A method for preparing an inverted light emitting diode and an inverted light emitting diode

By using technical means such as BOE corrosion liquid and metal reflective layer in flipped light emitting diode chips, the high voltage and heating problems after ICP etching are solved, and the product quality and reliability are improved.

CN118825156BActive Publication Date: 2024-12-06JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411296398.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

Before preparing the connecting electrode, the existing flip-emitting diode chips will remove the current barrier layer on the conductive steps of the N-type semiconductor layer, resulting in high voltage and concentrated heating, affecting product quality.

Method used

The BOE corrosion solution is used to corrode the through hole of the Bragg reflective layer to form the through hole of the current barrier layer and the Bragg reflective layer in the P-type region, and then the AL203 and SiO2 films are deposited on the epitaxial layer. The first insulating layer is formed, and then a through hole is formed on the first insulating layer to prepare the contact electrode, and the connecting electrode and the second insulating layer are deposited on the contact electrode, and the current on the conductive steps of the N-type semiconductor layer is removed by BOE wet corrosion. Barrier layer, evaporated contact and connection electrodes to solve high voltage and heating problems.

Benefits of technology

It effectively solves the high voltage and heating problems after ICP etching, and improves the quality and reliability of flip-floped light-emitting diodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825156B_ABST
    Figure CN118825156B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an inverted light emitting diode and an inverted light emitting diode, the preparation method comprising: providing a substrate, and depositing an epitaxial layer on the surface of the substrate, the epitaxial layer comprising an N-type semiconductor layer, an active light emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate; forming an N-type semiconductor layer conductive step in a partial area of ​​the epitaxial layer surface, and preparing a current expansion layer in the remaining area; preparing a current blocking layer and a Bragg reflection layer on the surface of the epitaxial layer, and then etching to form a Bragg reflection layer through hole and a current blocking layer through hole, preparing a metal reflection layer and a first insulating layer on the epitaxial layer, using a BOE etching solution to treat a part of the first insulating layer, forming a first insulating layer through hole, and then preparing a contact electrode; depositing a connecting electrode, a second insulating layer, and a pad layer on the contact electrode to obtain a target inverted light emitting diode. The inverted light emitting diode prepared by the present application has low internal voltage and less heat generation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of optoelectronic technology, and in particular to a method for preparing an inverted light emitting diode and the inverted light emitting diode. Background Art

[0002] Flip-chip LED chips are widely used due to their advantages such as back-emitting light, strong heat dissipation, good weldability, large thrust, and strong reliability. Initially, people used Bragg reflectors as reflectors to enable flip-chip LEDs to emit light from the back. In recent years, people have begun to add Bragg reflector layers to the Bragg reflectors to improve the reflection effect of the reflectors, and ultimately improve the external quantum efficiency of flip-chip LED chips.

[0003] Before preparing the connection electrodes of the existing flip-chip light-emitting diode chips, it is necessary to use the ICP (Inductively Coupled Plasma) etching process to remove the current blocking layer on the conductive steps of the N-type semiconductor layer. However, after the ICP etching process removes the current blocking layer on the conductive steps of the N-type semiconductor layer, high voltage will be generated, resulting in concentrated heat around the conductive steps of the N-type semiconductor layer, affecting product quality. Summary of the invention

[0004] Based on this, the purpose of the present invention is to provide a method for preparing a flip-chip light emitting diode and a flip-chip light emitting diode to solve the problems existing in the prior art.

[0005] The present invention provides a method for preparing a flip-chip light-emitting diode, comprising the following steps:

[0006] S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer comprises an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate;

[0007] S20, etching a portion of the surface area of ​​the epitaxial layer to a depth as deep as the N-type semiconductor layer to obtain a conductive step of the N-type semiconductor layer to form an N-type region on the epitaxial layer, and preparing a current spreading layer on other unetched areas on the surface of the epitaxial layer to form a P-type region on the epitaxial layer;

[0008] S30, preparing a current blocking layer and a Bragg reflection layer on the surfaces of the N-type region and the P-type region, and etching the Bragg reflection layer to form a Bragg reflection layer through hole on the Bragg reflection layer;

[0009] S40, using a BOE etching solution to perform etching in the Bragg reflective layer through hole to form a current blocking layer through hole on the current blocking layer, preparing a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region, and preparing an AL203 film and a SiO2 film on the epitaxial layer after the metal reflective layer is prepared to obtain a first insulating layer, wherein the temperature for preparing the SiO2 film is greater than the temperature for preparing the AL203 film, and the temperature difference is above 100° C.;

[0010] S50, treating a portion of the first insulating layer with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, and preparing a contact electrode in the first insulating layer through hole, wherein the ratio of the thickness of the contact electrode to the depth of the first insulating layer is less than 1:4;

[0011] S60, depositing a connection electrode on the contact electrode, and preparing a second insulating layer and a pad layer on the surface of the epitaxial layer after the connection electrode is deposited, so as to obtain a target flip-chip light emitting diode.

[0012] Preferably, the step of etching a partial area of ​​the surface of the epitaxial layer to a depth reaching the N-type semiconductor layer to obtain a conductive step of the N-type semiconductor layer to form an N-type region on the epitaxial layer, and preparing a current spreading layer on other unetched areas on the surface of the epitaxial layer to form a P-type region on the epitaxial layer comprises:

[0013] Coating a photoresist on the surface of the P-type semiconductor layer, then exposing and developing to remove a portion of the photoresist and expose a portion of the P-type semiconductor layer;

[0014] Performing ICP etching on the exposed P-type semiconductor layer, removing the exposed P-type semiconductor layer and the active light-emitting layer at the bottom thereof in sequence, and then removing the remaining photoresist on the P-type semiconductor layer to obtain an N-type semiconductor layer conductive step, so as to form an N-type region on the epitaxial layer;

[0015] Depositing an indium tin oxide layer on the surface of the epitaxial layer forming the N-type region and the remaining P-type semiconductor layer by a magnetron sputtering process, coating the indium tin oxide layer with a photoresist, exposing and developing to remove a portion of the photoresist, and exposing the indium tin oxide layer on the N-type region;

[0016] An indium tin oxide etching solution is used to remove the exposed indium tin oxide layer, and then the remaining photoresist on the indium tin oxide layer is removed, a current spreading layer is prepared on the P-type semiconductor layer, and a P-type region is formed on the epitaxial layer.

[0017] Preferably, the steps of preparing a current blocking layer and a Bragg reflection layer on the surfaces of the N-type region and the P-type region, and etching the Bragg reflection layer to form a Bragg reflection layer through hole on the Bragg reflection layer include:

[0018] Depositing SiO2 as a current blocking layer on the surface of the N-type region and the P-type region by using a PECVD process;

[0019] Using electron beam evaporation technology to alternately evaporate several cycles of TiO2 and SiO2 stacked layers on the surface of the current blocking layer as a Bragg reflection layer, the cycle of the alternating evaporation of TiO2 and SiO2 is 2-10;

[0020] Coating a photoresist on the Bragg reflection layer, then exposing and developing to remove the photoresist on a portion of the Bragg reflection layer, and removing the exposed Bragg reflection layer by an inductively coupled plasma etching process to form a Bragg reflection layer through hole on the Bragg reflection layer;

[0021] The Bragg reflection layer through holes include an N-type Bragg reflection layer through hole located in the N-type region and a P-type Bragg reflection layer through hole located in the P-type region.

[0022] Preferably, the step of using BOE etching solution to perform etching in the Bragg reflective layer through hole to form a current blocking layer through hole on the current blocking layer, preparing a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region, and preparing an AL203 film and a SiO2 film on the epitaxial layer after the metal reflective layer is prepared to obtain a first insulating layer comprises:

[0023] Coating photoresist on the surface of the Bragg reflection layer and the through hole of the Bragg reflection layer, and then removing part of the photoresist in the through hole of the Bragg reflection layer by exposure and development to expose the current blocking layer under the through hole of the Bragg reflection layer;

[0024] Using BOE etching solution to remove the exposed current blocking layer to form current blocking layer through holes on the current blocking layer, wherein the current blocking layer through holes include N-type current blocking layer through holes located in the N-type region and P-type current blocking layer through holes located in the P-type region;

[0025] Coating photoresist on the surface of the epitaxial layer forming the current blocking layer through hole, and then removing the photoresist on the P-type region by exposure and development;

[0026] Using an electron beam evaporation process to sequentially evaporate Ag / Ni / Ti / Pt / Ti metals on the surface of the epitaxial layer as a metal reflective layer, using a blue film stripping process to remove the metal on the remaining photoresist, and then removing the photoresist to prepare a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region;

[0027] An AL203 film is prepared on the metal reflective layer and the surface not covered by the metal reflective layer by atomic layer deposition, and then a SiO2 film is prepared on the AL203 film by PECVD process to obtain a first insulating layer.

[0028] Preferably, the temperature for preparing the AL203 film is 150°C-200°C, and the temperature for preparing the SiO2 film is 270°C-300°C.

[0029] Preferably, the step of treating a portion of the first insulating layer with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, and preparing a contact electrode in the first insulating layer through hole comprises:

[0030] Coating a positive photoresist on the first insulating layer, then exposing and developing the positive photoresist to form a photoresist opening, exposing the first insulating layer below the photoresist opening;

[0031] The first insulating layer is exposed by etching with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, wherein the size of the first insulating layer through hole is larger than the size of the photoresist opening;

[0032] Depositing a metal layer on the surface of the epitaxial layer after forming the through hole of the first insulating layer by electron beam evaporation process, wherein the metal layer is a Cr / Al / Ti stacked layer or a Cr / Ag / Ni stacked layer;

[0033] The metal layer on the photoresist is removed by a blue film stripping process, and finally the remaining photoresist is removed to prepare contact electrodes in the through holes of the first insulating layer, wherein the contact electrodes include an N-type contact electrode located in the N-type region and a P-type contact electrode located in the P-type region.

[0034] Preferably, the angle between the side and bottom of the photoresist opening is greater than 80°, the angle between the side and bottom of the first insulating layer through hole is less than 20°, the edge of the first insulating layer through hole is not less than 2μm away from the edge of the photoresist opening, the thickness of the Al layer in the Cr / Al / Ti stack is greater than 0.1μm, and the thickness of the Ag layer in the Cr / Ag / Ni stack is greater than 0.1μm.

[0035] Preferably, the step of depositing a connecting electrode on the contact electrode comprises:

[0036] Coating a negative photoresist on the first insulating layer and the contact electrode, and then exposing and developing to remove a portion of the photoresist;

[0037] Using electron beam evaporation process, AL / Ti / Pt / Ti / Ni / Ti metals are sequentially deposited on the surface of the epitaxial layer as connecting electrodes, and finally the remaining photoresist is removed;

[0038] Wherein, the connection electrodes include an N-type connection electrode located in the N-type region and a P-type connection electrode located in the P-type region.

[0039] Preferably, the step of preparing a second insulating layer and a pad layer on the surface of the epitaxial layer after depositing the connecting electrode comprises:

[0040] Using PECVD process to deposit SiO2 as the second insulating layer on the surface of the epitaxial layer after the connection electrode is prepared;

[0041] Coating a negative photoresist on the surface of the second insulating layer, then exposing and developing to remove a portion of the negative photoresist, exposing the second insulating layer below the negative photoresist;

[0042] The exposed second insulating layer is removed by using BOE etching solution, the second insulating layer is through-hole, and then Al / Ti / Al / Ni / AuSn metals are sequentially evaporated as pad layers by electron beam evaporation process;

[0043] The pad layer includes an N-type pad layer located in the N-type region and a P-type pad layer located in the P-type region.

[0044] The present application also provides a flip-chip light emitting diode, which is prepared using the above-mentioned flip-chip light emitting diode preparation method.

[0045] The beneficial effects of the present invention are as follows: the method for preparing a flip-chip light-emitting diode provided by the present application first provides a substrate, and deposits an epitaxial layer on the surface of the substrate; prepares an N-type semiconductor layer conductive step and a current expansion layer on the surface of the epitaxial layer; then prepares a current blocking layer and a Bragg reflection layer on the surface of the epitaxial layer; after forming through holes on the current blocking layer and the Bragg reflection layer, prepares a metal reflection layer and a first insulating layer, then etches the first insulating layer, forms an insulating layer through hole, and then prepares a contact electrode, then prepares a connecting electrode, a second insulating layer and a pad layer on the contact electrode, and the diode is turned on from top to bottom. The present application removes part of the current blocking layer on the conductive step of the N-type semiconductor layer through a BOE wet etching process, then evaporates the contact electrode in the current blocking layer through hole on the conductive step of the N-type semiconductor layer, and then evaporates the connecting electrode; evaporates the contact electrode between the conductive step of the N-type semiconductor layer and the connecting electrode, so as to solve the problems of high voltage and concentrated heat around the conductive step of the N-type semiconductor layer caused by etching the current blocking layer in the existing method for preparing a flip-chip light-emitting diode chip.

[0046] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1A flow chart of the method for preparing a flip-chip light-emitting diode provided by the present invention;

[0048] Figure 2 is a schematic diagram of the cross-sectional structure of a diode after an epitaxial layer is deposited on a substrate;

[0049] Figure 3 for Figure 2 A schematic diagram of the cross-sectional structure of a diode after the current spreading layer is prepared;

[0050] Figure 4 for Figure 3 A schematic diagram of the cross-sectional structure of a diode after the Bragg reflection layer is prepared;

[0051] Figure 5 for Figure 4 A schematic diagram of the cross-sectional structure of a diode after the through hole of the Bragg reflection layer is prepared;

[0052] Figure 6 for Figure 5 A schematic diagram of the cross-sectional structure of a diode after preparing a through hole in the current blocking layer;

[0053] Figure 7 for Figure 6 A schematic diagram of the cross-sectional structure of a diode after the metal reflective layer is prepared;

[0054] Figure 8 for Figure 7 A schematic diagram of the cross-sectional structure of a diode after the first insulating layer is prepared;

[0055] Fig. 9 for Figure 8 A schematic diagram of the cross-sectional structure of a diode after coating with positive photoresist;

[0056] Fig.10 for Fig. 9 A schematic diagram of the cross-sectional structure of a diode after preparing a photoresist opening;

[0057] Fig.11 for Fig.10 A schematic diagram of the cross-sectional structure of a diode after preparing a through hole in the first insulating layer;

[0058] Fig.12 for Fig.11 A schematic diagram of the partially enlarged structure at center A;

[0059] Fig.13 for Fig.11 A schematic diagram of the cross-sectional structure of a diode after the contact electrode is prepared;

[0060] Fig.14 for Fig.13 A schematic diagram of the cross-sectional structure of a diode after preparing the connection electrodes;

[0061] Fig.15 for Fig.14 A schematic diagram of the cross-sectional structure of the diode after the second insulating layer is prepared;

[0062] Fig.16 for Fig.15 A schematic diagram of the cross-sectional structure of the diode after preparing the through hole of the second insulating layer;

[0063] Fig.17 for Fig.16 Schematic diagram of the cross-sectional structure of the diode after preparing the pad layer.

[0064] Description of main component symbols:

[0065] 10. substrate; 111. N-type semiconductor layer; 112. active light emitting layer; 113. P-type semiconductor layer; 114. N-type semiconductor layer conductive step; 12. current spreading layer; 13. current blocking layer; 131. P-type current blocking layer through hole; 132. N-type current blocking layer through hole; 14. Bragg reflection layer; 141. P-type Bragg reflection layer through hole; 142. N-type Bragg reflection layer through hole; 15. metal reflection layer; 16. first insulating layer; 16 1. P-type first insulating layer through hole; 162. N-type first insulating layer through hole; 17. Positive photoresist; 171. P-type photoresist opening; 172. N-type photoresist opening; 181. P-type contact electrode; 182. N-type contact electrode; 191. P-type connecting electrode; 192. N-type connecting electrode; 20. Second insulating layer; 201. P-type second insulating layer through hole; 202. N-type second insulating layer through hole; 211. P-type pad layer; 212. N-type pad layer.

[0066] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0067] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0068] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0069] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing optional embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0070] Example 1

[0071] The present invention provides a method for preparing a flip-chip light-emitting diode, such as Figure 1 As shown, the method for preparing a flip-chip light-emitting diode includes S10 to S60:

[0072] S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer comprises an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate;

[0073] In a specific implementation, the epitaxial layer can be deposited by metal chemical vapor deposition (MOCVD), such as Figure 2 As shown, an N-type semiconductor layer 111, an active light-emitting layer 112, and a P-type semiconductor layer 113 are sequentially prepared on a substrate 10, and the substrate may be one of GaN, Al2O3, and Si.

[0074] S20, etching a portion of the surface area of ​​the epitaxial layer to a depth as deep as the N-type semiconductor layer to obtain a conductive step of the N-type semiconductor layer to form an N-type region on the epitaxial layer, and preparing a current spreading layer on other unetched areas on the surface of the epitaxial layer to form a P-type region on the epitaxial layer;

[0075] Optionally, S20 specifically includes:

[0076] Applying photoresist on the surface of the P-type semiconductor layer 113, and then removing part of the photoresist by exposure and development to expose part of the P-type semiconductor layer;

[0077] The exposed P-type semiconductor layer is subjected to ICP etching to sequentially remove the exposed P-type semiconductor layer and the active light-emitting layer at the bottom thereof, and then the remaining photoresist on the P-type semiconductor layer is removed to obtain an N-type semiconductor layer conductive step 114, thereby forming an N-type region. Figure 2 As shown;

[0078] Depositing an indium tin oxide layer on the surface of the epitaxial layer forming the N-type region and the remaining P-type semiconductor layer by a magnetron sputtering process, coating the indium tin oxide layer with a photoresist, exposing and developing to remove a portion of the photoresist, and exposing the indium tin oxide layer on the N-type region;

[0079] The exposed indium tin oxide layer is removed by using an indium tin oxide etching solution, and then the remaining photoresist on the indium tin oxide layer is removed, and a current spreading layer 12 is prepared on the P-type semiconductor layer to form a P-type region, such as Figure 3 shown.

[0080] S30, preparing a current blocking layer and a Bragg reflection layer on the surfaces of the N-type region and the P-type region, and etching the Bragg reflection layer to form a Bragg reflection layer through hole on the Bragg reflection layer;

[0081] Optionally, S30 specifically includes:

[0082] Depositing SiO2 as a current blocking layer 13 on the surface of the N-type region and the P-type region by using a PECVD process;

[0083] The electron beam evaporation process is used to alternately evaporate several cycles of TiO2 and SiO2 stacked layers on the surface of the current blocking layer as the Bragg reflection layer 14, and the cycle of the alternate evaporation of TiO2 and SiO2 is 2-10. Figure 4 As shown;

[0084] Coating a photoresist on the Bragg reflection layer, then exposing and developing to remove the photoresist on a portion of the Bragg reflection layer, and removing the exposed Bragg reflection layer by an inductively coupled plasma etching process to form a Bragg reflection layer through hole on the Bragg reflection layer;

[0085] The Bragg reflection layer through hole includes an N-type Bragg reflection layer through hole 142 located in the N-type region and a P-type Bragg reflection layer through hole 141 located in the P-type region. Figure 5 shown.

[0086] S40, using a BOE etching solution to perform etching in the Bragg reflective layer through hole to form a current blocking layer through hole on the current blocking layer, preparing a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region, and preparing an AL203 film and a SiO2 film on the epitaxial layer after the metal reflective layer is prepared to obtain a first insulating layer, wherein the temperature for preparing the SiO2 film is greater than the temperature for preparing the AL203 film, and the temperature difference is above 100° C.;

[0087] Optionally, S40 specifically includes:

[0088] Coating photoresist on the surface of the Bragg reflection layer and the through hole of the Bragg reflection layer, and then removing part of the photoresist in the through hole of the Bragg reflection layer by exposure and development to expose the current blocking layer under the through hole of the Bragg reflection layer;

[0089] The exposed current blocking layer 13 is removed by using a BOE (Buffered Oxide Etch) etching solution to form a current blocking layer through hole on the current blocking layer, wherein the current blocking layer through hole includes an N-type current blocking layer through hole 132 located in the N-type region and a P-type current blocking layer through hole 131 located in the P-type region, such as Figure 6 shown.

[0090] Coating photoresist on the surface of the epitaxial layer forming the current blocking layer through hole, and then removing the photoresist on the P-type region by exposure and development;

[0091] Ag / Ni / Ti / Pt / Ti metals are sequentially deposited on the surface of the epitaxial layer by electron beam evaporation process as a metal reflective layer 15, and the metal on the remaining photoresist is removed by blue film stripping process, and then the photoresist is removed to prepare a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region, such as Figure 7 As shown;

[0092] An AL203 film is prepared on the metal reflective layer and the surface not covered by the metal reflective layer by atomic layer deposition, and then a SiO2 film is prepared on the AL203 film by PECVD process to obtain a first insulating layer 16. In this embodiment, the thickness of the first insulating layer 16 can be determined according to the thickness of the contact electrode; Figure 8 shown.

[0093] Optionally, in this implementation, the temperature for preparing the AL203 film is 150℃-200℃, the temperature for preparing the SiO2 film is 270℃-300℃, and the temperature for preparing the SiO2 film is greater than the temperature for preparing the AL203 film, and the temperature difference is above 100℃; in this embodiment, the temperature for preparing the SiO2 film is greater than the temperature for preparing the AL203 film, and the temperature difference is above 100℃, and in the subsequent BOE etching process of the prepared first insulating layer, the etching rates of the AL203 film and the SiO2 film are matched to obtain a first insulating layer through hole with a smooth slope.

[0094] S50, treating a portion of the first insulating layer with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, and preparing a contact electrode in the first insulating layer through hole, wherein the ratio of the thickness of the contact electrode to the depth of the first insulating layer is less than 1:4;

[0095] Optionally, S50 specifically includes:

[0096] A positive photoresist 17 is coated on the first insulating layer. Fig. 9As shown, the positive photoresist is then exposed and developed to form a photoresist opening, exposing the first insulating layer located below the photoresist opening, as shown in FIG. Fig.10 As shown, the photoresist openings include an N-type photoresist opening 172 and a P-type photoresist opening 171;

[0097] The first insulating layer is exposed by etching with BOE etching solution to form a first insulating layer through hole on the first insulating layer. The size of the first insulating layer through hole is larger than the size of the photoresist opening. During the etching process, the through hole will extend to both sides of the first insulating layer 16. Fig.11 and Fig.12 As shown, the first insulating layer through hole includes an N-type first insulating layer through hole 162 and a P-type first insulating layer through hole 161;

[0098] Depositing a metal layer on the surface of the epitaxial layer after forming the through hole of the first insulating layer by electron beam evaporation process, wherein the metal layer is a Cr / Al / Ti stacked layer or a Cr / Ag / Ni stacked layer;

[0099] like Fig.13 As shown, the metal layer on the photoresist is removed by a blue film stripping process, and finally the remaining photoresist is removed to prepare contact electrodes in the through holes of the first insulating layer, wherein the contact electrodes include an N-type contact electrode 182 located in the N-type region and a P-type contact electrode 181 located in the P-type region, as shown in FIG. Fig.14 shown.

[0100] Optionally, in this embodiment, the angle between the side and bottom of the photoresist opening is greater than 80°, so that the angle between the side and bottom of the first insulating layer through hole after corrosion is less than 20°, and the ratio of the thickness of the contact electrode to the depth of the first insulating layer is less than 1:4, that is, the distance between the contact electrode and the photoresist opening is relatively large; so that when the contact electrode is evaporated, it is easier for metal molecules to grow from both ends into the through hole of the first insulating layer; the corrosion rates of the AL203 film and the SiO2 film are adapted to each other, so that the edge of the through hole of the first insulating layer is not less than 2μm away from the edge of the photoresist opening, so as to ensure that the first insulating layer is completely corroded in the vertical direction, the thickness of the Al layer in the Cr / Al / Ti stack is greater than 0.1μm, and the thickness of the Ag layer in the Cr / Ag / Ni stack is greater than 0.1μm.

[0101] S60, depositing a connection electrode on the contact electrode, and preparing a second insulating layer and a pad layer on the surface of the epitaxial layer after the connection electrode is deposited, so as to obtain a target flip-chip light emitting diode.

[0102] Optionally, S60 specifically includes:

[0103] Coating a negative photoresist on the first insulating layer and the contact electrode, and then exposing and developing to remove a portion of the photoresist;

[0104] Using electron beam evaporation process, AL / Ti / Pt / Ti / Ni / Ti metals are sequentially deposited on the surface of the epitaxial layer as connecting electrodes, and finally the remaining photoresist is removed;

[0105] The connecting electrodes include an N-type connecting electrode 192 located in the N-type region and a P-type connecting electrode 191 located in the P-type region. Fig.15 shown.

[0106] SiO2 is deposited on the surface of the epitaxial layer after the connection electrode is prepared by PECVD process as the second insulating layer 20. Fig.16 As shown;

[0107] Coating a negative photoresist on the surface of the second insulating layer, then exposing and developing to remove a portion of the negative photoresist, exposing the second insulating layer below the negative photoresist;

[0108] The exposed second insulating layer and the second insulating layer through-holes are removed by using BOE etching solution, wherein the second insulating layer through-holes include an N-type second insulating layer through-hole 202 and a P-type second insulating layer through-hole 201; Fig.17 As shown, Al / Ti / Al / Ni / AuSn metals are sequentially evaporated as pad layers using an electron beam evaporation process;

[0109] The pad layer includes an N-type pad layer 212 located in the N-type region and a P-type pad layer 211 located in the P-type region.

[0110] In summary, the method for preparing a flip-chip light-emitting diode provided by the present application first provides a substrate, and deposits an epitaxial layer on the surface of the substrate; prepares an N-type semiconductor layer conductive step and a current expansion layer on the surface of the epitaxial layer; then prepares a current blocking layer and a Bragg reflection layer on the surface of the epitaxial layer; after forming through holes on the current blocking layer and the Bragg reflection layer, a metal reflection layer and a first insulating layer are prepared, and then the first insulating layer is corroded to form an insulating layer through hole and then a contact electrode is prepared, and then a connecting electrode, a second insulating layer and a pad layer are prepared on the contact electrode, and the diode is turned on and off. The present application removes part of the current blocking layer on the conductive step of the N-type semiconductor layer through a BOE wet etching process, and then evaporates the contact electrode in the current blocking layer through hole on the conductive step of the N-type semiconductor layer, and then evaporates the connecting electrode; evaporates the contact electrode between the conductive step of the N-type semiconductor layer and the connecting electrode, so as to solve the problems of high voltage caused by etching the current blocking layer and concentrated heat around the conductive step of the N-type semiconductor layer in the existing method for preparing a flip-chip light-emitting diode chip.

[0111] Example 2

[0112] The present application also provides a flip-chip light emitting diode, which is manufactured using the above-mentioned flip-chip light emitting diode manufacturing method.

[0113] It should be noted that the above implementation process is only to illustrate the feasibility of the present application, but it does not mean that the flip-chip light-emitting diode of the present application has only the above-mentioned implementation processes. On the contrary, as long as the flip-chip light-emitting diode of the present application can be implemented, it can be included in the feasible implementation scheme of the present application. In addition, the structural part in the embodiment of the present invention corresponds to the preparation method part of the present invention, and the specific implementation details are also the same, which will not be repeated here.

[0114] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0115] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.

Claims

1. A method for preparing a flip-chip light-emitting diode, characterized in that: The following steps are involved: S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer includes an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate; S20, etching a portion of the surface of the epitaxial layer to a depth down to the N-type semiconductor layer to obtain a conductive step of the N-type semiconductor layer, thereby forming an N-type region on the epitaxial layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer to form a P-type region on the epitaxial layer; S30, forming a current blocking layer and a Bragg reflective layer on the surfaces of the N-type region and the P-type region, and etching the Bragg reflective layer to form a Bragg reflective layer through hole on the Bragg reflective layer; S40, etching the Bragg reflector through-hole with a BOE etching solution to form a current blocking layer through-hole on the current blocking layer, forming a metal reflective layer on the current blocking layer through-hole in the P-type region and the Bragg reflective layer in the P-type region, and forming an Al2O3 film and a SiO2 film on the epitaxial layer after the metal reflective layer is formed to obtain a first insulating layer, wherein the temperature for forming the SiO2 film is higher than the temperature for forming the Al2O3 film, and the temperature difference is greater than 100° C.; S50, treating a portion of the first insulating layer with a BOE etching solution to form a first insulating layer through-hole on the first insulating layer, and preparing a contact electrode in the first insulating layer through-hole, wherein the ratio of the thickness of the contact electrode to the depth of the first insulating layer is less than 1:4; S60, depositing a connecting electrode on the contact electrode, and preparing a second insulating layer and a pad layer on the surface of the epitaxial layer after the connecting electrode is deposited, so as to obtain a target flip-chip light-emitting diode; The steps of preparing a current blocking layer and a Bragg reflective layer on the surfaces of the N-type region and the P-type region, and etching the Bragg reflective layer to form a Bragg reflective layer through hole on the Bragg reflective layer include: Depositing SiO2 as a current blocking layer on the surfaces of the N-type region and the P-type region using a PECVD process; Using an electron beam evaporation process, a stack of TiO2 and SiO2 layers is alternately deposited on the surface of the current blocking layer in a plurality of cycles as a Bragg reflection layer, wherein the cycle of the TiO2 and SiO2 alternate evaporation is 2-10; Coating a photoresist on the Bragg reflective layer, then exposing and developing to remove a portion of the photoresist on the Bragg reflective layer, and removing the exposed Bragg reflective layer using an inductively coupled plasma etching process to form a Bragg reflective layer through hole on the Bragg reflective layer; Wherein, the Bragg reflective layer through holes include an N-type Bragg reflective layer through hole located in the N-type region and a P-type Bragg reflective layer through hole located in the P-type region; The steps of using a BOE etching solution to perform etching in the Bragg reflective layer through hole to form a current blocking layer through hole on the current blocking layer, forming a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region, and forming an Al2O3 film and a SiO2 film on the epitaxial layer after the metal reflective layer is formed to obtain a first insulating layer include: coating a photoresist on the surface of the Bragg reflective layer and the through hole of the Bragg reflective layer, and then removing a portion of the photoresist in the through hole of the Bragg reflective layer by exposure and development to expose the current blocking layer below the through hole of the Bragg reflective layer; Using a BOE etching solution to remove the exposed current blocking layer to form current blocking layer through holes on the current blocking layer, wherein the current blocking layer through holes include an N-type current blocking layer through hole located in the N-type region and a P-type current blocking layer through hole located in the P-type region; Coating photoresist on the surface of the epitaxial layer forming the current blocking layer through hole, and then exposing and developing to remove the photoresist on the P-type region; Using an electron beam evaporation process, Ag / Ni / Ti / Pt / Ti metals are sequentially deposited on the surface of the epitaxial layer as a metal reflective layer, a blue film stripping process is used to remove the metal located on the remaining photoresist, and then the photoresist is removed to prepare a metal reflective layer on the current blocking layer through hole and the Bragg reflective layer in the P-type region; An Al2O3 film is formed on the metal reflective layer and the surface not covered by the metal reflective layer by atomic layer deposition, and a SiO2 film is formed on the Al2O3 film by PECVD process to obtain a first insulating layer; The step of treating a portion of the first insulating layer with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, and preparing a contact electrode in the first insulating layer through hole comprises: coating a positive photoresist on the first insulating layer, then exposing and developing the positive photoresist to form a photoresist opening, exposing the first insulating layer below the photoresist opening; The first insulating layer is exposed by etching with a BOE etching solution to form a first insulating layer through hole on the first insulating layer, wherein the size of the first insulating layer through hole is larger than the size of the photoresist opening; Depositing a metal layer on the surface of the epitaxial layer after forming the through hole in the first insulating layer by electron beam evaporation, wherein the metal layer is a Cr / Al / Ti stacked layer or a Cr / Ag / Ni stacked layer; The metal layer on the photoresist is removed by a blue film stripping process, and the remaining photoresist is finally removed to prepare contact electrodes in the through holes of the first insulating layer. The contact electrodes include an N-type contact electrode located in the N-type region and a P-type contact electrode located in the P-type region.

2. The method for preparing a flip-chip light-emitting diode according to claim 1, wherein: The step of etching a portion of the surface of the epitaxial layer to a depth down to the N-type semiconductor layer to obtain a conductive step of the N-type semiconductor layer to form an N-type region on the epitaxial layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer to form a P-type region on the epitaxial layer comprises: Coating a photoresist on the surface of the P-type semiconductor layer, then exposing and developing to remove a portion of the photoresist and expose a portion of the P-type semiconductor layer; Performing ICP etching on the exposed P-type semiconductor layer to sequentially remove the exposed P-type semiconductor layer and the active light-emitting layer at the bottom thereof, and then removing the remaining photoresist on the P-type semiconductor layer to obtain an N-type semiconductor layer conductive step, thereby forming an N-type region on the epitaxial layer; Depositing an indium tin oxide layer on the surface of the epitaxial layer forming the N-type region and the remaining P-type semiconductor layer using a magnetron sputtering process, coating the indium tin oxide layer with a photoresist, exposing and developing to remove a portion of the photoresist, and exposing the indium tin oxide layer on the N-type region; An indium tin oxide etching solution is used to remove the exposed indium tin oxide layer, and then the remaining photoresist on the indium tin oxide layer is removed, a current spreading layer is prepared on the P-type semiconductor layer, and a P-type region is formed on the epitaxial layer.

3. The method for preparing a flip-chip light-emitting diode according to claim 1, wherein: The temperature for preparing the AL203 film is 150°C-200°C, and the temperature for preparing the SiO2 film is 270°C-300°C.

4. The method for preparing a flip-chip light-emitting diode according to claim 1, wherein: The angle between the side and bottom of the photoresist opening is greater than 80°, the angle between the side and bottom of the first insulating layer through hole is less than 20°, the edge of the first insulating layer through hole is not less than 2μm away from the edge of the photoresist opening, the thickness of the Al layer in the Cr / Al / Ti stack is greater than 0.1μm, and the thickness of the Ag layer in the Cr / Ag / Ni stack is greater than 0.1μm.

5. The method for preparing a flip-chip light-emitting diode according to claim 1, wherein: The step of depositing a connecting electrode on the contact electrode comprises: coating a negative photoresist on the first insulating layer and the contact electrode, and then exposing and developing to remove a portion of the photoresist; Using electron beam evaporation process, Al / Ti / Pt / Ti / Ni / Ti metals are sequentially deposited on the surface of the epitaxial layer as connecting electrodes, and finally the remaining photoresist is removed; The connecting electrodes include an N-type connecting electrode located in the N-type region and a P-type connecting electrode located in the P-type region.

6. The method for preparing a flip-chip light-emitting diode according to claim 5, wherein: The step of preparing a second insulating layer and a pad layer on the surface of the epitaxial layer after depositing the connecting electrode comprises: Using PECVD process to deposit SiO2 as the second insulating layer on the surface of the epitaxial layer after the connection electrode is prepared; Coating a negative photoresist on the surface of the second insulating layer, then exposing and developing to remove a portion of the negative photoresist, exposing the second insulating layer below the negative photoresist; Use BOE etching solution to remove the exposed second insulating layer, make through holes in the second insulating layer, and then use electron beam evaporation process to sequentially deposit Al / Ti / Al / Ni / AuSn metal as the pad layer; The pad layer includes an N-type pad layer located in the N-type region and a P-type pad layer located in the P-type region.

7. A flip-chip light emitting diode, characterized in that: The flip-chip light-emitting diode is prepared according to the method for preparing the flip-chip light-emitting diode according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • LED (Light Emitting Diode) chip provided with stepped current blocking structure and fabricating method thereof

    CN102751410A

  • Flip light emitting diode chip and preparation method thereof

    CN118588824A