability to initiate photoradical polymerization.

[0247] In formula (1), R 1 Represents R 11 , OR 11 , COR 11 , SR 11 ,CONR 12 R 13 or CN.

[0248] R 11 , R 12 and R 13 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0249] R 11 , R 12 or R 13The hydrogen atoms of the group represented by OR 21 , COR 21 , SR 21 NR 22 Ra 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 , CN, halogen atom or COOR 21 replace.

[0250] R 21 , R 22 and R 23 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0251] R 21 , R 22 or R 23 The hydrogen atom of the group represented may be substituted with CN, a halogen atom, a hydroxyl group or a carboxyl group.

[0252] When R 11 , R 12 , R 13 , R 21 , R 22 or R 23 When the group represented by has an alkylene portion, the alkylene portion may be replaced by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-、-NR 24 COO-、-OCONR 24 -, -SCO-, -COS-, -OCS- or -CSO- interrupts 1 to 5 times.

[0253] R 24 It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0254] When R 11 , R 12 , R 13 , R 21 , R 22 or R23 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 12 With R 13 and R 22 With R 23 They can form a ring together.

[0255] * represents a bonding site of another molecular structure other than the first molecular structure of the oxime compound (1), that is, the second molecular structure.

[0256] As R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The alkyl group having 1 to 20 carbon atoms represented by alkyl group includes, for example, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, tert-pentyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, tert-octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclopentyl, cyclohexyl, cyclohexylmethyl, cyclohexylethyl and the like.

[0257] As R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 Examples of the aryl group having 6 to 30 carbon atoms represented by phenyl include phenyl, tolyl, xylyl, ethylphenyl, naphthyl, anthracenyl, phenanthryl, phenyl substituted with one or more of the above alkyl groups, biphenyl, naphthyl, anthracenyl, and the like.

[0258] As R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the aralkyl group having 7 to 30 carbon atoms include benzyl, α-methylbenzyl, α,α-dimethylbenzyl, and phenylethyl.

[0259] As R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R24 The heterocyclic group having 2 to 20 carbon atoms represented by , for example, pyridyl, pyrimidinyl, furanyl, thienyl, tetrahydrofuranyl, dioxolanyl, benzoxazol-2-yl, tetrahydropyranyl, pyrrolidinyl, imidazolidinyl, pyrazolidinyl, thiazolidinyl, isothiazolidinyl, oxazolidinyl, isoxazolidinyl, piperidinyl, piperazinyl, morpholinyl and the like, preferably a 5- to 7-membered heterocyclic ring.

[0260] R in formula (1) 12 With R 13 and R 22 With R 23 can form a ring together, R 12 With R 13 and R 22 With R 23 These respectively mean that they can form a ring together with the nitrogen atom, carbon atom or oxygen atom to which they are connected.

[0261] As Ra in formula (1) 12 With Ra 13 and Ra 22 With Ra 23 Examples of the ring that can be formed together include a cyclopentane ring, a cyclohexane ring, a cyclopentene ring, a benzene ring, a piperidine ring, a morpholine ring, a lactone ring, a lactam ring and the like, and a 5- to 7-membered ring is preferred.

[0262] As R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 and R 23 Examples of the halogen atom which may be present as a substituent include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0263] R in formula (1) 1 Preferably R 11 , more preferably an alkyl group having 1 to 20 carbon atoms, further preferably an alkyl group having 1 to 10 carbon atoms, and further preferably an alkyl group having 1 to 6 carbon atoms.

[0264] An example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (2): The second molecular structure refers to another molecular structure portion of the oxime compound (1) other than the first molecular structure.

[0265] In formula (2), the bonding site represented by "*" is directly bonded to the bonding site represented by "*" in formula (1). That is, when the second molecular structure is the structure represented by formula (2), the benzene ring having "-*" in formula (2) is directly bonded to the carbonyl group having "-*" in formula (1).

[0266]

[0267] In formula (2), R 2 and R 3 Each independently represents R 11 , OR 11 , SR 11 , COR 11 ,CONR 12 R 13 NR 12 COR 11 ,OCOR 11 、COOR 11 SCOR 11 , OCSR 11 、COSR 11 ,CSOR 11 , CN or halogen atom.

[0268] When there are multiple R 2 These may be the same or different.

[0269] When there are multiple R 3 These may be the same or different.

[0270] R 11 , R 12 and R 13 Means the same as above.

[0271] s and t each independently represent an integer of 0-4.

[0272] L represents a sulfur atom, CR 31 R 32 , CO or NR 33 .

[0273] R 31 , R 32 and R 33 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms.

[0274] When R 31 , R 32 or R 33 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 31 , R 32 and R 33 Each independently may form a ring together with an adjacent benzene ring.

[0275] R 4It is a hydroxyl group, a carboxyl group or a group represented by the following formula (2-1).

[0276] (R 4a ) v —L 2 —L 1 — (2-1)

[0277] (In formula (2-1), L 1 Indicates -O-, -S-, -NR 22 -, -NR 22 CO-, -So2-, -CS-, -OCO- or -COO-.

[0278] R 22 Means the same as above.

[0279] L 2 It represents a group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, a group obtained by removing v hydrogen atoms from an aryl group having 6 to 30 carbon atoms, a group obtained by removing v hydrogen atoms from an aralkyl group having 7 to 30 carbon atoms, or a group obtained by removing v hydrogen atoms from a heterocyclic group having 2 to 20 carbon atoms.

[0280] When L 2 When the group represented by has an alkylene moiety, the alkylene moiety may be represented by -O-, -S-, -COO-, -OCO-, -NR 22 -, -NR 22 COO-、-OCONR 22 The alkylene moiety may be branched or cyclic.

[0281] R 4a Represents OR 41 , SR 41 ,CONR 42 R 43 NR 42 COR 43 ,OCOR 41 、COOR 41 SCOR 41 , OCSR 41 、COSR 41 ,CSOR 41 , CN or halogen atom.

[0282] When there are multiple R 4a , they may be the same or different.

[0283] R 41 , R 42 and R43 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. 41 , R 42 and R 43 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 42 With R 43 Can form a ring together.

[0284] v represents an integer from 1 to 3. )

[0285] * represents the bonding site of the oxime compound (1) to the first molecular structure.

[0286] R in formula (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 , R 31 , R 32 and R 33 , and R in the above formula (2-1) 22 , R 41 , R 42 and R 43 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, and the aralkyl group having 7 to 30 carbon atoms represented by 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Same as the example.

[0287] R in formula (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 , and R in the above formula (2-1) 22 Examples of heterocyclic groups having 2 to 20 carbon atoms represented by are the same as those of R in formula (1). 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Same as the example.

[0288] R in formula (2) 31 , R 32 and R 33 Each of the following can independently form a ring with an adjacent benzene ring: 31 , R 32 and R 33 Each independently forms a ring together with an adjacent benzene ring and the nitrogen atom to which it is connected.

[0289] R in formula (2) 31 , R 32 and R 33 Examples of a ring that can be formed together with an adjacent benzene ring include: 12 With Ra 13 and Ra 22 With Ra 23 The rings that can be formed together are the same.

[0290] In the above formula (2-1), L 2 It represents a group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0291] Examples of the group formed by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms include, for example, when v is 1, an alkylene group such as a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 3-methylbutylene group, a 4-methylbutylene group, a 2,4-dimethylbutylene group, a 1,3-dimethylbutylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, an ethane-1,1-diyl group, and a propane-2,2-diyl group.

[0292] Examples of the group obtained by removing v hydrogen atoms from an aryl group having 6 to 30 carbon atoms include arylene groups such as 1,2-phenylene, 1,3-phenylene, 1,4-phenylene, 2,6-naphthylene, 1,4-naphthylene, 2,5-dimethyl-1,4-phenylene, diphenylmethane-4,4'-diyl, 2,2-diphenylpropane-4,4'-diyl, diphenylsulfide-4,4'-diyl and diphenylsulfone-4,4'-diyl when v is 1.

[0293] Examples of the group obtained by removing v hydrogen atoms from an aralkyl group having 7 to 30 carbon atoms include, for example, a group represented by the following formula (a) and a group represented by the following formula (b) when v is 1.

[0294]

[0295] [In formulas (a) and (b), L 3 and L 5 represents an alkylene group having 1 to 10 carbon atoms, L 4 and L 6 represents a single bond or an alkylene group having 1 to 10 carbon atoms.]

[0296] Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, propylene, methylethylene, butylene, 1-methylpropylene, 2-methylpropylene, 1,2-dimethylpropylene, 1,3-dimethylpropylene, 1-methylbutylene, 2-methylbutylene, 3-methylbutylene, 4-methylbutylene, 2,4-dimethylbutylene, 1,3-dimethylbutylene, pentylene, hexylene, heptylene, octylene, nonylene, and decylene.

[0297] Examples of the group obtained by removing v hydrogen atoms from a heterocyclic group having 2 to 20 carbon atoms include, for example, when v is 1, divalent heterocyclic groups such as 2,5-pyridinediyl, 2,6-pyridinediyl, 2,5-pyrimidinediyl, 2,5-thiophenediyl, 3,4-tetrahydrofurandiyl, 2,5-tetrahydrofurandiyl, 2,5-furandiyl, 3,4-thiazoldiyl, 2,5-benzofurandiyl, 2,5-benzothiophenediyl, N-methylindole-2,5-diyl, 2,5-benzothiazoldiyl, and 2,5-benzooxazolediyl.

[0298] As R in formula (2) 2 and R 3 , and R in the above formula (2-1) 4a Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0299] From the viewpoint of solubility in the solvent (J) and / or developability of the composition I, a preferred example of the structure represented by the formula (2) is a structure represented by the following formula (2a).

[0300]

[0301] [In formula (2a), L' represents a sulfur atom or NR 50 , R 50 represents a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, R 2 , R 3 , R 4 , s and t have the same meanings as above.]

[0302] From the same viewpoint as above, another preferred example of the structure represented by formula (2) is a structure represented by the following formula (2b).

[0303]

[0304] [In formula (2b), R 44 It is a hydroxyl group, a carboxyl group or a group represented by the following formula (2-2).

[0305] R 44a —L 12 —L 11 — (2-2) (In formula (2-2), L 11 Indicates -O- or *-OCO-, * indicates L 12 The bonding site, L 12 represents an alkylene group having 1 to 20 carbon atoms, which may be interrupted by 1 to 3 -O- groups, R 44a Represents OR 55 or COOR 55 , R 55 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. )]

[0306] R 44 The group represented by the formula (2-2) is preferred. In this case, it is advantageous in terms of the solubility of the oxime compound (1) in the solvent (J) and the developability of the composition I.

[0307] L 12 The alkylene group represented by is preferably 1-10, more preferably 1-4.

[0308] R 44a It is preferably a hydroxyl group or a carboxyl group, and more preferably a hydroxyl group.

[0309] The method for producing the oxime compound (1) having the second molecular structure represented by formula (2) is not particularly limited, and it can be produced, for example, according to the method described in JP-A-2011-132215.

[0310] Another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (3).

[0311] The bonding site represented by "*" in formula (3) is directly bonded to the bonding site represented by "*" in formula (1). That is, when the second molecular structure is the structure represented by formula (3), the benzene ring having "-*" in formula (3) is directly bonded to the carbonyl group having "-*" in formula (1).

[0312]

[0313] In formula (3), R 5It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0314] When R 5 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic.

[0315] R 5 The hydrogen atoms of the group represented by R 21 , OR 21 , COR 21 , SR 21 NR 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 NR 22 COR 21 ,OCOR 21 、COOR 21 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 SCOR 21 , OCSR 21 、COSR 21 ,CSOR 21 , hydroxyl, nitro, CN, halogen atoms, or COOR 21 replace.

[0316] R 21 , R 22 and R 23 Means the same as above.

[0317] R 21 , R 22 or R 23 The hydrogen atom of the group represented may be substituted with CN, a halogen atom, a hydroxyl group or a carboxyl group.

[0318] When R 21 , R 22 and R 23 When the group represented by has an alkylene moiety, the alkylene moiety may be replaced by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-、-NR 24 COO-、-OCONR 24-, -SCO-, -COS-, -OCS- or -CSO- interrupts 1 to 5 times.

[0319] R 24 Means the same as above.

[0320] When R 21 , R 22 and R 23 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 22 With R 23 They can also form a ring together.

[0321] R 6 , R 7 , R 8 and R 9 Each independently represents R 61 , OR 61 , SR 61 , COR 62 ,CONR 63 R 64 NR 65 COR 61 ,OCOR 61 、COOR 62 SCOR 61 , OCSR 61 、COSR 62 ,CSOR 61 , hydroxyl, nitro, CN or halogen atom.

[0322] R 61 , R 62 , R 63 , R 64 and R 65 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0323] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , COR 21 , SR 21 NR 22 Ra 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR22 )-OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 , CN, halogen atoms, or COOR 21 replace.

[0324] R 6 With R 7 , R 7 With R 8 and R 8 With R 9 They can form a ring together.

[0325] * represents the bonding site of the oxime compound (1) to the first molecular structure.

[0326] R in formula (3) 5 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 30 carbon atoms, aralkyl groups having 7 to 30 carbon atoms, and heterocyclic groups having 2 to 20 carbon atoms are shown in the formula (1). 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Same as the example.

[0327] R in formula (3) 22 With R 23 Can form a ring together means that R 22 With R 23 It means that it can form a ring together with the nitrogen atom, carbon atom or oxygen atom to which it is connected.

[0328] R in formula (3) 22 With R 23 Examples of the rings that can be formed together are: 12 With Ra 13 and Ra 22 With Ra 23 The examples of rings that can be formed together are the same.

[0329] As R in formula (3)6 , R 7 , R 8 and R 9 The halogen atom represented by R 5 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the halogen atom replacing the hydrogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0330] From the viewpoint of solubility in the solvent (J) and / or developability of the composition I, in a preferred embodiment, R 5 It is a group represented by the following formula (3-1).

[0331]

[0332] [In the formula (3-1), Z represents a group obtained by removing one hydrogen atom from an alkyl group having 1 to 20 carbon atoms, a group obtained by removing one hydrogen atom from an aryl group having 6 to 30 carbon atoms, a group obtained by removing one hydrogen atom from an aralkyl group having 7 to 30 carbon atoms, or a group obtained by removing one hydrogen atom from a heterocyclic group having 2 to 20 carbon atoms,

[0333] When the group represented by Z has an alkylene moiety, the alkylene moiety may be -O-, -S-, -COO-, -OCO-, -NR- 24 -, -NR 24 COO-、-OCONR 24 -, -SCO-, -COS-, -OCS- or -CSO- are interrupted 1 to 5 times, and the alkylene part may be branched or cyclic.

[0334] R 21 , R 22 and R 24 Means the same as above.]

[0335] From the same viewpoint as described above, Z in formula (3-1) is preferably a methylene group, an ethylene group or a phenylene group.

[0336] From the same point of view as above, R in formula (3-1) 21 and R 22 It is preferably an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 30 carbon atoms, and more preferably a methyl group, an ethyl group or a phenyl group.

[0337] From the same viewpoint as above, in another preferred embodiment, R7 For nitro.

[0338] The method for producing the oxime compound (1) having the second molecular structure represented by the formula (3) is not particularly limited, and it can be produced, for example, by the method described in JP-A-2000-80068 and JP-A-2011-178776.

[0339] Still another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (4).

[0340] The bonding site represented by "*" in formula (4) is directly bonded to the bonding site represented by "*" in formula (1). That is, when the second molecular structure is the structure represented by formula (4), the benzene ring having "-*" in formula (4) is directly bonded to the carbonyl group having "-*" in formula (1).

[0341]

[0342] In formula (4), R 71 It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0343] When R 71 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic.

[0344] R 71 The hydrogen atoms of the group represented by R 21 , OR 21 , COR 21 , SR 21 NR 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 NR 22 COR 21 ,OCOR 21 、COOR 21 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 SCOR 21 , OCSR 21 、COSR 21 ,CSOR21 , hydroxyl, nitro, CN, halogen atoms, or COOR 21 replace.

[0345] R 21 , R 22 and R 23 Means the same as above.

[0346] R 21 , R 22 or R 23 The hydrogen atom of the group represented may be substituted with CN, a halogen atom, a hydroxyl group or a carboxyl group.

[0347] When R 21 , R 22 and R 23 When the group represented by has an alkylene moiety, the alkylene moiety may be replaced by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-、-NR 24 COO-、-OCONR 24 -, -SCO-, -COS-, -OCS- or -CSO- interrupts 1 to 5 times.

[0348] R 24 Means the same as above.

[0349] When R 21 , R 22 and R 23 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 22 With R 23 They can also form a ring together.

[0350] R 72 , R 73 and 3 Rs 74 Each independently represents R 61 , OR 61 , SR 61 , COR 62 ,CONR 63 R 64 NR 65 COR 61 ,OCOR 61 、COOR 62 SCOR 61 , OCSR 61 、COSR 62 ,CSOR 61 , hydroxyl, nitro, CN or halogen atom.

[0351] R61 , R 62 , R 63 , R 64 and R 65 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0352] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented can be OR 21 , COR 21 , SR 21 NR 22 Ra 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 , CN, halogen atoms, or COOR 21 replace.

[0353] R 72 With R 73 and 2 R 74 They can form a ring together.

[0354] * represents the bonding site of the oxime compound (1) to the first molecular structure.

[0355] R in formula (4) 71 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 30 carbon atoms, aralkyl groups having 7 to 30 carbon atoms, and heterocyclic groups having 2 to 20 carbon atoms are shown in the formula (1). 11 , R 12 , R 13 , R 21 , R 22 , R23 and R 24 Same as the example.

[0356] R in formula (4) 22 With R 23 Can form a ring together means: R 22 With R 23 It means that it can form a ring together with the nitrogen atom, carbon atom or oxygen atom to which it is connected.

[0357] R in formula (4) 22 With R 23 Examples of the rings that can be formed together are: 12 With Ra 13 and Ra 22 With Ra 23 The examples of rings that can be formed together are the same.

[0358] As R in formula (4) 72 , R 73 and R 74 The halogen atom represented by R 71 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the halogen atom replacing the hydrogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0359] The method for producing the oxime compound (1) having the second molecular structure represented by formula (4) is not particularly limited, and it can be produced, for example, according to the methods described in International Publication Nos. 2017 / 051680 and 2020 / 004601.

[0360] Still another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (5).

[0361] The bonding site represented by "*" in formula (5) is directly bonded to the bonding site represented by "*" in formula (1). That is, when the second molecular structure is the structure represented by formula (5), the pyrrole ring having "-*" in formula (5) is directly bonded to the carbonyl group having "-*" in formula (1).

[0362]

[0363] In formula (5), R 81It represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0364] When R 81 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic.

[0365] R 81 The hydrogen atoms of the group represented by R 21 , OR 21 , COR 21 , SR 21 NR 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 NR 22 COR 21 ,OCOR 21 、COOR 21 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 SCOR 21 , OCSR 21 、COSR 21 ,CSOR 21 , hydroxyl, nitro, CN, halogen atoms, or COOR 21 replace.

[0366] R 21 , R 22 and R 23 Means the same as above.

[0367] By R 21 , R 22 or R 23 The hydrogen atom of the group represented may be substituted with CN, a halogen atom, a hydroxyl group or a carboxyl group.

[0368] When R 21 , R 22 and R 23 When the group represented by has an alkylene moiety, the alkylene moiety may be replaced by -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-、-NR 24 COO-、-OCONR24 -, -SCO-, -COS-, -OCS- or -CSO- interrupts 1 to 5 times.

[0369] R 24 Means the same as above.

[0370] When R 21 , R 22 and R 23 When the group represented by has an alkyl portion, the alkyl portion may be branched or cyclic. 22 With R 23 They can also form a ring together.

[0371] R 82 , R 83 , R 84 , R 85 and R 86 Each independently represents R 61 , OR 61 , SR 61 , COR 62 ,CONR 63 R 64 NR 65 COR 61 ,OCOR 61 、COOR 62 SCOR 61 , OCSR 61 、COSR 62 ,CSOR 61 , hydroxyl, nitro, CN or halogen atom.

[0372] R 61 , R 62 , R 63 , R 64 and R 65 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0373] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , COR 21 , SR 21 NR 22 Ra 23 ,CONR 22 R 23 , -NR 22 -OR23 , -N(COR 22 )-OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 , CN, halogen atoms, or COOR 21 replace.

[0374] R 83 With R 84 , R 84 With R 85 and R 85 With R 86 They can form a ring together.

[0375] * represents the bonding site of the oxime compound (1) to the first molecular structure.

[0376] R in formula (5) 81 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 30 carbon atoms, aralkyl groups having 7 to 30 carbon atoms, and heterocyclic groups having 2 to 20 carbon atoms are shown in the formula (1). 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Same as the example.

[0377] R in formula (5) 22 With R 23 Can form a ring together means: R 22 With R 23 It means that it can form a ring together with the nitrogen atom, carbon atom or oxygen atom to which it is connected.

[0378] R in formula (5) 22 With R 23 Examples of the rings that can be formed together are: 12 With Ra 13 and Ra 22 With Ra 23 The examples of rings that can be formed together are the same.

[0379] As R in formula (5) 82 , R 83 , R 84 , R 85 and R 86 The halogen atom represented by R 81 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the halogen atom replacing the hydrogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0380] The method for producing the oxime compound (1) having the second molecular structure represented by formula (5) is not particularly limited, and it can be produced, for example, according to the methods described in International Publication Nos. 2017 / 051680 and 2020 / 004601.

[0381] Still another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (6).

[0382] The bonding site represented by "*" in formula (6) is directly bonded to the bonding site represented by "*" in formula (1). That is, when the second molecular structure is the structure represented by formula (6), the benzene ring having "-*" in formula (6) is directly bonded to the carbonyl group having "-*" in formula (1).

[0383]

[0384] In formula (6), the four R 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 Each independently represents R 61 , OR 61 , SR 61 , COR 62 ,CONR 63 R 64 NR 65 COR 61 ,OCOR 61 、COOR 62 SCOR 61 , OCSR 61 、COSR 62 ,CSOR 61, hydroxyl, nitro, CN or halogen atom.

[0385] R 61 , R 62 , R 63 , R 64 and R 65 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0386] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , COR 21 , SR 21 NR 22 Ra 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 , CN, halogen atoms, or COOR 21 replace.

[0387] R 21 , R 22 and R 23 Means the same as above.

[0388] R 92 With R 93 , R 94 With R 95 , R 95 With R 96 , and R 96 With R 97 They can form a ring together.

[0389] * represents the bonding site of the oxime compound (1) to the first molecular structure.

[0390] R in formula (6) 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R64 and R 65 The example of an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms represented by the formula (1) is 11 , R 12 , R 13 , R 21 , R 22 and R 23 Same as the example.

[0391] R in formula (6) 22 With R 23 Can form a ring together means: R 22 With R 23 It means that it can form a ring together with the nitrogen atom, carbon atom or oxygen atom to which it is connected.

[0392] R in formula (6) 22 With R 23 Examples of the rings that can be formed together are: 12 With Ra 13 and Ra 22 With Ra 23 The examples of rings that can be formed together are the same.

[0393] As R in formula (6) 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 The halogen atom represented by R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the halogen atom replacing the hydrogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0394] The method for producing the oxime compound (1) having the second molecular structure represented by formula (6) is not particularly limited, and it can be produced, for example, according to the methods described in International Publication Nos. 2017 / 051680 and 2020 / 004601.

[0395] Other examples of the photopolymerization initiator include photopolymerization initiators other than the oxime compound (1). Examples of the photopolymerization initiator include oxime compounds other than the oxime compound (1), biimidazole compounds, triazine compounds, and acylphosphine compounds.

[0396] Examples of oxime compounds other than the oxime compound (1) include oxime compounds having a partial structure represented by the following formula (d1): * represents a bonding site.

[0397]

[0398] Examples of the oxime compound having a partial structure represented by the formula (d1) include N-benzoyloxy-1-(4-phenylthiophenyl)butane-1-one-2-imine, N-benzoyloxy-1-(4-phenylthiophenyl)octane-1-one-2-imine, N-benzoyloxy-1-(4-phenylthiophenyl)-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethane-1-imine, N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxolane]propane-1-imine, cyclopentylmethyloxy)benzoyl}-9H-carbazole-3-yl]ethane-1-imide, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-3-cyclopentylpropane-1-imide, N-benzoyloxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-3-cyclopentylpropane-1-one-2-imide; compounds described in Japanese Unexamined Patent Publication No. 2011-132215, International Publication No. 2008 / 78678, International Publication No. 2008 / 78686, and International Publication No. 2012 / 132558, etc. Commercially available products such as Irgacure OXE01, OXE02 (above, manufactured by BASF), and N-1919 (manufactured by ADEKA) can also be used.

[0399] Among them, the oxime compound having a partial structure represented by formula (d1) is preferably at least one selected from N-benzoyloxy-1-(4-phenylthiophenyl)butane-1-one-2-imine, N-benzoyloxy-1-(4-phenylthiophenyl)octane-1-one-2-imine, and N-benzoyloxy-1-(4-phenylthiophenyl)-3-cyclopentylpropane-1-one-2-imine, and more preferably N-benzoyloxy-1-(4-phenylthiophenyl)octane-1-one-2-imine.

[0400] Examples of the biimidazole compound include compounds represented by formula (d5).

[0401]

[0402] [In formula (d5), R E ~R Jrepresents an aryl group having 6 to 10 carbon atoms which may have a substituent.]

[0403] Examples of the aryl group having 6 to 10 carbon atoms include phenyl, tolyl, xylyl, ethylphenyl and naphthyl, and a phenyl group is preferred.

[0404] Examples of the substituent include a halogen atom and an alkoxy group having 1 to 4 carbon atoms. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, preferably a chlorine atom. Examples of the alkoxy group having 1 to 4 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group, preferably a methoxy group.

[0405] Examples of the biimidazole compound include 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole (see, for example, Japanese Patent Application Laid-Open No. 06-75372 and Japanese Patent Application Laid-Open No. 06-75373), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, (Alkoxyphenyl) biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetrakis(dialkoxyphenyl) biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetrakis(trialkoxyphenyl) biimidazole (see, for example, Japanese Patent Publication No. 48-38403, Japanese Patent Application Laid-Open No. 62-174204, etc.), imidazole compounds in which the phenyl groups at the 4,4',5,5'-positions are substituted with alkoxycarbonyl groups (see, for example, Japanese Patent Application Laid-Open No. 7-10913, etc.). Among them, compounds represented by the following formula or mixtures thereof are preferred.

[0406]

[0407] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[ 2-(5-methylfuran-2-yl)vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)vinyl]-1,3,5-triazine, etc. Among them, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine is preferred.

[0408] Examples of the acylphosphine compound include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and (2,4,6-trimethylbenzoyl)diphenylphosphine oxide.

[0409] Other examples of photopolymerization initiators other than the oxime compound (1) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether and benzoin isobutyl ether; benzophenone compounds such as benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetrakis(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone and 4,4'-bis(diethylamino)benzophenone; quinone compounds such as 9,10-phenanthrenequinone, 2-ethylanthraquinone and camphorquinone; 10-butyl-2-chloroacridone, benzyl, methyl phenylglyoxylate and titanocene compounds.

[0410] The content of the polymerization initiator (E) in the composition I is preferably 0.1 to 300 parts by mass, and more preferably 0.1 to 200 parts by mass, relative to 100 parts by mass of the polymerizable compound (D). In addition, the content of the polymerization initiator (E) in the composition I is preferably 0.1 to 30 parts by mass, and more preferably 0.5 to 20 parts by mass, relative to 100 parts by mass of the total amount of the resin (C) and the polymerizable compound (D). If the content of the polymerization initiator (E) is within the above range, there is a tendency for the sensitivity of the composition I to be increased and the exposure time to be shortened, and therefore the productivity of the wavelength conversion layer tends to be improved.

[0411] From the viewpoint of improving the luminescent intensity of the wavelength conversion layer, the content of the oxime compound (1) in the polymerization initiator (E) is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, further preferably 80% by mass to 100% by mass, further preferably 90% by mass to 100% by mass, particularly preferably 95% by mass to 100% by mass, and most preferably 100% by mass, relative to the total amount of the polymerization initiator (E).

[0412] (1-7) Polymerization initiator aid (E1)

[0413] Composition I may further include a polymerization initiator aid (E1) together with the polymerization initiator (E). The polymerization initiator aid (E1) is a compound or sensitizer used to promote the polymerization of the polymerizable compound (D) initiated by the polymerization initiator (E). Examples of the polymerization initiator aid (E1) include photopolymerization initiators such as amine compounds, alkoxyanthracene compounds, thioxanthone compounds, and carboxylic acid compounds, and thermal polymerization initiators. Composition I may include two or more polymerization initiators (E1).

[0414] Examples of the amine compound include triethanolamine, methyldiethanolamine, triisopropanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isopentyl 4-dimethylaminobenzoate, 2-dimethylaminoethyl benzoate, 2-ethylhexyl 4-dimethylaminobenzoate, N,N-dimethyl-p-toluidine, 4,4'-bis(dimethylamino)benzophenone (commonly known as Michler's ketone), 4,4'-bis(diethylamino)benzophenone, and 4,4'-bis(ethylmethylamino)benzophenone.

[0415] Examples of the alkoxyanthracene compound include 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 2-ethyl-9,10-diethoxyanthracene, 9,10-dibutoxyanthracene, and 2-ethyl-9,10-dibutoxyanthracene.

[0416] Examples of the thioxanthone compound include 2-isopropylthioxanthone (IPTX), 4-isopropylthioxanthone (IPTX), 2,4-diethylthioxanthone (DETX), 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone.

[0417] Examples of the carboxylic acid compound include phenylthioacetic acid, methylphenylthioacetic acid, ethylphenylthioacetic acid, methylethylphenylthioacetic acid, dimethylphenylthioacetic acid, methoxyphenylthioacetic acid, dimethoxyphenylthioacetic acid, chlorophenylthioacetic acid, dichlorophenylthioacetic acid, N-phenylglycine, phenoxyacetic acid, naphthylthioacetic acid, N-naphthylglycine, and naphthoxyacetic acid.

[0418] When the composition I contains a polymerization initiator aid (E1), the content of the polymerization initiator aid (E1) in the composition I is preferably 0.1 to 300 parts by mass, and more preferably 0.1 to 200 parts by mass, relative to 100 parts by mass of the polymerizable compound (D). In addition, the content of the polymerization initiator aid (E1) in the composition I is preferably 0.1 to 30 parts by mass, and more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the total amount of the resin (C) and the polymerizable compound (D). If the content of the polymerization initiator aid (E1) is within the above range, higher sensitivity of the composition I can be achieved.

[0419] (1-8) Antioxidant (F)

[0420] Composition I may further include an antioxidant (F). The antioxidant (F) is not particularly limited as long as it is an antioxidant commonly used in industry, and phenol-based antioxidants, phosphorus-based antioxidants, phosphorus / phenol composite antioxidants, and sulfur-based antioxidants may be used. Composition I may include two or more antioxidants (F).

[0421] The phosphorus / phenol complex antioxidant is, for example, a compound having one or more phosphorus atoms and a phenol structure in each molecule. Among them, the antioxidant (F) preferably contains a phosphorus / phenol complex antioxidant from the viewpoint of the developability of the composition I and the luminescence intensity of the wavelength conversion layer.

[0422] Examples of the phenolic antioxidant include Irganox (registered trademark) 1010 (Irganox 1010: pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, manufactured by BASF Corporation), Irganox 1076 (Irganox 1076: octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, manufactured by BASF Corporation), and Irganox 1330 (Irganox 1330: 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-triyl)tri-p-cresol, manufactured by BASF Corporation), Irganox 3114 (Irganox 3114: 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Corporation), Irganox 3790 (Irganox 3790: 1,3,5-tris((4-tert-butyl-3-hydroxy-2,6-xylene)methyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Corporation), Irganox 1035 (Irganox Irganox 1035: 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate of thiodiethylene bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), manufactured by BASF Corporation), Irganox 1135 (Irganox 1135: 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester of phenylpropionic acid, manufactured by BASF Corporation), Irganox 1520L (Irganox 1520L: 4,6-bis(octylthiomethyl)-o-cresol, manufactured by BASF Corporation), Irganox 3125 (Irganox 3125, manufactured by BASF Corporation), Irganox 565 (Irganox 565: 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylphenylamino)-1,3,5-triazine, manufactured by BASF Corporation), Adekastab (registered trademark) AO-80 (Adekastab AO-80: 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, manufactured by Adeka Corporation), Sumilizer (registered trademark) BHT, Sumilizer GA-80, Sumilizer rGS (all manufactured by Sumitomo Chemical Corporation), Cyanox (registered trademark) 1790 (Cyanox 1790, manufactured by Cytec Corporation), Vitamin E (manufactured by Eisai Co., Ltd.), etc.

[0423] Examples of the phosphorus-based antioxidant include Irgafos (registered trademark) 168 (Irgafos 168: tris(2,4-di-tert-butylphenyl)phosphite, manufactured by BASF Corporation), Irgafos 12 (Irgafos 12: tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphin-6-yl]oxy]ethyl]amine, manufactured by BASF Corporation), Irgafos 38 (Irgafos 38: bis(2,4-bis(1,1-dimethylethyl)-6-methylphenyl)ethyl phosphite, manufactured by BASF Corporation), Adekastab (registered trademark) 329K, Adekastab PEP36, and Adekastab PEP-8 (all manufactured by ADEKA Corporation), and Sandstab P-EPQ (manufactured by Clariant), Weston (registered trademark) 618, Weston 619G (all manufactured by GE), UltRanox 626 (manufactured by GE), etc.

[0424] Examples of the phosphorus / phenol composite antioxidant include Sumilizer (registered trademark) GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1.3.2]dioxaphosphophepane) (manufactured by Sumitomo Chemical Co., Ltd.).

[0425] Examples of the sulfur-based antioxidant include dialkyl thiodipropionate compounds such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate; and β-alkylmercaptopropionate compounds of polyhydric alcohols such as tetrakis[methylene(3-dodecylthio)propionate]methane.

[0426] The content of the antioxidant (F) in the composition I is, for example, 1 to 50 parts by mass, relative to 100 parts by mass of the resin (C), preferably 5 to 40 parts by mass, and more preferably 7 to 30 parts by mass, from the viewpoint of the luminous intensity and heat resistance of the wavelength conversion layer.

[0427] (1-9) Leveling agent (H)

[0428] Composition I may further include a leveling agent (H). Examples of the leveling agent (H) include silicone surfactants, fluorine surfactants, and silicone surfactants having fluorine atoms. They may also have polymerizable groups on the side chains. From the viewpoint of the developability of composition I and the luminous intensity of the wavelength conversion layer, the leveling agent (H) is preferably a fluorine surfactant. Composition I may include two or more leveling agents (H).

[0429] Examples of the silicone-based surfactant include surfactants having a siloxane bond in the molecule. Specific examples include Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, Toray Silicone SH8400 (trade name: Toray, manufactured by Dow Corning Co., Ltd.), KP321, KP322, KP323, KP324, KP326, KP340, KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF4446, TSF4452, and TSF4460 (manufactured by Momentive Performance Materials Japan LLC).

[0430] Examples of the fluorine-based surfactant include surfactants having a fluorine carbon chain in the molecule. Specific examples include Fluorad (registered trademark) FC430, Fluorad FC431 (manufactured by Sumitomo 3M Co., Ltd.), MEGAFACE (registered trademark) F142D, MEGAFACE F171, MEGAFACE F172, MEGAFACE F173, MEGAFACE F177, MEGAFACE F183, MEGAFACE F554, MEGAFACE F575, MEGAFACE R30, MEGAFACE RS-718-K (manufactured by DIC Corporation), EFTOP (registered trademark) EF301, EFTOP EF303, EFTOP EF351, EFTOP EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Surflon (registered trademark) S381, Surflon S382, Surflon SC101, Surflon SC105 (manufactured by Asahi Glass Co., Ltd.) and E5844 (manufactured by Daikin Fine Chemical Laboratories, Ltd.), etc.

[0431] Examples of the organosilicon-based surfactant having a fluorine atom include surfactants having a siloxane bond and a fluorocarbon chain in the molecule, and more specifically, MEGAFACE (registered trademark) R08, MEGAFACE BL20, MEGAFACE F475, MEGAFACE F477, and MEGAFACE F443 (manufactured by DIC Corporation).

[0432] When the composition I contains a leveling agent (H), the content of the leveling agent (H) in the composition I is, for example, 0.001 mass % to 1.0 mass %, preferably 0.005 mass % to 0.75 mass %, more preferably 0.01 mass % to 0.5 mass %, and further preferably 0.02 mass % to 0.5 mass % relative to the total amount of the composition I. If the content of the leveling agent (H) is within the above range, the flatness of the wavelength conversion layer can be improved.

[0433] (1-10) Solvent (J)

[0434] Composition I may contain one or more solvents (J). The solvent (J) is preferably a solvent that dissolves the resin (C), the polymerizable compound (D) and the polymerization initiator (E). Examples of the solvent (J) include ester solvents (solvents that contain -COO- in the molecule and do not contain -O-), ether solvents (solvents that contain -O- in the molecule and do not contain -COO-), ether ester solvents (solvents that contain -COO- and -O- in the molecule), ketone solvents (solvents that contain -CO- in the molecule and do not contain -COO-), alcohol solvents (solvents that contain OH in the molecule and do not contain -O-, -CO- and COO-), aromatic hydrocarbon solvents, amide solvents, dimethyl sulfoxide, and the like.

[0435] Examples of the ester solvent include methyl lactate, ethyl lactate, n-butyl lactate, methyl 2-hydroxyisobutyrate, ethyl acetate, n-butyl acetate, isobutyl acetate, n-amyl formate, isoamyl acetate, n-butyl propionate, isopropyl butyrate, ethyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, cyclohexanol acetate, and γ-butyrolactone.

[0436] Examples of the ether solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, 3-methoxy-1-butanol, 3-methoxy-3-methylbutanol, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, anisole, phenethyl ether, and methyl anisole.

[0437] Examples of the ether ester solvent include methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0438] Examples of the ketone solvent include 4-hydroxy-4-methyl-2-pentanone, acetone, 2-butanone, 2-heptanone, 3-heptanone, 4-heptanone, 4-methyl-2-pentanone, cyclopentanone, cyclohexanone, and isophorone.

[0439] Examples of the alcohol solvent include methanol, ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, and glycerin.

[0440] Examples of the aromatic hydrocarbon solvent include benzene, toluene, xylene, and mesitylene.

[0441] Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0442] The solvent (J) preferably contains one or more selected from propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone, and aromatic hydrocarbon solvents.

[0443] The solvent (J) may be propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone or toluene, or a mixture of two or more thereof.

[0444] The solvent (J) is a component other than the solid component, and for example, the solvent contained in the dispersion of the semiconductor particles (A) and the solution of the resin (C) is also included in the solvent (J).

[0445] The content of the solvent (J) in the composition I is the ratio of the total mass of all solvents contained in the composition to the total mass of the composition I, and is, for example, 40% to 95% by mass, preferably 55% to 90% by mass, relative to the total mass of the composition I. In other words, the solid content of the composition I is, for example, 5% to 60% by mass, preferably 10% to 45% by mass. When the content of the solvent (J) is within the above range, the flatness of the composition layer during coating becomes better, and there is a tendency to easily form a wavelength conversion layer of an appropriate thickness.

[0446] (1-11) Other ingredients

[0447] The composition I may further contain additives known in the art such as a polymerization inhibitor, a filler, other polymer compounds, an adhesion promoter, a light stabilizer, and a chain transfer agent, as required.

[0448] (1-12) Method for producing composition I

[0449] Composition I can be produced by a method including the step of mixing predetermined components and other components used as needed. The method for producing composition II may further include the step of preparing resin (C).

[0450] (2) Wavelength conversion layer and method for manufacturing the same

[0451] The wavelength conversion layer is formed from composition I. The wavelength conversion layer can be disposed on the substrate, for example, by the following method:

[0452] Method a comprising the steps of applying composition I on a substrate and then drying it, or

[0453] Method b: a method in which the wavelength conversion layer is produced by a method including the steps of applying the composition I to a support and then drying the composition, and then the wavelength conversion layer is peeled from the support and bonded to a substrate via an adhesive layer.

[0454] In one embodiment, the composition I further comprises a resin (C) including a resin composition R1. The wavelength conversion layer (resin film) formed of the resin composition R1 can be formed by applying the composition I to a substrate or a support and then drying it.

[0455] In other embodiments, composition I is a curable composition R2 further comprising a polymerizable compound (D) and a polymerization initiator (E). The curable composition R2 may further comprise a resin (C). The wavelength conversion layer formed by the curable composition R2 is a cured film. The cured film can be obtained by applying the curable composition R2 to a substrate or a support, drying it, and curing it by the action of light and / or heat.

[0456] One embodiment of the curable composition R2 is a photocurable composition R3 containing a photopolymerizable compound and a photopolymerization initiator. The photocurable composition R3 may further contain a resin (C).

[0457] The wavelength conversion layer may be provided on the entire surface of the substrate, or may be provided in a pattern on a portion of the substrate. As a method for forming the wavelength conversion layer in a pattern on the substrate, photolithography, inkjet method, printing method, etc. may be cited. As a printing method, a template printing method, a screen printing method, a printing coating method using an applicator, etc. may be cited.

[0458] Examples of the substrate include glass plates such as quartz glass, borosilicate glass, aluminosilicate glass, and soda-lime glass coated with silicon dioxide; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; materials on which aluminum, silver, and silver / copper / palladium alloy thin films are formed; and components included or included in the display device. Examples of components included or included in the display device include a primary light source (e.g., a blue light source), a light guide plate, a diffusion film (diffusion layer), a light reflecting member (reflection film, etc.), a brightness enhancing member, a prism sheet, a barrier layer, and a protective layer (cover layer).

[0459] The patterned resin film (wavelength conversion layer) formed by the resin composition R1 can be formed on the substrate, for example, as follows. First, the resin composition R1 is applied to the substrate via a mask to form a patterned composition layer. Examples of the coating method of the resin composition include spin coating, slit coating, slit and spin coating, and the like.

[0460] Next, the resin film (wavelength conversion layer) is obtained by drying the composition layer (removing volatile components such as solvents). As drying methods, heating drying, reduced pressure drying or a combination thereof can be cited. The temperature for heating drying is preferably 30°C to 250°C, more preferably 50°C to 235°C. The heating time is preferably 10 seconds to 180 minutes, more preferably 30 seconds to 90 minutes. When reduced pressure drying is performed, it is preferably carried out under a pressure of 50Pa to 150Pa. The drying of the composition layer can be implemented in multiple stages, for example, by implementing multiple drying steps with different drying temperatures.

[0461] The patterned cured film (wavelength conversion layer) formed of the photocurable composition R3 can be formed on a substrate by, for example, using a photolithography method as follows. First, the photocurable composition R3 is applied to a substrate, and heated and dried (prebaked) and / or dried under reduced pressure to remove volatile components such as a solvent to obtain a composition layer. As a coating method, the same method as described above can be cited.

[0462] The temperature for heat drying is preferably 30° C. to 120° C., more preferably 50° C. to 110° C. The heating time is preferably 10 seconds to 60 minutes, more preferably 30 seconds to 30 minutes. When reduced pressure drying is performed, it is preferably performed at a pressure of 50 Pa to 150 Pa and a temperature range of 20° C. to 25° C.

[0463] Next, the composition layer is exposed through a photomask for forming a target pattern shape. As a light source used for exposure, a light source that generates light with a wavelength of 250nm to 450nm is preferred. For example, it is also possible to selectively extract light near 436nm, near 408nm, or near 365nm from the light of this wavelength using a bandpass filter according to the absorption wavelength of the photopolymerization initiator. As the light source, specifically, a mercury lamp, a light emitting diode, a metal halide lamp, a halogen lamp, etc. can be cited.

[0464] In order to evenly irradiate the entire exposure surface with parallel light or to accurately align the exposure surface with the substrate on which the photomask and the composition layer are formed, it is preferred to use an exposure device such as a mask aligner and a stepper. The composition layer after exposure is cured by polymerization of the photopolymerizable compound contained in the composition layer.

[0465] By bringing the exposed composition layer into contact with a developer for development, the unexposed portion of the composition layer is dissolved in the developer and removed, and a patterned cured film (wavelength conversion layer) can be obtained. As a developer, for example, aqueous solutions of alkaline compounds such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, and organic solvents can be cited. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% to 10% by mass, and more preferably 0.03% to 5% by mass. As an organic solvent, the same solvent as the above-mentioned solvent (J) can be cited. The developer may also contain a surfactant.

[0466] The developing method may be any of a coating method, an immersion method, a spray method, etc. Furthermore, the substrate may be tilted at any angle during the development.

[0467] The patterned film obtained by development is preferably further heated (post-baked). The heating temperature is preferably 150°C to 250°C, more preferably 160°C to 235°C. The heating time is preferably 1 minute to 120 minutes, more preferably 10 minutes to 60 minutes. By heating after development, the unreacted photopolymerizable compounds contained in the film can be polymerized, so that a cured film with better drug resistance can be obtained. Even if development is not performed, it is preferred to further heat the exposed composition layer (post-bake).

[0468] On the other hand, as a method for forming a cured film (wavelength conversion layer) on the entire surface of a substrate, there can be cited a method of applying a curable composition on a substrate, drying it as needed to form a composition layer, heating the composition layer and / or exposing the entire surface of the composition layer.

[0469] The cured film formed by the curable composition R2 includes a curing reaction product of a polymerizable compound and a polymerization initiator contained in the curable composition R2. The curing reaction product is a substance containing a structure caused by the structure of the polymerizable compound and the polymerization initiator. The structure caused by the structure of the polymerizable compound and the polymerization initiator refers to, for example, a skeleton structure or a part thereof other than the curing reaction site of the polymerizable compound and the polymerization initiator.

[0470] The thickness of the wavelength conversion layer is, for example, 1 μm to 20 μm, preferably 1.5 μm to 18 μm, more preferably 2 μm to 14 μm, and further preferably 2 μm to 12 μm. If the thickness of the wavelength conversion layer is too small, when the primary light is irradiated to the wavelength conversion layer, the primary light is not fully absorbed or scattered by the wavelength conversion layer, and the proportion of light passing through the wavelength conversion layer tends to increase.

[0471] The shape and size of the patterned wavelength conversion layer are not particularly limited. The patterned wavelength conversion layer has, for example, a square shape in plan view.

[0472] The wavelength conversion layer involved in one embodiment is a layer that absorbs primary light from a primary light source and emits green light, and is preferably a layer that converts the wavelength of blue light, which is the primary light, into the wavelength of green light. The green light generated by the wavelength conversion layer preferably includes a peak with a local maximum in the wavelength region of 500nm to 560nm, more preferably includes a peak with a local maximum in the wavelength region of 520nm to 545nm, and further preferably includes a peak with a local maximum in the wavelength region of 525nm to 535nm in the emission spectrum. The full width at half maximum of the peak is preferably 15nm to 80nm, more preferably 15nm to 60nm, further preferably 15nm to 50nm, and particularly preferably 15nm to 45nm.

[0473] The wavelength conversion layer involved in other embodiments is a layer that absorbs the primary light from the primary light source and emits red light, and is preferably a layer that converts the wavelength of the blue light as the primary light into the wavelength of red light. The red light generated by the wavelength conversion layer preferably includes a peak with a local maximum in the wavelength region of 610nm to 750nm in the emission spectrum, more preferably includes a peak with a local maximum in the wavelength region of 620nm to 650nm, and further preferably includes a peak with a local maximum in the wavelength region of 625nm to 645nm. The full width at half maximum of the peak is preferably 15nm to 80nm, more preferably 15nm to 60nm, further preferably 15nm to 50nm, and particularly preferably 15nm to 45nm.

[0474] The laminated body and the display device described later may include both a wavelength conversion layer that emits green light and a wavelength conversion layer that emits red light.

[0475] The wavelength conversion layer may be a layer that absorbs a portion of the primary light and transmits the rest of the primary light. From the viewpoint of wide color gamut and energy efficiency of the display device, the light transmittance of the wavelength conversion layer at a wavelength of 450nm is preferably 90% or less, more preferably 85% or less, further preferably 75% or less, further preferably 60% or less, particularly preferably 40% or less, more particularly preferably 30% or less, and most preferably 20% or less. The amount of primary light that transmits the wavelength conversion layer is preferably small.

[0476] <Composition for forming protective layer and protective layer>

[0477] (1) Composition II for protective layer

[0478] The protective layer is a layer arranged on the wavelength conversion layer. The protective layer contains a multifunctional polymerizable compound (K) or a polymer thereof, and is formed by a protective layer-forming composition (hereinafter, also referred to as "composition II") that does not contain semiconductor particles (A). Composition II is a curable composition. By configuring the protective layer formed by composition II on the wavelength conversion layer, the decrease in the luminous intensity of the wavelength conversion layer caused by heat can be suppressed compared to the case where no protective layer is configured. Composition II may contain two or more multifunctional polymerizable compounds (K) or polymers thereof.

[0479] Arranging the protective layer on the wavelength conversion layer means that the protective layer is arranged directly or via other layers on at least a portion of the surface of the wavelength conversion layer. The above-mentioned surface may be the main surface of the wavelength conversion layer or the side surface. The main surface is preferably the main surface on the light output direction side of the wavelength conversion layer. The protective layer may be arranged to cover the entire main surface of the wavelength conversion layer or may be arranged to cover a portion of the main surface. The protective layer is preferably arranged to cover the entire main surface on the light output direction side of the wavelength conversion layer. The protective layer may also be arranged to cover the entire surface of the wavelength conversion layer.

[0480] (1-1) Polyfunctional polymerizable compound (K) or polymer thereof

[0481] Composition II contains a polyfunctional polymerizable compound (K) or a polymer thereof having two or more ethylenically unsaturated bonds in the molecule. The polymer refers to an oligomer or polymer obtained by polymerizing the polyfunctional polymerizable compound (K). Examples of the ethylenically unsaturated bond include (meth)acryloyloxy and vinyl groups, and (meth)acryloyloxy groups are preferred.

[0482] The polyfunctional polymerizable compound (K) is preferably a polyfunctional (meth)acrylic compound having a (meth)acryloyloxy group as an ethylenically unsaturated bond.

[0483] Examples of the difunctional (meth)acrylic compound include alkylene glycol di(meth)acrylates, polyoxyalkylene glycol di(meth)acrylates, halogen-substituted alkylene glycol di(meth)acrylates, di(meth)acrylates of aliphatic polyols, di(meth)acrylates of hydrogenated dicyclopentadiene or tricyclodecane dialkanol, di(meth)acrylates of dicyclopentadiene, dicyclodecane dialkanol, and di(meth)acrylates of dicyclopentadiene. Alkanediol or diol Alkanedialkanol di(meth)acrylate, bisphenol A or bisphenol F alkylene oxide adduct di(meth)acrylate, bisphenol A or bisphenol F epoxy di(meth)acrylate, and the like.

[0484] More specific examples of the difunctional (meth)acrylate compounds include ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and diethylene glycol di(meth)acrylate. Ester, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, hydroxy neopentyl glycol di(meth)acrylate, 2,2-bis[4-(meth)acryloyloxyethoxyethoxyphenyl]propane, 2,2-bis[4-(meth)acryloyloxyethoxyethoxycyclohexyl]propane, hydrogenated biscyclopentadienyl di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-dimethacrylate Alkane-2,5-diyl di(meth)acrylate Acetal compound of 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-hydroxymethyl-1,3-dimethacrylate], hydroxypivalaldehyde and trimethylolpropane [Chemical name: 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-hydroxymethyl-1,3-dimethacrylate] di(meth)acrylate of ethoxylated bisphenol A, di(meth)acrylate of propoxylated bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, di(meth)acrylate of propoxylated bisphenol F, and the like.

[0485] Examples of the trifunctional or higher-functional (meth)acrylic compound include glycerol tri(meth)acrylate, alkoxylated glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, and the like. ) acrylate, tripentaerythritol hepta(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tris(2-(meth)acryloyloxyethyl)isocyanurate, ethylene glycol-modified pentaerythritol tetra(meth)acrylate, ethylene glycol-modified dipentaerythritol hexa(meth)acrylate, propylene glycol-modified pentaerythritol tetra(meth)acrylate, propylene glycol-modified dipentaerythritol hexa(meth)acrylate, caprolactone-modified pentaerythritol tetra(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and the like.

[0486] From the viewpoint of suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat and the viewpoint of pattern formation when forming a patterned protective layer, the multifunctional polymerizable compound (K) preferably has three or more ethylenically unsaturated bonds in the molecule, and more preferably has three or more (meth)acryloyloxy groups. The number of ethylenically unsaturated bonds possessed by the multifunctional polymerizable compound (K) is preferably six or less.

[0487] In addition, from the viewpoint of more effectively suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat, the multifunctional polymerizable compound (K) preferably has an acidic functional group. As the acidic functional group, for example, a carboxyl group, a sulfonic acid group, a phosphoric acid group, etc. can be cited. Among them, the acidic functional group is preferably a carboxyl group. From the viewpoint of more effectively suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat, the number of acidic functional groups that the multifunctional polymerizable compound (K) can have is preferably 1 to 3, more preferably 1 or 2. When having two or more acidic functional groups, each acidic functional group may be different or the same.

[0488] Examples of the polyfunctional polymerizable compound (K) having an acidic functional group include compounds obtained by subjecting a compound having two or more (preferably three or more) (meth)acryloyloxy groups and one or more hydroxyl groups in the molecule to polybasic acid modification. Examples of such compounds include compounds obtained by monoesterifying pentaerythritol triester (meth)acrylate with a dibasic acid (e.g., succinic acid, maleic acid) or an anhydride thereof, and compounds obtained by monoesterifying dipentaerythritol penta(meth)acrylate with a dibasic acid (e.g., succinic acid, maleic acid) or an anhydride thereof.

[0489] As commercially available products of the polyfunctional polymerizable compound (K) having an acidic functional group, for example, there can be cited "Aronix M-510" manufactured by Toagosei Co., Ltd., which has a dibasic acid anhydride adduct of pentaerythritol tri(meth)acrylate as a main component, and "Aronix M-520D" manufactured by Toagosei Co., Ltd., which has a dibasic acid anhydride adduct of dipentaerythritol penta(meth)acrylate as a main component. These commercially available products have a carboxyl group as an acidic functional group and belong to a polyfunctional polymerizable compound (K) having three or more (meth)acryloyloxy groups.

[0490] From the viewpoint of suppressing a decrease in the light emission intensity of the wavelength conversion layer due to heat, it is preferred that the polyfunctional polymerizable compound (K) or its polymer does not contain a silicon atom in the molecule.

[0491] The content of the multifunctional polymerizable compound (K) or its polymer in the composition II is preferably 7% to 80% by mass, more preferably 10% to 75% by mass, further preferably 15% to 70% by mass, further preferably 30% to 70% by mass, particularly preferably 40% to 70% by mass, and most preferably 45% to 65% by mass, relative to the total amount of the solid content of the composition II. If the content is within the above range, it is advantageous in suppressing the decrease in the luminous intensity of the wavelength conversion layer due to heat.

[0492] (1-2) Other ingredients

[0493] In addition to the multifunctional polymerizable compound (K) or its polymer, composition II preferably further contains a resin (C) and a polymerization initiator (E). Regarding the resin (C) and the polymerization initiator (E) in composition II, except for the content in the composition, the relevant description of composition I is cited. The polymerization initiator (E) is preferably a photopolymerization initiator. Composition II may further contain at least one selected from a polymerization initiation aid (E1), an antioxidant (F), a leveling agent (H) and a solvent (J). Regarding the polymerization initiation aid (E1), an antioxidant (F), a leveling agent (H) and a solvent (J) in composition II, except for the content in the composition, the relevant description of composition I is cited.

[0494] The content of the resin (C) in the composition II is, for example, 0.00001% by mass to 99.99999% by mass, preferably 1% by mass to 99% by mass, more preferably 1% by mass to 97% by mass, further preferably 1% by mass to 95% by mass, further preferably 3% by mass to 90% by mass, particularly preferably 5% by mass to 80% by mass, and most preferably 10% by mass to 70% by mass, relative to the total amount of solid components of the composition II.

[0495] The content of the polymerization initiator (E) in the composition II is preferably 0.001 to 60% by mass, more preferably 0.01 to 50% by mass, based on the total amount of the resin (C) and the polyfunctional polymerizable compound (K) or its polymer.

[0496] When a polymerization initiator aid (E1) is used, the content of the polymerization initiator aid (E1) in the composition II is preferably 0.00001% by mass to 60% by mass, and more preferably 0.0001% by mass to 50% by mass, relative to the total amount of the resin (C) and the polyfunctional polymerizable compound (K) or its polymer.

[0497] When an antioxidant (F) is used, the content of the antioxidant (F) in composition II is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, and even more preferably 4 to 30 parts by mass, relative to 100 parts by mass of the total amount of the resin (C) and the multifunctional polymerizable compound (K) or its polymer.

[0498] When a leveling agent (H) is used, the content of the leveling agent (H) in the composition II is, for example, 0.001% to 1.0% by mass, preferably 0.005% to 0.75% by mass, more preferably 0.01% to 0.5% by mass, and further preferably 0.02% to 0.5% by mass, relative to the total amount of the composition II. If the content of the leveling agent (H) is within the above range, the flatness of the protective layer can be improved.

[0499] Composition II does not contain semiconductor particles (A). Composition II may contain a colorant other than semiconductor particles (A), but preferably does not contain a colorant. The colorant may be a pigment or a dye. As the pigment, a known pigment may be used, for example, a pigment classified as a pigment in the Color Index (published by The Society of Dyers and Colourists). Only one type of pigment may be used, or two or more types may be used at the same time. As the dye, a known dye may be used, for example, a dye described in the Color Index (published by The Society of Dyers and Colourists) and the Dyeing Guide (Color Dyeing Company). Only one type of dye may be used, or two or more types may be used at the same time.

[0500] The colorant may be subjected to rosin treatment, surface treatment using a colorant derivative having an acidic group or a basic group introduced therein, grafting treatment on the colorant surface using a polymer compound, micronization treatment using a sulfuric acid micronization method, washing treatment using an organic solvent or water for removing impurities, removal treatment of ionic impurities using an ion exchange method, etc. The particle size of the colorant is preferably substantially uniform.

[0501] When composition II contains a colorant, the content of the colorant in composition II is, for example, 0.01% by mass to 99.99% by mass, preferably 0.1% by mass to 99.9% by mass, more preferably 1% by mass to 99% by mass, further preferably 10% by mass to 90% by mass, and further preferably 15% by mass to 70% by mass, relative to the total amount of solid components of composition II.

[0502] The composition II may further contain additives known in the art, such as a polymerization inhibitor, a filler, other polymer compounds, an adhesion promoter, a light stabilizer, and a chain transfer agent, as required.

[0503] The solid content of composition II, relative to the total amount of composition II, is preferably 0.01% to 100% by mass, more preferably 0.1% to 99.9% by mass, further preferably 0.1% to 99% by mass, further preferably 1% to 90% by mass, further preferably 1% to 80% by mass, particularly preferably 1% to 70% by mass, extremely preferably 1% to 60% by mass, and most preferably 1% to 50% by mass.

[0504] The content of the solvent (J) in the composition II is preferably 0% to 99.99% by mass, more preferably 0.1% to 99.9% by mass, further preferably 1% to 99.9% by mass, further preferably 10% to 99% by mass, further preferably 20% to 99% by mass, particularly preferably 30% to 99% by mass, extremely preferably 40% to 99% by mass, and most preferably 50% to 99% by mass, relative to the total amount of the composition II.

[0505] (1-3) Method for producing composition II

[0506] Composition II can be manufactured by a method comprising a step of mixing the prescribed components and other components used as needed. The method for manufacturing composition II may further include a step of preparing resin (C). When a colorant is used, the colorant is preferably used in a state where the colorant is pre-mixed with a part or all of the solvent (J) and the colorant is dispersed into a colorant dispersion having an average particle size of about 0.2 μm or less using a bead mill or the like. At this time, a part or all of the dispersant and the resin (C) may also be combined as needed. As a dispersant, the records related to the dispersant described in the light scattering agent (B) column are cited.

[0507] (2) Protective layer and method for manufacturing the same

[0508] The protective layer is formed from composition II. The protective layer is formed on the wavelength conversion layer. The protective layer may be in contact with the wavelength conversion layer, or another layer may be inserted between the wavelength conversion layer and the protective layer. As another layer, a light absorbing layer may be mentioned.

[0509] In one embodiment, composition II is a curable composition comprising a multifunctional polymerizable compound (K) or a polymer thereof, and a polymerization initiator (E). The curable composition may further comprise a resin (C). The protective layer formed by the curable composition is a cured film. The cured film can be obtained by applying the curable composition to a substrate, drying it, and curing it by light and / or heat.

[0510] One embodiment of the curable composition is a photocurable composition comprising a polyfunctional polymerizable compound (K) or a polymer thereof, and a photopolymerization initiator. The photocurable composition may further comprise a resin (C).

[0511] The substrate forming the protective layer is the wavelength conversion layer or a layer (e.g., a light absorbing layer) formed on the wavelength conversion layer. As a method for forming the protective layer on the substrate, photolithography, inkjet method, printing method, etc. can be cited. As a printing method, template printing method, screen printing method, printing coating using an applicator, etc. can be cited.

[0512] The curable composition or photocurable composition as composition II can be used to form a patterned protective layer in the same manner as the above-mentioned method for forming a patterned wavelength conversion layer using resin composition R1, curable composition R2, or photocurable composition R3.

[0513] The thickness of the protective layer is, for example, 0.1 μm to 20 μm. From the viewpoint of suppressing warping and wrinkling generated during curing and suppressing the decrease in the luminous intensity of the wavelength conversion layer caused by heat, the thickness of the protective layer is preferably 0.1 μm to 15 μm, more preferably 0.5 μm to 10 μm, further preferably 0.5 μm to 6 μm, and further preferably 0.5 μm to 4.5 μm.

[0514] <Laminated body>

[0515] (1) Structure of laminate

[0516] The laminate according to the present invention (hereinafter simply referred to as “laminate”) is an optical laminate including the wavelength conversion layer containing semiconductor particles (A) and the protective layer according to the present invention. Figure 1 is a schematic cross-sectional view showing an example of a laminate according to the present invention. Figure 2 is a schematic cross-sectional view showing another example of the laminated body according to the present invention. Figure 3 This is a schematic cross-sectional view showing another example of the laminated body according to the present invention.

[0517] Figure 1 to Figure 3 The stacked body shown includes a wavelength conversion layer 10 and a protective layer 20 disposed thereon. Figure 1 and Figure 2 In the laminate shown in FIG. 1 , the protective layer 20 is directly laminated on the wavelength conversion layer 10, and the protective layer 20 may be in contact with the wavelength conversion layer 10. Alternatively, as Figure 3 In the laminate shown in the figure, other layers may be inserted between the wavelength conversion layer 10 and the protective layer 20. As the other layer, a light absorbing layer 30 may be mentioned. When other layers are inserted, heat is applied to the wavelength conversion layer in the process of forming the other layers, so the luminous intensity of the wavelength conversion layer may decrease. If this aspect is taken into consideration, Figure 1 and Figure 2 In the laminate shown, the protective layer 20 is preferably directly laminated on the wavelength conversion layer 10 .

[0518] Figure 4 FIG. 2 is a schematic cross-sectional view showing yet another example of the laminated body according to the present invention. Figure 4As shown in FIG. 1 , the laminate includes: a first wavelength conversion layer 11 emitting red light, a first protective layer 21 disposed thereon, a second wavelength conversion layer 12 emitting green light, and a second protective layer 22 disposed thereon. The first protective layer 21 and the second protective layer 22 are both protective layers of the present invention. Instead of the first protective layer 21 and the second protective layer 22 disposed separately, a single (integrated) protective layer may be disposed on the first wavelength conversion layer 11 and the second wavelength conversion layer 12. In addition, in the case of Figure 4 In the stack shown, it is possible to Figure 2 , Figure 3 The stacked body is similarly provided with a light absorbing layer 30 .

[0519] In such Figure 4 In the laminate shown, when the light absorbing layer 30 is provided, the first light absorbing layer may be provided on the first wavelength conversion layer 11 or the first protective layer 21, and the second light absorbing layer may be provided on the second wavelength conversion layer 12 or the second protective layer 22. Alternatively, one (integrated) light absorbing layer may be provided on the first wavelength conversion layer 11 and the second wavelength conversion layer 12, or on the first protective layer 21 and the second protective layer 22.

[0520] The laminated body can be suitably used as a color conversion member disposed on a primary light source (blue light source) of a display device. According to the laminated body of the present invention, it is possible to suppress a decrease in the light emission intensity of the wavelength conversion layer due to heat.

[0521] (2) Composition for forming a light absorbing layer III

[0522] The light absorbing layer is a layer that transmits light in a specific wavelength range and absorbs light in at least a portion of the other wavelength ranges. The light released from the wavelength conversion layer passes through the light absorbing layer and is released from the display device. By providing the light absorbing layer on the wavelength conversion layer, it is possible to suppress the leakage of the primary light to the visual recognition side of the light absorbing layer, thereby realizing a wide color gamut of the display device.

[0523] The wavelength region of light transmitted by the light absorbing layer is preferably a green or red wavelength region. The green wavelength region is, for example, a wavelength region included in 495nm to 585nm. The red wavelength region is, for example, a wavelength region included in 585nm to 780nm. The wavelength region of light absorbed by the light absorbing layer is preferably a blue wavelength region, more preferably a wavelength range including 450nm, for example, a wavelength region above 380nm and included in 495nm.

[0524] In one embodiment, the average light transmittance of the composition III and the light absorbing layer in the wavelength region of 520 nm to 780 nm is 98% or more. By making the average light transmittance 98% or more, the luminous intensity can be further improved. The average light transmittance can be determined based on the absorption spectrum measured by a UV-visible-near infrared spectrophotometer equipped with an integrating sphere.

[0525] (2-1) Coloring agent

[0526] The light absorbing layer is formed from a light absorbing layer forming composition containing a colorant (hereinafter, also referred to as "composition III"). Composition III may be a curable composition that is cured by light irradiation or heat.

[0527] The coloring agent may be a pigment or a dye. As the pigment, a known pigment may be used, for example, a pigment classified as a pigment in the Color Index (published by The Society of Dyers and Colourists) may be cited. The pigment may be used alone or in combination of two or more. As the dye, a known dye may be used, for example, a dye described in the Color Index (published by The Society of Dyers and Colourists) and the Dyeing Guide (Color Dyeing Company) may be cited. The dye may be used alone or in combination of two or more. The coloring agent is preferably a yellow coloring agent.

[0528] Composition III preferably contains a first colorant satisfying the following formulae (i) and (ii). max (nm) represents the wavelength showing the maximum absorbance in the visible light wavelength region of the absorption spectrum. max Indicates the maximum absorbance above. A 480 Indicates the absorbance at a wavelength of 480nm.

[0529] 425≤λ max ≤470 (i)

[0530] A 480 / A max <0.5 (ii)

[0531] By satisfying equation (i), it is possible to suppress the leakage of the primary light (blue light) to the visual recognition side of the light absorbing layer, thereby achieving a wide color gamut of the display device. max It is preferable to satisfy any one of the following formulae.

[0532] 425≤λ max ≤460、425≤λ max ≤450、425≤λ max ≤440、430≤λ max≤460、430≤λ max ≤450, or 430≤λ max ≤440.

[0533] By satisfying the formula (ii), it is possible to suppress a decrease in luminous intensity. The decrease in luminous intensity here refers to a decrease in luminous intensity when a light absorbing layer is disposed on the wavelength conversion layer compared to a case where no light absorbing layer is disposed.

[0534] The left side of formula (ii) is preferably 0.45 or less, more preferably 0.4 or less, and may be 0.35 or less. The left side of formula (ii) is usually 0.001 or more, and may be 0.005 or more, 0.01 or more, or 0.05 or more.

[0535] By disposing a light absorbing layer formed of composition III on the wavelength conversion layer, it is possible to suppress leakage of primary light (e.g., blue light) to the visual recognition side of the light absorbing layer, and to suppress a decrease in luminous intensity when a light absorbing layer is disposed on the wavelength conversion layer compared to a case where no light absorbing layer is disposed. The amount of primary light passing through the wavelength conversion layer is preferably small, but by disposing a light absorbing layer formed of composition III containing a first colorant on the wavelength conversion layer, it is possible to suppress leakage of primary light to the visual recognition side, and to suppress a decrease in luminous intensity, even when a portion of the primary light passes through the wavelength conversion layer. From this viewpoint, the light transmittance of the wavelength conversion layer at a wavelength of 450 nm can be 10% or more, further 15% or more, and further 20% or more.

[0536] From the viewpoint of suppressing leakage of primary light and suppressing a decrease in luminous intensity, composition III preferably satisfies the above formulae (i) and (ii). Furthermore, the light absorbing layer formed from composition III preferably satisfies the above formulae (i) and (ii).

[0537] The absorption spectrum of the light absorbing layer can be measured by using a UV-visible-near infrared spectrophotometer equipped with an integrating sphere, using the light absorbing layer formed on a glass substrate as a measurement sample. The absorption spectrum of composition III can be measured as the absorption spectrum of the composition layer formed by applying the composition on a glass substrate or the like.

[0538] In addition, the absorption spectrum of the first colorant can be measured as the absorption spectrum of a light absorbing layer containing only the first colorant as a colorant.

[0539] The first colorant is preferably a yellow colorant. The yellow colorant may be a pigment or a dye. As the pigment, a known pigment may be used. Only one pigment may be used, or two or more pigments may be used at the same time. As the dye, a known dye may be used. Only one dye may be used, or two or more pigments may be used at the same time.

[0540] The yellow pigment that can be used as the first colorant is preferably selected from quinophthalone yellow pigments and azo yellow pigments, and more preferably quinophthalone yellow pigments. As quinophthalone yellow pigments, for example, CI Pigment Yellow 138, 231, etc. can be cited. As azo yellow pigments, for example, CI Pigment Yellow 150, etc. can be cited.

[0541] Composition III may contain only the first colorant as a colorant, or may contain a second colorant other than the first colorant in addition to the first colorant. When composition III further contains a second colorant, from the viewpoint of suppressing the leakage of primary light and suppressing the decrease in luminous intensity, it is preferred that the combination of the first colorant and the second colorant satisfies the above formulas (i) and (ii). The second colorant may be a pigment or a dye. Only one type of pigment and dye may be used, or two or more types may be used simultaneously.

[0542] The second colorant is preferably selected from a green colorant and a red colorant.

[0543] Examples of the green colorant include green pigments such as CI Pigment Green 7, 36, 58, 59, 62, and 63. Other examples of the green colorant include the following dyes.

[0544] CI solvent dyes such as CI Solvent Green 1, 3, 4, 5, 7, 28, 29, 32, 33, 34, 35;

[0545] CI acid green 1, 3, 5, 6, 7, 8, 9, 11, 13, 14, 15, 16, 22, 25, 27, 28, 41, 50, 50:1, 58, 63, 65, 80, 104, 105, 106, 109 and other CI acid dyes;

[0546] CI direct dyes such as CI Direct Green 25, 27, 31, 32, 34, 37, 63, 65, 66, 67, 68, 69, 72, 79, 82;

[0547] CI basic dyes such as CI basic green;

[0548] CI mordant green 1, 3, 4, 5, 10, 13, 15, 19, 21, 23, 26, 29, 31, 33, 34, 35, 41, 43, 53 and other CI mordant dyes;

[0549] CI vat dyes such as CI vat green 1, etc.

[0550] Examples of the red colorant include CI Pigment Red 9, 97, 105, 122, 123, 144, 149, 166, 168, 176, 177, 178, 179, 180, 190, 192, 209, 215, 216, 224, 242, 254, 255, 264, 265, 266, 268, 269, and 273. Other examples of the red colorant include the following dyes.

[0551] CI solvent dyes such as CI Solvent Red 24, 45, 49, 90, 91111, 118, 119, 122, 124, 125, 127, 130, 132, 143, 145, 146, 150, 151, 155, 160, 168, 169, 172, 175, 181, 207, 218, 222, 227, 230, 245, 247;

[0552] CI Acid Red 1, 4, 8, 14, 17, 18, 26, 27, 29, 31, 33, 34, 35, 37, 40, 42, 44, 50, 51, 52, 57, 66, 73, 76, 80, 87, 88, 91, 92, 94, 95, 97, 98, 103, 106, 111, 114, 129, 133, 134, 138, 143, 145, 150, 151, 155, 158, 160, 172, 176, 182, 183 , 195, 198, 206, 211, 215, 216, 217, 227, 228, 249, 252, 257, 258, 260, 261, 266, 268, 270, 274, 277, 280, 281, 289, 308, 312, 315, 316, 339, 341, 345, 346, 349, 382, ​​383, 388, 394, 401, 412, 417, 418, 422, 426 and other CI acid dyes;

[0553] CI direct dyes such as CI Direct Red 79, 82, 83, 84, 91, 92, 96, 97, 98, 99, 105, 106, 107, 172, 173, 176, 177, 179, 181, 182, 184, 204, 207, 211, 213, 218, 220, 221, 222, 232, 233, 234, 241, 243, 246, 250;

[0554] CI basic dyes such as CI Basic Red 1, 9, 10;

[0555] CI mordant red 1, 2, 3, 4, 9, 11, 12, 14, 17, 18, 19, 22, 23, 24, 25, 26, 27, 29, 30, 32, 33, 36, 37, 38, 39, 41, 42, 43, 45, 46, 48, 52, 53, 56, 62, 63, 71, 74, 76, 78, 85, 86, 88, 90, 94, 95 and other CI mordant dyes, etc.

[0556] The colorant may be subjected to rosin treatment, surface treatment using a colorant derivative having an acidic group or a basic group introduced therein, grafting treatment on the colorant surface using a polymer compound, micronization treatment using a sulfuric acid micronization method, washing treatment using an organic solvent or water for removing impurities, removal treatment of ionic impurities using an ion exchange method, etc., etc., as required. The particle size of the colorant is preferably substantially uniform.

[0557] When composition III contains a second colorant, when the wavelength conversion layer is a layer emitting green light, the second colorant is preferably a green colorant, and when the wavelength conversion layer is a layer emitting red light, the second colorant is preferably a red colorant. The green colorant and the red colorant may be used alone or in combination of two or more.

[0558] The content of the colorant in the composition III is, for example, 0.01% by mass to 99.99% by mass, preferably 0.1% by mass to 99.9% by mass, more preferably 1% by mass to 99% by mass, further preferably 10% by mass to 90% by mass, further preferably 15% by mass to 70% by mass, and particularly preferably 20% by mass to 70% by mass, relative to the total amount of the solid content of the composition III. When the composition III contains only the first colorant as the colorant, the colorant refers to the first colorant, and when the composition III contains the first colorant and the second colorant, the colorant refers to these first colorant and the second colorant.

[0559] (2-2) Other ingredients

[0560] In addition to the colorant, composition III preferably contains a resin (C), a polymerizable compound (D) and a polymerization initiator (E). Regarding the resin (C), the polymerizable compound (D) and the polymerization initiator (E) in composition III, except for the content ratio in the composition, the relevant description of composition I is cited. Composition III may further contain at least one selected from a self-polymerization initiation aid (E1), an antioxidant (F), a leveling agent (H) and a solvent (J). Regarding the polymerization initiation aid (E1), the antioxidant (F), the leveling agent (H) and the solvent (J) in composition III, except for the content ratio of these in the composition, the relevant description of composition I is cited.

[0561] The content of the resin (C) in the composition III, relative to the total amount of the solid content of the composition III, is, for example, 0.00001% by mass to 99.99999% by mass, preferably 1% by mass to 99% by mass, more preferably 1% by mass to 97% by mass, further preferably 1% by mass to 95% by mass, further preferably 3% by mass to 90% by mass, particularly preferably 5% by mass to 80% by mass, and most preferably 10% by mass to 70% by mass.

[0562] The content of the polymerizable compound (D) in the composition III, relative to the total amount of the solid content of the composition III, is, for example, 0.00001% by mass to 99.99999% by mass, preferably 1% by mass to 99% by mass, more preferably 1% by mass to 97% by mass, further preferably 1% by mass to 95% by mass, further preferably 1% by mass to 90% by mass, particularly preferably 2% by mass to 80% by mass, and most preferably 3% by mass to 70% by mass.

[0563] The content of the polymerization initiator (E) in the composition III is preferably 0.001 to 60% by mass, more preferably 0.01 to 50% by mass, based on the total amount of the resin (C) and the polymerizable compound (D).

[0564] When the polymerization initiator aid (E1) is used, the content of the polymerization initiator aid (E1) in the composition III is preferably 0.00001 to 60% by mass, more preferably 0.0001 to 50% by mass, based on the total amount of the resin (C) and the polymerizable compound (D).

[0565] When the antioxidant (F) is used, the content of the antioxidant (F) in the composition III is, for example, 1 to 50 parts by mass, preferably 5 to 40 parts by mass, more preferably 7 to 30 parts by mass, based on 100 parts by mass of the resin (C).

[0566] When a leveling agent (H) is used, the content of the leveling agent (H) in the composition III is, for example, 0.001% to 1.0% by mass, preferably 0.005% to 0.75% by mass, more preferably 0.01% to 0.5% by mass, and further preferably 0.02% to 0.5% by mass, relative to the total amount of the composition III. If the content of the leveling agent (H) is within the above range, the flatness of the light absorbing layer can be improved.

[0567] The solid content of composition III, relative to the total amount of composition III, is preferably 0.01% to 100% by mass, more preferably 0.1% to 99.9% by mass, further preferably 0.1% to 99% by mass, further preferably 1% to 90% by mass, further preferably 1% to 80% by mass, particularly preferably 1% to 70% by mass, and extremely preferably 1% to 60% by mass.

[0568] The content of the solvent (J) in composition III, relative to the total amount of composition III, is preferably 0% to 99.99% by mass, more preferably 0.1% to 99.9% by mass, further preferably 1% to 99.9% by mass, further preferably 10% to 99% by mass, further preferably 20% to 99% by mass, particularly preferably 30% to 99% by mass, and extremely preferably 40% to 99% by mass.

[0569] The composition III may further contain additives known in the art, such as a polymerization inhibitor, a filler, other polymer compounds, an adhesion promoter, a light stabilizer, and a chain transfer agent, as required.

[0570] (2-3) Method for producing composition III

[0571] Composition III can be manufactured by a method including a step of mixing a colorant and other components used as needed. The colorant is preferably used in a state where the colorant is pre-mixed with a part or all of the solvent (J) and the colorant is dispersed into a colorant dispersion having an average particle size of about 0.2 μm or less using a bead mill or the like. At this time, a part or all of the dispersant and resin (C) may be added as needed. As the dispersant, the records related to the dispersant described in the light scattering agent (B) column are cited.

[0572] (3) Light absorbing layer and method for manufacturing the same

[0573] The light absorbing layer is formed by composition III. The light absorbing layer is formed on the wavelength conversion layer. The light absorbing layer is, for example, arranged on the light output direction side of the wavelength conversion layer. The light absorbing layer may be in contact with the wavelength conversion layer, or other layers may be inserted between the wavelength conversion layer and the light absorbing layer. As other layers, a protective layer (covering layer) may be cited.

[0574] The light absorbing layer can be formed on the wavelength converting layer by a method including the steps of applying the composition III to a substrate and then drying the coating.

[0575] In one embodiment, the composition III further comprises a resin (C) including a resin composition R4. The light absorbing layer (resin film) formed of the resin composition R4 can be formed by applying the composition III to a substrate and then drying it.

[0576] In other embodiments, composition III further comprises a curable composition R5 of a polymerizable compound (D) and a polymerization initiator (E). The curable composition R5 may further comprise a resin (C). The light absorbing layer formed by the curable composition R5 is a cured film. The cured film can be obtained by applying the curable composition R5 to a substrate, drying it, and curing it by light and / or heat.

[0577] One embodiment of the curable composition R5 is a photocurable composition R6 containing a photopolymerizable compound and a photopolymerization initiator. The photocurable composition R6 may further contain a resin (C).

[0578] The substrate forming the light absorbing layer is the wavelength conversion layer or a layer (e.g., a protective layer) formed on the wavelength conversion layer. Methods for forming the light absorbing layer on the substrate include photolithography, inkjet printing, and printing. Printing methods include template printing, screen printing, and printing using an applicator.

[0579] The resin composition R4, curable composition R5, or photocurable composition R6 can be used to form a patterned light absorbing layer in the same manner as the above-mentioned method for forming a patterned wavelength conversion layer using the resin composition R1, curable composition R2, or photocurable composition R3.

[0580] The patterned cured film (light absorbing layer) formed of the photocurable composition R6 can be formed on a substrate as follows, for example, by using a photolithography method. First, the photocurable composition R6 is applied to a substrate, and heated and dried (prebaked) and / or dried under reduced pressure to remove volatile components such as a solvent to obtain a composition layer. Examples of the coating method include spin coating, slit coating, slit and spin coating, and the like.

[0581] The temperature for heat drying is preferably 30° C. to 120° C., more preferably 50° C. to 110° C. The heating time is preferably 10 seconds to 60 minutes, more preferably 30 seconds to 30 minutes. When reduced pressure drying is performed, it is preferably performed at a pressure of 50 Pa to 150 Pa and a temperature range of 20° C. to 25° C.

[0582] Next, the composition layer is exposed through a photomask for forming a target pattern shape. As a light source used for exposure, a light source that generates light with a wavelength of 250nm to 450nm is preferred. For example, it is also possible to selectively extract light near 436nm, near 408nm, or near 365nm from the light of this wavelength using a bandpass filter according to the absorption wavelength of the photopolymerization initiator. As the light source, specifically, a mercury lamp, a light emitting diode, a metal halide lamp, a halogen lamp, etc. can be cited.

[0583] In order to evenly irradiate the entire exposure surface with parallel light or to accurately align the exposure surface with the substrate on which the photomask and the composition layer are formed, it is preferred to use an exposure device such as a mask aligner and a stepper. The composition layer after exposure is cured by polymerization of the photopolymerizable compound contained in the composition layer.

[0584] By bringing the exposed composition layer into contact with a developer for development, the unexposed portion of the composition layer is dissolved in the developer and removed, and a patterned cured film (light absorbing layer) can be obtained. As the developer, for example, aqueous solutions of alkaline compounds such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, and organic solvents can be cited. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% to 10% by mass, and more preferably 0.03% to 5% by mass. As the organic solvent, the same solvent as the above-mentioned solvent (J) can be cited. The developer may also contain a surfactant.

[0585] The developing method may be any of a coating method, an immersion method, a spray method, etc. Furthermore, the substrate may be tilted at any angle during the development.

[0586] The patterned film obtained by development is preferably further heated (post-baked). The heating temperature is preferably 150°C to 250°C, more preferably 160°C to 235°C. The heating time is preferably 1 minute to 120 minutes, more preferably 10 minutes to 60 minutes. By heating after development, the unreacted photopolymerizable compounds contained in the film can be polymerized, so that a cured film with better drug resistance can be obtained. Even if development is not performed, it is preferred to further heat the exposed composition layer (post-bake).

[0587] The thickness of the light absorbing layer is, for example, 0.1 μm to 30 μm, preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 10 μm, and further preferably 0.5 μm to 6 μm from the viewpoint of effectively suppressing leakage of primary light (blue light) to the visual recognition side of the light absorbing layer.

[0588] The content of the colorant in the light absorbing layer is, for example, 0.01 to 99.99 mass %, preferably 0.1 to 99.9 mass %, more preferably 1 to 99 mass %, further preferably 10 to 90 mass %, and further preferably 15 to 70 mass %.

[0589] The wavelength region of light transmitted by the light absorbing layer is preferably a green or red wavelength region. The green wavelength region is, for example, a wavelength region included in 495nm to 585nm. The red wavelength region is, for example, a wavelength region included in 585nm to 780nm. The wavelength region of light absorbed by the light absorbing layer is preferably a blue wavelength region, more preferably a wavelength range including 450nm, for example, a wavelength region above 380nm and included in 495nm.

[0590] In one embodiment, the average light transmittance of the composition III and the light absorbing layer in the wavelength range of 520 nm to 780 nm is 98% or more. By setting the average light transmittance to 98% or more, the luminous intensity can be further increased.

[0591] <Display device>

[0592] The display device of the present invention (hereinafter referred to as "display device") comprises a primary light source and the laminate of the present invention. The display device is a device that emits light from the primary light source to the wavelength conversion layer, and outputs the emitted light through the light absorption layer.

[0593] Figure 5 This is a schematic cross-sectional view showing an example of a display device according to the present invention. Figure 5 The display device shown comprises Figure 4 The stacked body shown in FIG. 1 includes: a blue light source 40 as a primary light source, having a first region, a second region, and a third region that are different from each other; a first wavelength conversion layer 11, which is arranged on the first region of the blue light source 40, for example, emitting red light; a first protective layer 21, which is arranged on the first wavelength conversion layer 11; a second wavelength conversion layer 12, which is arranged on the second region of the blue light source 40, for example, emitting green light; and a second protective layer 22, which is arranged on the second wavelength conversion layer 12. The display device has a red light emitting region (i.e., the first region), a green light emitting region (i.e., the second region), and a blue light emitting region (i.e., the third region). Thus, the display device has a blue light source, a wavelength conversion layer, and a protective layer in the optical path of light from the blue light source 40.

[0594] The first wavelength conversion layer 11 and the second wavelength conversion layer 12 may be directly disposed on the blue light source 40 , or may be disposed on a light guide plate disposed between the blue light source 40 and the first wavelength conversion layer 11 and the second wavelength conversion layer 12 in the optical path of light from the blue light source 40 .

[0595] The display device may further include a transparent layer or a layer containing a light diffusing agent that is arranged on the third area of ​​the blue light source 40 and transmits blue light. Figure 2 , Figure 3The laminated body similarly has a light absorbing layer 30. On the transparent layer or the layer containing a light diffusing agent that transmits the blue light, a third light absorbing layer that transmits the blue light and absorbs light other than the blue light may be provided.

[0596] As the blue light source 40, for example, a known light source such as a blue light emitting diode (LED), a laser, an EL, etc. can be used. From the viewpoint of color gamut and energy efficiency, the blue light source 40 is preferably a light source that emits light having a peak below 495nm, and more preferably a light source that emits light having a peak at 425nm to 495nm.

[0597] The display device may further include, for example, a light guide plate, a diffusion film (diffusion layer), a light reflecting component (reflection film, etc.), a brightness enhancing component, a prism sheet, a barrier layer, etc.

[0598] Any appropriate light guide plate may be used as the light guide plate. For example, a light guide plate having a lens pattern formed on the back side, a light guide plate having a prism shape formed on the back side and / or the visual recognition side, etc. may be used to deflect light from the lateral direction in the thickness direction.

[0599] The diffusion film is a film used to diffuse the light emitted from the primary light or the wavelength conversion layer, and may also be an amplifying diffusion film, etc. The light reflecting component is a component used to reflect the primary light toward the wavelength conversion layer, and may be, for example, a reflector, a film of reflective particles, a reflective metal film, or a reflector, etc. The brightness enhancement component is a component used to reflect a part of the light toward the direction of light propagation and return it.

[0600] The prism sheet typically has a substrate portion and a prism portion. The substrate portion may be omitted depending on the adjacent components. The prism sheet may be bonded to the adjacent components via any appropriate bonding layer (e.g., adhesive layer, pressure-sensitive adhesive layer). The prism sheet is composed of a plurality of unit prisms protruding to the opposite side (back side) of the visual recognition side arranged in parallel. By arranging the convex portion of the prism sheet toward the back side, light passing through the prism sheet is easily focused. In addition, if the convex portion of the prism sheet is arranged toward the back side, the light that is not incident on the prism sheet and is reflected is less compared to the case where the convex portion is arranged toward the visual recognition side, and a display device with high luminous intensity can be obtained.

[0601] The barrier layer is a layer for protecting the wavelength conversion layer from water vapor in the outside air and oxygen in the atmosphere. In one embodiment, the display device includes both the protective layer and the barrier layer, and the barrier layer is used to protect the wavelength conversion layer from water vapor in the outside air and oxygen in the atmosphere.

[0602] The display device may include a layer composed of one or more dielectric materials on the optical path between adjacent elements (layers). The one or more dielectric materials include, for example, vacuum, air, gas, optical material, adhesive, optical adhesive, glass, polymer, solid, liquid, gel, curing material, optical bonding material, refractive index matching or refractive index mismatching material, refractive index gradient material, cladding or anti-cladding material, spacer, silica gel, brightness enhancement material, scattering or diffusion material, reflection or anti-reflection material, wavelength selective material, wavelength selective anti-reflection material or other suitable media known in the art, but are not limited to these and may include any appropriate material.

[0603] Specific examples of display devices include EL displays and display devices equipped with wavelength conversion materials for liquid crystal displays. Display devices are not limited to those using Figure 5 The example shown may be, for example, a display device in which a wavelength conversion layer is arranged between a blue light source and a light guide plate along an end surface (side surface) of the light guide plate, and a backlight (side tube package type backlight) that emits white light is provided, and a light absorption layer is arranged on the light guide plate side;

[0604] A display device in which a wavelength conversion layer is disposed on a light guide plate, a backlight (surface mounted backlight) is provided in which light irradiated from a blue light source placed on an end face (side face) of the light guide plate to the wavelength conversion layer is released as white light, and a light absorption layer is disposed on the wavelength conversion layer;

[0605] A display device in which a wavelength conversion layer is provided near the light emitting portion of a blue light source to release the irradiated light in the form of white light (chip package type backlight), and a light absorbing layer is arranged on the wavelength conversion layer; etc.

[0606] Example

[0607] The present invention is further described in detail below with reference to Examples. Unless otherwise specified, "%" and "parts" in the Examples are % by mass and parts by mass.

[0608] <Measurement>

[0609] (1) Measurement of the thickness of the wavelength conversion layer and the protective layer

[0610] The measurement was performed using a film thickness measuring device (DEKTAKXT; manufactured by Bruker).

[0611] (2) Measurement of the luminous intensity EI of the wavelength conversion layer and the laminate

[0612] A light diffusion plate is arranged as a backlight unit on a backlight using a blue LED lamp with a peak wavelength of 450nm as a point light source. The backlight unit is placed on the light diffusion plate facing upward, and a spectroradiometer ("SR-UL1R" manufactured by Topcon Co., Ltd.) is set at a height of 60cm from the surface of the light diffusion plate. A wavelength conversion layer formed on a glass substrate or a laminate of a wavelength conversion layer and a protective layer formed on a glass substrate is used as a measurement sample, and the measurement sample is arranged on the surface of the light diffusion plate with the wavelength conversion layer or the laminate facing upward. In this state, the backlight is turned on, and the spectroradiometer is used to measure the spectroradiometer spectrum of the light emitted from the wavelength conversion layer or the laminate, and the luminous intensity EI (μW) of the maximum peak wavelength of the green luminous peak is calculated based on the spectrum.

[0613] The maximum peak wavelength of the green emission peak is the maximum peak wavelength of the green emission peak in the emission spectrum of the semiconductor particles (A) contained in the wavelength conversion layer, which is 530 nm. The full width at half maximum of the green emission peak is 42 nm.

[0614] The emission spectrum of the semiconductor particles (A) was measured using an absolute PL quantum yield measuring apparatus ("C9920-02" manufactured by Hamamatsu Photonics, excitation light 450 nm, room temperature, atmospheric air) using a dispersion of the semiconductor particles (A) diluted so that the absorbance at a wavelength of 450 nm was 0.4 as a measurement sample.

[0615] (3) Determination of weight average molecular weight (Mw) of resin

[0616] The polystyrene-equivalent weight average molecular weight (Mw) of the resin (C) can be measured by the GPC method under the following conditions.

[0617] Equipment: HLC-8120GPC (Tosoh Corporation)

[0618] Column: TSK-GELG2000HXL

[0619] Column temperature: 40°C

[0620] Solvent: Tetrahydrofuran

[0621] Flow rate: 1.0mL / min

[0622] Solid content concentration of the analysis sample: 0.001 to 0.01 mass%

[0623] Injection volume: 50μL

[0624] Detector: RI

[0625] Calibration standard substances: TSK STANDARD POLYSTYRENE F-40, F-4, F-288, A-2500, A-500 (manufactured by Tosoh Corporation)

[0626] <Synthesis Example 1: Synthesis of Resin (C1)>

[0627] An appropriate amount of nitrogen gas was flowed into a flask equipped with a reflux cooler, a dropping funnel, and a stirrer to replace the atmosphere with nitrogen, and 80 parts of propylene glycol monomethyl ether acetate (PGMEA) was added and heated to 85°C while stirring. Next, a mixed solution prepared by dissolving 6 parts of methacrylic acid, 25 parts of dicyclopentyl methacrylate, 40 parts of methyl methacrylate, and 29 parts of 1-[2-(acryloyloxy)ethyl] succinate in 20 parts of PGMEA was dripped into the flask over 4 hours. On the other hand, a solution prepared by dissolving 9 parts of a polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) in 40 parts of PGMEA was dripped over 5 hours. After the dripping of the initiator solution was completed, it was kept at 85°C for 4 hours and then cooled to room temperature to obtain a copolymer (resin (C1)) solution. The solid content of the resin (C1) solution was 40%, and the weight average molecular weight Mw was 11500.

[0628] <Synthesis Example 2: Synthesis of Resin (C2)>

[0629] An appropriate amount of nitrogen gas was introduced into a flask equipped with a reflux cooler, a dropping funnel and a stirrer to replace the atmosphere with nitrogen, and 371 parts of PGMEA was added and heated to 85°C while stirring. Next, 54 parts of acrylic acid and 3,4-epoxytricyclo[5.2.10 2,6 ]decane-8-yl ester and 3,4-epoxytricyclo[5.2.10 2,6 A mixed solution prepared by dissolving 225 parts of a mixture of decane-9-yl ester (containing a molar ratio of 50:50) and 81 parts of vinyltoluene (isomer mixture) in 80 parts of PGMEA was added dropwise to the flask over 4 hours. On the other hand, a solution prepared by dissolving 30 parts of a polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) in 160 parts of PGMEA was added dropwise over 5 hours. After the addition of the initiator solution was completed, it was kept at 85°C for 4 hours and then cooled to room temperature to obtain a copolymer (resin (C2)) solution. The solid content of the resin (C2) solution was 37%, and the weight average molecular weight Mw was 10600.

[0630] <Preparation Example 1: Preparation of Semiconductor Particle (A1) Dispersion Liquid>

[0631] A toluene dispersion a of semiconductor particles (A1) (green luminescent InP / ZnSeS quantum dots) containing oleic acid as an organic ligand (G1) was prepared. As described above, the maximum peak wavelength of the green luminescent peak of the quantum dots was 530 nm, and the full width at half maximum of the green luminescent peak was 42 nm.

[0632] Toluene was removed from the toluene dispersion a by vacuum distillation, and then 70 parts of cyclohexyl acetate (J3) were added to 30 parts of the total amount of semiconductor particles (A1) and organic ligand (G1) to obtain semiconductor particle (A1) dispersion b. The composition of semiconductor particle (A1) dispersion b is shown in Table 1.

[0633] [Table 1]

[0634]

[0635] The composition ratio of the semiconductor particles (A1) to the organic ligand (G1) was determined by TG-DTA measurement. The remaining amount when the mixture was heated to 550°C at a heating rate of 5°C / min after toluene was removed was measured and the remaining amount was calculated as the weight of the organic ligand (G1).

[0636] <Preparation Example 2: Preparation of Composition (I) for Forming Wavelength Conversion Layer>

[0637] The semiconductor particle (A1) dispersion liquid b was mixed with the components shown in Table 2 to prepare a wavelength conversion layer-forming composition (I). In Table 2, the number of parts of the components other than the solvent (J) is expressed in terms of solid content.

[0638] [Table 2]

[0639]

[0640] The details of the abbreviations of the components shown in Table 2 are as follows.

[0641] Light scattering agent (B1): In the preparation of composition (I), 10 parts of resin C1 (solid content conversion) and 30 parts of PGMEA were mixed with 60 parts of titanium oxide particles, and the titanium oxide particles were fully dispersed using a bead mill. The number of parts of light scattering agent (B1) listed in Table 2 is the number of parts of titanium oxide particles.

[0642] Polymerizable compound (D1): Carboxyl group-containing polyfunctional (meth)acrylate (trade name "Aronix M-510" manufactured by Toagosei Co., Ltd.)

[0643] Polymerization initiator (E1): "Irgacure (registered trademark) OXE-02" manufactured by BASF

[0644] Antioxidant (F1): Sumitomo Chemical Co., Ltd., trade name "Sumilizer GP"

[0645] Leveling agent (H1): polyether-modified silicone oil (trade name "Toraysilicone SH8400" manufactured by Toray Dow Corning Co., Ltd.)

[0646] Solvent (J1): Propylene glycol monomethyl ether acetate (PGMEA)

[0647] <Examples 1 to 6, Comparative Examples 1 and 2: Preparation of protective layer-forming composition (II)>

[0648] The components shown in Table 3 were mixed to obtain protective layer-forming compositions (II-1) to (II-8). In Table 3, the number of parts of the resin indicates a value based on solid content.

[0649] Table 3

[0650]

[0651] The details of the abbreviations of the components shown in Table 3 are as follows.

[0652] Polyfunctional polymerizable compound (K1): Carboxyl group-containing polyfunctional (meth)acrylate (trade name "Aronix M-510" manufactured by Toagosei Co., Ltd.)

[0653] Polyfunctional polymerizable compound (K2): Carboxyl group-containing polyfunctional (meth)acrylate (trade name "Aronix M-520D" manufactured by Toagosei Co., Ltd.)

[0654] Polyfunctional polymerizable compound (K3): trimethylolpropane triacrylate (trade name "NK Ester A-TMPT" manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0655] Polyfunctional polymerizable compound (K4): dipentaerythritol hexaacrylate (trade name "KAYARAD (registered trademark) DPHA" manufactured by Nippon Kayaku Co., Ltd.)

[0656] Monofunctional polymerizable compound (M1): 2-ethylhexyl acrylate

[0657] Monofunctional polymerizable compound (M2): 2-hydroxyethyl acrylate

[0658] Polymerization initiator (E2): N-benzoyloxy-1-(4-phenylthiophenyl)octan-1-one-2-imine (trade name "Irgacure (registered trademark) OXE-01" manufactured by BASF)

[0659] <Example 7>

[0660] The composition (I) for forming a wavelength conversion layer was applied to a 5 cm square glass substrate ("Eagle XG" manufactured by Corning) by spin coating so that the thickness of the layer after post-baking was 3 μm, and then pre-baked at 100°C for 3 minutes to form a composition layer. The substrate with the composition layer formed thereon was exposed to light at 80 mJ / cm in an air atmosphere using an exposure machine ("TME-150RSK" manufactured by Topcon Corporation). 2 The wavelength conversion layer was formed by irradiating with an exposure amount (365 nm reference) of 1.5 % and developing, and then post-baking was performed at 180°C for 30 minutes. The luminous intensity of the obtained wavelength conversion layer (luminous intensity before lamination of the protective layer) EI b Carry out determination.

[0661] Next, the protective layer-forming composition (II-1) was applied on the wavelength conversion layer by spin coating so that the thickness of the layer after post-baking was 1 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate on which the composition layer was formed was exposed to light at 100 mJ / cm2 in an air atmosphere using an exposure machine (“TME-150RSK” manufactured by Topcon Corporation). 2 The light was irradiated with an exposure amount of 100 nm (365 nm reference) and post-baked at 180° C. for 30 minutes to form a laminate of a wavelength conversion layer and a protective layer. The luminous intensity of the obtained laminate (luminous intensity after the protective layer was laminated) EI a The measurement was performed and the maintenance rate of the emission intensity EI before and after lamination of the protective layer was calculated according to the following formula.

[0662] The maintenance rate of the luminous intensity EI before and after the protective layer is stacked (%) = [EI a / EI b ]×100

[0663] <Examples 8 to 12>

[0664] A laminate of a wavelength conversion layer and a protective layer was formed in the same manner as in Example 7 except that protective layer-forming compositions (II-2) to (II-6) were used instead of protective layer-forming composition (II-1), and the maintenance rate of emission intensity EI before and after lamination of the protective layer was determined. The results are shown in Table 4.

[0665] <Comparative Example 3>

[0666] A wavelength conversion layer was formed on a glass substrate in the same manner as in Example 7, and the emission intensity of the wavelength conversion layer (the emission intensity before the protective layer formation step) was measured. bNext, without applying the protective layer forming composition, the film was baked at 100°C for 3 minutes, and then an exposure machine (TME-150RSK manufactured by Topcon Corporation) was used to expose the film at 100 mJ / cm 2 The laminate was irradiated with an exposure amount (365 nm reference) and then baked at 180°C for 30 minutes. In this way, a wavelength conversion layer was obtained that had undergone the same process as the protective layer formation process, except that the protective layer forming composition was not applied. The luminescence intensity of the obtained laminate (luminescence intensity after the protective layer formation process) EI was measured. a The maintenance rate of the luminous intensity EI before and after the protective layer forming step was calculated according to the following formula. The results are shown in Table 4.

[0667] The maintenance rate of the luminous intensity EI before and after the protective layer formation step (%) = [EI a / EI b ]×100

[0668] <Comparative Examples 4 and 5>

[0669] A laminate of a wavelength conversion layer and a protective layer was formed in the same manner as in Example 7 except that the protective layer-forming composition (II-7) or (II-8) was used instead of the protective layer-forming composition (II-1), and the maintenance rate of the emission intensity EI before and after the protective layer was determined. The results are shown in Table 4.

[0670] [Table 4]

[0671] Composition for forming protective layer (II) Luminous intensity EI maintenance rate (%) Example 7 II-1 94 Example 8 II-2 95 Example 9 II-3 90 Example 10 II-4 91 Embodiment 11 II-5 96 Example 12 II-6 98 Comparative Example 3 none 86 Comparative Example 4 II-7 88 Comparative Example 5 II-8 88

[0672] Explanation of symbols

[0673] 10 wavelength conversion layer, 11 first wavelength conversion layer, 12 second wavelength conversion layer, 20 protective layer, 21 first protective layer, 22 second protective layer, 30 light absorption layer, 40 blue light source.

Claims

1. A composition for forming a protective layer disposed on a wavelength conversion layer containing light-emitting inorganic semiconductor particles, The composition does not contain luminescent inorganic semiconductor particles, Furthermore, it includes a polyfunctional polymerizable compound having two or more ethylenically unsaturated bonds in the molecule or a polymer thereof.

2. The composition according to claim 1, wherein The polyfunctional polymerizable compound is a polyfunctional (meth)acrylic compound.

3. The composition according to claim 1, wherein The multifunctional polymerizable compound has an acidic functional group.

4. The composition according to claim 1, wherein The polyfunctional polymerizable compound has three or more ethylenically unsaturated bonds in the molecule. 5 . A protective layer formed from the composition according to claim 1 .

6. A laminate comprising: a wavelength conversion layer containing luminescent inorganic semiconductor particles, and The protective layer according to claim 5 is disposed on the wavelength conversion layer.

7. A display device comprising the laminated body according to claim 6.