High-performance low-emission composite modified rubber asphalt and preparation method thereof
By using composite modification technology of diatomaceous earth and alcoholic odorant in rubber asphalt, the problems of harmful gas emissions and storage stability during construction are solved, and high and low temperature performance and low emission effects are achieved.
Patent Information
- Application Number
- CN202411297215.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-05
AI Technical Summary
Rubber asphalt emits a large amount of harmful gases during mixing and construction, and has poor storage stability, resulting in health risks and degradation of performance.
The rubber asphalt is compositely modified by diatomaceous earth and alcoholic odorant. Diatomaceous earth is used to adsorb harmful gases and prevent the sedimentation of rubber powder. Alcohol odorant produces macromolecular aromatic hydrocarbons to inhibit harmful gas emissions.
It significantly reduces the harmful gas emissions of rubber asphalt, improves its high and low temperature performance and storage stability, and ensures construction safety and performance optimization.
Smart Images

Figure BDA0005046383440000051 
Figure BDA0005046383440000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road asphalt, and in particular relates to a high-performance, low-emission composite modified rubber asphalt and a preparation method thereof. Background Art
[0002] Using waste rubber powder as an asphalt modifier to prepare rubber asphalt can effectively absorb waste tires and improve asphalt performance. The addition of waste rubber powder can improve the high and low temperature performance of asphalt, improve the deformation resistance and fatigue resistance of asphalt, make rubber asphalt pavement superior to traditional asphalt pavement in terms of performance and service life, and the cost of rubber asphalt pavement can be reduced by about 20% compared with the common SBS modified asphalt pavement. However, despite the many advantages of rubber asphalt, there are still two serious problems that are difficult to solve: serious volatilization of harmful gas pollution and poor storage stability. Rubber asphalt has a high viscosity, and its mixing temperature is usually above 180°C, which causes it to emit a large amount of harmful gases during mixing and construction. In addition, waste rubber powder itself will also volatilize some toxic and irritating gases under high temperature conditions, which greatly affects the health of construction workers and the surrounding people. On the other hand, the solubility parameters of rubber powder and asphalt are different. Rubber powder can only swell in asphalt but cannot be completely dissolved. Phase separation is easy to occur between rubber powder and asphalt, resulting in poor storage stability of rubber asphalt. The higher the amount of rubber powder, the worse the storage stability of rubber asphalt. Therefore, the problems of harmful gas volatilization and storage instability of rubber asphalt need to be solved urgently.
[0003] Researchers at home and abroad often reduce the harmful gas emissions of asphalt by adding inorganic adsorbents or flame retardants, but the addition of these inorganic powders will significantly reduce the low-temperature crack resistance of asphalt. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, wherein the rubber asphalt has excellent high and low temperature performance, storage stability and low emission characteristics.
[0005] The present invention provides a high-performance, low-emission composite modified rubber asphalt, which is prepared by compositely modifying rubber asphalt with diatomaceous earth and an alcohol deodorant;
[0006] Diatomaceous earth accounts for 2-3% of the mass of rubber asphalt;
[0007] The alcohol deodorant accounts for 2-3% of the rubber powder in the rubber asphalt;
[0008] The specific surface area of the diatomaceous earth is 25 to 35 m 2 / g.
[0009] The present invention utilizes the effect of diatomaceous earth on improving the high-temperature performance of rubber asphalt and the adsorption of harmful gases, the effect of alcohol deodorizers on improving the low-temperature performance of rubber asphalt and the inhibition of harmful gases, and the synergistic effect of diatomaceous earth and alcohol deodorizers; that is, the composite modification of rubber asphalt with diatomaceous earth and alcohol deodorizers can simultaneously improve the high and low temperature performance of rubber asphalt and the storage stability of rubber asphalt; and reduce the harmful gas emission of rubber asphalt.
[0010] The diatomaceous earth used in the present invention is used as one of the composite modifiers, and its disc-shaped structure can prevent the rubber powder from settling and improve the storage stability of the rubber asphalt.
[0011] The alcohol deodorant used in the present invention as another component of the composite modifier can react with the small molecular Volatile Organic Compounds (VOCs) in rubber asphalt to generate macromolecular aromatic hydrocarbons, and diatomaceous earth can efficiently adsorb such macromolecular aromatic hydrocarbons. The synergistic effect of the alcohol deodorant and diatomaceous earth can significantly reduce the harmful gas emissions of rubber asphalt.
[0012] The specific surface area of the diatomaceous earth in the present invention is 25 to 35 m 2 / g. Using diatomite with a specific surface area within the above range is not only easy to disperse, but also can prevent the rubber powder from settling; when it exceeds the above range, the diatomite particle size is too small, and it is difficult to use its disc-shaped structure to prevent the rubber powder from settling; when it is below the above range, the diatomite particle size is too large, and it is difficult to evenly distribute, which reduces the low-temperature performance of rubber asphalt. In a specific embodiment, the specific surface area of diatomite is 25m 2 / g, 30m 2 / g or 35m 2 / g. Diatomaceous earth accounts for 2% or 3% of rubber asphalt.
[0013] The content of rubber powder in the rubber asphalt of the present invention is 18-23%; in a specific embodiment, the content of rubber powder in the rubber asphalt is 20%.
[0014] In the present invention, diatomite accounts for 2-3% of the mass of rubber asphalt; the alcohol deodorant accounts for 2-3% of the mass of rubber powder in rubber asphalt. Within the above specific dosage range, diatomite and alcohol deodorant can work together to significantly reduce the harmful gas emission of rubber asphalt, and can improve its high and low temperature performance and storage stability.
[0015] The present invention provides a method for preparing the high-performance, low-emission composite modified rubber asphalt described in the above technical solution, comprising the following steps:
[0016] Heat the rubber asphalt to 140-150°C, add diatomaceous earth, stir, then add an alcohol deodorant, continue stirring, and obtain high-performance, low-emission rubber asphalt.
[0017] The stirring rate of the present invention is 3000-4000 rpm, the stirring time is 30-40 min, and the stirring time is 20-30 min. In a specific embodiment, the stirring rate is 300 rpm, the stirring time is 30 min, and the stirring time is 30 min.
[0018] The present invention provides a high-performance, low-emission composite modified rubber asphalt, which is prepared by compositely modifying rubber asphalt with diatomaceous earth and an alcohol deodorant; the diatomaceous earth accounts for 2-3% of the mass of the rubber asphalt; the alcohol deodorant accounts for 2-3% of the mass of the rubber powder in the rubber asphalt; the specific surface area of the diatomaceous earth is 25-35m 2 / g. Diatomaceous earth and alcohol deodorizers are used to carry out composite modification of rubber asphalt. The composite modified rubber asphalt not only has excellent high and low temperature performance, but also has low emission characteristics, by utilizing the improvement effect of diatomaceous earth on the high temperature performance of rubber asphalt and the adsorption effect of harmful gases, the improvement effect of alcohol deodorizers on the low temperature performance of rubber asphalt and the inhibition effect of harmful gases, and the synergistic effect of diatomaceous earth and alcohol deodorizers. The disc-shaped structure of diatomaceous earth can also prevent the rubber powder from settling, thereby improving the storage stability of rubber asphalt. DETAILED DESCRIPTION
[0019] In order to further illustrate the present invention, a high-performance, low-emission composite modified rubber asphalt and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0020] Example 1
[0021] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000rpm, stir for 30min, then add 0.4 parts of alcohol deodorant (polyol asphalt deodorant produced by Zhengzhou Huilin Chemical Co., Ltd., model 951, the deodorant is also used in Comparative Examples 2 to 9), and continue stirring for 30min to obtain high-performance and low-emission rubber asphalt.
[0022] Comparative Example 1 (no deodorant added):
[0023] Heat 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, add 3 parts of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, and stir for 30 minutes to obtain comparative asphalt 1.
[0024] Comparative Example 2 (without addition of diatomaceous earth):
[0025] 100 parts of rubber asphalt (rubber powder content is 20%) are heated to 150°C, 0.4 parts of alcohol deodorant are added, the stirring paddle is turned on, the stirring speed is controlled to 3000 rpm, and stirring is carried out for 30 minutes to obtain comparative asphalt 2.
[0026] Comparative Example 3 (too much diatomaceous earth added)
[0027] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 4 parts of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 min, then add 0.4 parts of alcohol deodorant, continue stirring for 30 min, and obtain comparative asphalt 3.
[0028] Comparative Example 4 (too little diatomaceous earth added)
[0029] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 1 part of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 minutes, then add 0.4 parts of alcohol deodorant, continue stirring for 30 minutes, and obtain comparative asphalt 4.
[0030] Comparative Example 5 (Too much deodorant added)
[0031] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 min, then add 0.7 parts of alcohol deodorant, continue stirring for 30 min, and obtain comparative asphalt 5.
[0032] Comparative Example 6 (too little deodorant added)
[0033] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 minutes, then add 0.3 parts of alcohol deodorant, continue stirring for 30 minutes, and obtain comparative asphalt 6.
[0034] Comparative Example 7 (diatomaceous earth specific surface area is too low)
[0035] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 20m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 minutes, then add 0.4 parts of alcohol deodorant, continue stirring for 30 minutes, and obtain comparative asphalt 7.
[0036] Comparative Example 8 (diatomaceous earth specific surface area is too high)
[0037] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 40m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 min, then add 0.4 parts of alcohol deodorant, continue stirring for 30 min, and obtain comparative asphalt 8.
[0038] Comparative Example 9 (Calcium hydroxide zeolite replaces diatomaceous earth)
[0039] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of calcium hydroxide zeolite (specific surface area is 35m 2 / g), turn on the stirring paddle, control the stirring speed to 3000 rpm, stir for 30 min, then add 0.4 parts of alcohol deodorant, continue stirring for 30 min, and obtain comparative asphalt 9.
[0040] Embodiment 2:
[0041] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 3 parts of diatomaceous earth (specific surface area is 25m 2 / g), turn on the stirring paddle, control the stirring speed to 3000rpm, stir for 30min, then add 0.5 parts of alcohol deodorant (liquid asphalt deodorant purchased from Dongguan Wanqing Environmental Protection Co., Ltd.), continue stirring for 30min, and obtain high-performance and low-emission rubber asphalt.
[0042] Embodiment 3:
[0043] A high-performance, low-emission composite modified rubber asphalt and a preparation method thereof, comprising the following steps: heating 100 parts of rubber asphalt (rubber powder content is 20%) to 150°C, adding 2 parts of diatomaceous earth (specific surface area is 30m 2 / g), turn on the stirring paddle, control the stirring speed to 3000rpm, stir for 30min, then add 0.6 parts of alcohol deodorant (liquid asphalt masking agent purchased from Dongguan Wanqing Environmental Protection Co., Ltd.), continue stirring for 30min, and obtain high-performance and low-emission rubber asphalt.
[0044] According to the "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011), the rubber asphalt, the high-performance and low-emission rubber asphalt in Examples 1 to 3, and the comparative asphalt 1 to the comparative asphalt 9 were subjected to three major indexes, low-temperature bending beam and segregation tests. According to the reference document Construction and Building Materials 416 (2024) 135276, the VOCs emissions of the rubber asphalt, the high-performance and low-emission composite modified rubber asphalt in Examples 1 to 3, and the comparative asphalt 1 to the comparative asphalt 9 were tested. The test results are shown in Table 1.
[0045] Table 1
[0046]
[0047]
[0048] Needle penetration is a measure of the viscosity (hardness) of asphalt. The lower the needle penetration, the harder the asphalt and the higher its high-temperature resistance. Ductility is an indicator of the plasticity of asphalt. The higher the ductility, the higher the ductility and deformation capacity of the asphalt, and the better the low-temperature crack resistance. The softening point difference is a measure of the storage stability of asphalt. The smaller the softening point difference, the better the storage stability of the asphalt. The lower the stiffness modulus, the higher the low-temperature performance of the asphalt.
[0049] It can be seen from the scheme of Example 1 that, under the condition of composite modification, the high-performance, low-emission rubber asphalt of Example 1 has better high and low temperature performance, storage stability and harmful gas inhibition effect than ordinary rubber asphalt.
[0050] By comparing Example 1 with Comparative Example 1, it can be seen that when diatomaceous earth is added, the high-performance, low-emission rubber asphalt of Example 1 has better high and low temperature performance than Comparative Asphalt 1; by comparing Example 1 with Comparative Example 2, it can be seen that when alcohol deodorant is added, the high-performance, low-emission rubber asphalt of Example 1 has better harmful gas inhibition effect than Comparative Asphalt 2; by comparing Example 1 with Comparative Examples 3 and 6, it can be seen that when too much diatomaceous earth is added or too little alcohol deodorant is added, the low-temperature performance of Comparative Asphalt 3 and Comparative Asphalt 6 is reduced compared with the rubber asphalt in Example 1. Low, it is difficult to achieve the performance of high-performance low-emission rubber asphalt; By comparing Example 1 with Comparative Examples 4 and 5, it can be seen that when too little diatomaceous earth is added or too much alcohol deodorant is added, the needle penetration of Comparative Asphalt 4 and Comparative Asphalt 5 is higher, and the high-temperature performance is lower than that of the rubber asphalt in Example 1, and it is difficult to achieve the performance of high-performance low-emission rubber asphalt; By comparing Example 1 with Comparative Example 7, it can be seen that when the specific surface area of diatomaceous earth is too low, the low-temperature performance (ductility) and storage stability of Comparative Asphalt 7 are both lower than those of the rubber asphalt in Example 1, and the composite modified performance of Example 1 cannot be achieved. By comparing Example 1 with Comparative Example 8, it can be seen that when the specific surface area of diatomaceous earth is too high, the high-temperature performance (higher needle penetration) and storage stability of Comparative Asphalt 8 are both lower than those of the rubber asphalt in Example 1, and the composite modified performance of Example 1 cannot be achieved. By comparing Example 1 with Comparative Asphalt 9, it can be seen that when diatomaceous earth is not added but other powdered adsorbents (calcium hydroxide zeolite) are added, Comparative Asphalt 9 is difficult to achieve the storage stability of high-performance low-emission rubber asphalt in Example 1.
[0051] As can be seen from the above embodiments, the present invention provides a high-performance, low-emission composite modified rubber asphalt, which is prepared by composite modification of rubber asphalt with diatomaceous earth and alcohol deodorant; the diatomaceous earth accounts for 2-3% of the mass of the rubber asphalt; the alcohol deodorant accounts for 2-3% of the mass of the rubber powder in the rubber asphalt; the specific surface area of the diatomaceous earth is 25-35m 2 / g. Diatomaceous earth and alcohol deodorizers are used to carry out composite modification of rubber asphalt. The composite modified rubber asphalt not only has excellent high and low temperature performance, but also has low emission characteristics, by utilizing the improvement effect of diatomaceous earth on the high temperature performance of rubber asphalt and the adsorption effect of harmful gases, the improvement effect of alcohol deodorizers on the low temperature performance of rubber asphalt and the inhibition effect of harmful gases, and the synergistic effect of diatomaceous earth and alcohol deodorizers. The disc-shaped structure of diatomaceous earth can also prevent the rubber powder from settling, thereby improving the storage stability of rubber asphalt. The experimental results show that the penetration of the composite modified rubber asphalt is 56.0-58.2 (25℃, 0.1mm); the elongation is 147-155 (5cm / min, 5℃, mm); the stiffness modulus is 51-56MPa at -12℃, 125-132MPa at -18℃, and 292-318MPa at -24℃; the total VOCs release is 377.41-437.60μg / m 3 .
[0052] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high-performance, low-emission composite modified rubber asphalt, which is prepared by composite modification of rubber asphalt with diatomaceous earth and alcohol deodorizer; Diatomaceous earth accounts for 2-3% of the mass of rubber asphalt; The alcohol deodorant accounts for 2-3% of the rubber powder in the rubber asphalt; The specific surface area of the diatomaceous earth is 25 to 35 m 2 / g.
2. The high-performance, low-emission composite modified rubber asphalt according to claim 1, characterized in that: The content of rubber powder in rubber asphalt is 18-23%.
3. The high performance and low emission composite modified rubber asphalt according to claim 1, characterized in that: Diatomaceous earth makes up 2% or 3% of rubber asphalt.
4. The high-performance, low-emission composite modified rubber asphalt according to claim 1, characterized in that: The specific surface area of diatomaceous earth is 25m 2 / g, 30m 2 / g or 35m 2 / g.
5. The high performance and low emission composite modified rubber asphalt according to claim 1, characterized in that: The alcohol deodorant accounts for 2%, 2.5% or 3% of the mass of the rubber powder in the rubber asphalt.
6. A method for preparing the high-performance, low-emission composite modified rubber asphalt according to claim 1, comprising the following steps: Heat the rubber asphalt to 140-150°C, add diatomaceous earth, stir, then add an alcohol deodorant, continue stirring, and obtain a high-performance, low-emission composite modified rubber asphalt.
7. The preparation method according to claim 6, characterized in that: The stirring rate is 3000-4000 rpm, and the stirring time is 30-40 min; Continue stirring for 20 to 30 minutes.
Citation Information
Cited By
Preparation and application of damp-heat-resistant high-elasticity toughening crosslinked rubber asphalt